A powder preparation method and powder stirring mill for 3D printing

Through the methods of screening and circulating powder grinding in aerosolized powdering technology, the problem of low fine particle yield in aerosolized powdering technology is solved, the yield and preparation efficiency of metal powder are improved, and the cost of production is reduced. Production costs are reduced and more efficient metal powder preparation is achieved.

CN114226738BActive Publication Date: 2024-10-22CHINA RAILWAY ENGINEERING EQUIPMENT GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111428848.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-29
Publication Date
2024-10-22
Estimated Expiration
2041-11-29

AI Technical Summary

Technical Problem

Existing gas atomization powdering technology has problems with low yield and slow preparation rate of fine-grained metal powder in batch production, resulting in limitations in production efficiency and cost of metal 3D printing technology.

Method used

Metal powder is prepared using gas atomization powdering technology and then screened. The screened large particle size powder enters the powder stirring mill for circulation grinding. Combined with crucible-less electrode induction melting gas atomization technology and inert gas protection, the finished product of the powder is improved. rate and preparation efficiency.

Benefits of technology

It significantly improves the yield and preparation efficiency of metal powder, reduces production costs, reduces the waste of repeated melting processing, and improves the quality and stability of the powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114226738B_ABST
    Figure CN114226738B_ABST
Patent Text Reader

Abstract

The present invention proposes a powder preparation method and a powder stirring mill for 3D printing, which are used to solve the technical problems of low fine-particle metal powder yield and slow metal powder preparation rate in the existing gas atomization powder making technology. The present invention is based on the gas atomization powder making technology, obtains some qualified metal powders through the gas atomization powder making technology, and then uses the high processing efficiency of the powder stirring mill for small-particle powders to obtain qualified metal powders, effectively improving the yield of metal powders and reducing production costs; using the crucible-free electrode induction melting gas atomization technology, the diameter of the metal rod is reduced during melting, and the deviation of the metal liquid flow from the axis is reduced; the length of the metal rod is increased, the descending speed is accelerated, and the segregation of the alloy components is prevented; the internal structure of the powder stirring mill is optimized by calculation, which can fully realize the grinding and crushing of fine powders, and the stirring mill processing process is accompanied by inert gas protection to prevent the oxidation of powder during the grinding process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of powder metallurgy, and in particular to a powder preparation method and a powder stirring mill for 3D printing. Background Art

[0002] As a new type of additive manufacturing technology for metal parts processing, metal 3D printing technology has a unique additive processing method that makes it widely used in aerospace, medical, electronics, automobiles, molds and other fields. The emergence of metal 3D printing technology has promoted the development of high-end manufacturing and shortened the technological gap between China and foreign countries in the processing of complex metal structures.

[0003] H13 steel is widely used in the mold industry due to its good resistance to thermal cracking, wear resistance and thermal fatigue. As a typical hot working die steel, H13 steel can serve stably in high temperature and high bearing pressure environments, and is a very important steel type in the mold industry at this stage. Studies have shown that the smaller the grain size in the steel structure, the better its comprehensive mechanical properties. However, the existing casting and forging technology cannot solve the problem of grain growth in the steel structure during cooling. Metal 3D printing technology greatly reduces the grain size of steel structure through the principle of powder metallurgy. The technical research on 3D printing H13 steel has extremely high application value.

[0004] The prerequisite for obtaining H13 steel for 3D printing is to prepare H13 powder suitable for printing. With the development of 3D printing technology and the continuous expansion of the application market, there is a greater demand and higher quality requirements for the metal powder required for 3D printing technology. The quality of the powder seriously affects the performance of the 3D printed product, among which the particle size index of the metal powder has an important influence on the mechanical properties of 3D printed metal parts.

[0005] Existing powder preparation methods are divided into physical and chemical methods and mechanical methods according to their production principles. Physical and chemical methods generally use reduction, synthesis, and electrolysis to produce powder. Mechanical methods mainly use atomization and mechanical crushing. At present, the production technology of fine powder is mainly gas atomization. Gas atomization production is limited by its technical principles. The powder particle size range is wide and normally distributed. Fine powder accounts for only about 20%. The low powder formation rate and high powder production cost have seriously limited the widespread application of metal 3D printing technology in mass production. Improving powder production efficiency and reducing powder costs are important technical means to promote the development of 3D printing technology.

