Multilayer structures for transporting or storing hydrogen
By using a multi-layer structure in hydrogen storage tanks and pipelines, using the combination of high-strength composite reinforcement and semi-crystalline polymer liner, the problems of insufficient adhesion between composite reinforcement and sealing sheath and high temperature failure are solved, and high-temperature failure is achieved Mechanical strength and chemical stability improve the safety and efficiency of hydrogen storage and transportation.
Patent Information
- Application Number
- CN202080055439.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-30
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-07-28
AI Technical Summary
In the existing hydrogen storage and transportation technology, insufficient adhesion between the composite reinforcement and the sealing sheath causes the liner to collapse, and the sealing sheath fails at high temperatures, affecting the mechanical strength and chemical stability of the hydrogen storage tank and pipeline.
Using a multilayer structure, the excellent adhesion between the liner and the composite is ensured by depositing a fiber layer of high-strength composite reinforcement at low temperatures on the semi-crystalline polymer liner, and through the composition of different polymers Ensure that the substrate remains glassy at high temperatures, improves mechanical strength and fatigue resistance.
High mechanical strength and chemical stability of hydrogen storage tanks and pipelines at high temperatures are achieved, avoiding liner collapse and seal sheath failure, and improving the safety and efficiency of hydrogen storage and transportation.
Smart Images

Figure BDA0003495039790000191 
Figure BDA0003495039790000201
Abstract
Description
Technical Field
[0001] The present patent application relates to multilayer composite structures for transporting, distributing, or storing hydrogen, and methods of making the same. Background Art
[0002] One of the goals sought in the automotive sector is to propose vehicles that pollute less and less. Thus, electric or hybrid vehicles comprising batteries are intended to gradually replace internal combustion vehicles, such as petrol or diesel vehicles. It has been shown that batteries are relatively complex vehicle parts. Depending on the positioning of the battery in the vehicle, it may be necessary to protect it from impacts and the external environment (which may have extreme temperatures and variable humidity). It is also necessary to avoid any risk of combustion.
[0003] Furthermore, in order not to damage the cells of the battery and to preserve its life, it is important that its operating temperature does not exceed 55° C. Conversely, for example in winter, it may be necessary to increase the battery temperature in order to optimize its operation.
[0004] Furthermore, electric vehicles today still suffer from several issues, namely the range of the batteries, the use of rare earths in these batteries whose resources are not inexhaustible, and the availability of electricity production in various countries to charge the batteries.
[0005] Hydrogen is therefore an alternative to electric batteries, since hydrogen can be converted into electricity by means of fuel cells and thus power electric vehicles.
[0006] However, due to its very low molar mass and very low liquefaction temperature, the storage of hydrogen is technically difficult and costly, especially when it comes to mobile storage. However, in order to be efficient, the storage must be implemented in small volumes, which means that the hydrogen must be kept at high pressures, given the temperatures at which the vehicle is used. This is particularly the case for fuel cell hybrid road vehicles, which aim for a range of about 600 to 700 km, or even less, for essentially urban use, in addition to a battery-powered electric basis.
[0007] Hydrogen storage tanks are usually made of a metal liner that must prevent the hydrogen from escaping. This first liner must itself be protected by a second liner (usually made of composite material) designed to withstand the internal pressure of the tank (e.g. 700 bar) and to withstand any impact or heat sources. The valve system must also be safe.
[0008] According to the French Hydrogen and Fuel Cell Federation (AFHYPAC) Hydrogen Memorandum 4.2 (December 2016 edition), pressurized hydrogen storage and distribution has been standard practice for many years, with cylindrical cylinders or cylinder assemblies filled to 20 or 25 MPa (Type I and II). The disadvantage of this storage method is the size - only 14 kg / m at 20 MPa and normal temperature (21°C). 3 (In comparison, methane is 100 kg / m 3 ) - and, most importantly, weight, which results from the use of low-stress steels in order to avoid problems with hydrogen embrittlement. The situation has changed radically with the advent of composite tank technology, known as type III or IV. The basic principle is to separate the two essential functions of sealing and mechanical strength and to manage them independently of one another. In this type of tank, a bladder (also known as a liner (or sealing sheath)) made of resin (thermosetting or thermoplastic) is combined with a reinforcing structure (also known as a reinforcement layer or sleeve) made of fibers (glass, aramid, carbon), which allows the tank to operate at much higher pressures while reducing its mass and avoiding the risk of explosive rupture in the event of severe external erosion. Thus, 70 MPa (700 bar) has practically become the current standard.
[0009] In Type IV tanks, the liner and reinforcement layer are made of different materials, which has the disadvantage of insufficient adhesion between the liner and the reinforcement layer, which leads to the problem of liner collapse when there is both gas accumulation at the interface between the liner and the composite and the internal pressure of the tank drops.
[0010] This problem has led to the development of V-tanks based on the use of the same polymer for the liner and the composite matrix, in order to ensure excellent and durable adhesion between the liner and the composite.
[0011] When hydrogen is transported or distributed by rigid or flexible pipes, it is also preferred that the hydrogen is at low volume and therefore high pressure to ensure adequate flow. Thus, for the storage, transportation, or distribution of hydrogen, it is of interest to use a composite pipe that is composed of a sealing sheath reinforced by an outer layer made of a composite material (ensuring air tightness and chemical resistance), which is made by winding a unidirectional (UD) tape deposited on a liner in successive layers by filaments. When it is desired to make this pipe flexible, one possibility is to wind the UD tape at one or more orientation angles relative to the pipe axis so that the composite reinforcement can support the deformation of the composite pipe during its use. The composite reinforcement allows the pipe to withstand the internal pressure generated by the transported fluid.
[0012] As for storage tanks, it is essential that the sealing sheath resists collapse, especially during production stops that lead to a sudden drop in pressure. This collapse risk exists when the sheath is not adhered to the composite reinforcement and gas can be present between the sealing sheath and the composite reinforcement. In order to avoid this phenomenon, one solution is to add an internal reinforcement called a skeleton to the pressure jacket: this reinforcement (usually metal) is perforated to make it flexible, and therefore it is not sealed to the fluid being transported. It adds weight, complexity and cost to a flexible pipe. Furthermore, in order to reduce the weight of the composite pipe or even eliminate the internal skeleton of the composite pipe, it is essential that the composite reinforcement is adhered to the sealing sheath, as in the case of a V-type storage tank.
[0013] Furthermore, the sealing sheath must be capable of being continuously extruded, possibly on an internal skeleton support as described above. This sealing sheath must be sufficiently chemically stable so that its mechanical and sealing properties do not deteriorate in a prohibitive manner during the life of the tank or flexible pipe.
