A polypropylene-agar salt bridge and its preparation method and application
By using a salt bridge of agar gel electrolyte filled with acrylic emulsion in a polypropylene tube, the problem of poor stability of the existing glass-agar salt bridge when measuring autophoretic coatings containing hydrofluoric acid is solved, and a more stable redox potential is achieved. measurement, potential fluctuations are reduced, and the materials are common and low-cost.
Patent Information
- Application Number
- CN202111625452.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-28
AI Technical Summary
The existing glass-agar salt bridge has poor stability when measuring autophoretic coatings containing hydrofluoric acid and cannot effectively withstand the corrosiveness of hydrofluoric acid, resulting in unstable measurement results.
A polypropylene (PP) tube is used as the salt bridge support, filled with agar gel electrolyte of acrylic emulsion, to reduce the reactivity between the salt bridge material and the autophoretic paint components and improve the stability of the salt bridge.
It significantly improves the measurement stability of autophoretic paint potential, reduces the fluctuation of redox potential, meets the requirements for salt bridge stability, and has common materials, simple production and low cost.
Smart Images

Figure BDA0003439828740000021 
Figure BDA0003439828740000031 
Figure BDA0003439828740000051
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemical measurement and coatings, and particularly relates to a polypropylene-agar salt bridge and a preparation method thereof and application thereof in stably measuring the redox potential of a self-phoretic coating containing hydrofluoric acid. Background Art
[0002] The control of the redox potential of the bath liquid of self-phoretic coating has a great influence on the quality of the paint film. The main components of commonly used self-phoretic coatings containing hydrofluoric acid are FeF3, HF, H2O2, organic polymer latex, pigments, etc. Therefore, self-phoretic coatings have strong oxidizing, acidic and corrosive properties, which requires that the part of the self-phoretic coating measuring device that is in contact with the self-phoretic coating has good corrosion resistance, with the focus on tolerance to hydrofluoric acid. Since common reference electrodes such as saturated calomel electrodes cannot be directly used in self-phoretic coatings during measurement, a salt bridge is required. The conventional salt bridge is a glass U-tube filled with KCl solution and agar gel. The stability of the glass-agar salt bridge in self-phoretic coatings is poor. This is because SiO2 in the glass reacts with F - Agar not only reacts with F - The reaction will also cause acid decomposition. Summary of the invention
[0003] In view of the shortcomings of the prior art such as poor stability, the present invention provides a polypropylene-agar salt bridge and a preparation method thereof and an application thereof in the stable measurement of the potential of a self-phoretic coating containing hydrofluoric acid. The present invention uses a polypropylene (PP) tube resistant to hydrofluoric acid corrosion as a U-shaped tube, and fills the PP tube with agar gel added with an acrylic emulsion (pure acrylic emulsion, silicone acrylic emulsion, styrene acrylic emulsion), which greatly reduces the reactivity of the salt bridge material with the self-phoretic coating component, greatly improves the stability of the prepared PP-agar salt bridge in the self-phoretic coating, and greatly improves the potential stability of the measured self-phoretic coating.
[0004] The process flow of preparing the salt bridge of the present invention is as follows: bending a straight PP tube into a U-shaped tube → dissolving agar → adding KCl into agar → adding acrylic emulsion into agar → injecting agar into the U-shaped tube → inserting PP nets at both ends of the U-shaped tube.
[0005] In order to achieve the above object, the technical solution of the present invention is as follows:
[0006] The present invention provides a polypropylene-agar salt bridge, wherein the polypropylene-agar salt bridge uses a polypropylene U-shaped tube as a support body, the polypropylene U-shaped tube is filled with gel electrolyte, and both ends of the polypropylene U-shaped tube are respectively plugged with polypropylene filter nets (to prevent gel from falling off and losing water);
[0007] The gel electrolyte is prepared as follows: KCl and acrylic emulsion are added to 2-4wt% (preferably 3wt%) agar aqueous solution at 80-95° C. (preferably 90° C.), and the mixture is uniformly mixed to obtain the gel electrolyte; the mass ratio of the agar aqueous solution, KCl and acrylic emulsion is 100:20-35:0.25-4 (preferably 100:30:0.25-4).
[0008] The gel electrolyte is injected into the polypropylene U-shaped tube while hot, and cooled to form a tube.
