Long-acting super-hydrophobic ceramic tile nano anti-slip agent and preparation method thereof

By forming a transparent protective layer on the surface of the tiles, and using modified nano silica to improve the anti-slip performance of the tiles, the problem of anti-slip agent affecting the aesthetics and anti-slip effects of the tiles in the prior art is solved, and the wear resistance and safety improvement is achieved .

CN119039826APending Publication Date: 2024-11-29JIANGMEN JIAHONG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411145605.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing anti-slip agent of tiles is treated with acidic liquid, which causes holes to form on the surface of the tiles, destroying the smoothness and affecting the beauty, and it is difficult to provide long-term anti-slip effect.

Method used

Homemade inorganic resin and wear-resistant nanoparticles are used to form a transparent protective layer on the surface of the ceramic tile, and the friction and anti-slip properties are improved by modifying nanosilicon dioxide.

Benefits of technology

It achieves the long-term excellent anti-slip effect without damaging the aesthetics of the ceramic tiles, improves the wear resistance and safety of the ceramic tiles, reduces slip accidents, simplifies the application process and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a long-acting super-hydrophobic ceramic tile nano anti-slip agent and a preparation method thereof. The long-acting super-hydrophobic ceramic tile nano anti-slip agent is mainly prepared from lactic acid, a surfactant, a defoaming agent, ethylene glycol, self-made modified nano silicon dioxide and deionized water. The self-made modified nano silicon dioxide is prepared from acidic silica sol, heptadecafluorodecyl triethoxy silane and a silane coupling agent KH560. The preparation method comprises the following steps: heating and stirring acidic silica sol, adjusting the pH value, and dropwise adding heptadecafluorodecyl triethoxy silane and a silane coupling agent KH560 to obtain uniformly dispersed modified nano silicon dioxide. According to the nano anti-slip agent, the anti-slip effect of the ceramic tile is improved by forming the uniformly dispersed modified nano silicon dioxide layer, the friction force is enhanced, and the slip risk is reduced. And the added heptadecafluorodecyl triethoxy silane endows superhydrophobicity, so that the friction force is further increased. The anti-slip agent provides a long-term effect, saves time and cost, does not damage the aesthetic property of tiles, and is suitable for various types of tiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anti-skid materials, and in particular relates to a long-acting super-hydrophobic nano anti-skid agent for ceramic tiles and a preparation method thereof. Background Art

[0002] Ceramic tiles are an indispensable basic building material for modern buildings and are widely used. However, the surface of ceramic tiles is smooth and easy to slip when walking, especially when the surface of ceramic tiles is wet with water, it is very easy to slip. Therefore, the anti-slip treatment of ceramic tile surface is getting more and more attention. Therefore, the research and development and preparation of ceramic tile anti-slip agents have become a hot topic of research.

[0003] Most of the current tile anti-slip agents use acidic liquids to treat the surface of tiles, mainly by using acidic substances to react chemically with silicates and other components on the surface of tiles, thereby forming tiny holes on the surface of tiles. These holes can increase the friction of the tile surface and improve the anti-slip performance of the tiles. However, this treatment method does destroy the original smoothness of the tile surface and affect the appearance of the tiles. Specifically, acidic substances react with silicates on the surface of tiles to generate some silicate acid salts and water. These acid salts form tiny holes on the surface of tiles, thereby increasing the roughness of the surface. This roughness can increase the friction of the tile surface, making it difficult for tiles to slip when wet or in water. However, this treatment method will also make the surface of the tile no longer smooth, thereby affecting the aesthetics of the tile. Especially in public places or residential areas, people may pay more attention to the aesthetics of tiles and are unwilling to accept the appearance of tiles after anti-slip treatment.

[0004] In view of this, we propose a long-lasting super-hydrophobic nano anti-slip agent for tiles and its preparation method to solve the above problems. The present invention uses a homemade inorganic resin to form a wear-resistant and transparent tile protective layer on the surface of the tile, and adds wear-resistant nanoparticles to achieve an excellent anti-slip effect on the surface of the tile. Summary of the invention

[0005] The present invention aims to solve the technical problem that most of the tile anti-slip agents in the above-mentioned prior art use acidic liquids to treat the tile surface, thereby forming a large number of capillary pores on the tile surface, thereby improving the tile anti-slip coefficient. This treatment method will damage the tile surface and affect the appearance of the tile. The present invention proposes to use a homemade inorganic resin to form a wear-resistant and transparent tile protective layer on the tile surface, and at the same time add wear-resistant nanoparticles, so as to achieve an excellent anti-slip effect on the tile surface. A long-lasting super hydrophobic tile nano anti-slip agent and a preparation method thereof are provided.