[0014] In the case of flexible pipes with an internal metal skeleton, the sealing gasket must also be able to withstand the creep effects of the material from which it is made (caused by the internal pressure of the pipe creating stresses on the sealing sheath). When the pipe is subjected to the pressure of the effluent being transported, creep occurs in the joints (gaps or gaps) between the metal armoring (e.g. self-locking Z or T geometries) on which the gasket is located, thereby generating material protrusions that create stress concentrations and are therefore preferential failure zones for the sealing sheath: the material constituting the sealing sheath must therefore also withstand these stress concentrations.
[0015] For example, Airborne has developed various flexible pipes that do not have an internal skeleton and have a sealing sheath adhered to a composite reinforcement. The flexible pipes include: a PA11 liner having a PA11 FC composite (completed by JIP in 2011) or a PA12 liner having a PA12 FC composite, or even a PVDF liner having a PVDF FC composite. However, all of these structures have the following disadvantages: the matrix of the composite reinforcement has a glass transition temperature Tg that is lower than the service temperature Tu of the pipe; that is, in the case of pipes based on PA11 or PA12, Tg in the dry state is 50 °C, while the pipe service temperature Tu is 60 to 80 °C; and in the case of PVDF, Tg is -40 °C, while the service temperature in continuous operation is above 100 °C and typically close to 130 °C. In the specific case of PVDF, the hardness (rigidity, stiffness) (modulus) of the matrix remains high above its Tg until it reaches another transition (α-transition) around 100 °C, beyond which the behavior of the matrix becomes purely rubbery. Thus, in all of the above industrial and commercial cases of TP matrix composite pipes, the matrix of the composite reinforcement is in a fully rubberized state at the composite pipe service temperature Tu.
[0016] To solve this problem and to have a composite reinforcement whose matrix has a Tg higher than the maximum service temperature and is not in a rubberized state at the service temperature (in this case 130 °C), Kutting&Total, and then Vitrex and Magma have developed the following solution: consisting of a PEEK sealing sheath (or liner) that is reinforced by a composite having a PEEK matrix. The Tg of PEEK is 140 °C and thus meets the requirement of high rigidity, since this Tg is higher than the maximum service temperature. The disadvantage is that, as a result, the sealing sheath is also very rigid, which can limit its fatigue life and is a major drawback for the production of flexible pipes. In addition, the processing temperature of this type of sealing sleeve is very high (typically 380 - 400 °C), and this causes major difficulties in terms of tool operation and process control in the case of common conversion processes, which are pipe extrusion.
[0017] In addition, Ticona (Celanese), together with Airborne, has provided composite pipes having a PPS FC reinforcement and a PPS sealing sheath.
[0018] For Tu > 90 °C, this structure causes the same problem for the composite matrix as the PVDF-based solution (i.e., Tg < Tu), and there is additionally a problem with the transition temperature (for PPS and PVDF, typically 350 °C vs. 250 °C, respectively).
[0019] For Tu < 90°C, PPS is suitable for the composite matrix, but the problem of sealing liner extrusion temperature still exists, as well as the problem of its high stiffness (which limits the flexibility of the composite pipe).
[0020] The case of hydrogen tanks poses similar technical problems, since their rapid filling with hydrogen causes the tank temperature to increase due to the compression of the hydrogen, especially to about 110°C, which in the case where the matrix of the composite has a Tg below this temperature requires the composite to be oversized.
[0021] It is therefore still necessary to optimize, on the one hand, the matrix of the composite in order to optimize its mechanical strength at high temperatures and, on the other hand, the material constituting the sealing gasket in order to optimize its application temperature without deteriorating the adhesion of the composite reinforcement to the sealing gasket. Thus, the changes to be made in the composition of the material constituting the sealing gasket in order to ensure at least partial miscibility with the matrix of the composite should not lead to a significant increase in the manufacturing temperature of this gasket (extrusion-blow molding, injection, rotational molding, etc.) compared to that practiced today for polyamides and PVDF.
[0022] These problems are solved by providing the multilayer structure of the present invention which is a fully bonded, "dual material" composite pipe or tank and is constructed of a high strength composite reinforcement (i.e. comprising a high Tg matrix) deposited (particularly by filament winding) on a liner previously extruded at relatively low temperatures. The adhesion between the composite and the liner is very good.
[0023] Throughout this specification, the terms "gasket", "sealing sheath" and "pressure jacket" have the same meaning.
[0024] Thus, the present invention relates to a multilayer structure chosen from tanks, pipes or tubes intended to transport or store hydrogen, comprising, from the inside to the outside, at least one sealing layer and at least one composite reinforcement layer,
[0025] The innermost composite reinforcement layer is welded to the outermost adjacent sealing layer,
[0026] The sealing layer is composed of a composition that mainly comprises at least one semi-crystalline thermoplastic polymer P1i (i=1 to n, n is the number of sealing layers), whose Tm measured according to ISO 11357-3:2013 is less than 280°C, in particular less than 265°C,
[0027] The at least one thermoplastic polymer of each sealing layer may be the same or different, and at least one of the composite reinforcement layers is composed of a fibrous material in the form of continuous fibers, which is impregnated with the following composition: the composition mainly comprises at least one thermoplastic polymer P2j (j=1 to m, m is the number of reinforcement layers), the thermoplastic polymer P2j is particularly semi-crystalline, and the thermoplastic polymer P2j has a Tg measured according to ISO 11357-3:2013 that is greater than the maximum use temperature (Tu) of the structure, wherein Tg≥Tu+20°C, particularly Tg≥Tu+30°C, and Tu is greater than 50°C, particularly greater than 100°C.
[0028] Thus, the inventors unexpectedly discovered that using different polymers for the composite matrix and the liner, and in particular:
[0029] The matrix of the composite reinforcement is composed of a polymer having a Tg significantly greater than the maximum use temperature Tu of the tank or pipeline (typically, Tg>Tu+20°C, in particular Tg≥Tu+30°C), so as to still be in its glassy region and have high stiffness, thereby enabling the composite to have high mechanical strength,
[0030] The semi-crystalline polymer constituting the liner has a low melting point Tm, allowing it to be processed by extrusion, extrusion blow molding, rotational molding, injection or by winding a pure resin film (as the case may be) at moderate temperatures common to those skilled in the art, relative to the Tm of this polymer (less than 280°C, preferably less than 265°C). The currently known low-Tm semi-crystalline polymers also have a low Tg, which in most cases will be below the maximum use temperature. As a result, the polymer constituting the liner will work in its rubberized zone and will therefore be very flexible and therefore very resistant to fatigue. Its semi-crystalline nature ensures good resistance to chemical attack, wear and creep,
[0031] Furthermore, the two aforementioned polymers (the polymer constituting the matrix of the composite and the polymer constituting the liner) are sufficiently miscible with each other to ensure weldability of the composite to the liner and thus excellent adhesion between the liner and the composite. The durability of the adhesion will be ensured by the durability of the materials constituting the mixture at the interface of the two materials, i.e. in the welded joint. The miscibility of the two polymers is expressed as follows: preferably by a single Tg; or when that is not possible, by the characteristic signature of a partially homogeneous mixture, for example by the presence of two Tg values intermediate to those of the two pure polymers.
