Synergistic solidification treatment method for radioactive waste
By sorting and melting and solidifying the radioactive waste, using the glass additive function in non-combustible non-metallic waste, the problems of slow processing speed and low tolerance in the prior art are solved, and efficient capacity reduction for a variety of wastes and Stable solidification, suitable for a variety of waste treatments in nuclear facilities.
Patent Information
- Application Number
- CN202111512903.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-11
AI Technical Summary
The existing radioactive waste treatment methods have problems such as slow processing speed, low waste tolerance, high leaching rate of compressed waste nuclides, high cost and low applicability of curing equipment, and cannot effectively deal with various types of radioactive waste, especially Non-combustible metals and non-metallic wastes.
Classify the radioactive waste to be treated into combustible waste, non-combustible metal waste and non-combustible non-metal waste, and perform smelting and decontamination and calcining treatment. Use the function of glass additives in non-combustible non-metal waste to form glass ceramic solidified bodies through melt solidification treatment. , achieve efficient capacity reduction and stable solidification of waste.
It has achieved extensive treatment of almost all types of radioactive waste, improved treatment efficiency and curing effect, reduced dependence on glass additives, achieved efficient capacity reduction and stable curing of waste, and is suitable for a variety of waste treatments in nuclear facilities.
Smart Images

Figure CN114188061B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radioactive waste treatment, and in particular to a synergistic solidification treatment method for radioactive waste. Background Art
[0002] A large amount of radioactive waste is generated during the production and decommissioning of the nuclear industry. The main process flow of the traditional treatment method for radioactive waste is as follows: classification - compression and volume reduction, cement solidification or concrete fixation - packaging and storage in a temporary storage warehouse - shallow stratum disposal. This treatment method is widely used by nuclear industry units, especially nuclear power plants, due to its mature technology, but it has disadvantages such as slow processing speed, low waste inclusion rate, and high leaching rate of waste nuclides after compression. With the continuous development of my country's nuclear industry and the increasing attention to nuclear safety, the traditional cement solidification or concrete fixation method has gradually failed to meet the requirements of stable treatment of radioactive waste and volume reduction of solidified bodies.
[0003] A technology provides a cement solidification system, method and application for radioactive waste treatment, the system includes a three-axle rail car, a track, a scale detection system and a wireless control system, and is intended to solve the problems of high equipment cost, complexity and poor applicability caused by the existing use of cement solidification lines to treat radioactive waste. The system is only applicable to the cement solidification treatment of radioactive waste, and cannot realize other advanced solidification treatment technologies such as radioactive waste glass solidification.
[0004] Another technology provides a radioactive waste treatment system and a treatment method thereof. The treatment system includes a fixed bed gasification furnace, a fine ash separation device, a second combustion chamber, a quenching tower and a purification system connected in sequence. By combining the fixed bed gasification technology with the steam reforming technology, it can treat waste resin, dry active waste, clothing, chemical waste liquid, waste oil and sludge, etc., and can significantly reduce the volume of radioactive waste and stabilize the nuclides. However, this method has the following main problems: ① It is impossible to treat radioactive waste metals, filter elements, waste glass, concrete, insulation materials and other wastes; ② The solidified bed gasification furnace used is a refractory brick fixed gasification furnace. The refractory material has high requirements for temperature control, is easily damaged under extremely cold and hot conditions, is greatly corroded by waste, and has a short lifespan.
[0005] Another technology provides a plasma low-medium radioactive solid waste treatment method, including: classifying radioactive solid waste, placing different types of solid waste in different waste barrels according to categories, and measuring; adding additives of corresponding formulas to the above-measured wastes according to categories, crushing the whole barrel, and transporting them to the plasma melting furnace for melting treatment; discharging the molten material discharged from the melting furnace into a receiving container, and when the receiving container is full, transferring it to the insulation annealing station for insulation, annealing, and slow cooling to form a glass solid body with uniform texture; transporting the receiving container after solidification to the dose detection station for radioactive dose detection and transportation and storage. Through this invention, a glass solid body with uniform texture and good performance can be formed, and the processing efficiency can be improved. However, this invention also has certain shortcomings, mainly including: ① It is impossible to treat non-combustible radioactive wastes such as scrap metal, sludge, concentrate, concrete, and waste glass, and the scope of radioactive waste treatment is limited; ② Scrap metal and sludge are directly barreled and fixed for treatment and storage, which on the one hand causes waste of metal resources, and on the other hand increases the cost of geological disposal.
