Test device and method for simulating corrosion environment of compacted bentonite with different water contents
By designing experimental devices and methods to simulate the corrosion environment of bentonite, the problems of bentonite wetting and uneven distribution of groundwater ions were solved, enabling more accurate simulation of the corrosion environment and acquisition of corrosion data, and supporting research on the corrosion behavior of high-level radioactive waste geological disposal container materials.
Patent Information
- Application Number
- CN202010963372.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-09-14
AI Technical Summary
Existing technologies make it difficult to achieve uniform mixing of groundwater and bentonite in simulated bentonite corrosion environments, resulting in uneven wetting and groundwater ion distribution, which affects the accuracy of corrosion data.
An experimental device was designed to simulate the corrosion environment of compacted bentonite with different water contents. The device includes a bentonite block compaction device and a closed electrolytic cell. The bentonite blocks are compacted by a hydraulic system, and an electrochemical testing method is used to ensure that the groundwater solution and bentonite are uniformly mixed.
It significantly improved the uniformity of bentonite wetting and the uniformity of groundwater ion distribution, achieving more realistic corrosion environment simulation and accurate corrosion data, and supporting research on the corrosion behavior of high-level radioactive waste geological disposal container materials.
Smart Images

Figure HDA0002681371400000011 
Figure HDA0002681371400000012 
Figure HDA0002681371400000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal corrosion and protection research, and specifically relates to a test device and method for simulating the corrosion environment of compacted bentonite with different water contents, which is suitable for simulating the corrosion environment of bentonite, a buffer material for geological disposal of high-level radioactive waste. Background Art
[0002] As a green and clean energy, nuclear energy has become an important part of the global electricity source. At the same time, a large amount of harmful radioactive waste is also produced. If it is not properly disposed of, it will cause serious damage to the human living environment. Therefore, how to safely and effectively deal with radioactive waste has become an important issue that needs to be urgently solved for the sustainable development of nuclear energy. At present, countries around the world generally believe that deep geological disposal is the best disposal solution for high-level radioactive nuclear waste, that is, a multiple barrier system is used to bury high-level radioactive waste in a geological environment about 500 to 1000 meters deep from the surface to isolate it from the human living environment. The multiple barrier system includes surrounding rock, buffer material bentonite, metal disposal container and glass solid body from the outside to the inside, and its main function is to prevent the leakage of nuclides. As a key component, the disposal container is an important safety barrier for isolating nuclides, and its corrosion resistance is the first factor to meet the safe disposal of high-level radioactive waste. In the thousands of years of geological disposal process, as the buffer material bentonite is gradually infiltrated by groundwater, the disposal container will face severe corrosion problems.
[0003] In recent years, scholars from all over the world have conducted a lot of research on the corrosion behavior of high-level radioactive waste geological disposal container materials in simulated different geological disposal environments. The results show that the evolution of the surrounding environment, such as groundwater ion composition, dissolved oxygen concentration and bentonite properties, is the key factor determining the corrosion mode and corrosion rate of the disposal container. However, in the early stage of geological disposal, due to the continuous infiltration of groundwater, the bentonite around the container gradually changes from an unsaturated state to a water-saturated state. In this process, the water content in the bentonite will also have a great influence on the corrosion evolution of the disposal container. In order to further study the influence of groundwater content in compacted bentonite on the corrosion behavior of the disposal container, it is necessary to carry out simulation research to simulate the corrosion environment of compacted bentonite with a predetermined groundwater content. Traditional simulation methods generally use a spraying method to spray the prepared groundwater solution into the bentonite or directly pour the solution into the bentonite in a certain proportion and stir it. However, due to the agglomeration of bentonite, there is often an uneven degree of bentonite wetting and uneven distribution of groundwater ion components, which brings great difficulties to the realization of corrosion electrochemical testing of candidate materials in a low-water content compacted bentonite environment and the acquisition of accurate corrosion data. Summary of the invention