[0006] To achieve the above object, the present invention provides the following technical solutions: A long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles, comprising the following components by weight: Lactic acid 5-20 parts; 2-10 parts of surfactant; Defoaming agent 0.01-1 part; 1-10 parts of ethylene glycol; 0.5-5 parts of homemade modified nano-silicon dioxide; 40-60 parts of deionized water; The homemade modified nano-silica comprises the following components by weight: 50-100 parts of acidic silica sol, 1-5 parts of heptadecafluorodecyltriethoxysilane, 10-20 parts of silane coupling agent KH560, Among them, the preparation method of homemade modified nano-silicon dioxide is: Acidic silica sol was weighed, stirred and heated, and then the pH was adjusted with fluorosilicic acid; heptafluorodecyltriethoxysilane was slowly added dropwise, stirred and hydrolyzed; and silane coupling agent KH560 was slowly added dropwise, stirred and hydrolyzed to obtain uniformly dispersed homemade modified nano-silica.

[0007] Preferably, the surfactant is one or more of an alkyl trimethyl ammonium salt surfactant, a dialkyl dimethyl ammonium salt surfactant, an alkyl dimethyl benzyl ammonium salt surfactant, an alkyl isoquinolinium salt quaternary ammonium salt surfactant, and a benzyl chloride quaternary ammonium salt surfactant.

[0008] Preferably, the defoaming agent is one or more of polydimethylsiloxane, emulsified silicone oil, polyoxyethylene polyoxypropylene pentaerythritol ether, and polyoxypropylene glycerol ether.

[0009] Preferably, in the preparation of homemade modified nano-silica, the silica content in the acidic silica sol is 25%-30% and the pH value is 4-5.

[0010] Preferably, in the preparation of the homemade modified nano-silica, the acidic silica sol is stirred and heated to 50-80° C., and fluorosilicic acid is added to adjust the pH of the acidic silica sol to 2-3.

[0011] Preferably, in the preparation of the homemade modified nano-silica, the stirring and hydrolysis time of adding heptadecafluorodecyltriethoxysilane is 2 hours; the stirring and hydrolysis time of adding silane coupling agent KH560 is 2 hours.

[0012] A method for preparing a long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles comprises the following steps: S1. Weigh the surfactant and deionized water by weight, mix them evenly, continue heating and stirring, and then cool; S2, adding lactic acid, homemade nano-silicon dioxide and ethylene glycol to the mixed solution obtained in step S1, and stirring to mix evenly; S3, adding a defoamer to the mixed solution obtained in step S2, continuing to stir and mix evenly, and then discharging the material to obtain a long-lasting super-hydrophobic nano anti-slip agent for tiles.

[0013] Preferably, the surfactant and deionized water are mixed and continuously heated and stirred at a temperature of 50-80°C, stirred for 5 minutes, and cooled to 25-30°C.

[0014] Preferably, the stirring time after adding lactic acid, homemade nano-silicon dioxide and ethylene glycol is 5 minutes; the stirring time after adding the defoaming agent is 15-30 minutes.

[0015] Compared with the prior art, the technical effects and advantages of the present invention are: The long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles and its preparation method, the addition of wear-resistant nanoparticles is to enhance the anti-slip effect of ceramic tiles by forming a layer of uniformly dispersed modified nano-silica on the surface of the ceramic tiles. The addition of modified nano-silica can increase the roughness of the ceramic tile surface, thereby increasing the friction between the soles or other surfaces and reducing the risk of slipping. Specifically, the introduction of heptadecafluorodecyltriethoxysilane makes the surface of the modified nano-silica super-hydrophobic, which means that water droplets form spheres on the surface instead of forming flakes in contact with the surface, thereby further increasing the friction when the surface contacts objects. Therefore, the addition of wear-resistant nanoparticles not only improves the wear resistance of ceramic tiles, but also enhances their anti-slip performance, which is very beneficial for improving the safety and durability of ceramic tile surfaces.

[0016] Once applied to tiles, nano-anti-slip agents can provide long-term effects, rather than just short-term anti-slip treatments. This reduces the frequency of re-treatments, saving time and costs. Traditional acid treatments may damage the surface of tiles and affect their aesthetics. Nano-anti-slip agents are designed to provide anti-slip effects without damaging the appearance of tiles. Nano-anti-slip agents increase the anti-slip properties by increasing the coefficient of friction on the surface of tiles, while ensuring the safety of surface-treated tiles in wet environments. The composition of nano-anti-slip agents is designed to make them suitable for all types of tiles, including tiles of different colors, textures and materials, providing a wide range of application options.

[0017] The application process of nano anti-slip agent is relatively simple and can be carried out by conventional mixing and spraying equipment, without the need for complex technology or special construction conditions. The durability and reduced maintenance costs of nano anti-slip agent can provide a more economical choice. Due to its durability, nano anti-slip agent reduces the need for daily maintenance, making the tile surface easier to clean and maintain.