[0032] The immiscibility of the two polymers results in the presence of two Tg's in the mixture of the two polymers, which correspond to the respective Tg's of the pure polymers taken separately.
[0033] "Multilayer structure" means, for example, a tank, a pipe or a pipeline comprising or consisting of several layers, in particular two layers.
[0034] The sealing layer(s) are the innermost layers compared to the composite reinforcement layer which is the outermost layer.
[0035] The sealing layer is in contact with hydrogen even when there is an inner and therefore innermost non-sealing metal layer used to form the skeleton, which is formed by a spirally wound profiled metal strip, such as a cut strip, on which the sealing layer(s) are coated by extrusion.
[0036] When several sealing layers are present, only the innermost of said sealing layers is in direct contact with the hydrogen.
[0037] When only the sealing layer and the composite reinforcing layer are present, resulting in a multilayer structure of two layers, the two layers are welded and thereby adhered to each other, being in direct contact with each other.
[0038] When there are several sealing layers and / or several composite reinforcing layers, the outermost layer of the sealing layer (and thus the layer opposite to the layer in contact with hydrogen) is welded to the innermost layer of the composite reinforcing layers and thus adheres to each other, being in direct contact with each other.
[0039] Other composite reinforcement layers are also welded together.
[0040] The other sealing layers are also welded together.
[0041] About Sealant Layers and Thermoplastic Polymers P1i
[0042] One or more sealing layers may be present.
[0043] Each of the layers consists of a composition that essentially comprises at least one thermoplastic polymer P1i, i corresponding to the number of layers present. i is from 1 to 10, in particular from 1 to 5, in particular from 1 to 3, preferably i=1.
[0044] The term "predominantly" means that the at least one polymer is present in more than 50% by weight, relative to the total weight of the composition.
[0045] Advantageously, said at least one principal polymer is present in an amount greater than 60% by weight, particularly greater than 70% by weight, particularly greater than 80% by weight, more particularly greater than or equal to 90% by weight relative to the total weight of the composition.
[0046] The composition may further comprise impact modifiers and / or additives.
[0047] The additive may be selected from antioxidants, heat stabilizers, UV absorbers, light stabilizers, lubricants, inorganic fillers, flame retardants, nucleating agents, plasticizers, dyes, carbon black, and carbonaceous nanofillers.
[0048] Advantageously, the composition consists essentially of the thermoplastic polymer P1i, 0 to 5% by weight of an impact modifier, 0 to 5% by weight of additives, the sum of the constituents of the composition being equal to 100% (based on a maximum of 90% P2i).
[0049] The at least one principal polymer in each layer may be the same or different.
[0050] In one embodiment, a single primary polymer is present in at least the sealing layer welded to the composite reinforcement layer.
[0051] Thermoplastic polymer P1i
[0052] Thermoplastics or thermoplastic polymers refer to semi-crystalline materials that are generally solid at ambient temperature and soften during temperature increase, particularly after exceeding their glass transition temperature (Tg), and may exhibit a sharp transition above what is known as their melting point (Tm), and become solid again when the temperature is reduced below their crystallization temperature.
[0053] Tg, Tc and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0054] The number average molecular weight Mn of the thermoplastic polymer is preferably in the range from 10 000 to 40 000, preferably from 12 000 to 30 000. These Mn values may correspond to an intrinsic viscosity greater than or equal to 0.8, as determined according to standard ISO 307:2007 but by changing the solvent in m-cresol (m-cresol is used instead of sulfuric acid and the temperature is 20° C.).
[0055] Examples of suitable semi-crystalline thermoplastic polymers in the present invention include:
[0056] Polyamides, including copolymers such as polyamide-polyether copolymers, polyesters, and PVDF, and PVDF / PEI blends (where PVDF is predominant).
[0057] Very particular preference is given among the semi-crystalline polymers to polyamides and their semi-crystalline copolymers.
[0058] The nomenclature used to define polyamides is described in ISO Standard 1874-1:2011 “Plastiques—Material aux polyamides (PA) pour moulage et extrusion—Partie 1: Designation”, in particular on page 3 (Tables 1 and 2), and is familiar to the skilled person.
[0059] The polyamide may be a homopolyamide, or a copolyamide, or a mixture thereof.
[0060] Advantageously, the thermoplastic polymer is a long-chain aliphatic polyamide, ie a polyamide having an average number of carbon atoms greater than 8.5, preferably greater than 9, per nitrogen atom.
[0061] In particular, the long-chain aliphatic polyamide is selected from:
[0062] Polyamide 11 (PA11), polyamide 12 (PA12), polyamide 1010 (PA1010), polyamide 1012 (PA1012), polyamide 1212 (PA1012), or mixtures or copolyamides thereof, in particular PA11 and PA12.
[0063] Advantageously, the thermoplastic polymer is a long-chain semiaromatic polyamide, ie a polyamide having an average number of carbon atoms greater than 8.5, preferably greater than 9, per nitrogen atom and a melting point ranging from 240 to less than 280°C.
[0064] In particular, the long-chain semiaromatic polyamide is selected from polyamide 11 / 5T or 11 / 6T or 11 / 10T. In this context it is obvious that the ratio of 11 should be carefully chosen so that the Tm of the polymer is below 280°C, preferably below 265°C.
[0065] Advantageously, each sealing layer consists of a composition comprising the same type of polymer, in particular a polyamide.
[0066] Advantageously, said composition comprising said polymer P1i is black in colour and is capable of absorbing radiation suitable for welding.
[0067] There are various methods for welding thermoplastic polymer parts (parts). Thus, contact or non-contact heating blades, ultrasound, infrared, vibration, rotating one element to be welded relative to the other, or even laser welding can be used.
[0068] The welding of thermoplastic polymer elements, in particular by laser welding, requires that the two elements to be welded have different properties with respect to radiation, in particular laser radiation: one of the elements must be transparent to the radiation, in particular laser radiation, and the other must absorb the radiation, in particular laser radiation. Thus, the radiation, in particular laser radiation, passes through the transparent component and then reaches the absorbing element, where it is converted into heat. This allows the contact area between the two elements to melt and thus for welding to occur.
[0069] In some applications, it is desirable that both parts to be welded be black, including parts that are transparent to laser radiation.
[0070] In order to make them absorptive, it is known to add various additives, including for example carbon black, which gives the polymer a black color and allows it to absorb radiation suitable for welding.
[0071] In one embodiment, the welding is performed by a system selected from laser, infrared (IR) heating, LED heating, induction or microwave heating, or high frequency (HF) heating.
