An extrusion die, polytetrafluoroethylene film, and preparation method and application thereof

The extrusion die with varying cavity roughnesses addresses the challenge of producing PTFE films with high strength, filtration efficiency, and air permeability by controlling fiberization and pore size, resulting in improved PTFE films for diverse applications.

CN114225713BActive Publication Date: 2024-12-06NANJING FIBERGLASS RES & DESIGN INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210002331.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-04
Publication Date
2024-12-06
Estimated Expiration
2042-01-04

AI Technical Summary

Technical Problem

Existing methods struggle to produce polytetrafluoroethylene microporous membranes with simultaneous high strength, filtration efficiency, and air permeability due to inconsistent pore structures and complex processes.

Method used

An extrusion die with a first and second shell, featuring cavities with varying roughnesses and fixed connections, is used to prepare polytetrafluoroethylene films through extrusion, calendering, and stretching, allowing control over fiberization and pore size.

Benefits of technology

The method produces PTFE films with improved strength, filtration efficiency, and air permeability, achieving pore sizes less than 2μm, elongation at break greater than 190%, and air permeability of 20-100 L/dm²·min, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114225713B_ABST
    Figure CN114225713B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of microporous membrane preparation, and specifically relates to an extrusion die, a polytetrafluoroethylene film, and a preparation method and application thereof. The extrusion die comprises a first shell and a second shell connected to each other, the first shell is provided with at least one cavity, and at least two different roughnesses are provided on the surface of the cavity in contact with the material. The polytetrafluoroethylene film prepared by the extrusion die can have the advantages of strength, high filtration efficiency and good air permeability, and can be prepared without using a complicated process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microporous membrane preparation, and specifically relates to an extrusion die, a polytetrafluoroethylene film, and a preparation method and application thereof. Background Art

[0002] Polytetrafluoroethylene expanded microporous membrane (PTFE) is widely used in the filtration industry due to its excellent chemical stability, temperature resistance and high porosity. However, since PTFE is a non-melting material, it cannot flow even when the decomposition temperature is reached, and the processing is difficult. The existing technology generally adopts an extrusion stretching molding process to prepare the PTFE membrane. Specifically, the existing polytetrafluoroethylene microporous membrane preparation process is to mix polytetrafluoroethylene resin with an oil agent, fill it into a blank, and after pressing, a compact blank with uniform density is formed, and a film is made by squeezing, calendering, and asynchronously stretching in the longitudinal and transverse directions through a circular die to obtain a film with a uniform pore structure. However, the film has some problems. When the film thickness is small, the air permeability increases and the resistance is low, but the filtration effect and strength decrease; when the film thickness is large, the strength and filtration efficiency increase, but the resistance becomes larger and the air permeability decreases. The film with a uniform pore structure prepared by the existing technology cannot make the film have good strength, filtration efficiency and air permeability at the same time.

[0003] PTFE microporous membrane is a "node + fiber" structure. The higher the degree of fibrosis, the higher the porosity, the better the filtration performance of the microporous membrane. In order to achieve high efficiency and low resistance filtration performance at the same time, many studies have been carried out at home and abroad. For example, patent document US5476589A discloses a porous PTFE membrane and a method for manufacturing the same. The method uses PTFE fine powder with low amorphous content and at least 98% crystallinity as raw material. Although the air permeability and efficiency of the obtained film are good, the pore structure of the PTFE membrane is inconsistent and the uniformity of the film is poor. Chinese patent document CN107088369A discloses an application of a mixed powder and a molding material in the manufacture of a porous membrane and a porous membrane. The method realizes the degree of fibrosis of the PTFE membrane by modifying the raw material formula, and realizes high air permeability and high filtration performance. However, the method also has the problem that the pore structure of the PTFE membrane is inconsistent and the uniformity of the film is poor. When improving the uniformity of the microporous membrane, the improvement effect is limited. Chinese patent document CN1030690C discloses a method for producing a multilayer polytetrafluoroethylene porous membrane, which requires filling at least two polytetrafluoroethylene fine powders mixed with a liquid lubricant, followed by extrusion to obtain a multilayer extrudate, and then roller pressing to obtain a polytetrafluoroethylene film. This method requires separate fillers, the process is cumbersome, and is affected by a variety of components, temperature and other environmental factors. The degree of fiberization cannot be differentially controlled during the extrusion process. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects in the prior art that it is difficult to produce a polytetrafluoroethylene microporous membrane with good strength, filtration efficiency and air permeability through a simple process, thereby providing an extrusion mold, a polytetrafluoroethylene film and a preparation method and application thereof.