[0004] The problem to be solved by the present invention is: to provide a test device and method for simulating the corrosion environment of compacted bentonite with different water contents, so that the simulated groundwater solution and bentonite are evenly mixed in different proportions to form a corrosion environment, effectively solve the problems of bentonite wetting degree and uneven distribution of groundwater ions, and more realistically simulate the corrosion environment of compacted bentonite with a predetermined groundwater content, which is used to realize the corrosion behavior research of disposal container candidate materials in the simulated compacted bentonite environment with different groundwater contents.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A test device simulating the corrosion environment of bentonite compacted with different water contents, the test device is provided with a bentonite block compacting device, the bentonite block compacting device is composed of a steel stand, a mold pressure head, a mold base, a separate hydraulic jack, and a hydraulic pump. The specific structure is as follows:
[0007] The steel stand is composed of an upper steel plate, a middle steel plate, a lower steel plate, 4 steel columns, 8 nuts, and 8 washers. The horizontal upper steel plate, middle steel plate, and lower steel plate are arranged relatively parallel to each other at the upper, middle, and lower positions. The 4 steel columns with threads at both ends are respectively passed along the four corners of the upper steel plate, the middle steel plate, and the lower steel plate. The upper and lower ends of each steel column are respectively connected to the upper steel plate and the lower steel plate by threads. The upper steel plate and the lower steel plate are fixed by nuts and washers installed at the upper and lower ends of the steel column. The middle steel plate and the steel column are in sliding fit.
[0008] The separate hydraulic jack is arranged on the lower steel plate, the top output end thereof is connected to the bottom of the middle steel plate, the power input end thereof is connected to the hydraulic pump, and the mold base is arranged on the top of the middle steel plate;
[0009] The dry bentonite powder and ice powder are placed in the mold base and mixed evenly. A mold pressing head is installed on the mold base. The lower end of the mold pressing head is in sliding fit with the mold base, and the upper end of the mold pressing head corresponds to the bottom of the upper steel plate.
[0010] In the test device simulating the corrosion environment of compacted bentonite with different water contents, the hydraulic pump drives the output end of the separate hydraulic jack to rise and fall, so that the mold base can move freely up and down with the middle steel plate, which is convenient for discharging materials into the mold base and demoulding the compacted bentonite block.
[0011] In the test device for simulating the corrosion environment of compacted bentonite with different water contents, the mold pressure head cooperates with the mold base to make compacted bentonite blocks from dry bentonite powder and ice powder.
[0012] The test device for simulating the corrosion environment of compacted bentonite with different water contents is also provided with a stainless steel closed electrolytic cell, which is composed of a stainless steel electrolytic cell, a compacted bentonite block, a counter electrode, a working electrode, and a reference electrode. The specific structure is as follows:
[0013] The compacted bentonite block made by the bentonite block compacting device is placed in the electrolyte in the stainless steel electrolytic cell, one end of the counter electrode, the working electrode and the reference electrode are respectively arranged in the compacted bentonite block, and the other ends of the counter electrode, the working electrode and the reference electrode are led out to the electrochemical workstation through wires, and the corrosion electrochemical test is carried out through the electrochemical workstation.