[0072] In the case where the welding is carried out by laser welding, then the composition P1i comprises a non-agglomerated or non-aggregated carbonaceous filler.
[0073] In the case where welding is carried out by induction, then said composition P1i comprises metal particles.
[0074] Advantageously, the welding is performed by means of a laser system.
[0075] About composite reinforcements and thermoplastic polymers P2j
[0076] There may be one or more composite reinforcement layers.
[0077] Each of the layers consists of a composition consisting essentially of at least one thermoplastic polymer P2j, j corresponding to the number of layers present.
[0078] j comprises 1 to 10, particularly 1 to 5, particularly 1 to 3, preferably j=1.
[0079] The term “predominantly” means that the at least one polymer is present in more than 50% by weight, relative to the total weight of the composition.
[0080] Advantageously, said at least one principal polymer is present in an amount greater than 60% by weight, particularly greater than 70% by weight, particularly greater than 80% by weight, more particularly greater than or equal to 90% by weight relative to the total weight of the composition.
[0081] The composition may further comprise impact modifiers and / or additives.
[0082] The additive may be selected from antioxidants, heat stabilizers, UV absorbers, light stabilizers, lubricants, inorganic fillers, flame retardants, nucleating agents, plasticizers, and dyes.
[0083] Advantageously, said composition consists essentially of said thermoplastic polymer P2j, 0 to 5% by weight of impact modifier, 0 to 5% by weight of additives, the sum of the constituents of the composition being equal to 100% (based on a maximum of 90% of P2j).
[0084] The at least one principal polymer in each layer may be the same or different.
[0085] In one embodiment, a single primary polymer is present in at least the composite reinforcement layer that is welded to the sealing layer.
[0086] In one embodiment, each reinforcement layer comprises the same type of polymer, in particular polyamide.
[0087] Thermoplastic polymer P2j
[0088] Thermoplastics or thermoplastic polymers refer to materials that are generally solid at ambient temperature, that may be semi-crystalline or amorphous, in particular semi-crystalline, and that soften during temperature increase, in particular after exceeding their glass transition temperature (Tg), and that flow at higher temperatures when they are amorphous, or that may exhibit a sharp transition as soon as their so-called melting temperature (Tm) is exceeded when they are semi-crystalline, and that become solid again when the temperature is lowered below their crystallization temperature (for semi-crystalline) or below their glass transition temperature (for amorphous).
[0089] Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0090] The polymer P2j of the composition of at least one of the composite reinforcing layers is such that its Tg is greater than the maximum use temperature (Tu) of the structure and in particular Tg ≥ Tu+20°C, especially Tg ≥ Tu+30°C.
[0091] In one embodiment, polymer P2j has a Tg ≥ Tu + 20°C, in particular a Tg ≥ Tu + 30°C, regardless of the position of said reinforcement layer.
[0092] In another embodiment, the reinforcing layer consisting of a composition comprising a polymer P2j having a Tg ≥ Tu + 20°C, in particular a Tg ≥ Tu + 30°C, is a layer welded to the sealing layer.
[0093] In one embodiment, the polymer P2j of the composition of at least one of the composite reinforcement layers is such that its Tg is greater than the maximum use temperature (Tu) of the structure, Tg≥Tu+20°C, and the reinforcement layer composed of the composition containing the polymer P2j is a layer welded to the sealing layer.
[0094] In one embodiment, the polymer P2j of the composition of at least one of the composite reinforcement layers is such that its Tg is greater than the maximum use temperature (Tu) of the structure, Tg≥Tu+30°C, and the reinforcement layer composed of the composition containing the polymer P2j is a layer welded to the sealing layer.
[0095] In another embodiment, the reinforcing layer consisting of a composition comprising a polymer P2j having a Tg ≥ Tu + 20° C., in particular a Tg ≥ Tu + 30° C., is the outermost reinforcing layer of the structure. The number average molecular weight Mn of the thermoplastic polymer is preferably in the range of 10 000 to 40 000, preferably 12 000 to 30 000. These Mn values may correspond to an intrinsic viscosity greater than or equal to 0.8, as determined according to standard ISO 307:2007 but by changing the solvent in m-cresol (m-cresol is used instead of sulfuric acid and the temperature is 20° C.).
[0096] Examples of suitable semi-crystalline thermoplastic polymers in the present invention include:
[0097] Polyamides, in particular polyamides containing aromatic and / or cycloaliphatic structures, including copolymers, for example polyamide-polyether copolymers, polyesters,
[0098] Polyaryletherketone (PAEK),
[0099] Polyetheretherketone (PEEK),
[0100] Polyetherketoneketone (PEKK),
[0101] Polyetherketoneetherketoneketone (PEKEKK),
[0102] Polyimides, in particular polyetherimide (PEI) or polyamide-imide,
[0103] Polysulfones (PSU), in particular polyarylsulfones, such as polyphenylsulfone (PPSU),
[0104] Polyethersulfone (PES).
[0105] Semi-crystalline polymers are particularly preferred, and in particular polyamides and semi-crystalline copolymers thereof.
[0106] The nomenclature used to define polyamides is described in ISO Standard 1874-1:2011 “Plastiques—Material aux polyamides (PA) pour moulage et extrusion—Partie 1: Designation”, in particular on page 3 (Tables 1 and 2), and is familiar to the skilled person.
[0107] The polyamide may be a homopolyamide, or a copolyamide, or a mixture thereof.
[0108] Advantageously, the semicrystalline polyamide is a semiaromatic polyamide, in particular a semiaromatic polyamide of formula X / YAr as described in EP1505099, in particular a semiaromatic polyamide of formula A / XT, in which A is chosen from units obtained from amino acids, units obtained from lactams, and units corresponding to the formula (Ca diamine).(Cb diacid), in which a represents the number of carbon atoms of the diamine and b represents the number of carbon atoms of the diacid, a and b are each between 4 and 36, advantageously between 9 and 18, the units (Ca diamine) are chosen from linear or branched aliphatic diamines, cycloaliphatic diamines and alkylaromatic diamines, and the units (Cb diacid) are chosen from linear or branched aliphatic diacids, cycloaliphatic diacids and aromatic diacids;
[0109] XT represents a unit obtained by the polycondensation of a Cx diamine and terephthalic acid, wherein x represents the number of carbon atoms of the Cx diamine, x being between 5 and 36, advantageously between 9 and 18, in particular a polyamide of formula A / 5T, A / 6T, A / 9T, A / 10T, or A / 11T, A being as defined above, in particular a polyamide selected from the group consisting of PA MPMDT / 6T, PA11 / 10T, PA 5T / 10T, PA 11 / BACT, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA11 / MXDT / 10T, 11 / 5T / 10T.
[0110] T corresponds to terephthalic acid, MXD to meta-xylylenediamine, MPMD to methylpentamethylenediamine and BAC to bis(aminomethyl)cyclohexane. The semiaromatic polyamide as defined above has in particular a Tg greater than or equal to 80°C.
