A method for synthesizing bone-shaped gold nanorods
By using CTAC and oleamine as bisurfactants and 1,2,4 trihydroxybenzene as reducing agents, the problems of high reactants, high cost and low purity in the synthesis of existing gold nanorods were solved, and high Purity and high yield of bone-shaped gold nanorods, suitable for a wide range of applications in the medical field.
Patent Information
- Application Number
- CN202111401927.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-11-19
AI Technical Summary
In the existing gold nanorod synthesis methods, the reactants are large, the cost is high, the purity is low, and the size and dispersion of the gold nanorods are poor, which limits the prospects for their industrial applications.
Using CTAC and oleamine as bisurfactants and 1,2,4 trihydroxybenzene as reducing agents, bone-shaped gold nanorods were synthesized by seed-mediated method, and the reaction conditions were controlled to improve purity and yield. CTAC and oil were used. As a bisurfactant, amines use 1,2,4 trihydroxybenzene as reducing agents to adjust pH and temperature, reduce the amount of reactants, and reduce costs.
It has achieved high purity, high yield and good dispersion of gold nanorods. It is suitable as a self-assembly material for gold nanorods and is suitable for a wide range of applications in the medical field.
Smart Images

Figure CN114192794B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal nano material synthesis, in particular to a method for synthesizing gold nanorods. Background Art
[0002] In recent years, the research in the field of precious metal nanoparticles has entered the field of vision of researchers. Gold nanorods, due to their unique one-dimensional nanostructure, can display size- and shape-dependent localized surface plasmon resonances (LSPRs). Therefore, they have attracted widespread attention and have broad application prospects in electronics, optics, catalysis, diagnostics or treatment.
[0003] Therefore, the industrialization of the synthesis of gold nanorods has become one of the key research directions of researchers.
[0004] For example, the Chinese patent with application publication number CN112974829A and application publication date June 18, 2021 discloses a method for preparing gold nanorod materials by reducing hydroquinone under dual surfactants. Under the joint action of hexadecyltrimethylammonium bromide (CTAB) and sodium oleate (NaOL), the seed-mediated method is used to synthesize gold nanorods, including the following steps: a certain amount of CTAB and chloroauric acid (HAuCl4) are mixed in a bottle, and sodium borohydride (NaBH4) prepared by ice-water mixture is added. After vigorous stirring with a magnetic stirrer for 2 minutes, the solution changes from golden yellow to brown yellow. Let it stand for 30 minutes, which is the seed solution; dissolve the corresponding low concentration of CTAB and NaOL in another bottle at 50°C as the growth solution, cool to about 30°C, and then add silver nitrate (AgNO3) and chloroauric acid. After stirring at room temperature for 60-90 minutes, the solution changes from golden yellow to clear; hydroquinone and seed solution are added in sequence. The mixture was stirred vigorously with a magnetic stirrer and then allowed to stand at a constant temperature of 30°C for 12 hours to obtain the final product. In the synthesis method, NaOL and CTAB are used together as surfactants, and the purity of the gold nanorods is reduced due to the reaction of the carboxyl group in NaOL with the hydroxyl group in the phenolic substance. Summary of the invention
[0005] The present invention aims to solve the above-mentioned technical problems existing in the prior art gold nanorod synthesis method, and provides a method for synthesizing bone-shaped gold nanorods with a small amount of required reactants, low cost, easy control of reaction conditions, longer gold nanorod size, good dispersibility, high purity and high yield.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme: A method for synthesizing a rod-shaped gold nanorod of the present invention comprises the following steps:
[0007] (1) Preparation of seed solution
[0008] After mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, add 0.6 mL of 0.01 M NaBH4 solution, stir and let stand at a constant temperature to obtain a seed solution.
[0009] (2) Preparation of growth solution
[0010] Dissolve 10 mL of 0.1 M CTAC solution and 0.054 g of oleylamine in 8.4 mL of water, add 40 μL of 0.1 M AgNO3 solution, let stand at a constant temperature, then add 1 mL of 10 mM HAuCl4, stir and let stand at a constant temperature until the solution becomes clear; adjust the pH to 1.7, add 1.6 mL of 0.1 M 1,2,4-trihydroxybenzene, let stand at a constant temperature to obtain a growth solution.
[0011] (3) Growth of bone-like gold nanorods
[0012] Take 32 μL of seed solution and add it to the growth solution, keep it at a constant temperature, and remove the supernatant by centrifugation. The centrifugal product is the rod-shaped gold nanorods.
[0013] Preferably, in step (1), the NaBH4 solution is prepared by the following method: mixing an ice-water mixture with a required amount of NaBH4.
[0014] Preferably, in step (1), the stirring conditions are: a rotation speed of 1500 rpm, and a stirring time of 1 to 2 min; and the constant temperature standing conditions are: heating in a water bath at 30° C. and standing for 30 min.
[0015] Preferably, in step (2), 10 mL of 0.1 M CTAC solution and 0.054 g of oleylamine are dissolved in water at 50° C., and the temperature is lowered to 30° C. after dissolution.
[0016] Preferably, in step (2), the pH is adjusted to 1.7 using 5 M H2SO4.
[0017] Preferably, in step (2), the stirring conditions are: a rotation speed of 1500 rpm, and a stirring time of 1 to 2 min; and the constant temperature standing conditions are: heating in a water bath at 30° C. and standing for 30 min.
[0018] Preferably, in step (3), the constant temperature static condition is: heating in a water bath at 30° C. and static for 3 hours. Heating in a water bath at 30° C. can greatly improve the purity of the gold nanorods and ensure a higher final yield.