[0014] A test method for simulating the corrosion environment of compacted bentonite with different water contents, comprising the following steps:
[0015] (1) Prepare groundwater simulation solution using analytical grade reagents and deionized water;
[0016] (2) Pour the simulated solution into an ice box and freeze it in a low-temperature freezer at -40°C to prepare ice cubes; crush and grind the ice cubes into ice powder using an ice crusher, filter it through a 200-mesh filter sieve to obtain fine ice powder, and store it in a freezer for later use;
[0017] (3) preheating the oven to 100-120° C., spreading the bentonite powder on a cardboard and placing it in the oven, drying for 0.5-2 hours to obtain dry bentonite powder, then immediately pouring it into a sealed bag, sealing it, and placing it in a freezer for frozen storage;
[0018] (4) Calculating the mass of dry bentonite and ice powder required to prepare a compacted bentonite block based on the predetermined bentonite block volume, dry density and water content, and weighing them using a weighing balance;
[0019] (5) According to the thickness of the bentonite block to be compacted (20 to 40 mm) and the size of the mold base, calculate the distance that the mold pressure head needs to be pressed into the mold base and mark it;
[0020] (6) Under low temperature conditions of -40°C, freeze-dried bentonite powder is mixed with ice powder, stirred evenly, and then poured into a -40°C low temperature mold base, and then the mold pressure head is placed into the mold base, and a compaction test is performed using a bentonite block compaction device; the mold pressure head should be stored in a -40°C low temperature freezer in advance to ensure that the bentonite is in a low temperature environment during the compaction process;
[0021] (7) Manually operate the hydraulic pump to lift the separate hydraulic jack and move the middle steel plate and the mold base upward. The top of the mold pressure head contacts the upper steel plate of the steel stand and is pressed into the mold base;
[0022] (8) When the mold pressing head is pressed into the mold base to the marked position in step 5, the pressing is stopped and the mold is demolded, the compacted bentonite block is taken out, and it is placed in a freezer for frozen storage;
[0023] (9) Under low temperature conditions of -40°C, the corrosion weight loss samples and electrochemical sensors were buried in different ice-containing compacted bentonite blocks, and then placed in a stainless steel electrolytic cell in a stacking order and completely sealed;
[0024] (10) When the ice in the compacted bentonite block is completely melted and the temperature reaches the temperature required for the corrosion test, a corrosion electrochemical test is performed.
[0025] The test method for simulating the corrosion environment of bentonite compacted with different water contents, in step (1), according to the chemical environment characteristics of groundwater, the corrosive ions include HCO3 - , Cl - and SO4 2- , prepare the groundwater simulation solution as follows: NaHCO3 with a molar concentration of 0.01M, NaCl with a molar concentration of 0.1M, Na2SO4 with a molar concentration of 0.1M, and water as the balance.
[0026] The test method for simulating the corrosion environment of compacted bentonite with different water contents, in step (4), according to the corrosion test conditions and the size of the stainless steel electrolytic cell, a compacted bentonite block with a water content of 10wt% to 40wt% is prepared.
[0027] The design concept of the present invention is:
[0028] In order to simulate the corrosion environment characteristics of high-level radioactive waste geological disposal as close to reality, the present invention designs a method and device for preparing compacted bentonite blocks with predetermined groundwater content, and effectively solves the problems of uneven wetting degree of compacted bentonite and uneven distribution of groundwater ions, and realizes electrochemical in-situ measurement of corrosion of disposal container candidate materials in a compacted bentonite environment through a closed electrolytic cell device.
[0029] The advantages and beneficial effects of the present invention are:
[0030] 1. The test device and method described in the present invention are simple to operate and feasible, and significantly improve the forming rate and preparation efficiency of ice-containing compacted bentonite blocks.
[0031] 2. The present invention can simulate the compacted bentonite corrosion environment of a predetermined groundwater content more realistically and accurately according to different groundwater chemical environment characteristics.
[0032] 3. The research method of the present invention effectively avoids the problems of uneven wetting degree of compacted bentonite blocks and uneven distribution of groundwater ions.
[0033] 4. The device and method provided by the present invention are used to realize the electrochemical in-situ monitoring of corrosion of candidate materials for high-level radioactive waste geological disposal containers in an environment simulating compacted bentonite with different groundwater contents. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of bentonite block compacting device. In the figure, 1, steel stand; 11, upper steel plate; 12, middle steel plate; 13, lower steel plate; 14, steel column; 15, nut; 16, gasket; 2, mold pressure head; 3, mold base; 4, separate hydraulic jack; 5, hydraulic pump.
[0035] Figure 2 Schematic diagram of a stainless steel sealed electrolytic cell. In the figure, 6, stainless steel electrolytic cell; 7, compacted bentonite block; 8, counter electrode; 9, working electrode; 10, reference electrode.
[0036] Figure 3 Schematic diagram of a compacted bentonite block with a water content of 20 wt%.