[0111] Advantageously, each composite reinforcing layer consists of a composition comprising the same type of polymer, in particular a polyamide.
[0112] Advantageously, said composition comprising said polymer P2j is transparent to radiation suitable for welding.
[0113] For the purposes of welding, especially laser welding, thermoplastic polymers are generally transparent. Carbonaceous nanofillers make it possible to impart a black color to a layer of a composition comprising a thermoplastic polymer while maintaining the transparency of said layer to laser radiation.
[0114] Advantageously, the carbonaceous nanofiller is non-agglomerated or non-aggregated.
[0115] Advantageously, the carbonaceous nanofiller is incorporated into the composition in an amount ranging from 100 ppm to 500 ppm and preferably from 100 ppm to 250 ppm.
[0116] Advantageously, the carbonaceous nanofiller is selected from carbon nanotubes (CNTs), carbon nanofibers, graphene, nanoscale carbon black, and mixtures thereof.
[0117] Advantageously, the carbonaceous nanofiller does not contain nano carbon black.
[0118] In one embodiment, the welding is performed by a system selected from laser, IR heating, or induction heating.
[0119] Advantageously, the welding is performed by a laser system.
[0120] Advantageously, the laser radiation is infrared laser radiation and preferably has a wavelength between 700 nm and 1200 nm and preferably between 800 nm and 1100 nm.
[0121] About Structure
[0122] Thus, the multilayer structure comprises at least one sealing layer and at least one composite reinforcement layer welded together.
[0123] In one embodiment, in the multilayer structure, each polymer P1i of each sealing layer is partially or fully miscible with each polymer P1i of an adjacent layer, each polymer P2j of each reinforcing layer is partially or fully miscible with each polymer P2j of an adjacent layer, and each polymer P2j is partially or fully miscible with each polymer P1i (when they are adjacent), and polymer P21 is partially or fully miscible with polymer P11 adjacent to it,
[0124] The complete or partial miscibility of the polymers is defined by the difference in the glass transition temperatures of the two resins in the mixture relative to the difference in the glass transition temperatures of the two resins before mixing, and the miscibility is complete when the difference is equal to 0 and partial when the difference is different from 0, excluding the immiscibility of polymer P2j with polymer P1i.
[0125] When the miscibility of the polymers is partial, the difference is such that the greater the miscibility, the smaller the difference.
[0126] Advantageously, when the miscibility of said polymers is partial, said difference is less than 30%, preferably less than 20%, in absolute terms.
[0127] In one embodiment, the glass transition temperature of the mixture, depending on whether the miscibility is complete or partial, is necessarily between the glass transition temperatures of the polymers before blending and differs from them by at least 5°C, preferably at least 10°C.
[0128] The expression "completely miscible" means that when, for example, two polymers P1 1 and P1 2 (They have Tg1 1 and Tg1 2 ) is present in two adjacent sealing layers or two adjacent reinforcing layers, then the mixture of the two polymers has only one Tg1 1 1 2 , its value is at Tg1 1 and Tg1 2 between.
[0129] Furthermore, this Tg1 1 1 2 Value ratio Tg1 1 At least 5°C, in particular at least 10°C, and greater than Tg1 2 At least 5°C lower, in particular at least 10°C lower.
[0130] The expression "partially miscible" means that when, for example, two polymers P1 1 and P1 2 (They have Tg1 1 and Tg1 2 ) exists in two adjacent sealing layers or two adjacent reinforcing layers, the mixture of the two polymers has two Tg: Tg'1 1 and Tg'1 2 , where Tg1 1 <Tg’1 1 <Tg’1 2 <Tg1 2 .
[0131] Furthermore, these Tg'1 1 and Tg'1 2 Value ratio Tg1 1 At least 5°C, in particular at least 10°C, and greater than Tg1 2 At least 5°C lower, in particular at least 10°C lower.
[0132] The immiscibility of the two polymers results in the presence of two Tgs in the mixture of the two polymers: Tg1 1 and Tg1 2 , which corresponds to the Tg of each pure polymer taken separately, Tg1 1 and Tg1 2 .
[0133] Advantageously, the welded sealing layer and the reinforcing layer are made of compositions comprising different polymers, respectively.
[0134] Nevertheless, the different polymers may be of the same type.
[0135] Thus, if one of the two welded composite reinforcement and sealing layers is made of a composition comprising an aliphatic polyamide, the other layer is made of a composition comprising a polyamide that is non-aliphatic and is, for example, a semiaromatic polyamide, to have a high Tg polymer as matrix for the composite reinforcement.
[0136] The multilayer structure may comprise up to 10 sealing layers and up to 10 composite reinforcement layers.
[0137] It is obvious that the multilayer structure does not have to be symmetrical and it may therefore comprise more sealing layers than composite layers, or vice versa.
[0138] Advantageously, the multilayer structure comprises one, two, three, four, five, six, seven, eight, nine, or ten sealing layers and one, two, three, four, five, six, seven, eight, nine, or ten composite reinforcement layers.
[0139] Advantageously, the multilayer structure comprises one, two, three, four or five sealing layers and one, two, three, four or five composite reinforcement layers.
[0140] Advantageously, the multilayer structure comprises one, two, or three sealing layers, and one, two, or three composite reinforcement layers.
[0141] Advantageously, they consist of compositions each comprising different polymers.
[0142] Advantageously, they consist of a composition comprising the polyamides corresponding to polyamides P1i and P2j, respectively.
[0143] Advantageously, they consist of compositions each comprising different polyamides.
[0144] In one embodiment, the multilayer structure comprises a single sealing layer and several reinforcement layers, the sealing layer being welded to the adjacent reinforcement layers.
[0145] In another embodiment, the multilayer structure comprises a single reinforcement layer and several sealing layers, the reinforcement layer being welded to the adjacent sealing layers.
[0146] In an advantageous embodiment, the multilayer structure comprises a single sealing layer and a single composite reinforcement layer welded together.
[0147] Therefore, all combinations of these two layers are within the scope of the present invention, provided that at least the innermost composite reinforcement layer is fused to the outermost adjacent sealing layer, and the other layers are either fused together or not fused together.
[0148] Advantageously, in said multilayer structure, each sealing layer consists of a composition comprising polymers P1i of the same type, in particular polyamides.
[0149] The expression "same type of polymer" means, for example, polyamide which may be the same or different polyamide depending on the layer.
[0150] Advantageously, said polymer P1i is a polyamide and said polymer P2j is a polyamide.
[0151] Advantageously, the polyamide P1i is the same for all sealing layers.
[0152] Advantageously, the polymer P1i is a long-chain aliphatic polyamide, in particular PA1010, PA 1012, PA 1212, PA11, PA12, in particular PA 11 or PA12.
