A method for preparing an artificial lens for reducing after-cataract

The femtosecond laser processing to form an array protruding structure and hydrophobic coating treatment solves the problem of post-cataract suppression, achieves effective lens epithelial cell suppression and stability improvement, and avoids damage to the optical zone of the lens surface and glare.

CN114159188BActive Publication Date: 2024-10-18TIANJIN SHI JI KANG TAI BIOMEDICAL ENG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111365733.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-18
Publication Date
2024-10-18
Estimated Expiration
2041-11-18

AI Technical Summary

Technical Problem

Post-cataract often occurs after cataract surgery, causing the patient's vision to be affected. Existing technologies such as right-angled square edge design and polishing process have problems with edge damage and residual processing lines in the optical area, and it is difficult to effectively inhibit the migration and adsorption of lens epithelial cells.

Method used

Using femtosecond laser processing to form a micron-scale array protrusion structure, combined with water-soluble wax coating and hydrophobic material treatment, a super-hydrophobic structure is formed to inhibit the migration and adsorption of lens epithelial cells, and active groups are introduced through low-temperature plasma treatment to enhance the surface Hydrophobicity.

Benefits of technology

It effectively reduces the incidence of post-implantation cataracts, enhances the hydrophobic ability of the surface of the intraocular lens, avoids the proliferation and accumulation of lens epithelial cells, and improves the stability and visual quality after implantation without damaging the optical performance of the lens surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114159188B_ABST
    Figure CN114159188B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an artificial lens for reducing after-cataract, comprising the following steps: S1: polishing; S2: fixing; S3: processing an array protrusion structure; S4: surface treatment; S5: preparing a hydrophobic coating; S6: cleaning and drying; wherein the order of S3 and S4 can be reversed, the method has simple steps and convenient operation, and the prepared artificial lens forms a physical super-hydrophobic structure through the array protrusion structure, which can effectively inhibit the migration and adsorption of lens epithelial cells, avoid the proliferation and accumulation of lens epithelial cells, and further reduce the occurrence of after-cataract; by preparing a hydrophobic coating on the surface of the artificial lens, the hydrophobic ability of the surface of the artificial lens can be further enhanced, the adsorption of epithelial cells can be restricted, and the occurrence of posterior capsule turbidity can be further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of artificial lenses, and in particular to a method for preparing an artificial lens for reducing after-cataract. Background Art

[0002] Cataract ranks first among blinding eye diseases. It is a serious and common eye disease, with more than 20 million cataract patients worldwide. Phacoemulsification combined with intraocular lens implantation is recognized as the most effective method for treating cataracts. Cataract surgery is one of the common ophthalmic surgeries. Cataract surgery first makes an incision in the anterior capsule of the lens, and uses phacoemulsification and other methods to remove the cataractous lens. Except for the incision in the anterior capsule, the lens capsule is basically intact. After the cataractous lens is removed, an intraocular lens is implanted in the lens capsule to achieve normal visual function for the patient.

[0003] Cataract surgery can restore the visual quality of cataract patients and greatly improve the quality of life of patients. However, many patients will develop posterior capsule opacity after surgery, namely, post-cataract (PCO). The main cause of post-cataract is that the residual lens epithelial cells after cataract surgery migrate to the surface of the artificial lens, proliferate and fibrose on the surface of the artificial lens, thereby affecting vision. The incidence of post-cataract in adults is 30% to 50%, which seriously affects the quality of life of patients after surgery. For post-cataract, YAG laser posterior capsule incision is the main method for treating post-cataract, but it also brings some complications, such as artificial lens damage, fundus damage and other problems. In recent years, in view of the cause of posterior capsule opacity, a right-angle square edge design has been proposed in the design of artificial lenses to block the migration of lens epithelial cells, thereby reducing the occurrence of post-cataract. The right-angle square edge technology is to form a sharp edge on the edge of the artificial lens through milling during the processing of the artificial lens, thereby inhibiting the migration of lens epithelial cells and further inhibiting the occurrence of after-cataracts. After the artificial lens is processed by turning, milling, etc., there will be processing lines remaining in the optical area of ​​the artificial lens, which will affect the imaging quality of the artificial lens. The method for dealing with these processing lines in production is physical polishing, that is, using polishing balls, rolling polishing and other methods, combined with the use of polishing agents and other additives to remove the processing lines in the optical area of ​​the artificial lens. However, this polishing process will cause the sharp edges formed in the processing of the artificial lens to be destroyed, forming a smooth edge, which reduces its ability to inhibit the migration of lens epithelial cells, thereby reducing its ability to inhibit posterior capsule opacity. Therefore, it is urgent to develop a method for preparing an artificial lens that reduces after-cataracts to solve the above technical problems.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing an artificial lens for reducing post-cataract, with simple steps and convenient operation. The prepared artificial lens forms a physical super-hydrophobic structure through an array protrusion structure, which can effectively inhibit the migration and adsorption of lens epithelial cells, avoid the proliferation and accumulation of lens epithelial cells, and thus reduce the occurrence of post-cataract; by preparing a hydrophobic coating on the surface of the artificial lens, the hydrophobic ability of the surface of the artificial lens can be further enhanced, the adsorption of epithelial cells can be limited, and the occurrence of posterior capsule opacity can be further reduced.