[0005] To this end, the present invention provides the following technical solutions.

[0006] The present invention provides an extrusion die for preparing a polytetrafluoroethylene film, comprising a first shell and a second shell connected to each other;

[0007] The first shell is provided with at least one cavity;

[0008] At least two different roughnesses are arranged on the surface of the cavity contacting with the material.

[0009] Furthermore, at least a first region and a second region are provided on the surface of the cavity in contact with the material, and the first region and the second region have different roughnesses;

[0010] The first area is formed by a first arc line, a second arc line, a first bus line and a second bus line;

[0011] The second area is formed by the third arc line, the fourth arc line, the first generatrix and the second generatrix.

[0012] The arc length of the first arc is 1 / 10-1 / 2 of the circumference of the closed curve;

[0013] The roughness is 0.01-50.

[0014] The first shell is provided with at least a first cavity and a second cavity; the second cavity is sleeved in the first cavity;

[0015] The roughness of the inner surface of the first cavity is different from the roughness of the inner surface of the second cavity; and / or,

[0016] The roughness of the inner surface of the first cavity is different from the roughness of the outer surface of the second cavity; and / or,

[0017] The roughness of the inner surface of the first cavity, the roughness of the inner surface of the second cavity and the roughness of the outer surface of the second cavity are different.

[0018] The first shell is provided with a material inlet and a material outlet;

[0019] Adjacent cavities are fixedly connected at the material inlet and the material outlet.

[0020] The cavity is in a truncated cone shape, and the ratio of the inner diameter of the cross section where the material inlet is located to the inner diameter of the cross section where the material outlet is located is 2-17.

[0021] The present invention also provides a method for preparing a polytetrafluoroethylene film, using the above extrusion die, comprising the following steps:

[0022] The green body is extruded, calendered and stretched to obtain a polytetrafluoroethylene film.

[0023] The preparation step of the green body comprises: mixing polytetrafluoroethylene resin and oil agent and then beating the green body to obtain the green body; wherein the mass ratio of polytetrafluoroethylene resin to oil agent is 100:(10-40).

[0024] The oil agent may be, but is not limited to, aviation kerosene and paraffin oil.

[0025] The extrusion step in the preparation method is carried out using the above extrusion die.

[0026] In the stretching step, the material is stretched along the flow direction to 2-12 times of the original length;

[0027] Stretched in a direction perpendicular to the material flow direction to 4-28 times the original length;

[0028] After the calendering, a sheet is formed, and the thickness of the sheet is 100-300 μm.

[0029] The invention also provides a polytetrafluoroethylene film prepared by the preparation method.

[0030] In addition, the present invention also provides a polytetrafluoroethylene film obtained by the above preparation method or the application of the above polytetrafluoroethylene film in air filtration, liquid filtration, hydrogen energy or electronic communication.

[0031] The technical solution of the present invention has the following advantages:

[0032] 1. The extrusion die for preparing polytetrafluoroethylene film provided by the present invention comprises a first shell and a second shell connected to each other, the first shell has at least one cavity, and the surface of the cavity in contact with the material is provided with at least two different roughnesses. The polytetrafluoroethylene film prepared by the extrusion die can have the advantages of strength, high filtration efficiency and good air permeability, and can be prepared without using complicated processes.