[0153] Advantageously, the polyamide P1i is a long-chain semiaromatic polyamide, in particular PA 11 / 5T, PA 11 / 6T or PA11 / 10T. In this case it is obvious that the ratios 11 must be carefully chosen so that the Tm of the polymer is below 280°C, preferably 265°C.
[0154] Advantageously, in said multilayer structure, each reinforcing layer consists of a composition comprising the same type of polymer P2j, in particular a polyamide.
[0155] Advantageously, the polyamide P2j is the same for all the reinforcement layers.
[0156] Advantageously, the polymer P2j is a semiaromatic polyamide chosen from the group consisting of PA MXDT / 6T, PA 11 / 10T, PA 11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T, PA 5T / 10T.
[0157] Advantageously, in said multilayer structure, each sealing layer consists of a composition comprising the same type of polymer P1i, in particular a polyamide, and each reinforcing layer consists of a composition comprising the same type of polymer P2j, in particular a polyamide, with the proviso that the polyamides P1i and P2j are different, i.e. if the sealing layer consists of a composition comprising a long-chain aliphatic polyamide, then the sealing layer consists of a composition comprising a semiaromatic polyamide.
[0158] Advantageously, the polymer P1i is a long-chain aliphatic polyamide, in particular PA1010, PA 1012, PA 1212, PA11, PA12, especially PA 11 or PA12, and the polymer P2j is a semiaromatic polyamide, in particular chosen from PAMPMDT / 6T, PA PA11 / 10T, PA 11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T, and PA 5T / 10T.
[0159] Advantageously, the multilayer structure consists of a single reinforcement layer and a single sealing layer, wherein the polymer P1i is a long-chain aliphatic polyamide, in particular PA1010, PA 1012, PA 1212, PA11, PA12, in particular PA 11 or PA12; and the polymer P2j is a semi-aromatic polyamide, in particular chosen from PA MPMDT / 6T, PA PA11 / 10T, PA 11 / BACT, PA11 / 6T / 10T a PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T.
[0160] According to one embodiment, the multilayer structure is a storage tank.
[0161] According to another embodiment, the multilayer structure is a flexible pipe.
[0162] The maximum use temperature Tu of the multilayer structure is 50° C. or higher, particularly 100° C. or higher.
[0163] In one embodiment, the multilayer structure defined above has reduced pressure resistance and drying capability.
[0164] Indeed, when storing or transporting hydrogen, hydrogen may diffuse from the interior of the pipe or tank through the sealing layer, due to its permeability to the transported or stored hydrogen, to the interface between the final sealing layer and the first composite reinforcement. The accumulation of hydrogen at this location may generate pressure which will lead to the collapse of the sealing layer when the internal pressure of the pipe or tank is lower than the pressure at the interface with the composite reinforcement (this may occur in particular when the pumping or transport of hydrogen is stopped during a production stoppage, resulting in a pressure drop of hundreds of bars to atmospheric pressure, or when the storage tank is empty). The same applies to internal water pressure testing of the tank: this water may migrate to the interface between the composite reinforcement and the final sealing layer by permeation and will then be very difficult to remove, leading to long and expensive drying cycles of the storage tank, especially under vacuum.
[0165] In another embodiment, the multilayer structure defined above further comprises a metal skeleton located within the sealing layer.
[0166] This metal skeleton is not leak-proof and is the innermost layer.
[0167] Advantageously, the multilayer structure further comprises at least one outer layer, in particular a metal layer, said layer being the outermost layer of the multilayer structure.
[0168] The outer layer is a second reinforcement layer, but is metallic rather than composite (composite).
[0169] There may also be a polymeric protective layer (outermost layer) on the structure which has an anti-wear effect or which allows an inscription to be placed on the structure.
[0170] About Fibrous Materials
[0171] As regards the fibres constituting the fibrous material, these are in particular mineral, organic or vegetable fibres.
[0172] Advantageously, the fibrous material may be sized or unsized.
[0173] Thus, the fibrous material may contain up to 0.1% by weight of an organic material (thermosetting or thermoplastic resin type) known as a sizing.
[0174] The mineral fibers include, for example, carbon fibers, glass fibers, basalt or basalt-based fibers, silica fibers, or silicon carbide fibers. Organic fibers include fibers based on thermoplastic or thermosetting polymers, such as semi-aromatic polyamide fibers, aramid fibers, or polyolefin fibers. Preferably, they are based on amorphous thermoplastic polymers and have a glass transition temperature Tg that is higher than the Tg of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is amorphous), or the Tg is higher than the Tm of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is semi-crystalline). Advantageously, they are based on semi-crystalline thermoplastic polymers and have a melting temperature Tm that is higher than the Tg of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is amorphous), or the Tm is higher than the Tm of the polymer or thermoplastic polymer mixture constituting the prepreg matrix (when the latter is semi-crystalline). Thus, there is no risk of melting of the organic fibers constituting the fibrous material during the impregnation with the thermoplastic matrix of the final composite. The plant fibers include natural flax, hemp, lignin, bamboo, silk, in particular spider silk, sisal, and other cellulosic fibers, in particular viscose. These plant fibers can be used pure, treated, or coated with a coating to facilitate the attachment and impregnation of the thermoplastic polymer matrix.
[0175] The fibrous material may also be woven, knitted, or woven from fibers.
[0176] It may also correspond to a fiber having a support thread.
[0177] These component fibers can be used alone or in a mixture. Thus, organic fibers can be mixed with mineral fibers to be pre-impregnated with thermoplastic polymer powder and form a pre-impregnated fibrous material.
[0178] The organic fiber strands may have several gram weights. They may further have several geometric shapes. The constituent fibers of the fibrous material may further be in the form of a mixture of these reinforcing fibers having different geometric shapes. The fibers are continuous fibers.
[0179] Preferably, the fibrous material consists of continuous carbon or glass fibers or mixtures thereof, in particular carbon fibers. It is used in the form of a roving or several rovings.
[0180] According to another aspect, the invention relates to a method for manufacturing a multilayer structure as defined above, characterized in that it comprises a step of welding a reinforcing layer as defined above to a sealing layer as defined above.
[0181] Advantageously, the welding step is performed by a system selected from laser, infrared (IR) heating, LED heating, induction or microwave heating, or high frequency (HF) heating.
[0182] Advantageously, the method comprises a step of extruding the sealing layer onto the metal skeleton and a step of welding the reinforcing layer onto the sealing layer.