[0006] In order to achieve the above object, the present invention provides a method for preparing an artificial lens for reducing after-cataract, characterized in that it comprises the steps of:

[0007] S1: Polishing: polishing the intraocular lens blank to remove the processing lines on the surface of the optical zone;

[0008] S2: Fixing: fix the polished intraocular lens in the slot, exposing the surface facing the posterior capsule of the human eye;

[0009] S3: Processing an array protrusion structure, using a femtosecond laser to process a micrometer-scale array protrusion structure for inhibiting the migration and adsorption of lens epithelial cells in the area to be processed, wherein the area to be processed is one or more of the support haptics, the buffer zone and the side of the optical zone;

[0010] S4: Surface treatment: apply a layer of water-soluble wax on the optical zone, wait for it to dry, and then use a low-temperature plasma instrument to treat the surface of the intraocular lens. The treatment power is 5-1000w and the treatment time is 1-120min. The purpose of waxing is to protect the optical zone to prevent the optical zone from being treated by plasma. The purpose of low-temperature plasma treatment is to use high-energy plasma to react with the surface molecules of the lens to introduce active groups on the surface of the lens, such as -OH, -COOH and other groups.

[0011] S5: preparing a hydrophobic coating, dissolving a hydrophobic material in an organic solvent at a concentration of 1-50%, applying the coating on the surface of the intraocular lens, absorbing excess liquid, reacting at 40-70° C. for 10 min, and then reacting at 70-100° C. for 10 h, wherein the hydrophobic material is heptafluorodecyl acrylate, heptafluorodecyl triethoxysilane, octadecyl trimethoxysilane, polydimethylsiloxane, dodecafluoroheptyl methacrylate, methyl triethoxysilane, phenyl triethoxysilane, vinyl triethylsilane, octyl triethoxysilane, trimethylchlorosilane or octadecyl trimethoxysilane, and the organic solvent is ethanol, ethyl acetate or isopropanol;

[0012] S6: Clean and dry: clean the surface of the intraocular lens with pure water at 60-90°C and dry at room temperature;

[0013] The order of S3 and S4 can be reversed.

[0014] Preferably, in S1, the method for preparing the intraocular lens blank is: using a high-precision machine tool to process a mold with an optical shape, injecting the intraocular lens material into the mold and then solidifying and shaping it to obtain the intraocular lens blank.

[0015] Preferably, in S1, the method for preparing the intraocular lens blank is: injection molding the intraocular lens material into a small disc, machining the optical surface using a lathe, and milling the desired contour shape using a milling machine to obtain the intraocular lens blank.

[0016] Preferably, in S2, the polished intraocular lens is fixed in the slot by gluing wax.

[0017] Preferably, in S4, the gas source of the low-temperature plasma instrument is argon, ammonia, oxygen, carbon dioxide or air.

[0018] Preferably, in S5, the coating method is spraying or brushing.

[0019] Preferably, in S3, the array protrusion structure is formed by an array of columnar, conical, hemispherical or ellipsoidal protrusions.

[0020] Preferably, in S3, the height and width of the protrusions are 1-100 μm, and the spacing between them is 1-100 μm.

[0021] Preferably, in S3, the array protrusion structure is a non-uniform height structure, which increases step by step from the outer circle to the inner circle, or decreases step by step, or has high and low points in the middle.

[0022] Preferably, in S3, the array protrusion structure is a single-layer protrusion structure, or a multi-layer protrusion structure having one or more layers of small protrusions added to the single-layer protrusion structure.

[0023] The present invention provides a method for preparing an artificial lens for reducing after-cataract, which has the following beneficial effects.