[0006] In the prior art, people have conducted a lot of research on gas atomization powder making technology. Chinese invention patent CN200710121435.1 discloses a method for preparing nitrogen-containing / high-nitrogen stainless steel powder by gas atomization; Chinese invention patent CN108546875A proposes a technology for preparing ultrafine powder by recycling silicon steel waste using a melting atomization process; Chinese invention patent CN111570814A proposes a method for improving the quality of carbon steel powder prepared by gas atomization by adjusting the process and adding liquid film. However, the above preparation processes all require remelting of the large-size powder screened out, and repeated melting and processing wastes electricity resources, resulting in large losses in mass production and low production efficiency. Summary of the invention

[0007] In view of the technical problems of low fine-particle metal powder yield and slow metal powder preparation rate in the existing gas atomization powder making technology, the present invention proposes a powder preparation method and a powder stirring mill for 3D printing. The method is based on the gas atomization powder making technology, and the metal powder prepared by the gas atomization powder making technology is screened to obtain partially qualified metal powder. The large-particle metal powder obtained by screening is then cyclically ground by the powder stirring mill to obtain qualified metal powder. The whole process is designed as an integrated process, and the efficiency of metal powder preparation is significantly improved, which effectively improves the metal powder yield and reduces production costs.

[0008] In order to achieve the above object, the technical solution of the present invention is achieved as follows:

[0009] A method for preparing powder for 3D printing, comprising the following steps:

[0010] S1. Smelting and preparing metal bars for gas atomization processing;

[0011] S2, using gas atomization powder making technology to atomize and powder the metal rod prepared in step S1 to obtain atomized metal powder;

[0012] S3, collecting the metal powder obtained by atomization powder making in step S2;

[0013] S4, sieving the metal powder collected in step S3 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulating it;

[0014] S5, adding the metal powder with a particle size larger than the appropriate particle size screened out in step S4 into a powder stirring mill for grinding;

[0015] S6. Collect and sieve the metal powder ground in step S5 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulate it, and repeatedly grind the metal powder with a particle size larger than the suitable particle size.

[0016] Furthermore, the mesh size of the sieve used for metal powder screening in step S4 and step S6 is 240-350 meshes.

[0017] Furthermore, the powder stirring mill in step S5 includes a power component, a fixed bracket, a barrel and a stirring component. The power component is connected to the rotating main shaft in the barrel. The barrel and the power component are installed on the fixed bracket. The stirring component is located in the barrel and is coaxially arranged with the barrel and the stirring component is arranged on the rotating main shaft. The barrel is provided with a feed port and a discharge port. The grinding medium arranged in the barrel corresponds to the stirring component.

[0018] Furthermore, the power assembly includes a motor and a reducer located on a fixed bracket, the reducer is connected to the motor through a coupling, and the reducer is connected to the rotating main shaft; the stirring assembly includes an agitator and an outlet grille, and the agitator and the outlet grille are synchronously installed on the rotating main shaft; the volume of the stirring medium accounts for 18% to 22% of the internal volume of the cylinder, and the stirring medium includes ball milling steel balls, and the diameter of the ball milling steel balls is 12 mm.

[0019] Furthermore, the rotation speed of the powder stirring mill is 200-240 r / min, the single grinding time of the powder stirring mill is 10-15 min, and inert gas is introduced during the grinding process of the powder stirring mill.

[0020] Furthermore, step S1 specifically includes:

[0021] Y1. Use metal bar raw materials for electric arc furnace steelmaking, and adopt refining and vacuum degassing treatment;

[0022] Y2. Pour the solution of the metal bar obtained in step Y1 into the mold, cool and shape it, and then perform fine processing to obtain the metal bar.

[0023] Further, the metal bar is H13 steel, the length of the metal bar is 300-360 mm, and the diameter of the metal bar is 50-60 mm. Preferably, the H13 steel is made of the following raw materials by mass fraction: 0.36% C, 1.02% Si, 0.35% Mn, 5.17% Cr, 1.33% Mo, 0.95% V, and the rest is Fe.

[0024] Furthermore, step S2 specifically includes:

[0025] T1. Use the crucible-free electrode induction melting gas atomization technology to atomize and powder the metal rods, and perform vacuum treatment in the atomization equipment and introduce inert gas;

[0026] T2, turn on the atomization equipment, energize the induction coil, and the metal bar rotates and starts to descend;

[0027] T3. The high-pressure inert gas sprayed from the atomizing nozzle breaks up and atomizes the molten metal droplets. The powder particles produced by atomization cool and solidify and enter the collection bin.

[0028] Furthermore, the vacuum degree in the atomizing device after the vacuum treatment in step T1 is ≤1×10 -1 The Pa inert gas is argon with a purity of 99.9%; in step T2, the rotation speed of the metal bar is 20-40 r / min, and the descending speed is 100-120 mm / min; the flow rate of the high-pressure inert gas in step T3 is 800-1200 m / min. 3 / h. Preferably, the inert gas in step T1 is argon with a purity of 99.9%, and the atomizing nozzle in step T3 is a free-fall nozzle.