[0183] According to another aspect, the invention relates to the use of a multilayer structure selected from a tank or a pipe or a pipeline for the production of a tank or a pipe or a pipeline for the transport, distribution or storage of hydrogen, the multilayer structure comprising, from the inside to the outside, at least one sealing layer as defined above and at least one composite reinforcement layer as defined above,
[0184] The innermost composite reinforcement layer is welded to the outermost adjacent sealing layer,
[0185] The sealing layer is composed of a composition that mainly comprises at least one semi-crystalline thermoplastic polymer P1i (i=1 to n, n is the number of sealing layers), whose Tm measured according to ISO 11357-3:2013 is less than 280°C, in particular less than 265°C,
[0186] The at least one thermoplastic polymer of each sealing layer may be the same or different, and at least one of the composite reinforcement layers is composed of a fibrous material in the form of continuous fibers, which is impregnated with the following composition: the composition mainly comprises at least one thermoplastic polymer P2j (especially semi-crystalline), (j=1 to m, m is the number of reinforcement layers), and the thermoplastic polymer P2j has a Tg measured according to ISO11357-3:2013 that is greater than the maximum use temperature (Tu) of the structure, wherein Tg≥Tu+20°C, especially Tg≥Tu+30°C, and Tu is greater than 50°C, especially greater than 100°C. Example
[0187] In all the examples, the tanks are obtained by rotomoulding of the liner at a temperature adapted to the nature of the thermoplastic resin used, but in all cases below 280°C.
[0188] In the case of epoxy, a wet filament winding process is used, which consists of winding a fiber around the mat, the fiber being pre-impregnated in a bath of liquid epoxy. The tank is then polymerized in an oven for 2 hours.
[0189] In all other cases, a fibrous material (tape) previously impregnated with a thermoplastic resin was used. This tape was deposited by filament winding using an automatic machine with a 1500 W laser heater at a speed of 12 m / min and without a polymerization step.
[0190] Example 1 (Comparative Example)
[0191] Type IV hydrogen storage tank, consisting of T700SC31E (produced by Toray) carbon fiber epoxy composite reinforcement (Tg 80°C) and PA6 sealing layer: there is no miscibility between the two resins (see Table 1), which hinders any welding between the fibrous reinforcement and the sealing layer.
[0192] Example 2 (Comparative Example)
[0193] Type IV hydrogen storage tank, consisting of T700SC31E (produced by Toray) carbon fiber epoxy composite reinforcement (Tg 80°C) and HDPE sealing layer: there is no miscibility between the two resins (see Table 1), which hinders any welding between the fibrous reinforcement and the sealing layer.
[0194] Example 3: Type IV or V hydrogen storage tank consisting of T700SC31E (produced by Toray) BACT / 10T carbon fiber composite reinforcement and PA6 sealing layer: good partial miscibility between the two resins (see Table 1), which allows good welding between the fibrous reinforcement and the sealing layer.
[0195] The selected BACT / 10T composition has a melting temperature Tm of 283°C, a crystallization temperature Tc of 250°C, and a glass transition temperature of 164°C.
[0196] Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0197] Example 4: IV or V type hydrogen storage tank, which is composed of T700SC31E (produced by Toray) BACT / 10T carbon fiber composite reinforcement and PA66 sealing layer: good partial miscibility between the two resins (see Table I), which allows good welding between the fibrous reinforcement and the sealing layer. The selected BACT / 10T composition has a melting temperature Tm of 283°C, a crystallization temperature Tc of 250°C, and a glass transition temperature of 164°C. Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0198] The higher melting point of the PA66 liner (268.8°C) compared to the PA6 liner in Example 3 (220°C) facilitates taping and fabrication of the tank.
[0199] Example 5: Type IV or V hydrogen storage tank, which is composed of CT24-5.0 / 270-T140 (produced by SGL Carbon) 11 / BACT / 10T carbon fiber composite reinforcement and PA11 sealing layer: good partial miscibility between the two resins (see Table 1), which leads to good welding between the fibrous reinforcement and the sealing layer. The selected 11 / BACT / 10T composition has a melting temperature Tm of 280°C, a crystallization temperature Tc of 220°C, and a glass transition temperature of 160°C. Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0200] Example 6: Type IV or V hydrogen storage tank consisting of CT24-5.0 / 270-T140 (produced by SGL Carbon) 11 / BACT / 10T carbon fiber composite reinforcement and PA11 / 10T sealing layer: good partial miscibility between the two resins (see Table 1), which leads to good welding between the fibrous reinforcement and the sealing layer.
[0201] The selected 11 / BACT / 10T composition has a melting temperature Tm of 280° C., a crystallization temperature Tc of 220° C., and a glass transition temperature of 160° C. Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0202] The 11 / 10T composition for the liner resulted in a Tm of 255°C.
[0203] The use of an 11 / 10T liner, which has a melting point of 255°C (close to the melting point of the 11 / BACT / 10T resin used as the matrix of the composite), facilitated processing of the tank.
[0204] Example 7: Type IV or V hydrogen storage tank, which is composed of CT24-5.0 / 270-T140 (produced by SGL Carbon) 11 / BACT carbon fiber composite reinforcement and PA11 sealing layer: good partial miscibility between the two resins (see Table 1), which leads to good welding between the fibrous reinforcement and the sealing layer. The selected 11 / BACT composition has a melting temperature Tm of 278°C, a crystallization temperature Tc of 210°C, and a glass transition temperature of 157°C. Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0205] The use of the slow crystallizing 11 / BACT polymer allows for lower wrapping temperatures compared to the 11 / BACT / 10T of the previous examples and facilitates the use of a PA11 liner.
[0206] Example 8: Type IV or V hydrogen storage tank, consisting of CT24-5.0 / 270-T140 T140 (produced by SGL Carbon) 11 / BACT carbon fiber composite reinforcement and PA11 / 10T sealing layer: good partial miscibility between the two resins (see Table 1), which leads to good welding between the fibrous reinforcement and the sealing layer.
[0207] The selected 11 / BACT composition has a melting temperature Tm of 278° C., a crystallization temperature Tc of 210° C., and a glass transition temperature of 157° C. Tg, Tc, and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.
[0208] The 11 / 10T composition for the liner resulted in a Tm of 255°C.
[0209] The implementation of the tank was facilitated using 11 / 10T liner which has a melting point of 255°C, close to 11 / BACT as the reinforcing resin of the composite.
[0210] In all examples in Table 1 below, to evaluate the miscibility of the resins, the mixtures were made from powders with a particle size of about 150 μm on a micro DSM with a recirculation time of 1 minute after melting. All mixtures were made at 300°C, except for the epoxy-polyethylene mixture, which was made at 220°C.
[0211] At the end of the mixing process, the mixture is injected into a mold to produce a test piece that will be characterized in the DMA.
[0212] Table 1
[0213]
[0214]
[0215] ***Tg measurements were done by DMTA according to ISO 4664-1
[0216] Miscibility test results:
[0217] - Column 4: Glass transition temperature of each resin before mixing
[0218] - Column 5: Glass transition temperature of the resin in the mixture
[0219] - Column 6: Ratio between the difference in glass transition temperature of the resins in the mixture and before mixing.