[0006] In order to ensure the sustainable development of the nuclear industry, it is necessary to propose a solidification treatment method with a wide range of applications and good solidification and volume reduction effects. Summary of the invention
[0007] Based on this, it is necessary to provide a synergistic solidification treatment method for radioactive waste with a wide range of applications and good solidification and volume reduction effects.
[0008] The present invention is achieved through the following technical solutions.
[0009] The present invention provides a method for synergistic solidification treatment of radioactive waste, comprising the following steps:
[0010] Classify the radioactive waste to be treated into combustible waste, non-combustible metallic waste and non-combustible non-metallic waste;
[0011] The non-combustible metal waste is subjected to smelting and decontamination treatment to obtain smelting residue containing radioactive nuclides and usable metals without radioactive nuclides;
[0012] Obtaining waste having glass additive function from the non-combustible non-metallic waste as a waste additive; and
[0013] The smelting residue, the combustible waste and one or more of the waste additives are mixed with a glass additive to form radioactive mixed waste, which is then melt-solidified.
[0014] In some embodiments, the collaborative curing process further comprises the following steps:
[0015] calcining the combustible waste to obtain a calcined product;
[0016] Wherein, the combustible waste in the melt solidification process is added in the form of the calcined product.
[0017] In some of the embodiments, the melt solidification treatment includes a melt treatment and a heat treatment performed in sequence, and the heat treatment is a heat preservation annealing treatment or a nucleation crystallization treatment; the heating melting temperature of the melt treatment is controlled at 1000-1800°C.
[0018] In some of the embodiments, the smelting decontamination treatment and the melting treatment are both performed by induction heating.
[0019] In some of the embodiments, the melt solidification treatment is a glass solidification process, and the heat treatment is a thermal insulation annealing treatment; the heating melting temperature in the melt treatment is controlled at 1000-1500°C, and the time is 0.5-5h; the temperature of the thermal insulation annealing treatment is 300-600°C, and the time is 0.5-3h.
[0020] In some of the embodiments, the melt solidification treatment is a glass ceramic solidification process, and the heat treatment is a nucleation crystallization treatment; the heating melting temperature in the melt treatment is controlled at 1300-1800°C, and the time is 0.5-5h; the nucleation crystallization treatment is: first nucleation treatment at 500-1000°C for 0.5-2h, and then crystallization treatment at 1000-1200°C for 0.5-3h.
[0021] In some of the embodiments, a decontamination additive is further added during the smelting decontamination treatment step.
[0022] In some embodiments, the step of obtaining the waste having glass additive function from the non-combustible non-metallic waste comprises the following steps:
[0023] Analyzing the content of characteristic elements in each of the non-combustible non-metallic wastes, wherein the characteristic elements are the same elements as those in the glass additive composition;
[0024] If the total content of the characteristic elements of the non-combustible non-metallic waste is within a preset range, the non-combustible non-metallic waste is waste having the function of a glass additive.
[0025] In some embodiments, the combustible waste includes at least one of absorbent paper, wood products, cotton fabrics, plastic products, rubber products, non-metallic parts in filter elements, and non-metallic parts in waste resin components;
[0026] The non-combustible non-metallic waste includes at least one of concentrate, insulation material, concrete, soil, sludge and waste glass.
[0027] In some embodiments, if the radioactive waste to be treated is at least one of a filter element and a waste resin group, the collaborative solidification treatment method further comprises the following steps:
[0028] Dismantling and crushing the radioactive waste to be treated to obtain scrap metal parts and non-metal parts, which are classified into non-combustible metal waste and non-combustible non-metal waste respectively; and / or
[0029] The glass additive added to the radioactive mixed waste is 5wt% to 65wt%.