[0033] At least two different roughnesses are set on the cavity surface in the extrusion die, which can increase the shearing effect on the material, improve the fiberization of the PTFE membrane, increase the number of fibrils, and thus improve the strength and filtration efficiency of the membrane; through the different roughnesses of the cavity surface, the material can be subjected to different shear forces, so that the PTFE film forms different microstructures in different directions.

[0034] 2. The extrusion die provided by the present invention can be adjusted and designed according to the different pore sizes, elongation at break and air permeability requirements of the PTFE membrane by controlling the size of the cavity surface where the roughness is located.

[0035] 3. The preparation method of the polytetrafluoroethylene film provided by the present invention comprises the steps of extruding, calendering and stretching a blank to obtain a polytetrafluoroethylene film, using the extrusion die provided by the present invention, by controlling the roughness of the die, while improving the film fiberization, the process difficulty will not be increased, and the strength, filtration efficiency and air permeability of the film are improved, while ensuring the ease of process operation. The pore size of the polytetrafluoroethylene film obtained by the present invention is less than 2μm, the elongation at break is higher than 190%, and the air permeability is 20-100L / dm 2 ·min.

[0036] 4. The preparation method of the polytetrafluoroethylene film provided by the present invention can obtain PTFE membranes with different pore sizes, elongation at break and air permeability by controlling the stretching ratio, so as to meet the application requirements in different fields or different working conditions in the same field. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 is the structural formula of the extrusion die provided in Example 1 of the present invention;

[0039] Figure 2 is a structural diagram of an extrusion die according to another embodiment of the present invention provided in Example 1;

[0040] Figure 3-5 is a structural diagram of an extrusion die provided in Example 2 of the present invention;

[0041] Reference numerals:

[0042] 1-first shell; 2-second shell; 3-welding point;

[0043] 1-1-first cavity; 1-2-second cavity; 1-3-third cavity;

[0044] 1-1-1-Material import; 1-1-2-Material export. DETAILED DESCRIPTION

[0045] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0046] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0047] In the description of the present invention, it should be noted that the terms "upper", "lower", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0048] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the term "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0049] Example 1

[0050] This embodiment provides an extrusion die, comprising a first shell 1 and a second shell 2 connected to each other.

[0051] like Figure 1 As shown, the first housing 1 is provided with at least one cavity 1-1, the cavity includes a material inlet 1-1-1 and a material outlet 1-1-2, after the material enters the first housing 1, it is extruded and discharged from the material outlet into the second housing 2, and at least two different roughnesses are set on the surface of the cavity in contact with the material. When the extrusion die is used to prepare a polytetrafluoroethylene film, the film can have the advantages of strength, high filtration efficiency, good air permeability, etc. At the same time, the extrusion die has no special requirements for the processing technology of the polytetrafluoroethylene film, and does not need to adopt a complicated process.

[0052] Specifically, at least two different roughnesses are set on the surface of the cavity, and the roughness (Ra) is any value in the range of 0.01-50. Ra can be at least one value in the range of 0.05, 0.1, 0.2, 0.4, 0.8, 1.6, 3.2, 6.3, 12.5, 25, and 50. The present embodiment does not specifically limit the number and value of roughnesses. In the present embodiment, the shape of the cavity is a cylinder, such as a cylinder, a truncated cone, etc., preferably a truncated cone. When the cavity is a truncated cone, the ratio of the inner diameter of the cross section where the material inlet is located to the inner diameter of the cross section where the material outlet is located is 2-17; the material of the cavity can be but not limited to brass, stainless steel, etc. The second shell is a cylinder, such as a cylinder, a truncated cone, etc., preferably a cylinder; the material of the second shell can be but not limited to brass, stainless steel, etc.

[0053] At least two different roughness levels are set on the cavity surface, which can make the material subject to different shear forces, improve the fiberization of the material, and thus improve the strength, filtration efficiency and air permeability of the PTFE film. b The ratio D of the maximum inner diameter to the second shell inner diameter can achieve differences in fiberization at different positions of the structure; by controlling the ratio of the maximum inner diameter to the minimum inner diameter of the cavity, the pore size of the PTFE membrane can be effectively adjusted to prepare filter membranes with different filtration performances.