[0009] Preferably, the acrylic emulsion is a pure acrylic emulsion, a silicone acrylic emulsion or a styrene acrylic emulsion (preferably a styrene acrylic emulsion). Further preferably, when the acrylic emulsion is a pure acrylic emulsion, the mass ratio of the agar aqueous solution, KCl and the acrylic emulsion is 100:20-35:0.25-1 (more preferably 100:20-35:0.25-0.5, most preferably 100:30:0.5); when the acrylic emulsion is a silicone acrylic emulsion or a styrene acrylic emulsion, the mass ratio of the agar aqueous solution, KCl and the silicone acrylic emulsion or the styrene acrylic emulsion is 100:20-35:0.25-4 (more preferably 100:20-35:0.25-2, most preferably 100:30:2).
[0010] Furthermore, the solid content of the acrylic emulsion is 20-50% (preferably 40-50%, more preferably 45%).
[0011] The added amounts of the pure acrylic emulsion, silicone acrylic emulsion and styrene acrylic emulsion calculated by mass are 0.25-1%, 0.25-4% and 0.25-4% respectively, and the added amounts calculated by solid content are 0.11-0.45%, 0.11-1.8% and 0.11-1.8% respectively.
[0012] The present invention also provides an application of the polypropylene-agar salt bridge in measuring the redox potential of a self-phoretic coating containing hydrofluoric acid.
[0013] Specifically, the application is: a Pt electrode is inserted into the self-phoretic coating containing hydrofluoric acid as a working electrode, a saturated calomel electrode is inserted into a saturated KCl solution as a reference electrode and an auxiliary electrode, the self-phoretic coating containing hydrofluoric acid and the saturated KCl solution are connected by a salt bridge, and after the power is turned on, the redox potential of the self-phoretic coating containing hydrofluoric acid is measured.
[0014] The redox potential of the hydrofluoric acid-containing self-phoretic coating ranges from 190 mV to 560 mV;
[0015] The self-swimming paint can be self-prepared (including emulsion synthesis) or commercially available (e.g., Henkel's Aquence 930 self-swimming paint);
[0016] The acrylic self-phoretic coating comprises: a film-forming substance, a surfactant, a pigment, HF and H2O2.
[0017] Compared with the prior art, the invention has the following beneficial effects: the PP-agar salt bridge is prepared by adding acrylic emulsion to agar gel, and the fluctuation of the redox potential of the self-phoretic coating measured by using this salt bridge is significantly smaller than the measurement result of the agar-PP salt bridge without acrylic emulsion, and the reduction is greater than that of the four salt bridges of PE, glass, 304 stainless steel and 316 stainless steel without acrylic emulsion. The requirements for the stability of the salt bridge in the redox potential measurement of the self-phoretic coating are met, and the raw materials used are common, the preparation is simple, and the cost of the finished salt bridge is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the self-phoretic coating redox potential measurement system.
[0019] Figure 2 Potential-time curves of Henkel self-phoretic coatings measured with 0.5% pure acrylic, 2% silicone acrylic, 2% styrene acrylic and glass, 304 and 316 stainless steel, PE, and blank PP salt bridge. (a) is the overall picture, and (b) is the enlarged picture. DETAILED DESCRIPTION
[0020] The technical solution of the present invention is further described below in conjunction with specific examples, but the protection scope of the present invention is not limited thereto.
[0021] The main experimental drugs used in the present invention are listed in Table 1, and the main experimental equipment and instruments used are listed in Table 2.
[0022] Table 1 Main experimental drugs
[0023]
[0024] Note: The outer diameter of the glass tube, 304 stainless steel tube and 316 stainless steel tube is 10mm and the inner diameter is 8mm.
[0025] The mass solid content of pure acrylic emulsion, silicone acrylic emulsion and styrene acrylic emulsion is 45%.
[0026] Table 2 Main experimental equipment
[0027]
[0028] Example 1: 0.25% pure propylene
[0029] (1) Preparation of U-shaped tube. Cut a 12 cm long straight PP tube with an outer diameter of 8 mm and an inner diameter of 6 mm, insert a spring with a diameter 1-2 mm smaller than the PP tube into the straight PP tube, heat and soften the straight PP tube with a heating splint, and then bend it into a U-shaped tube with a three-slot tube bender. After forming, pull out the spring.