[0037] Figure 4 Schematic diagram of a compacted bentonite block with a water content of 40 wt%. DETAILED DESCRIPTION
[0038] The invention discloses a test device for simulating the corrosion environment of bentonite compacted with different water contents, comprising a bentonite block compacting device, a low-temperature freezer, an ice crusher, a filter screen, a weighing balance, a 316L stainless steel closed electrolytic cell, and the like.
[0039] like Figure 1 As shown, the bentonite block compacting device is composed of a steel stand 1, a mold pressure head 2, a mold base 3, a separate hydraulic jack 4 (50T), a hydraulic pump 5, etc. The specific structure is as follows:
[0040] The steel stand 1 is composed of an upper steel plate 11, a middle steel plate 12, a lower steel plate 13, four steel columns 14, eight nuts 15, and eight washers 16. The horizontal upper steel plate 11, middle steel plate 12, and lower steel plate 13 are arranged relatively parallel to each other in the upper, middle, and lower directions. Four steel columns 14 with threads at both ends are respectively passed through the four corners of the upper steel plate 11, the middle steel plate 12, and the lower steel plate 13. The upper and lower ends of each steel column 14 are respectively connected to the upper steel plate 11 and the lower steel plate 13 by threads. The upper steel plate 11 and the lower steel plate 13 are fixed by nuts 15 and washers 16 installed at the upper and lower ends of the steel column 14, and the middle steel plate 12 is in sliding fit with the steel column 14.
[0041] The separate hydraulic jack 4 is arranged on the lower steel plate 13, and its top output end is connected to the bottom of the middle steel plate 12, and its power input end is connected to the hydraulic pump 5. The mold base 3 is arranged on the top of the middle steel plate 12. The hydraulic pump 5 drives the output end of the separate hydraulic jack 4 to rise and fall, so that the mold base 3 can move freely up and down with the middle steel plate 12, which is convenient for discharging materials into the mold base 3 and demolding the compacted bentonite block 7.
[0042] The dry bentonite powder and ice powder are placed in the mold base 3 and mixed evenly. The mold press head 2 is installed on the mold base 3. The lower end of the mold press head 2 is slidably matched with the mold base 3, and the upper end of the mold press head 2 corresponds to the bottom of the upper steel plate 11. The mold press head 2 cooperates with the mold base 3 to make the dry bentonite powder and ice powder into a compacted bentonite block 7.
[0043] like Figure 2 As shown, the 316L stainless steel closed electrolytic cell is composed of a stainless steel electrolytic cell 6, a compacted bentonite block 7, a counter electrode 8, a working electrode 9, a reference electrode 10, etc. The specific structure is as follows:
[0044] The compacted bentonite block 7 made by the bentonite block compacting device is placed in the electrolyte in the stainless steel electrolytic cell 6, one end of the relative electrode 8, the working electrode 9, and the reference electrode 10 are respectively arranged in the compacted bentonite block 7, and the other ends of the relative electrode 8, the working electrode 9, and the reference electrode 10 are led out to the electrochemical workstation through wires, and corrosion electrochemical testing is carried out through the electrochemical workstation.
[0045] In the specific implementation process, first, the prepared simulated groundwater solution is frozen into ice cubes and then ground into ice powder, which is then filtered through a fine sieve and mixed with dry bentonite powder in a certain mass ratio, and then poured into the mold base 3 for compaction under low temperature conditions. Subsequently, the metal corrosion test piece and the electrochemical sensor are buried in different compacted bentonite blocks, and are sequentially placed in a stainless steel electrolytic cell and sealed. After the frozen bentonite returns to room temperature, the corrosion test is carried out.
[0046] The technical solution of the present invention is clearly and completely described below in conjunction with specific embodiments. The preferred embodiments of the present invention are described in detail as follows:
[0047] Example 1
[0048] like Figure 1 , Figure 2 , Figure 3 As shown, the experimental method of this embodiment for simulating the corrosion environment of compacted bentonite with a water content of 20wt% comprises the following steps:
[0049] (1) According to the characteristics of groundwater chemical environment (corrosive ions mainly include HCO3 - , Cl - and SO4 2- ), a simulated groundwater solution was prepared using analytical grade reagents and deionized water: 0.01 M molar concentration of NaHCO3, 0.1 M molar concentration of NaCl, 0.1 M molar concentration of Na2SO4, and the balance of water.