[0054] As an improved embodiment, at least a first area and a second area are provided on the surface of the cavity, and the roughness of the first area and the second area are different; wherein the first area is formed by a first arc, a second arc, a first busbar and a second busbar; the second area is formed by a third arc, a fourth arc, a first busbar and a second busbar; the arc length of the first arc is any value between 1 / 10 and 1 / 2 of the circumference of the closed curve, such as 1 / 10, 1 / 8, 1 / 4, etc.

[0055] Figure 2 An improved implementation is shown, in which a plurality of cavities are sequentially arranged in the first shell 1 from large to small in inner diameter, which may be 2, 3, 4, etc., and the vertical spacing between adjacent cavities is at least 3 mm.

[0056] In the present embodiment, the first shell is provided with a first cavity 1-1 and a second cavity 1-2, and the second cavity 1-2 is sleeved in the first cavity 1-1, and the surfaces of the first cavity 1-1 and the second cavity 1-2 in contact with the material are provided with at least two different roughnesses; specifically, at least two different roughnesses are provided on the inner surface of the first cavity 1-1; or, the roughness of the inner surface of the first cavity 1-1 and the inner surface of the second cavity 1-2 are different; or, the roughness of the inner surface of the first cavity 1-1 and the outer surface of the second cavity 1-2 are different; or, the roughness of the inner surface of the first cavity 1-1, the inner surface of the second cavity 1-2 and the outer surface of the second cavity 1-3 are different; or, the roughness of the inner surface of the second cavity 1-2 and the outer surface of the second cavity 1-2 are different; or, the inner surface of the second cavity 1-2 is provided with at least two different roughnesses; or, the outer surface of the second cavity 1-2 is provided with at least two different roughnesses, or, it can also be a combination of two or more of these embodiments.

[0057] This embodiment can increase the number of fibrils and the degree of fiberization in the extrusion process by providing a plurality of cavities with different roughness, and further improve the strength, filtration efficiency and air permeability of the PTFE film.

[0058] As an improved implementation manner, the first cavity and the second cavity are both provided with a material inlet and a material outlet, and the first cavity and the second cavity are fixedly connected at the material inlet and the material outlet by welding points 3. Specifically, at least one welding point is provided at the material inlet for fixed connection, and at least one welding point is provided at the material outlet for fixed connection to ensure that the material can enter the first shell and the second shell.

[0059] The working principle of this embodiment is that after the material (polytetrafluoroethylene blank) enters the first shell, the first cavity and the second cavity are fixedly connected at the material inlet by welding points, the material is broken up at the material inlet, and then enters the first shell. Since the cavity surface in contact with the material in the first shell is provided with different roughnesses, the material can be fiberized and the broken up material can be reintegrated. When discharged from the material outlet of the first shell, since the first cavity and the second cavity are fixedly connected at the material inlet by welding points, the material will be broken up again. After entering the second shell, the material is reintegrated. The integrated material is discharged from the extrusion die and enters the next process in the preparation of PTFE.

[0060] Example 2

[0061] This embodiment provides an extrusion die for preparing a polytetrafluoroethylene film, such as Figure 3-5 As shown, including,