[0019] Therefore, the present invention has the following beneficial effects: CTAC and oleylamine are used as dual surfactants, 1,2,4-trihydroxybenzene is used as a reducing agent, a small amount of reactants is required, the cost is low, the reaction rate is extremely high, the reaction conditions are easy to control, the obtained gold nanorods have good dispersibility, a long size, large ends and a small middle, and a rod-like shape, which is more suitable as a material for self-assembly of gold nanorods, and has broader application prospects in the medical field. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a transmission electron microscope image of the gold nanorod material obtained in Example 1. DETAILED DESCRIPTION
[0021] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0022] Example 1
[0023] (1) Preparation of seed solution
[0024] After mixing 10mL of 0.1M CTAB solution and 0.25mL of 10mM HAuCl4 solution, add 0.6mL of 0.01M NaBH4 solution, stir and let stand at a constant temperature. The stirring conditions are: rotation speed of 1500rpm and stirring time of 2min. The constant temperature standing conditions are: heating in a water bath at 30°C and standing for 30min to obtain a seed solution. The NaBH4 solution is prepared by the following method: mixing an ice-water mixture with a required amount of NaBH4.
[0025] (2) Preparation of growth solution
[0026] Dissolve 10mL of 0.1M CTAC solution and 0.054g of oleylamine in 8.4mL of water at 50℃, cool to 30℃ after dissolution, add 40μL of 0.1M AgNO3 solution, let it stand at a constant temperature, then add 1mL of 10mM HAuCl4, stir and let it stand at a constant temperature until the solution becomes clear; adjust the pH to 1.7 with 5M H2SO4, add 1.6mL of 0.1M 1,2,4-trihydroxybenzene, let it stand at a constant temperature to obtain a growth solution; the stirring conditions are: the rotation speed is 1500rpm, and the stirring time is 2min; the constant temperature standing conditions are: heating in a water bath at 30℃ and standing for 30min.
[0027] (3) Rod-like gold nanorods
[0028] Take 32 μL of seed solution and add it to the growth solution, and let it stand at a constant temperature. The constant temperature and standing conditions are: heating in a water bath at 30°C, standing for 3 hours, and centrifuging to remove the supernatant. The centrifugal product is the bone-shaped gold nanorods.
[0029] The transmission electron microscopy image of the obtained rod-shaped gold nanorods is shown in Figure 1 shown.
[0030] from Figure 1 It can be seen that the length of the obtained gold nanorods is about 121.4nm, the diameter in the middle of the rod is about 21.2nm, the diameter at the head of the rod is about 28.4nm, the aspect ratio is about 5.7, the two ends are large and the middle is small, and it is in the shape of a rod bone. The gold nanorods are relatively long and have good monodispersity.
[0031] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.
Claims
1. A method for synthesizing rod-shaped gold nanorods, characterized in that: The following steps are involved: (1) Preparation of seed solution After mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, add 0.6 mL of 0.01 M NaBH4 solution, stir and let stand at a constant temperature to obtain a seed solution; (2) Preparation of growth solution Dissolve 10 mL of 0.1 M CTAC solution and 0.054 g of oleylamine in 8.4 mL of water, add 40 μL of 0.1 M AgNO3 solution, let stand at a constant temperature, then add 1 mL of 10 mM HAuCl4, stir and let stand at a constant temperature until the solution becomes clear; adjust the pH to 1.7, add 1.6 mL of 0.1 M 1,2,4-trihydroxybenzene, let stand at a constant temperature to obtain a growth solution; (3) Generation of rod-shaped gold nanorods Take 32 μL of seed solution and add it to the growth solution, keep it at a constant temperature, and remove the supernatant by centrifugation. The centrifugal product is the rod-shaped gold nanorods.
2. The method for synthesizing a rod-shaped gold nanorod according to claim 1, characterized in that: In step (1), the NaBH4 solution is prepared by the following method: mixing an ice-water mixture with a required amount of NaBH4.
3. The method for synthesizing a rod-shaped gold nanorod according to claim 1 or 2, characterized in that: In step (1), the stirring conditions are: a rotation speed of 1500 rpm, and a stirring time of 1 to 2 min; and the constant temperature standing conditions are: heating in a water bath at 30° C. and standing for 30 min.
4. The method for synthesizing a rod-shaped gold nanorod according to claim 1, characterized in that: In step (2), 10 mL of 0.1 M CTAC solution and 0.054 g of oleylamine were dissolved in 50° C. water, and the temperature was lowered to 30° C. after dissolution.
5. The method for synthesizing bone-shaped gold nanorods according to claim 1, characterized in that: In step (2), the pH was adjusted to 1.7 using 5 M H2SO4.
6. The method for synthesizing bone-shaped gold nanorods according to claim 1, characterized in that: In step (2), the stirring conditions are: a rotation speed of 1500 rpm, and a stirring time of 1 to 2 min; and the constant temperature standing conditions are: heating in a water bath at 30° C. and standing for 30 min.
7. The method for synthesizing bone-shaped gold nanorods according to claim 1, characterized in that: In step (3), the constant temperature standing condition is: heating in a water bath at 30°C and standing for 3 hours.
Citation Information
Patent Citations
Method for preparing gold nanorod material through reduction of hydroquinone under double surfactants
CN112974829A
Method for rapidly preparing gold nanorod
CN104209533A
Method for preparing gold nanorods
CN104907578A
Preparation method of gold nanorod material under low surfactant concentration
CN112756622A
Preparation method for growing mesoporous silica material on surface of gold nanorod