[0050] (2) Pour the prepared simulated solution into an ice box, and place it in a low-temperature freezer at a temperature of -40°C to freeze ice cubes; crush and grind the prepared ice cubes into ice powder using an ice crusher, and filter through a 200-mesh filter sieve to obtain fine ice powder, which is stored in a freezer for later use.
[0051] (3) Preheat the oven to 105° C. Spread the bentonite powder on a piece of cardboard and put it into the oven. Dry the bentonite powder for 1 hour to obtain dry bentonite powder. Then, immediately pour the powder into a sealed bag, seal it, and store it in a freezer.
[0052] (4) According to the corrosion test conditions and the size of the stainless steel electrolytic cell, four compacted bentonite blocks with a water content of 20 wt% and a diameter of 91 cm and a height of 25 cm were prepared; it was calculated that each compacted bentonite block required 244 g of dry bentonite powder and 61 g of ice powder, which were weighed using a weighing balance; the mixed dry density of the compacted bentonite block was 1.88 g / cm 3 .
[0053] (5) According to the thickness of the bentonite block to be compacted (20-40 mm) and the size of the mold base 3, calculate the distance that the mold pressure head 2 needs to be pressed into the mold base 3 and mark it.
[0054] (6) Under low temperature conditions of -40°C, freeze-dried bentonite powder and ice powder are mixed and stirred evenly, and then poured into a mold base 3 at a low temperature of -40°C. Then, the mold press head 2 is placed into the mold base 3, and the mold press head 2 is placed in the mold base 3. Figure 1 The bentonite block compacting device in the embodiment of the present invention is used for the compaction test. The mold pressure head 2 should be stored in a -40℃ low temperature freezer in advance to ensure that the bentonite is in a low temperature environment during the compaction process.
[0055] (7) The hydraulic pump 5 is manually operated to lift the separate hydraulic jack 4 and move the middle steel plate 12 and the mold base 3 upward. The top of the mold pressing head 2 contacts the upper steel plate 11 of the steel stand 1 and is pressed into the mold base 3.
[0056] (8) When the mold pressing head 2 is pressed into the mold base 3 to the marked position in step 5, the pressing is stopped and demolding is performed to obtain a compacted bentonite block with an ice content of 20 wt% ( Figure 3 ) and store it in the freezer.
[0057] (9) Under low temperature conditions of -40°C, the corrosion weight loss samples and electrochemical sensors were buried in different compacted bentonite blocks with an ice content of 20 wt% using tools such as a chisel and a hand drill, and then placed in a stainless steel electrolytic cell in a stacking order and completely sealed ( Figure 2 ).
[0058] (10) When the ice in the compacted bentonite block is completely melted and the temperature reaches the temperature required for the corrosion test, a corrosion electrochemical test is performed.
[0059] Example 2
[0060] like Figure 1 , Figure 2 , Figure 4 As shown, the experimental method of this embodiment for simulating the corrosion environment of compacted bentonite with a water content of 40wt% comprises the following steps:
[0061] (1) According to the characteristics of groundwater chemical environment (corrosive ions mainly include HCO3 - , Cl - and SO4 2- ), a simulated groundwater solution was prepared using analytical grade reagents and deionized water: 0.01 M molar concentration of NaHCO3, 0.1 M molar concentration of NaCl, 0.1 M molar concentration of Na2SO4, and the balance of water.
[0062] (2) Pour the prepared simulated solution into an ice box, and place it in a low-temperature freezer at a temperature of -40°C to freeze ice cubes; crush and grind the prepared ice cubes into ice powder using an ice crusher, and filter through a 200-mesh sieve to obtain fine ice powder, which is then stored in a freezer for later use.