[0062] The first shell is provided with a first cavity 1-1, a second cavity 1-2 and a third cavity 1-3. The first cavity, the second cavity and the third cavity are all truncated cone structures, and the axis of the truncated cone structure is parallel to the horizontal plane; the inner surface a of the first cavity 1-1 is provided with a first area and a second area, the roughness of the first area is 50, and the roughness of the second area is 0.025. The first area is formed by the first arc, the second arc, the first busbar and the second busbar, and the second area is formed by the third arc, the fourth arc, the first busbar and the second busbar. The arc length of the first area is 1 / 2 of the circumference of the circle, that is, the truncated cone structure is divided into an upper and lower part along the horizontal direction and through the axis of the truncated cone structure, the first area is the upper half, and the second area is the lower half; the inner surface b of the second cavity 1-2 is provided with The outer surface c of the second cavity 1-2 is provided with two different roughnesses of 0.025 and 50, and the truncated cone structure is divided into two parts, the upper part, and the lower part, along the horizontal direction and through the axis of the truncated cone structure. The roughness of the upper part is 50, and the lower part is 0.025; the outer surface c of the second cavity 1-2 is provided with two different roughnesses of 0.025 and 50, and the truncated cone structure is divided into two parts, the upper part, and the lower part, along the horizontal direction and through the axis of the truncated cone structure. The roughness of the upper part of the outer surface of the second cavity 1-2 is 50, and the lower part is 0.025; the outer surface d of the third cavity 1-3 is provided with two different roughnesses of 0.025 and 50, and the truncated cone structure is divided into two parts, the upper part, and the lower part, along the horizontal direction and through the axis of the truncated cone structure. The roughness of the upper part is 50, and the lower part is 0.025; the roughness of the inner surface e of the third cavity 1-3 is 0.025.

[0063] The maximum inner diameter D of the first cavity, the second cavity and the third cavity truncated cone structure b The ratio of the minimum inner diameter D is 10; the material is brass; the first cavity, the second cavity and the third cavity are all provided with a material inlet and a material outlet, and the adjacent cavities are fixedly connected at the material inlet and the material outlet by welding points, and the welding point fixed connection method can break up the material entering the extrusion die. The vertical distance between two adjacent cavities is 5mm.

[0064] The second shell is connected to the material outlet of the first cavity. The second shell is a cylinder, the axis of the cylinder is parallel to the horizontal plane, and the ratio of the length L of the second shell to its inner diameter D is 8. The second shell is made of brass.

[0065] Example 3

[0066] This embodiment provides an extrusion die for preparing a polytetrafluoroethylene film. Figure 3 ,include,

[0067] The first shell is provided with a first cavity 1-1, a second cavity 1-2 and a third cavity 1-3. The first cavity, the second cavity and the third cavity are all truncated cone structures, and the axis of the truncated cone structure is parallel to the horizontal plane; the inner surface a of the first cavity 1-1 is provided with a first area and a second area, the roughness of the first area is 50, and the roughness of the second area is 0.1. The first area is formed by the first arc, the second arc, the first busbar and the second busbar, and the second area is formed by the third arc, the fourth arc, the first busbar and the second busbar. The arc length of the first area is 1 / 2 of the circumference of the circle, that is, the truncated cone structure is divided into upper and lower parts along the horizontal direction and through the axis of the truncated cone structure, the first area is the upper half, and the second area is the lower half; the inner surface a of the second cavity 1-2 b is set with two different roughnesses of 12.5 and 10. The truncated cone structure is divided into two parts, upper and lower, along the horizontal direction and through the axis of the truncated cone structure. The roughness of the upper part is 12.5, and that of the lower part is 10; the outer surface c of the second cavity 1-2 is set with two different roughnesses of 50 and 0.1. The truncated cone structure is divided into two parts, upper and lower, along the horizontal direction and through the axis of the truncated cone structure. The roughness of the upper part of the outer surface of the second cavity 1-2 is 50, and that of the lower part is 0.1; the outer surface d of the third cavity 1-3 is set with two different roughnesses of 12.5 and 10. The truncated cone structure is divided into two parts, upper and lower, along the horizontal direction and through the axis of the truncated cone structure. The roughness of the upper part is 12.5, and that of the lower part is 10; the roughness of the inner surface e of the third cavity 1-3 is 0.1.

[0068] The maximum inner diameter to minimum inner diameter ratio of the first cavity, the second cavity and the third cavity in the truncated cone structure is 6; the material is brass; the first cavity, the second cavity and the third cavity are all provided with a material inlet and a material outlet, and the adjacent cavities are fixedly connected at the material inlet and the material outlet by welding points, and the welding point fixed connection method can break up the material entering the extrusion die. The vertical distance between two adjacent cavities is 5mm.