[0024] 1. The present invention has simple steps and convenient operation. The prepared artificial lens forms a physical super-hydrophobic structure through the array protrusion structure, which can effectively inhibit the migration and adsorption of lens epithelial cells, avoid the proliferation and accumulation of lens epithelial cells, and thus reduce the occurrence of post-cataracts; by preparing a hydrophobic coating on the surface of the artificial lens, the hydrophobic ability of the surface of the artificial lens can be further enhanced, the adsorption of epithelial cells can be limited, and the occurrence of posterior capsule opacity can be further reduced. The present invention processes the artificial lens by laser or other methods after polishing, which will not affect the surface quality of the artificial lens.

[0025] 2. The array protrusion structure on the side of the optical zone of the intraocular lens prepared by the present invention can reduce the light transmittance around the optical zone, thereby effectively reducing the glare phenomenon after the intraocular lens is implanted. The array protrusion structure of the support haptic can increase the friction of the support haptic, thereby increasing the friction between the support haptic and the lens capsule, reducing the possibility of lens rotation after intraocular lens implantation, and increasing the stability of the intraocular lens. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic diagram of the structure of an artificial lens for reducing after-cataract obtained by the preparation method of the present invention;

[0027] Figure 2 A side view of an array protrusion structure of an artificial lens embodiment 1 for reducing after-cataract obtained by the preparation method of the present invention;

[0028] Figure 3 A side view of an array protrusion structure of an artificial lens embodiment 2 for reducing after-cataract obtained by the preparation method of the present invention;

[0029] Figure 4 A side view of an array protrusion structure of an artificial lens embodiment 3 for reducing after-cataract obtained by the preparation method of the present invention;

[0030] Figure 5 A side view of an array protrusion structure of an artificial lens embodiment 4 for reducing after-cataract obtained by the preparation method of the present invention;

[0031] Figure 6 A side view of an array protrusion structure of an artificial lens embodiment 5 for reducing after-cataract obtained by the preparation method of the present invention;

[0032] Figure 7 A side view of an array protrusion structure of an artificial lens embodiment 6 for reducing after-cataract obtained by the preparation method of the present invention;

[0033] Figure 8 A side view of the array protrusion structure of Example 7 of an artificial lens for reducing after-cataract obtained by the preparation method of the present invention.

[0034] In the figure:

[0035] 1. Optical zone 2. Support loop 3. Buffer zone 4. Side of the optical zone. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with specific embodiments and drawings to help understand the content of the present invention.

[0037] The present invention provides a method for preparing an artificial lens for reducing after-cataract, comprising the steps of:

[0038] S1: Polishing, polishing the intraocular lens blank to remove the processing lines on the surface of the optical zone 1; the preparation method of the intraocular lens blank is: using a high-precision machine tool to process a mold with an optical shape, injecting the intraocular lens material into it and then solidifying it to obtain the intraocular lens blank; or injection molding the intraocular lens material into a small disc, using a lathe to process the optical surface, and using a milling machine to mill out the required contour shape to obtain the intraocular lens blank.

[0039] S2: Fixing, fixing the polished intraocular lens in the slot, exposing the surface facing the posterior capsule of the human eye; preferably, the polished intraocular lens is fixed in the slot by wax adhesion.

[0040] S3: Processing array protrusion structure, using femtosecond laser, processing micron-scale array protrusion structure for inhibiting migration and adsorption of lens epithelial cells in the area to be processed, the area to be processed is one or more of the support loop 2, buffer zone 3 and optical zone side 4; the array protrusion structure is arranged by columnar, conical, hemispherical or ellipsoidal protrusion array. The height and width of the protrusion are 1-100μm, and the spacing is 1-100μm. The array protrusion structure is a non-uniform height structure, which increases step by step from the outer circle to the inner circle, or decreases step by step, or has high and low in the middle. The array protrusion structure is a single-layer protrusion structure, or a multi-layer protrusion structure with one or more layers of small protrusions added to the single-layer protrusion structure.

[0041] S4: Surface treatment: apply a layer of water-soluble wax on the optical zone 1. After drying, use a low-temperature plasma instrument to treat the surface of the intraocular lens. The treatment power is 5-1000w and the treatment time is 1-120min. The gas source of the low-temperature plasma instrument is argon, ammonia, oxygen, carbon dioxide or air. The purpose of waxing is to protect the optical zone 1 to prevent the optical zone 1 from being treated by plasma. The purpose of low-temperature plasma treatment is to use high-energy plasma to react with the surface molecules of the lens to introduce active groups on the surface of the crystal, such as -OH, -COOH and other groups.