[0030] (2) Agar dissolving: Measure 3 g agar powder and 97 g distilled water into a beaker and heat the beaker in a water bath at 90°C until the agar is completely dissolved.
[0031] (3) Add KCl to agar. Add 30 g of KCl and stir thoroughly under heating at 90°C in a water bath until the KCl is completely dissolved.
[0032] (4) Adding acrylic emulsion to agar: Add 0.25 g of pure acrylic emulsion and stir under heating conditions at 90°C in a water bath to disperse the pure acrylic emulsion in the agar-KCl solution.
[0033] (5) Inject agar into the U-shaped tube. Use a syringe to add agar into the U-shaped tube while it is still hot and let it stand to condense into a jelly.
[0034] (6) Insert PP mesh into both ends of the U-shaped tube. Cut a 3mm thick 500-mesh PP filter mesh into small pieces with a diameter of 6mm, and insert the small pieces of PP mesh into both ends of the U-shaped tube.
[0035] (7) Measurement of the redox potential of the self-phoretic coating. The redox potential of the self-phoretic coating was measured using a two-electrode system. 50 g of Henkel 930 self-phoretic coating was measured in a 50 g PP beaker. A Pt electrode was inserted into the self-phoretic coating as a working electrode, and a saturated calomel electrode was placed in a saturated KCl solution as a reference electrode and auxiliary electrode. The self-phoretic coating and the saturated KCl solution were connected with a salt bridge, and the redox potential of the self-phoretic coating was measured using an Ivium electrochemical workstation. The measurement was carried out at room temperature, and the potential test time was 1800 s. The measurement system was connected as follows: Figure 1 As shown. The redox potential of Henkel 930 self-phoretic coating is 290-310 mV. Note: The preset value of the self-phoretic coating here is estimated by the average potential of the salt bridge 0.5% pure propylene and 2% silicone propylene obtained in Example 2 and Example 8.
[0036] Example 2: 0.5% pure propylene
[0037] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 1; Step 4 is the same as that in Example 1 except that the amount of pure acrylic emulsion added is changed to 0.5 g.
[0038] Example 3: 1% pure propylene
[0039] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 1; Step 4 is the same as that in Example 1 except that the amount of pure acrylic emulsion added is changed to 1 g.
[0040] Example 4: 2% pure propylene
[0041] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 1; Step 4 is the same as that in Example 1 except that the amount of pure acrylic emulsion added is changed to 2 g.
[0042] Example 5: 0.25% silicone acrylate
[0043] Steps 1, 2, 3, 5, 6, and 7 are the same as those in Example 1; Step 4 is to add 0.25 g of silicone acrylic emulsion instead of pure acrylic emulsion, and the rest is the same as Step 4 in Example 1.
[0044] Example 6: 0.5% silicone acrylate
[0045] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 5; Step 4 is the same as that in Example 5 except that the amount of silicone acrylic emulsion added is changed to 0.5 g.
[0046] Example 7: 1% Silicone Acrylic
[0047] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 5; Step 4 is the same as that in Example 5 except that the amount of silicone acrylic emulsion added is changed to 1 g.
[0048] Example 8: 2% Silicone Acrylic
[0049] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 5; Step 4 is the same as that in Example 5 except that the amount of silicone acrylic emulsion added is changed to 2 g.
[0050] Example 9: 4% Silicone Acrylate
[0051] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 5; Step 4 is the same as that in Example 5 except that the amount of silicone acrylic emulsion added is changed to 4 g.
[0052] Example 10: 0.25% Phenylpropane
[0053] Steps 1, 2, 3, 5, 6, and 7 are the same as those in Example 1; Step 4 is to add 0.25 g of styrene-acrylic emulsion instead of pure acrylic emulsion, and the rest is the same as Step 4 in Example 1.
[0054] Example 11: 0.5% Phenylpropane
[0055] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 10; Step 4 is the same as that in Example 10 except that the amount of styrene-acrylic emulsion added is changed to 0.5 g.
[0056] Example 12: 1% Phenylpropane
[0057] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 10; Step 4 is the same as that in Example 10 except that the amount of styrene-acrylic emulsion added is changed to 1 g.
[0058] Example 13: 2% Phenylpropane
[0059] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 10; Step 4 is the same as that in Example 10 except that the amount of styrene-acrylic emulsion added is changed to 2 g.