[0018] By using this long-lasting super-hydrophobic nano anti-slip agent for tiles, the anti-slip performance of tiles can be improved without sacrificing the aesthetics of the tiles, while providing long-term protection to meet the needs of modern buildings for safety, beauty and durability. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0020] Preparation of homemade modified nano-silica: weigh 50 parts of acidic silica sol, stir and heat to 50°C, then adjust the pH to 2-3 with fluorosilicic acid; slowly add 1 part of heptadecafluorodecyltriethoxysilane, stir and hydrolyze for 2 hours; slowly add 10 parts of silane coupling agent KH560, stir and hydrolyze for 2 hours to obtain uniformly dispersed modified nano-silica.

[0021] Preparation of long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles: weigh 2 parts of hexadecyltrimethylammonium bromide and 60 parts of deionized water by weight, mix well and heat to 50-80°C, stir for 5 minutes; cool to 25-30°C, then continue to add 5 parts of lactic acid, 0.5 parts of homemade modified nano-silica, and 1 part of ethylene glycol, stir for 5 minutes; finally, add 0.01 parts of emulsified silicone oil, continue stirring for 15-30 minutes, and the long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles is obtained. Example 2

[0022] Preparation of homemade modified nano-silica: weigh 80 parts of acidic silica sol, stir and heat to 50-80°C, then adjust the pH to 2-3 with fluorosilicic acid; slowly add 3 parts of heptadecafluorodecyltriethoxysilane, stir and hydrolyze for 2 hours; slowly add 15 parts of silane coupling agent KH560, stir and hydrolyze for 2 hours to obtain uniformly dispersed modified nano-silica.

[0023] Preparation of long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles: weigh 10 parts of dialkyldimethylammonium chloride and 40 parts of deionized water by weight, mix well and heat to 50-80°C, stir for 5 minutes; cool to 25-30°C, then continue to add 20 parts of lactic acid, 5 parts of homemade modified nano-silica, and 10 parts of ethylene glycol, stir for 5 minutes; finally add 1 part of polydimethylsiloxane, continue stirring for 15-30 minutes, and the long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles is obtained. Example 3

[0024] Preparation of homemade modified nano-silica: weigh 100 parts of acidic silica sol, stir and heat to 50-80°C, then adjust the pH to 2-3 with fluorosilicic acid; slowly add 5 parts of heptadecafluorodecyltriethoxysilane, stir and hydrolyze for 2 hours; slowly add 20 parts of silane coupling agent KH560, stir and hydrolyze for 2 hours to obtain uniformly dispersed modified nano-silica.

[0025] Preparation of long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles: weigh 5 parts of dodecyl dimethyl benzyl ammonium chloride and 50 parts of deionized water by weight, mix well and heat to 50-80°C, stir for 5 minutes; cool to 25-30°C, then continue to add 10 parts of lactic acid, 2 parts of homemade modified nano-silica, and 5 parts of ethylene glycol, stir for 5 minutes; finally add 0.5 parts of polyoxypropylene glycerol ether, continue stirring for 15-30 minutes, and the long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles is obtained.

[0026] Performance Test: Friction coefficient test: The ceramic tile is treated with the long-lasting super-hydrophobic ceramic tile nano anti-slip agent obtained from this formula, and then the ceramic tile is dried at 25°C for 60 minutes. In contrast, the ceramic tile anti-slip agent on the market is used to treat the ceramic tile surface with an acidic liquid, and then the changes in the ceramic tile surface after the anti-slip treatment are observed.

[0027] The friction coefficient of the long-lasting super-hydrophobic nano anti-slip agent for tiles is calculated through a friction coefficient test. During the test, a special friction coefficient tester is used to measure the friction coefficient of the tile surface. During the test, a certain pressure is applied to the tile surface and the sliding resistance between the two contact surfaces is measured to calculate the friction coefficient.

[0028] The test results are shown in Table 1: sample Friction coefficient Changes in tile surface after anti-slip treatment Example 1 0.95 No visible changes Example 2 0.91 No visible changes Example 3 0.89 No visible changes Comparative Example 0.73 Slightly matte The coefficient of friction is a dimensionless value that represents the ratio of the frictional resistance to the normal pressure between two contacting surfaces. The value range of the coefficient of friction is usually between 0 and 1. The larger the value, the better the anti-slip performance, that is, the less likely it is to slide.

[0029] Each of the three embodiments gives the test results of the friction coefficient. For example, the friction coefficient of embodiment 1 is 0.95, embodiment 2 is 0.91, embodiment 3 is 0.89, and the friction coefficient of the comparative example without the anti-slip agent is 0.73. These test results show that the anti-slip performance of the tiles treated with the anti-slip agent of the present invention is significantly improved.