[0030] The above-mentioned synergistic solidification treatment method of radioactive waste is applicable to the treatment of almost all wastes generated by nuclear facilities, including combustible waste, non-combustible metal waste and non-combustible non-metallic waste. The waste treatment range is wide, and it is classified into three categories of combustible waste, non-combustible metal waste and non-combustible non-metallic waste for synergistic solidification treatment; then make full use of the characteristics of non-combustible metal waste and non-combustible non-metallic waste, smelt and decontaminate the non-combustible metal waste, obtain smelting residue containing radioactive nuclides and usable metal without radioactive nuclides, realize high-temperature decontamination of waste metal and recycling of usable metal without radioactive nuclides, and use the waste with glass additive function in the non-combustible non-metallic waste as waste additive. Combustible waste can be directly used as raw material for melt solidification treatment, or it can be first calcined and added in the form of calcined products. Finally, the smelting residue, combustible waste or its calcined products, one or more of the waste additives and the glass additive are mixed for melt solidification treatment. In this way, waste volume reduction can be effectively achieved, and the solidified body obtained by melt solidification treatment can be directly disposed of geologically, with the advantages of good solidification effect and efficient volume reduction.
[0031] The synergistic solidification treatment method of radioactive waste of the present invention can be applied to the treatment of almost all wastes generated by nuclear facilities, and fully utilizes the composition characteristics of different wastes such as combustible waste, non-combustible metal waste and non-combustible non-metallic waste, and comprehensively synergistically solidifies them, so that the waste can serve as a waste additive (i.e., glass additive) as much as possible, so that only a small amount of glass additive needs to be added, and then the melting solidification treatment of the waste can be completed by adding a very small amount of additives, so as to achieve the purpose of making the best use of resources and "treating waste with waste" on the basis of realizing waste stabilization treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A flow chart of a method for co-solidification of radioactive waste according to an embodiment of the present invention;
[0033] Figure 2 A flow chart of a method for co-solidification of radioactive waste according to another embodiment of the present invention;
[0034] Figure 3 Schematic diagram of the process flow of the synergistic solidification treatment method for radioactive waste of Examples 1 to 2. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0037] In the description of the present invention, “plurality” means two or more than two, unless otherwise clearly and specifically defined.
[0038] See also Figure 1 The present invention provides a method for collaborative solidification treatment of radioactive waste, comprising the following steps S10 to S40.
[0039] Step S10: Classify the radioactive waste to be processed into combustible waste, non-combustible metal waste and non-combustible non-metal waste.
[0040] Step S20: The non-combustible metal waste is subjected to a smelting and decontamination treatment to obtain a smelting residue containing radioactive nuclides and a usable metal without radioactive nuclides.
[0041] Step S30: obtaining waste with glass additive function from incombustible non-metallic waste as a waste additive.
[0042] Step S40: mixing one or more of the smelting residue, combustible waste, waste additives and glass additives to form radioactive mixed waste, and then performing a melting and solidification process.
[0043] See also Figure 2 In other embodiments, the above-mentioned radioactive waste synergistic solidification treatment method further includes the following step S50: calcining the combustible waste to obtain a calcined product. Accordingly, the combustible waste in the original step S40 of melt solidification treatment is added in the form of a calcined product. That is, the original step S40 is the following step S60: mixing the smelting residue, the calcined product, the waste additive and the glass additive to form a radioactive mixed waste, and then performing a melt solidification treatment.
[0044] In other words, in this embodiment, step S50 can be performed before step S60; there is no particular order between step S50 and step S20 and step S30, and they can be performed one after the other or simultaneously.
[0045] Furthermore, the calcination temperature is 700-1000°C.
[0046] Among them, combustible waste includes but is not limited to at least one of absorbent paper contaminated with radionuclides, wood products, cotton fabrics, plastic products, rubber products, non-metallic parts in filter elements and non-metallic parts in waste resin components.
[0047] Among them, non-combustible non-metallic waste includes but is not limited to at least one of concentrates contaminated by radionuclides, insulation materials, concrete, soil, silt and waste glass.
[0048] The non-combustible metal waste includes but is not limited to at least one of scrap metal, metal parts in filter elements and metal parts in waste resin components.
[0049] The above-mentioned synergistic solidification treatment method of radioactive waste is applicable to the treatment of almost all wastes generated by nuclear facilities, including combustible waste, non-combustible metal waste and non-combustible non-metallic waste. The waste treatment range is wide, and it is classified into three categories of combustible waste, non-combustible metal waste and non-combustible non-metallic waste for synergistic solidification treatment; then make full use of the characteristics of non-combustible metal waste and non-combustible non-metallic waste, smelt and decontaminate the non-combustible metal waste, obtain smelting residue containing radioactive nuclides and usable metal without radioactive nuclides, realize high-temperature decontamination of waste metal and recycling of usable metal without radioactive nuclides, and use the waste with glass additive function in the non-combustible non-metallic waste as waste additive. Combustible waste can be directly used as raw material for melt solidification treatment, or it can be first calcined and added in the form of calcined products. Finally, the smelting residue, combustible waste or its calcined products, one or more of the waste additives and the glass additive are mixed for melt solidification treatment. In this way, waste volume reduction can be effectively achieved, and the solidified body obtained by melt solidification treatment can be directly disposed of geologically, with the advantages of good solidification effect and efficient volume reduction.