[0042] S5: preparing a hydrophobic coating, dissolving a hydrophobic material in an organic solvent at a concentration of 1-50%, and applying the coating on the surface of the intraocular lens by spraying or brushing. After removing excess liquid, reacting at 40-70° C. for 10 minutes, and then reacting at 70-100° C. for 10 hours. The hydrophobic material is heptafluorodecyl acrylate, heptafluorodecyl triethoxysilane, octadecyl trimethoxysilane, polydimethylsiloxane, dodecafluoroheptyl methacrylate, methyl triethoxysilane, phenyl triethoxysilane, vinyl triethylsilane, octyl triethoxysilane, trimethylchlorosilane or octadecyl trimethoxysilane. The organic solvent is ethanol, ethyl acetate or isopropanol.

[0043] S6: Clean and dry: clean the surface of the intraocular lens with pure water at 60-90°C and dry at room temperature;

[0044] The order of the above-mentioned S3 and S4 can be reversed.

[0045] like Figure 2 The figure shows a side view of an array protrusion structure of an artificial lens embodiment 1 for reducing after-cataract obtained by the preparation method of the present invention. The array protrusion structure is composed of an array of cone-shaped protrusions, with the same height from the outer circle to the inner circle, an equal height structure, and a single-layer protrusion structure.

[0046] like Figure 3 The figure shows a side view of an array protrusion structure of an artificial lens embodiment 2 for reducing after-cataract obtained by the preparation method of the present invention. The array protrusion structure is arranged by a columnar protrusion array, with different heights from the outer circle to the inner circle, high and low in the middle, a non-uniform height structure, and a single-layer protrusion structure.

[0047] like Figure 4 The figure shows a side view of an array protrusion structure of an artificial lens embodiment 3 for reducing after-cataract obtained by the preparation method of the present invention. The array protrusion structure is arranged by an array of columnar protrusions, with different heights from the outer circle to the inner circle, high and low in the middle, and a non-uniform height structure, and a layer of small protrusions is added to the single-layer protrusion structure, which is a multi-layer protrusion structure.

[0048] like Figure 5 The figure shows a side view of an array protrusion structure of an artificial lens embodiment 4 for reducing after-cataract obtained by the preparation method of the present invention. The array protrusion structure is arranged by an ellipsoidal protrusion array, and the height from the outer circle to the inner circle is the same, which is an equal height structure, and a layer of small protrusions is added to the single-layer protrusion structure, which is a multi-layer protrusion structure.

[0049] like Figure 6The figure shows a side view of an array protrusion structure of an artificial lens embodiment 5 for reducing after-cataract obtained by the preparation method of the present invention. The array protrusion structure is arranged in a columnar (without rounded corners on the top) protrusion array, and the height from the outer circle to the inner circle is the same, which is an equal height structure and a single-layer protrusion structure.

[0050] like Figure 7 The figure shows a side view of an array protrusion structure of an artificial lens embodiment 6 for reducing after-cataract obtained by the preparation method of the present invention. The array protrusion structure is arranged in a columnar (with rounded corners on the top) protrusion array, and the height from the outer circle to the inner circle is the same, which is an equal height structure and a single-layer protrusion structure.

[0051] like Figure 8 The figure shows a side view of an array protrusion structure of an artificial lens for reducing after-cataracts obtained by the preparation method of the present invention in Example 7. The array protrusion structure is arranged in a hemispherical protrusion array, and the height from the outer circle to the inner circle is the same, which is an equal height structure and a single-layer protrusion structure.

[0052] Taking the design patterns of the array protrusion structures of Examples 5-7 as an example, the water drop contact angles of the intraocular lens blanks before and after treatment were measured. The test results are shown in Table 1.

[0053] Table 1 Measurement results of water drop contact angle before and after treatment

[0054]

[0055] The smaller the water drop contact angle, the better the affinity between the water drop and the material, and the higher the hydrophilicity of the material. On the contrary, the larger the water drop contact angle, the worse the affinity between the water drop and the material, and the better the hydrophobicity of the material. It can be seen from the measurement results in Table 1 that the water drop contact angle on the surface of the intraocular lens treated by the preparation method of the present invention has increased significantly after treatment, indicating that the hydrophobicity of the surface of the crystal has been significantly improved after treatment.