[0030] The long-lasting super-hydrophobic nano-anti-slip agent for ceramic tiles and its preparation method are based on forming a layer of uniformly dispersed modified nano-silicon dioxide on the surface of ceramic tiles to increase the roughness of the ceramic tile surface and reduce the surface energy, thereby achieving super-hydrophobicity and excellent anti-slip effect. Specifically, the addition of modified nano-silicon dioxide can form a dual structure of micron and nanometer levels. These rough microstructures can increase the contact area between water droplets and the surface of ceramic tiles, so that water droplets form spheres on the surface instead of spreading into sheets, thereby reducing the contact area between water droplets and the ground, increasing the friction coefficient, and achieving an anti-slip effect. At the same time, the low surface energy modified nano-silicon dioxide also makes the surface of the ceramic tile less likely to be wetted by water and other liquids, further enhancing the anti-slip performance.

[0031] This long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles improves the anti-slip properties of the ceramic tile surface, reduces the occurrence of slip accidents, and improves safety in public places and homes. Since a transparent protective layer is used, it will not damage the original appearance of the ceramic tile while improving the anti-slip properties, thus maintaining the aesthetics of the ceramic tile. The protective layer formed by homemade inorganic resin and wear-resistant nanoparticles has a certain wear resistance, can resist daily wear and tear, and extend the service life of the ceramic tile. The super-hydrophobic surface can make water droplets roll off quickly, reducing the adhesion of dirt on the ceramic tile surface, making it easy to clean and maintain.

[0032] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles, characterized in that: By weight, it includes the following components: Lactic acid 5-20 parts; 2-10 parts of surfactant; Defoaming agent 0.01-1 part; 1-10 parts of ethylene glycol; 0.5-5 parts of homemade modified nano-silicon dioxide; The balance is deionized water; The homemade modified nano-silica comprises the following components by weight: 50-100 parts of acidic silica sol, 1-5 parts of heptadecafluorodecyltriethoxysilane, 10-20 parts of silane coupling agent KH560, Among them, the preparation method of homemade modified nano-silicon dioxide is: Acidic silica sol was weighed, stirred and heated, and then the pH was adjusted with fluorosilicic acid; heptafluorodecyltriethoxysilane was slowly added dropwise, stirred and hydrolyzed; and silane coupling agent KH560 was slowly added dropwise, stirred and hydrolyzed to obtain uniformly dispersed homemade modified nano-silica.

2. A long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to claim 1, characterized in that: The surfactant is one or more of an alkyltrimethyl quaternary ammonium salt surfactant, a dialkyldimethyl quaternary ammonium salt surfactant, an alkyldimethylbenzyl quaternary ammonium salt surfactant, an alkylisoquinolinium quaternary ammonium salt surfactant, and a benzylchloride quaternary ammonium salt surfactant.

3. A long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to claim 1, characterized in that: The defoaming agent is one or more of polydimethylsiloxane, emulsified silicone oil, polyoxyethylene polyoxypropylene pentaerythritol ether, and polyoxypropylene glycerol ether.

4. The long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to claim 1, characterized in that: In the preparation of homemade modified nano-silica, the silica content in the acidic silica sol is 25%-30% and the pH value is 4-5.

5. The long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to claim 1, characterized in that: In the preparation of homemade modified nano-silica, the acidic silica sol is stirred and heated to 50-80°C, and fluorosilicic acid is added to adjust the pH of the acidic silica sol to 2-3.

6. The long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to claim 5, characterized in that: In the preparation of the homemade modified nano-silica, the stirring and hydrolysis time of adding heptadecafluorodecyltriethoxysilane was 2 hours; the stirring and hydrolysis time of adding silane coupling agent KH560 was 2 hours.

7. A method for preparing the long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Weigh the surfactant and deionized water by weight, mix them evenly, continue heating and stirring, and then cool; S2, adding lactic acid, homemade nano-silicon dioxide and ethylene glycol to the mixed solution obtained in step S1, and stirring to mix evenly; S3, adding a defoamer to the mixed solution obtained in step S2, continuing to stir and mix evenly, and then discharging the material to obtain a long-lasting super-hydrophobic nano anti-slip agent for tiles.

8. The method for preparing a long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to claim 7, characterized in that: The surfactant and deionized water are mixed and heated and stirred continuously at a temperature of 50-80°C for 5 minutes and then cooled to 25-30°C.

9. The method for preparing a long-lasting super-hydrophobic nano anti-slip agent for ceramic tiles according to claim 7, characterized in that: The stirring time after adding lactic acid, self-made nano-silica and ethylene glycol is 5 minutes; the stirring time after adding the defoaming agent is 15-30 minutes.

Citation Information

Cited By

  • Efficient anti-slip agent for ceramic tiles and preparation method of efficient anti-slip agent

    CN120737666A

  • High-efficiency anti-slip agent for ceramic tiles and preparation method thereof

    CN120737666B