[0050] The synergistic solidification treatment method of radioactive waste of the present invention can be applied to the treatment of almost all wastes generated by nuclear facilities, and fully utilizes the composition characteristics of different wastes such as combustible waste, non-combustible metal waste and non-combustible non-metallic waste, and comprehensively synergistically solidifies them, so that the waste can serve as a waste additive (i.e., glass additive) as much as possible, so that only a small amount of glass additive needs to be added, and then the melting solidification treatment of the waste can be completed by adding a very small amount of additives, so as to achieve the purpose of making the best use of resources and "treating waste with waste" on the basis of realizing waste stabilization treatment.
[0051] It can be understood that in one embodiment, smelting residue, combustible waste or its calcined product, waste additives and glass additives are mixed and melt-solidified.
[0052] In some embodiments, the melt solidification process includes a melt process and a heat treatment performed sequentially, and the heat treatment is a heat preservation annealing process or a nucleation crystallization process.
[0053] Furthermore, the heating melting temperature of the melting treatment is controlled at 1000-1800°C.
[0054] Furthermore, both the smelting decontamination treatment and the melting treatment are carried out by induction heating.
[0055] Furthermore, the melting process is carried out in a melting furnace, and the above-mentioned induction heating is achieved by an induction heating device. Furthermore, a segmented induction heating device is arranged on the outside of the melting furnace so that the melting furnace can achieve segmented induction heating. The segmented induction heating device includes a plurality of induction coils, which are sequentially arranged in the axial direction of the melting furnace. Specifically, at least one segment of the induction coil is located at the top, middle and bottom of the melting furnace, respectively, and each segment of the induction coil is independently controlled by its own induction power supply, thereby achieving segmented induction heating control of materials at different positions in the melting furnace. In the melting stage of the melting process, a segmented induction heating device is used to achieve layered induction heating of the waste melt in the melting furnace, maintain a cold cap at the top of the melting furnace, and maintain a lower temperature furnace bottom melt at the bottom of the melting furnace, so as to meet the requirements of the glass solidification process or the glass ceramic solidification process, and control the radioactive mixed waste within a reasonable temperature range to complete the melting process.
[0056] In this way, the radioactive waste can be melted into a uniform molten body through induction heating technology, and the radioactive nuclides can be fully solidified at the atomic level through further heat preservation annealing or nucleation crystallization treatment to obtain a solid body.
[0057] It can be understood that, generally, the melting process includes a feeding melting stage, a heating melting stage, a discharging stage and a furnace bottom cooling stage, wherein the heating melting stage is the most critical and important stage.
[0058] In some of the embodiments, the melt solidification treatment is a glass solidification process, and the heat treatment is a thermal insulation annealing treatment; the heating melting temperature in the melt treatment is controlled at 1000-1500°C, and the time is 0.5-5h; the temperature of the thermal insulation annealing treatment is 300-600°C, and the time is 0.5-3h.
[0059] In some of the embodiments, the melt solidification treatment is a glass ceramic solidification process, and the heat treatment is a nucleation crystallization treatment; the heating melting temperature in the melt treatment is controlled at 1300-1800°C, and the time is 0.5-5h; the nucleation crystallization treatment is: first nucleation treatment at 500-1000°C for 0.5-2h, and then crystallization treatment at 1000-1200°C for 0.5-3h.
[0060] Preferably, the melting solidification method is mainly determined by the content of transuranic nuclides in the waste. Compared with glass solidification, glass ceramic solidification has a larger capacity for transuranic nuclides and better chemical stability. Therefore, when the content of transuranic nuclides is high, such as exceeding the preset value, it is recommended to use the glass ceramic solidification method. When there is no or only a small amount of transuranic nuclides, such as not more than the preset value, it is recommended to use the glass solidification method for waste treatment, which is relatively simpler.