[0063] (3) Preheat the oven to 105° C. Spread the bentonite powder on a piece of cardboard and put it into the oven. Dry the bentonite powder for 1 hour to obtain dry bentonite powder. Then, immediately pour the powder into a sealed bag, seal it, and store it in a freezer.
[0064] (4) According to the corrosion test conditions and the size of the stainless steel electrolytic cell, four compacted bentonite blocks with a water content of 40 wt% and a diameter of 91 cm and a height of 25 cm were prepared; it was calculated that each compacted bentonite block required 163 g of dry bentonite powder and 108 g of ice powder, which were weighed using a weighing balance; the mixed dry density of the compacted bentonite block was 1.67 g / cm 3 .
[0065] (5) According to the thickness of the bentonite block to be compacted (20-40 mm) and the size of the mold base 3, calculate the distance that the mold pressure head 2 needs to be pressed into the mold base 3 and mark it.
[0066] (6) Under low temperature conditions of -40°C, dry bentonite powder and ice powder are mixed and stirred evenly, and then poured into a mold base 3 at a low temperature of -40°C. Figure 1 The bentonite block compacting device in the embodiment of the present invention is used for the compaction test. The mold pressure head 2 should be stored in a -40℃ low temperature freezer in advance to ensure that the bentonite is in a low temperature environment during the compaction process.
[0067] (7) Manually operate the hydraulic pump 5 to lift the separate hydraulic jack 4 and move the middle steel plate 12 and the mold base 3 upward; the top of the mold pressing head 2 contacts the upper steel plate 11 of the steel stand 1 and is pressed into the mold base 3.
[0068] (8) When the mold pressing head 2 is pressed into the mold base 3 to the marked position in step 5, the pressing is stopped and demolding is performed to obtain a compacted bentonite block with an ice content of 40 wt% ( Figure 4 ) and store it in the freezer.
[0069] (9) Under low temperature conditions of -40°C, the corrosion weight loss samples and electrochemical sensors were buried in different compacted bentonite blocks with an ice content of 40 wt% using tools such as a chisel and a hand drill, and then placed in a stainless steel electrolytic cell in a stacking order and completely sealed ( Figure 2 ).
[0070] (10) When the ice in the compacted bentonite block is completely melted and the temperature reaches the temperature required for the corrosion experiment, a corrosion electrochemical test is performed.
[0071] The results of the embodiments show that the present invention truly and accurately simulates the corrosion environment of bentonite, a buffer material for high-level radioactive waste geological disposal, after being infiltrated by groundwater, and is used to study the corrosion behavior of candidate materials for high-level radioactive waste geological disposal containers in an environment simulating compacted bentonite with different groundwater contents.
[0072] Obviously, the examples described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
Claims
1. A test method for simulating the corrosion environment of compacted bentonite with different water contents, characterized in that: The test device used in this test method is equipped with a bentonite block compacting device, which consists of a steel stand, a mold pressure head, a mold base, a separate hydraulic jack, and a hydraulic pump. The specific structure is as follows: The steel stand is composed of an upper steel plate, a middle steel plate, a lower steel plate, 4 steel columns, 8 nuts, and 8 washers. The horizontal upper steel plate, middle steel plate, and lower steel plate are arranged relatively parallel to each other at the upper, middle, and lower positions. The 4 steel columns with threads at both ends are respectively passed along the four corners of the upper steel plate, the middle steel plate, and the lower steel plate. The upper and lower ends of each steel column are respectively connected to the upper steel plate and the lower steel plate by threads. The upper steel plate and the lower steel plate are fixed by nuts and washers installed at the upper and lower ends of the steel column. The middle steel plate and the steel column are in sliding fit. The separate hydraulic jack is arranged on the lower steel plate, the top output end thereof is connected to the bottom of the middle steel plate, the power input end thereof is connected to the hydraulic pump, and the mold base is arranged on the top of the middle steel plate; The dry bentonite powder and ice powder are placed in the mold base and mixed evenly. A mold pressing head is installed on the mold base. The lower end of the mold pressing head is in sliding fit with the mold base, and