[0069] The second shell is connected to the material outlet of the first cavity. The second shell is a cylinder, the axis of the cylinder is parallel to the horizontal plane, and the ratio of the length of the second shell to its inner diameter is 9. The second shell is made of brass.

[0070] Example 4

[0071] This embodiment provides an extrusion die for preparing a polytetrafluoroethylene film, comprising:

[0072] The first shell is provided with a first cavity, a second cavity and a third cavity. The inner surface a of the first cavity 1-1 is provided with a first area and a second area. The roughness of the first area is 50, and the roughness of the second area is 0.025. The first area is formed by the first arc, the second arc, the first busbar and the second busbar. The second area is formed by the third arc, the fourth arc, the first busbar and the second busbar. The arc length of the first area is 1 / 5 of the circumference of the circle. The roughness of the inner surface of the second cavity is 40, and the roughness of the outer surface of the second cavity is 0.025. The roughness of the outer surface and the inner surface of the third cavity are the same, both of which are 25.

[0073] The first cavity, the second cavity and the third cavity are all truncated cone structures, and the ratio of the maximum inner diameter to the minimum inner diameter is 4; the material is stainless steel; the first cavity, the second cavity and the third cavity are all provided with a material inlet and a material outlet, and adjacent cavities are fixedly connected at the material inlet and the material outlet by welding points, and the welding point fixed connection method can break up the material entering the extrusion die.

[0074] The second shell is connected to the material outlet of the first cavity. The second shell is a cylinder, the axis of the cylinder is parallel to the horizontal plane, and the ratio of the length of the second shell to its inner diameter is 12; the second shell is made of brass.

[0075] Example 5

[0076] This embodiment provides a method for preparing a polytetrafluoroethylene film, using the extrusion die in embodiment 2, the preparation method comprises:

[0077] The polytetraethylene resin is Daikin F104, and aviation kerosene is used as the oil agent. The mass ratio of Daikin F104 and aviation kerosene is 100:15. After aging and blanking, the blank is obtained.

[0078] After extrusion using the extrusion die of Example 2, the sheet with a thickness of 300 μm was obtained by calendering with upper and lower rollers. After deoiling, it was stretched at 350°C, and its length was stretched to 9 times the original length along the flow direction of the sheet, and stretched to 15 times the original length in the direction orthogonal to the flow direction of the sheet, to obtain a polytetrafluoroethylene film with a pore size of 0.78 μm, an elongation at break of 168%, and an air permeability of 80 L / dm 2 ·min, after compounding with non-woven fabric, the filtration efficiency reaches 99.9996% (test conditions @2.5cm / s, 0.19μm); the elongation at break is measured according to GB / T 7689.5, the air permeability is in accordance with GB / T 5453, and the effective area of ​​the sample is 50cm 2, fixed pressure difference 127Pa, the number of samples per unit sample is 10. The test standard for filtration efficiency is CRAA431.3, specifically: after compounding the PTFE membrane with the non-woven fabric, use TSI3140, the solvent is paraffin oil, the particle size is 0.19μm, and the test wind speed is 2.5cm / s.

[0079] Example 6

[0080] This embodiment provides a method for preparing a polytetrafluoroethylene film, using the extrusion die in embodiment 3, the preparation method comprises:

[0081] Dongyue DF-201 is used as polytetraethylene resin, aviation kerosene is used as oil, Daikin F104 and aviation kerosene are mixed in a mass ratio of 100:20, aged, and then blanked to obtain a blank;

[0082] After extrusion using the extrusion die of Example 2, the sheet with a thickness of 300 μm was obtained by calendering with upper and lower rollers. After deoiling, it was stretched at 350°C, and its length was stretched to 6 times the original length along the flow direction of the sheet, and stretched to 12 times the original length in the direction orthogonal to the flow direction of the sheet, to obtain a polytetrafluoroethylene film with a pore size of 0.92 μm, an elongation at break of 180%, and an air permeability of 100 L / dm 2 ·min, after being compounded with non-woven fabric, the filtration efficiency reaches 99.999% (test conditions @2.5cm / s, 0.19μm); wherein, the test method is the same as that in Example 5.