[0061] In some embodiments, a decontamination additive is also added in the step of smelting decontamination treatment. Further, in actual operation, the glass additive in the above step S40 and the decontamination additive in the step of smelting decontamination treatment can be derived from the same additive feeding system.
[0062] In some embodiments, the step S30 of obtaining waste having glass additive function from incombustible non-metallic waste includes the following steps S31-S32.
[0063] Step S31: analyzing the content of characteristic elements of each non-combustible non-metallic waste, wherein the characteristic elements are the same elements as those in the glass additive composition.
[0064] Further, the elements in the glass additive include at least one of B, Si, Al, Na, Fe, and P. The characteristic element is at least one of B, Si, Al, Na, Fe, and P. Further, the characteristic element is at least one of B, Si, Al, and Na.
[0065] Step S32: If the total content of characteristic elements of the non-combustible non-metallic waste is within a preset range, the non-combustible non-metallic waste is waste having glass additive function.
[0066] In a specific example, if the total content of characteristic elements of the non-combustible non-metallic waste is not less than 40 wt %, then the non-combustible non-metallic waste is waste having glass additive function.
[0067] It is understandable that the preset range is not fixed and can be set as needed, such as not less than 30wt%, not less than 45wt%, not less than 50wt%, preferably not less than 40wt%. The main consideration is to be able to make comprehensive and synergistic use of the waste in the non-combustible non-metallic waste as much as possible. Then, according to the actual situation, the amount of glass additive that needs to be added is calculated. In this way, the radioactive waste rich in glass additive components in the non-combustible non-metallic waste is used as a glass additive, and only a small amount of glass additive is evenly added on this basis.
[0068] The mixing scheme of radioactive waste mainly considers that the main components and proportions of various wastes such as smelting residues, combustible wastes or their calcination products, and waste additives can complement each other, so that the main components and proportions of the composed radioactive mixed wastes can meet or nearly meet the glass formation zone range of a common glass system phase diagram.
[0069] The composition of the above-mentioned additional glass additives is mainly determined based on the difference in composition between the radioactive mixed waste and the glass forming area, as well as the difference in composition between the radioactive mixed waste and the glass system commonly used for key nuclides such as volatile nuclides, yellowish phase nuclides, easily deposited nuclides, and major radioactive nuclides in the radioactive mixed waste.
[0070] In some embodiments, the glass additives added to the radioactive mixed waste are 5wt% to 65wt%, and accordingly, the total content of the smelting residue, the combustible waste or its calcined product, and the waste additives is 35wt% to 95wt%. In a specific example, the total amount of the glass additives, the smelting residue, the combustible waste or its calcined product, and the waste additives added is 100%.
[0071] In some embodiments, if the radioactive waste to be treated is at least one of a filter element and a waste resin group, the above-mentioned collaborative solidification treatment method further comprises the following steps: dismantling and crushing the radioactive waste to be treated to obtain scrap metal parts and non-metal parts, and classifying them into non-combustible metal waste and non-combustible non-metal waste respectively.
[0072] In some of the embodiments, the step S10 of classifying the radioactive waste to be treated into combustible waste, non-combustible metal waste and non-combustible non-metallic waste includes the following steps: selectively crushing and classifying the waste for temporary storage according to the type and form of the waste, and then analyzing the composition, characteristics and storage capacity of the classified waste through various pretreatment systems; and entering information such as the composition characteristics, waste content and storage capacity of the waste into the compatibility data analysis system.
[0073] In the subsequent step S30, waste with glass additive function in the non-combustible non-metallic waste can be obtained as a waste additive through the compatibility data analysis system. The composition and melting solidification treatment method of the radioactive mixed waste in the subsequent step S40 or step S60 can be obtained through manual compatibility data analysis or through the compatibility data analysis system according to the waste component characteristics, waste content and storage capacity.
[0074] The compatibility data analysis is based on the characteristics, composition and storage volume of the radioactive waste to be treated this time and the various types of waste that actually need to be treated in the waste repository. The characteristics and composition include information such as the composition of each element and its proportion, physical and chemical properties, form, and whether it can be calcined to reduce volume. In this way, a compatibility scheme recommendation is obtained that maximizes the waste package capacity of the radioactive waste to be treated this time, has excellent solidification performance, and is economical. The compatibility scheme (i.e., waste compatibility data) is recommended to include information such as radioactive mixed waste scheme, glass additive composition, and treatment process. Among them, the radioactive mixed waste scheme includes information such as the composition of radioactive mixed waste and the proportion of various types of waste.