the upper end of the mold pressing head corresponds to the bottom of the upper steel plate. The hydraulic pump drives the output end of the separate hydraulic jack to rise and fall, so that the mold base can move freely up and down along with the middle steel plate, which is convenient for releasing materials into the mold base and demoulding the compacted bentonite block; The mold pressing head cooperates with the mold base to form a compacted bentonite block from the dry bentonite powder and ice powder; The test device is also equipped with a stainless steel sealed electrolytic cell consisting of a stainless steel electrolytic cell, a compacted bentonite block, a counter electrode, a working electrode, and a reference electrode. The specific structure is as follows: The compacted bentonite block made by the bentonite block compacting device is placed in the electrolyte in the stainless steel electrolytic cell, one end of the counter electrode, the working electrode, and the reference electrode are respectively arranged in the compacted bentonite block, and the other ends of the counter electrode, the working electrode, and the reference electrode are led to the electrochemical workstation through wires, and the corrosion electrochemical test is performed through the electrochemical workstation; The test method for simulating the corrosion environment of compacted bentonite with different water contents comprises the following steps: (1) Prepare the simulated groundwater solution using analytical grade reagents and deionized water; (2) Pour the simulated solution into an ice box and freeze it in a low-temperature freezer at -40°C to prepare ice cubes; crush and grind the ice cubes into ice powder using an ice crusher, filter it through a 200-mesh filter sieve to obtain fine ice powder, and store it in a freezer for later use; (3) Preheat the oven to 100-120°C, spread the bentonite powder on a cardboard and put it into the oven. After drying for 0.5-2 hours, obtain dry bentonite powder, then immediately pour it into a sealed bag, seal it, and store it in a freezer; (4) Calculate the mass of dry bentonite and ice powder required to prepare a compacted bentonite block based on the predetermined bentonite block volume, dry density and water content, and weigh them using a weighing balance; (5) Based on the required thickness of the compacted bentonite block (20 to 40 mm) and the size of the mold base, calculate the distance that the mold pressure head needs to be pressed into the mold base and mark it; (6) Under low temperature conditions of -40°C, freeze-dried bentonite powder is mixed with ice powder, stirred evenly, and then poured into a -40°C low-temperature mold base. The mold pressure head is then placed into the mold base, and a compaction test is performed using a bentonite block compaction device; the mold pressure head should be stored in a -40°C low-temperature freezer in advance to ensure that the bentonite is in a low-temperature environment during the compaction process; (7) Manually operate the hydraulic pump to lift the separate hydraulic jack and move the middle steel plate and the mold base upward. The top of the mold pressure head contacts the upper steel plate of the steel stand and then presses into the mold base; (8) When the mold pressing head is pressed into the mold base to the marked position in step 5, stop pressing and demold, take out the compacted bentonite block, and put it into a freezer for frozen storage; (9) Under low temperature conditions of -40°C, the corrosion weight loss samples and electrochemical sensors were buried in different ice-containing compacted bentonite blocks, and then placed in a stainless steel electrolytic cell in a stacking order and completely sealed; (10) When the ice in the compacted bentonite block is completely melted and the temperature reaches the temperature required for the corrosion experiment, the corrosion electrochemical test is carried out.
2. The test method for simulating the corrosion environment of compacted bentonite with different water contents according to claim 1, characterized in that: In step (1), according to the characteristics of the groundwater chemical environment, the corrosive ions include HCO3 - , Cl - and SO4 2- , prepare the groundwater simulation solution as follows: NaHCO3 with a molar concentration of 0.01M, NaCl with a molar concentration of 0.1M, Na2SO4 with a molar concentration of 0.1M, and water as the balance.
3. The test method for simulating the corrosion environment of compacted bentonite with different water contents according to claim 1, characterized in that: In step (4), according to the corrosion test conditions and the size of the stainless steel electrolytic cell, a compacted bentonite block with a water content of 10 wt% to 40 wt% is prepared.