[0056] The present invention has simple steps and convenient operation. The prepared artificial lens forms a physical super-hydrophobic structure through the array protrusion structure, which can effectively inhibit the migration and adsorption of lens epithelial cells, avoid the proliferation and accumulation of lens epithelial cells, and thus reduce the occurrence of post-cataract; by preparing a hydrophobic coating on the surface of the artificial lens, the hydrophobic ability of the surface of the artificial lens can be further enhanced, the adsorption of epithelial cells can be restricted, and the occurrence of posterior capsule turbidity can be further reduced. The present invention processes the artificial lens by laser or other methods after polishing, which will not affect the surface quality of the artificial lens. The artificial lens prepared by the present invention has an array protrusion structure on the side surface 4 of the optical zone that can reduce the light transmittance around the optical zone 1, thereby effectively reducing the glare phenomenon after the artificial lens is implanted. The array protrusion structure of the support haptic 2 can increase the friction of the support haptic 2, thereby increasing the friction between the support haptic 2 and the lens capsule, reducing the possibility of lens rotation after the artificial lens is implanted, and increasing the stability of the artificial lens.

[0057] The invention concept is described in detail using specific examples herein, and the description of the above embodiments is only used to help understand the core idea of ​​the invention. It should be pointed out that any obvious modification, equivalent substitution or other improvement made by a person of ordinary skill in the art without departing from the invention concept should be included in the protection scope of the present invention.

Claims

1. A method for preparing an artificial lens for reducing after-cataract, characterized in that: Including steps such as: S1: Polishing: polishing the intraocular lens blank to remove the processing lines on the surface of the optical zone; S2: Fixing: fix the polished intraocular lens in the slot, exposing the surface facing the posterior capsule of the human eye; S3: Processing an array protrusion structure, using a femtosecond laser to process a micrometer-scale array protrusion structure for inhibiting the migration and adsorption of lens epithelial cells in the area to be processed, wherein the area to be processed is one or more of the support haptics, the buffer zone and the side of the optical zone; S4: Surface treatment: apply a layer of water-soluble wax on the optical area, wait for it to dry, and then use a low-temperature plasma instrument to treat the surface of the intraocular lens. The treatment power is 5-1000w and the treatment time is 1-120min. S5: preparing a hydrophobic coating, dissolving a hydrophobic material in an organic solvent at a concentration of 1-50%, applying the coating on the surface of the intraocular lens, absorbing excess liquid, reacting at 40-70° C. for 10 min, and then reacting at 70-100° C. for 10 h, wherein the hydrophobic material is heptafluorodecyl acrylate, heptafluorodecyl triethoxysilane, octadecyl trimethoxysilane, polydimethylsiloxane, dodecafluoroheptyl methacrylate, methyl triethoxysilane, phenyl triethoxysilane, vinyl triethylsilane, octyl triethoxysilane, trimethylchlorosilane or octadecyl trimethoxysilane, and the organic solvent is ethanol, ethyl acetate or isopropanol; S6: Clean and dry: clean the surface of the intraocular lens with pure water at 60-90°C and dry at room temperature; The order of S3 and S4 can be reversed.

2. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In S1, the method for preparing the intraocular lens blank is: using a high-precision machine tool to process a mold with an optical shape, injecting the intraocular lens material into the mold and then solidifying it to obtain the intraocular lens blank.

3. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In S1, the method for preparing the artificial lens blank is: injection molding the artificial lens material into a small disc, machining the optical surface using a lathe, and milling the required contour shape using a milling machine to obtain the artificial lens blank.

4. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In S2, the polished intraocular lens is fixed in the slot by wax adhesion.

5. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In S4, the gas source of the low-temperature plasma instrument is argon, ammonia, oxygen, carbon dioxide or air.

6. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In S5, the coating method is spraying or brushing.

7. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In S3, the array protrusion structure is formed by an array of columnar, conical, hemispherical or ellipsoidal protrusions.

8. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In the S3, the height and width of the protrusions are 1-100 μm, and the spacing between them is 1-100 μm.

9. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In the S3, the array protrusion structure is a non-uniform height structure, which increases step by step from the outer circle to the inner circle, or decreases step by step, or has high and low points in the middle.

10. The method for preparing an intraocular lens for reducing after-cataract according to claim 1, characterized in that: In S3, the array protrusion structure is a single-layer protrusion structure, or a multi-layer protrusion structure with one or more layers of small protrusions added to the single-layer protrusion structure.

Citation Information

Patent Citations

  • Super-hydrophobic posterior chamber intraocular lens with microstructures on surface and preparing method thereof

    CN104546223A

  • Artificial intraocular lens

    DE3431224A1