[0075] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments.
[0076] Example 1
[0077] The invention provides a method for co-solidification treatment of radioactive waste.
[0078] A method for the coordinated solidification treatment of radioactive waste utilizes the characteristics of various waste components to carry out mixed solidification treatment of different wastes in order to achieve the purpose of improving the waste containment rate, making the best use of waste, and treating waste with waste. Atomic solidification methods such as glass solidification and glass-ceramic solidification are used to achieve more stable solidification of radioactive nuclides at the atomic level.
[0079] The radioactive waste to be treated includes absorbent paper, wood and other wooden products, cotton fabrics, plastic products, rubber products contaminated with radionuclides, concentrated liquid, insulation materials, concrete, soil, silt, waste glass, waste metal, as well as filter cores and waste resin components contaminated with radionuclides.
[0080] The radioactive waste collaborative solidification treatment method mainly includes the following steps:
[0081] Selectively crush and classify radioactive waste for temporary storage according to its type and form.
[0082] Specifically, the filter element and the waste resin assembly are divided into waste metal parts and non-metal parts through disassembly. The waste metal parts are classified as non-combustible wastes, and the non-metal parts are classified as combustible wastes, so as to facilitate subsequent pre-processing and other operations.
[0083] Absorbent paper, wood and other wooden products, cotton fabrics, plastic products, and rubber products contaminated with radioactive nuclides are classified as combustible waste.
[0084] Concentrated liquids, insulation materials, concrete, soil, sludge, waste glass, and waste metal contaminated with radionuclides are classified as non-combustible wastes.
[0085] Among them, non-combustible waste is further classified into non-combustible metal waste and non-combustible non-metal waste according to whether it is metal material. Concentrated liquid, insulation materials, concrete, soil, sludge, and waste glass contaminated by radioactive nuclides are non-combustible non-metal wastes, and the scrap metal, filter cores, and scrap metal parts of the dismantled waste resin components are all classified as non-combustible metal wastes. In this way, the radioactive waste to be treated is classified into combustible waste, non-combustible metal waste, and non-combustible non-metal waste.
[0086] Analyze the composition and characteristics of each waste, and enter the information such as waste composition characteristics and waste content into the compatibility data analysis system.
[0087] Specifically, the compatibility data analysis system gives compatibility suggestions based on the storage volume and composition characteristics of the various types of waste that need to be treated, with maximum waste package capacity, excellent solidification performance, and good economic efficiency. The compatibility suggestions include information such as the composition of radioactive mixed waste, the composition of glass additives, and the solidification method (glass solidification, glass ceramic solidification).
[0088] In addition to scrap metal, other non-combustible wastes, such as concentrates, insulation materials, concrete, soil, sludge, waste glass, etc., are rich in the main components of glass additives such as B, Si, Al, and Na, and can be considered as radioactive wastes rich in glass additive components. Therefore, obtaining radioactive wastes rich in glass additive components from non-combustible non-metallic wastes is waste with glass additive functions, which is used as a waste additive. In a specific example, the total content of characteristic elements (B, Si, Al, Na) of each non-combustible non-metallic waste is analyzed. If the total content is ≥40wt%, it is used as a waste additive.
[0089] According to the recommended mixing scheme, carry out waste solidification treatment operations. The main steps are as follows:
[0090] The disassembled scrap metal parts and scrap metal are put into the pretreatment system 1 together, and then enter the melting system 1 through the feeding system 1, and the decontamination additive is added to the melting system 1 for smelting and decontamination treatment, and the non-radioactive usable metal and the smelting residue with radioactive nuclides are formed by induction heating smelting. The smelting residue enters the melting system 2 through the smelting residue transfer system.
[0091] The disassembled non-metallic parts and combustible wastes such as absorbent paper, wood, cotton fabrics, plastic products, rubber products, etc. enter the pretreatment system 2, and then enter the calcination system through the feeding system 2, and complete the calcination treatment (or inorganic treatment) in a high temperature environment of 700-1000℃. The calcined products produced after the inorganic treatment are then sent to the melting system 2 through the calcined product transfer system. Figure 3 As shown in method 1.