[0083] Comparative Example 1

[0084] This comparative example provides a method for preparing a polytetrafluoroethylene film. The difference between the extrusion die used and that of Example 2 is that the surface roughness of the first cavity, the second cavity and the third cavity in the extrusion die used in this comparative example are the same, which is 50. The other parts are the same as those of the extrusion die in Example 2. The preparation method comprises the following steps:

[0085] The polytetraethylene resin is Daikin F104, and aviation kerosene is used as the oil agent. The mass ratio of Daikin F104 and aviation kerosene is 100:15. After aging and blanking, the blank is obtained.

[0086] After extrusion using the extrusion die of this comparative example, the sheet with a thickness of 300 μm was obtained by calendering with upper and lower rollers. After deoiling, it was stretched at 350°C, and its length was stretched to 9 times the original length along the flow direction of the sheet, and stretched to 15 times the original length in the direction orthogonal to the flow direction of the sheet, to obtain a polytetrafluoroethylene film with a pore size of 0.96 μm, an elongation at break of 150%, and an air permeability of 70 L / dm 2·min, after being compounded with non-woven fabric, the filtration efficiency reaches 99.997% (test conditions @2.5cm / s, 0.19μm); wherein, the test method is the same as that in Example 5.

[0087] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. An extrusion die for preparing a polytetrafluoroethylene film, characterized in that: comprising a first shell and a second shell that are connected; The first shell is provided with at least one cavity; At least two different roughnesses are set on the surface of the cavity in contact with the material; At least a first area and a second area are provided on the surface of the cavity in contact with the material, and the first area and the second area have different roughnesses; The first area is formed by a first arc line, a second arc line, a first generatrix, and a second generatrix; The second area is formed by the third arc, the fourth arc, the first generatrix and the second generatrix. The arc length of the first arc is 1 / 10-1 / 2 of the circumference of the closed curve; The roughness is 0.01-50.

2. The extrusion die according to claim 1, characterized in that: The first shell is provided with at least a first cavity and a second cavity; the second cavity is sleeved in the first cavity.

3. The extrusion die according to claim 2, characterized in that: The roughness of the inner surface of the first cavity is different from the roughness of the inner surface of the second cavity.

4. The extrusion die according to claim 2, characterized in that: The roughness of the inner surface of the first cavity is different from the roughness of the outer surface of the second cavity.

5. The extrusion die according to claim 2, characterized in that: The roughness of the inner surface of the first cavity, the roughness of the inner surface of the second cavity and the roughness of the outer surface of the second cavity are different.

6. The extrusion die according to claim 2, characterized in that: The first shell is provided with a material inlet and a material outlet; Adjacent cavities are fixedly connected at the material inlet and the material outlet.

7. The extrusion die according to any one of claims 1 to 6, characterized in that: The cavity is in a truncated cone shape, and the ratio of the inner diameter of the cross section where the material inlet is located to the inner diameter of the cross section where the material outlet is located is 2-17.

8. A method for preparing a polytetrafluoroethylene film, characterized in that: Using the extrusion die according to any one of claims 1 to 7, comprising the following steps: The green body is extruded, calendered and stretched to obtain a polytetrafluoroethylene film.

9. The preparation method according to claim 8, characterized in that: In the stretching step, the material is stretched along the flow direction to 2-12 times of the original length; Stretched in a direction perpendicular to the material flow direction to 4-28 times the original length; After the calendering, a sheet is formed, and the thickness of the sheet is 100-300 μm.

10. The polytetrafluoroethylene film obtained by the preparation method according to claim 8 or 9.

11. Use of the polytetrafluoroethylene film obtained by the preparation method according to any one of claims 8 to 9 or the polytetrafluoroethylene film according to claim 10 in air filtration, liquid filtration, hydrogen energy or electronic communication.