[0060] Example 14: 4% Phenylpropane
[0061] Steps 1, 2, 3, 5, 6 and 7 are the same as those in Example 10; Step 4 is the same as that in Example 10 except that the amount of styrene-acrylic emulsion added is changed to 4 g.
[0062] Example 15: 0.5% pure propane - 200mV
[0063] Steps 1, 2, 3, 4, 5 and 6 are the same as those in Example 2; Step 7 is the same as Step 7 in Example 2 except that the redox potential of the self-phoretic coating is 190-210 mV.
[0064] Example 16: 0.5% pure propane - 550mV
[0065] Steps 1, 2, 3, 4, 5 and 6 are the same as those in Example 2. Step 7 is the same as those in Example 2 except that the redox potential of the self-phoretic coating is 540-560 mV.
[0066] Example 17: 2% Silicon Propylene - 200mV
[0067] Steps 1, 2, 3, 4, 5 and 6 are the same as those in Example 8; Step 7 is the same as that in Example 8 except that the redox potential of the self-phoretic coating is 190-210 mV.
[0068] Example 18: 2% Silicone Acrylic - 550mV
[0069] Steps 1, 2, 3, 4, 5 and 6 are the same as those in Example 8; Step 7 is the same as Step 7 in Example 8 except that the redox potential of the self-phoretic coating is 540-560 mV.
[0070] Example 20: 2% Phenylpropane-200mV
[0071] Steps 1, 2, 3, 4, 5, and 6 are the same as those in Example 13; Step 7 is the same as Step 7 in Example 13 except that the redox potential of the self-phoretic coating is 190-210 mV.
[0072] Example 21: 2% Phenylpropyl-550mV
[0073] Steps 1, 2, 3, 4, 5 and 6 are respectively the same as those in Example 13; Step 7 is the same as Step 7 in Example 13 except that the redox potential of the self-phoretic coating is 540-560 mV.
[0074] Comparative Example 1: Glass Salt Bridge
[0075] Steps 1, 2, 3, 4, and 5 are respectively the same as steps 2, 3, 5, 6, and 7 of Example 1. The difference between Comparative Example 1 and Example 1 is that the U-shaped tube uses an existing glass U-shaped tube and no acrylic emulsion is added to the agar solution.
[0076] Comparative Example 2: 304 Stainless Steel Salt Bridge
[0077] (1) Preparation of U-shaped tube: A 15 cm long straight 304 stainless steel tube was bent into a U-shaped tube using a 410M manual tube bender.
[0078] Steps 2, 3, 4, 5 and 6 are respectively the same as 1, 2, 3, 4 and 5 of Comparative Example 1.
[0079] Comparative Example 3: 316 Stainless Steel Salt Bridge
[0080] Step 1 is to bend a 15 cm long straight 316 stainless steel into a U-shaped tube using a 410M manual tube bender. Steps 2, 3, 4, 5, and 6 are the same as those in Comparative Example 2.
[0081] Comparative Example 4: PE Salt Bridge
[0082] The pipe used in step 1 is a straight PE pipe, and the rest is the same as step 1 of embodiment 1. Steps 2, 3, 4, 5, and 6 are respectively the same as steps 2, 3, 5, 6, and 7 of embodiment 1. The difference between comparative example 4 and embodiment 1 is that the pipe is a PE pipe and the gel does not contain acrylic emulsion.
[0083] Comparative Example 5: Blank PP
[0084] Steps 1, 2, 3, 4, 5, and 6 are respectively the same as steps 1, 2, 3, 5, 6, and 7 of Example 1, that is, compared with Example 1, step 4 is lacking (that is, no acrylic emulsion is added).
[0085] Comparative Example 6: Blank PP-200mV
[0086] Steps 1, 2, 3, 4, and 5 are the same as those in comparative example 5. Step 6 is the same as that in comparative example 5 except that the redox potential of the self-phoretic coating is 190-210 mV.
[0087] Comparative Example 7: Blank PP-550mV
[0088] Steps 1, 2, 3, 4 and 5 are the same as those in comparative example 5. Step 6 is the same as that in comparative example 5 except that the redox potential of the self-phoretic coating is 540-560 mV.
[0089] Definition: Maximum potential fluctuation = maximum potential - minimum potential, unit is mV.