[0092] Other non-combustible wastes except scrap metal, including concentrate, insulation materials, concrete, soil, sludge, waste glass, scrap metal, etc., rich in main glass additive components such as B, Si, Al, Na, and the total content of B, Si, Al, Na ≥ 40wt%, are considered to be radioactive wastes rich in glass additive components and are used as waste additives. According to the actual waste types, components and proportions to be treated and the requirements of the solidification formula component range, select part or all of them for compatibility and mixing, enter the pretreatment system 3 as a waste additive, and then enter the melting system 2 through the feeding system 3.
[0093] In summary, the smelting residue, calcined product and waste additives all enter the melting system 2; further, it also includes an additive feeding system for adding glass additives and decontamination additives, which is used to add the required glass additives to the melting system 2 and to add decontamination additives for participating in metal smelting decontamination to the melting system 1. The smelting residue, calcined product, waste additives and glass additives are mixed to form radioactive mixed waste. According to the composition of the radioactive mixed waste, the total content of the smelting residue, calcined product and waste additives is controlled to be 35wt% to 95wt%, and the glass additive accounts for 5wt% to 65wt%, and the total of the two is 100wt%.
[0094] Melting system 2 uses induction heating. During the furnace startup phase, the radioactive waste is isolated from the inner wall of the furnace by using a non-condensed shell. During the melting phase, a segmented induction heating device is used to achieve layered induction heating of the waste melt in the furnace. A cold cap is maintained at the top of the melting furnace and a relatively low temperature melt is maintained at the bottom of the melting furnace, thereby meeting the requirements of advanced glass solidification technology or glass-ceramic solidification technology, and the radioactive mixed waste formula mixture is controlled within a reasonable temperature range to complete the melting process.
[0095] According to the recommendations of the compatibility scheme, if the glass solidification treatment scheme is selected, Figure 3 As shown in method 1, the melting temperature of the melting system 2 is controlled at 1000-1500°C by induction heating technology, and the radioactive mixed waste formula mixture is melted in a melting furnace for 0.5-5 hours to obtain a glass melt. The glass melt enters a heat preservation annealing system through a discharging system. The glass melt is kept at 300-600°C for 0.5-3 hours and then annealed to form a glass solid body.
[0096] Or, according to the compatibility scheme, if the glass ceramic curing treatment scheme is selected, Figure 3 As shown in method 2, the heating melting temperature of the melting system 2 is controlled at 1300-1800°C by induction heating technology, and the radioactive mixed waste formula mixture is melted in a melting furnace for 0.5-5h to obtain a glass melt. The formed glass melt enters the nucleation crystallization system through a discharge system, is nucleated at 500-1000°C for 0.5-2h and crystallized at 1000-1200°C for 0.5-3h to form a glass ceramic solid body.
[0097] The produced glass solid body or glass ceramic solid body is stored and transported or directly disposed of near the geological environment with the packaging container.
[0098] Example 2
[0099] The invention provides a method for co-solidification treatment of radioactive waste.
[0100] It is basically the same as Example 1, except that:
[0101] The compatibility recommendations obtained by the manual calculation by engineers without using the compatibility data analysis system are basically the same, with the only difference being that the disassembled non-metallic parts and combustible wastes such as absorbent paper, wood, cotton fabrics, plastic products, and rubber products enter the pretreatment system 2, and then directly enter the melting system 2 instead of the calcination system via the feeding system 2, such as Figure 3 As shown in method 2.
[0102] In summary, the smelting residue, combustible waste and waste additives all enter the melting system 2; further, it also includes an additive feeding system for adding glass additives and decontamination additives, which is used to add the required glass additives to the melting system 2 and to add decontamination additives for participating in metal smelting decontamination to the melting system 1. The smelting residue, combustible waste, waste additives and glass additives are mixed to form radioactive mixed waste. According to the composition of the radioactive mixed waste, the total content of the smelting residue, combustible waste and waste additives is controlled to be 35wt% to 95wt%, and the glass additive accounts for 5wt% to 65wt%, and the two together are 100wt%.