[0220] 100% indicates the immiscibility of the resin,
[0221] <80% indicates low miscibility,
[0222] <30% indicates good but partial miscibility,
[0223] 0 indicates complete miscibility.
Claims
1. A multilayer structure selected from a tank or a pipeline intended for transporting, distributing, or storing hydrogen, comprising, from the inside to the outside, at least one sealing layer and at least one composite reinforcement layer, The innermost composite reinforcement layer is welded to the outermost adjacent sealing layer, The sealing layer is composed of the following composition: The composition mainly comprises at least one semi-crystalline thermoplastic polymer P1i, i=1 to n, n being the number of sealing layers, having a Tm measured according to ISO 11357-3: 2013 of less than 280°C, The at least one thermoplastic polymer of each sealing layer may be the same or different, and at least one of the composite reinforcement layers consists of a fibrous material in the form of continuous fibers, which is impregnated with a composition that essentially comprises at least one thermoplastic polymer P2j, j=1 to m, m being the number of reinforcement layers, the thermoplastic polymer P2j having a Tg greater than the maximum use temperature (Tu) of the structure measured according to ISO 11357-3: 2013, wherein Tg ≥ Tu+ 20°C, Tu is greater than 50°C, The polymer P1i is a long-chain aliphatic polyamide or a semi-aromatic polyamide, and the polymer P2j is a semi-aromatic polyamide.
2. The multilayer structure according to claim 1, wherein the multilayer structure is a pipe intended for transporting, distributing, or storing hydrogen.
3. The multilayer structure according to claim 1, wherein the semi-crystalline thermoplastic polymer P1i has a Tm measured according to ISO 11357-3: 2013 of less than 265°C.
4. The multilayer structure according to claim 1, wherein the thermoplastic polymer P2j is a semi-crystalline thermoplastic polymer P2j.
5. The multilayer structure according to claim 1, wherein Tg ≥ Tu + 30 °C.
6. The multilayer structure according to claim 1, wherein Tu is greater than 100°C.
7. A multilayer structure according to claim 1, wherein each polymer P1i of each sealing layer is partially or completely miscible with each polymer P1i of an adjacent layer, each polymer P2j of each reinforcing layer is partially or completely miscible with each polymer P2j of an adjacent layer, and polymer P21 is partially or completely miscible with polymer P11 adjacent thereto, The complete or partial miscibility of the polymers is defined by the difference in the glass transition temperatures of the two resins in the mixture relative to the difference in the glass transition temperatures of the two resins before mixing, the miscibility being complete when the difference is equal to 0 and partial when the difference is different from 0.
8. The multilayer structure according to any one of claims 1 to 7, characterized in that Each sealing layer comprises the same type of polymer.
9. The multilayer structure according to claim 8, characterized in that The same type of polymer is polyamide.
10. The multilayer structure according to any one of claims 1 to 7, characterized in that Each reinforcement layer comprises the same type of polymer.
11. The multilayer structure according to claim 10, characterized in that The same type of polymer is polyamide.
12. The multilayer structure according to any one of claims 1 to 7, characterized in that Each sealing layer comprises the same type of polymer, and each reinforcing layer comprises the same type of polymer.
13. The multilayer structure according to claim 12, characterized in that The same type of polymer in each sealing layer is polyamide, and the same type of polymer in each reinforcing layer is polyamide.
14. The multilayer structure according to any one of claims 1 to 7, characterized in that It has a single sealing layer and a single reinforcement layer.
15. The multilayer structure according to any one of claims 1 to 7, characterized in that The structure is a storage tank or a flexible pipe.
16. The multilayer structure according to any one of claims 1 to 7, characterized in that The composition comprising the polymers P1 and P2 also comprises additives enabling them to absorb radiation suitable for welding.
17. The multilayer structure according to claim 16, characterized in that The additive is selected from carbon black, carbon nanotubes (CNT), or graphene.
18. The multilayer structure according to any one of claims 1 to 7, characterized in that Said composition comprising said polymer P2j is transparent to radiation suitable for welding.
19. The multilayer structure according to any one of claims 1 to 7, characterized in that The welding is performed by a system selected from laser, infrared (IR) heating, LED heating, induction or microwave heating, or high frequency (HF) heating.
20. The multilayer structure according to any one of claims 1 to 7, characterized in that The polymer P1i is a long-chain aliphatic polyamide selected from PA1010, PA1012, PA1212, PA11, PA12; or a semi-aromatic one selected from PA11 / 5T, PA11 / 6T, and PA11 / 10T.
21. The multilayer structure according to claim 20, characterized in that The polymer P1i is a long-chain aliphatic polyamide selected from PA 11 or PA12.
22. The multilayer structure according to any one of claims 1 to 7, characterized in that The polymer P2j is a semi-aromatic polyamide selected from PA MPMDT / 6T, PA 11 / 10T, PA 11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PAMPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T, PA11 / 5T / 10T.
23. The multilayer structure according to any one of claims 1 to 7, characterized in that The polymer P1i is a long chain aliphatic polyamide selected from PA1010, PA 1012, PA 1212, PA11, PA12, or a semiaromatic one selected from PA 11 / 5T, PA 11 / 6T, or PA 11 / 10T; and the polymer P2j is a semiaromatic polyamide selected from PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA 5T / 10T, PA 11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA 11 / BACT / 6T, PA 11 / MPMDT / 6T, PA 11 / MPMDT / 10T, PA 11 / BACT / 10T, PA 11 / MXDT / 10T, PA11 / 5T / 10T.
24. The multilayer structure according to claim 23, characterized in that The polymer P1i is a long-chain aliphatic polyamide selected from PA11 or PA12.
25. The multilayer structure according to any one of claims 1 to 7, characterized in that It has reduced pressure tolerance and drying capabilities.
26. The multilayer structure according to any one of claims 1 to 7, characterized in that The structure further comprises a metal skeleton located within the sealing layer.
27. The multilayer structure according to any one of claims 1 to 7, characterized in that The structure further comprises at least one outer layer.
28. The multilayer structure according to claim 27, characterized in that The at least one outer layer is a metal layer, and the metal layer is the outermost layer of the multilayer structure.
29. The multilayer structure according to any one of claims 1 to 7, characterized in that The fibrous material is selected from glass fibers, carbon fibers, basalt fibers or basalt-based fibers.
30. Method for producing a multilayer structure as defined in any one of claims 1 to 29, characterized in that It comprises the step of welding a reinforcing layer as defined in claim 1 to a sealing layer as defined in claim 1 .
31. The method according to claim 30, characterized in that The welding step is performed by a system selected from laser, infrared (IR) heating, LED heating, induction or microwave heating, or high frequency (HF) heating.
32. The method according to claim 30 or 31, characterized in that The method comprises the steps of extruding the sealing layer onto the metal skeleton and welding the reinforcing layer onto the sealing layer.