[0090] Table 1 shows the maximum potential fluctuation of Henkel self-phoretic coatings measured by adding PP salt bridges with different concentrations of acrylic emulsions. Table 2 shows the maximum potential fluctuation of Henkel self-phoretic coatings with different redox potentials measured by using 0.5% pure acrylic, 2% silicone acrylic, and 2% styrene acrylic salt bridges.
[0091] Table 1 Maximum potential fluctuation of Henkel's self-phoretic coating measured by adding PP salt bridge with different concentrations of acrylic emulsion (unit: mV).
[0092]
[0093] Table 2 shows the maximum potential fluctuations measured in Henkel self-phoretic coatings with different redox potentials using three salt bridges: 0.5% pure acrylic, 2% silicone acrylic, and 2% styrene acrylic.
[0094]
[0095] from Figure 1 It can be seen that the potential change in the potential-time curve measured by the salt bridge with U-shaped tube made of glass and stainless steel is significantly greater than that of the PP salt bridge. Among them, the glass salt bridge is the largest, which is because the HF in the self-dipping paint will react with the silicon dioxide in the glass. Hydrofluoric acid will also react with 304 stainless steel. 316 stainless steel is resistant to hydrofluoric acid, but the measured potential fluctuation is also large, which may be because there is an oxide on the surface of 316 stainless steel and there is a stabilization process in hydrofluoric acid. In addition, the salt bridge electrolyte KCl may react with 316 stainless steel. The potential fluctuation measured by the PE salt bridge is larger than that of PP, which may be because PE is not as resistant to the corrosion of hydrofluoric acid and strong oxidizing media as PP. The addition of acrylic emulsion improves the stability of the potential measured by the PP salt bridge, because most of the components in the acrylic emulsion are resistant to hydrofluoric acid and oxidizing media, and the acrylic emulsion dispersed in agar reduces the contact between agar and self-dipping paint.
[0096] As shown in Table 1, the addition of acrylic emulsion significantly improves the stability of the salt bridge measurement potential. When the amount of emulsion added is large (pure acrylic is 2%, silicone acrylic and styrene acrylic are 4%), the potential stability decreases slightly, which may be because the emulsion destroys the gel structure.
[0097] As can be seen from Table 2, when the potential of the self-phoretic coating is different, the potentials measured using 0.5% pure acrylic, 2% silicone acrylic, and 2% styrene acrylic salt bridges are relatively stable. When the acidity is high, the potential stability of the blank PP salt bridge without acrylic emulsion becomes worse. This is because agar has poor acid resistance, and when the acidity increases, the stability of agar becomes worse.
[0098] It can be seen from Tables 1 and 2 that the improvement in the measured potential stability of the styrene-acrylic emulsion is more significant among the three acrylic emulsions.
Claims
1. A polypropylene-agar salt bridge, characterized in that: The polypropylene-agar salt bridge is supported by a polypropylene U-shaped tube, the polypropylene U-shaped tube is filled with gel electrolyte, and both ends of the polypropylene U-shaped tube are respectively plugged with polypropylene filter nets; The gel electrolyte is prepared as follows: adding KCl and acrylic emulsion to a 2-4 wt% agar aqueous solution at 80-95° C. and mixing them evenly to obtain the gel electrolyte; the mass ratio of the agar aqueous solution to KCl is 100:30; The acrylic emulsion is pure acrylic emulsion, silicone acrylic emulsion or styrene acrylic emulsion; the solid content of the acrylic emulsion is 45%; The addition amounts of the pure acrylic emulsion, silicone acrylic emulsion and styrene acrylic emulsion calculated based on the mass of the agar aqueous solution are 0.25-1%, 0.25-4% and 0.25-4% respectively.
2. Use of the polypropylene-agar salt bridge as claimed in claim 1 in measuring the redox potential of a self-phoretic coating containing hydrofluoric acid.
3. The use according to claim 2, characterized in that The application is: a Pt electrode is inserted into the self-phoretic coating containing hydrofluoric acid as a working electrode, a saturated calomel electrode is inserted into a saturated KCl solution as a reference electrode and an auxiliary electrode, the self-phoretic coating containing hydrofluoric acid and the saturated KCl solution are connected by a salt bridge, and after the power is turned on, the redox potential of the self-phoretic coating containing hydrofluoric acid is measured.
Citation Information
Patent Citations
Reference electrode
CN102971621A
A process of preparing saltbridge employing SAGO for fuel cells and product thereof
IN202041040013A