[0103] In Examples 1 to 2, the required pretreatment system, feeding system, and transfer system can be partially or completely combined according to actual conditions; non-combustible metal waste and non-combustible non-metal waste can be melted in different melting systems at the same time, or they can be melted in different batches through one melting system. That is, in the first case, there are melting systems 1 and 2, which are respectively used for melting non-combustible metal waste and melting non-combustible non-metal waste. In this case, non-combustible metal waste and non-combustible non-metal waste can be melted at the same time; in the second case, different melting periods of the same melting system, such as melting period 1 and melting period 2, are used for melting non-combustible metal waste in melting period 1, and in melting period 2, they are used for melting non-combustible non-metal waste; the melting system has the dual functions of inorganic treatment and melting treatment. The calcination system and the supporting transfer system as waste inorganic treatment devices can improve the melting efficiency and energy utilization rate, and can be set up or directly abandoned according to specific considerations such as actual needs and economy.
[0104] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0105] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A method for the synergistic solidification treatment of radioactive waste, characterized in that: The steps include: Classify the radioactive waste to be treated into combustible waste, non-combustible metallic waste and non-combustible non-metallic waste; The non-combustible metal waste is subjected to smelting and decontamination treatment to obtain smelting residue containing radioactive nuclides and usable metals without radioactive nuclides; Obtaining waste having glass additive function from the non-combustible non-metallic waste as a waste additive; and The smelting residue, the combustible waste and one or more of the waste additives and a glass additive are mixed to form radioactive mixed waste, and then melt-solidified; The step of obtaining the waste having the function of glass additive from the non-combustible non-metallic waste comprises the following steps: Analyzing the content of characteristic elements in each of the non-combustible non-metallic wastes, wherein the characteristic elements are the same elements as those in the glass additive composition; If the total content of the characteristic elements of the non-combustible non-metallic waste is within a preset range, the non-combustible non-metallic waste is waste having the function of a glass additive.
2. The collaborative solidification treatment method according to claim 1, characterized in that: The collaborative solidification treatment method further comprises the following steps: calcining the combustible waste to obtain a calcined product; Wherein, the combustible waste in the melt solidification process is added in the form of the calcined product.
3. The collaborative solidification treatment method according to any one of claims 1 to 2, characterized in that: The melt solidification treatment includes a melt treatment and a heat treatment performed in sequence, wherein the heat treatment is a heat preservation annealing treatment or a nucleation crystallization treatment; and the heating melting temperature of the melt treatment is controlled at 1000-1800°C.
4. The collaborative solidification treatment method according to claim 3, characterized in that: The smelting decontamination treatment and the melting treatment are both performed by induction heating.
5. The collaborative solidification treatment method according to claim 3, characterized in that: The melt solidification treatment is a glass solidification process, and the heat treatment is a heat preservation annealing treatment; the heating melting temperature in the melt treatment is controlled at 1000-1500°C for 0.5-5h; the temperature of the heat preservation annealing treatment is 300-600°C for 0.5-3h.
6. The collaborative solidification treatment method according to claim 3, characterized in that: The melt solidification treatment is a glass ceramic solidification process, and the heat treatment is a nucleation crystallization treatment; the heating melting temperature in the melt treatment is controlled at 1300-1800°C, and the time is 0.5-5h; the nucleation crystallization treatment is: first nucleation treatment at 500-1000°C for 0.5-2h, and then crystallization treatment at 1000-1200°C for 0.5-3h.
7. The collaborative solidification treatment method according to any one of claims 1 to 2, characterized in that: A decontamination additive is also added in the smelting decontamination treatment step.
8. The collaborative solidification treatment method according to any one of claims 1 to 2, characterized in that: The combustible waste includes at least one of absorbent paper, wood products, cotton fabrics, plastic products, rubber products, non-metallic parts in filter elements, and non-metallic parts in waste resin components; The non-combustible non-metallic waste includes at least one of concentrate, insulation material, concrete, soil, sludge and waste glass.
9. The collaborative solidification treatment method according to any one of claims 1 to 2, characterized in that: If the radioactive waste to be treated is at least one of a filter element and a waste resin group, the collaborative solidification treatment method further comprises the following steps: The radioactive waste to be treated is disassembled and crushed to obtain scrap metal parts and non-metal parts, which are respectively classified into incombustible metal waste and incombustible non-metal waste.
10. The collaborative solidification treatment method according to any one of claims 1 to 2, characterized in that: The glass additive added to the radioactive mixed waste is 5wt% to 65wt%.