[0029] A powder stirring mill comprises a motor, a reducer and a barrel, wherein the motor, the reducer and the barrel are all mounted on a fixed bracket, the reducer is connected to the motor through a coupling, the reducer is connected to a rotating main shaft in the barrel, a feed port and a discharge port are arranged on the barrel, an agitator, an outlet grid and a stirring medium are arranged in the barrel, the agitator and the outlet grid are synchronously mounted on the rotating main shaft, the stirring medium corresponds to the agitator and the outlet grid respectively, the volume of the stirring medium accounts for 18% to 22% of the internal volume of the barrel, the stirring medium comprises ball milling steel balls, and the diameter of the ball milling steel balls is 12 mm.

[0030] Beneficial effects of the present invention:

[0031] 1. The present invention is based on aerosol powder making technology. The metal powder prepared by aerosol powder making technology is screened to obtain partially qualified metal powder. The large-particle metal powder produced in the aerosol processing process is crushed and ground by utilizing the high processing efficiency of the powder stirring mill for small-particle powder to obtain qualified metal powder. The repeated melting processing of large-particle powder that does not meet the standards by aerosol powder making technology is reduced, a large amount of manpower and material resources are saved, and the whole process is designed as an integrated process. The efficiency of metal powder preparation is significantly improved, the yield of metal powder is effectively improved and the production cost is reduced.

[0032] 2. When the present invention prepares metal powder by the crucible-free electrode induction melting gas atomization technology, the length of the metal rod is adjusted, and the length of the metal rod is designed to be 300~360mm, which is larger than the diameter of the conventional metal rod. The descending speed of the metal rod can be accelerated. Under the cooperation of the rotation speed of 20~40r / min, the speed of metal melting is increased, and the alloy component segregation caused by the long existence time of the molten metal state is reduced, so as to ensure the quality of the metal powder obtained by the gas atomization powder making technology. In addition, the electrode induction melting gas atomization technology is used to atomize and powder the metal rod. The surface of the metal rod melts during the rotation process, which correspondingly reduces the diameter of the metal rod. The centrifugal force is too large during the rotation of the metal rod, which causes the metal liquid flow to deviate from the axis and then deviate from the atomization area, thereby ensuring the stability of the metal rod gas atomization powder making process.

[0033] 3. In the powder stirring mill of the present invention, the motor provides power for the whole set of equipment; the reducer is connected to the motor through a torque limiting coupling to reduce the rotation speed and increase the torque; the outlet grid and the agitator are coaxially installed to separate the grinding medium and the ultrafine powder; the fixed bracket is an integrated interconnecting design to provide support for the motor, the reducer and the cylinder; the ball mill steel balls collide randomly in the powder stirring mill, and the ratio of all the steel balls to the volume of the cylinder is 18%, which can fully grind the metal powder and improve the grinding quality; and the powder stirring mill processing process is accompanied by inert gas protection to prevent the powder from oxidizing during the grinding process, thereby further improving the grinding quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 It is a schematic diagram of the process of aerosol powder making of the present invention.

[0036] Figure 2 It is a front cross-sectional view of the powder stirring mill of the present invention.

[0037] Figure 3 It is a side cross-sectional view of the powder stirring mill of the present invention.

[0038] In the figure, 1-metal rod, 2-induction coil, 3-high-pressure inert gas, 4-atomized metal powder, 5-feed port, 6-rotating spindle, 7-agitator, and 8-discharge port. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Example 1

[0041] A method for preparing powder for 3D printing, comprising the following steps:

[0042] S1. Smelting and preparing metal bar material 1 for gas atomization processing.

[0043] S2. Atomize and powder the metal rod 1 prepared in step S1 using gas atomization powder making technology to obtain atomized metal powder 4.

[0044] S3, collecting the metal powder obtained by atomization powder making in step S2.

[0045] S4. Screening the metal powder collected in step S3 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulating it.

[0046] S5, adding the metal powder with a particle size larger than the appropriate particle size screened out in step S4 into a powder stirring mill for grinding.

[0047] S6. Collect and sieve the metal powder ground in step S5 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulate it, and repeatedly grind the metal powder with a particle size larger than the suitable particle size.

[0048] In application, the metal powder with suitable particle size suitable for 3D printing obtained in step S3 and the metal powder with suitable particle size suitable for 3D printing obtained in step S6 both meet the actual needs. This embodiment can be based on the gas atomization powder making technology, and the metal powder prepared by the gas atomization powder making technology is screened to obtain some qualified metal powders, and then the large-particle-size metal powder obtained by screening is circulated and ground by a powder stirring mill. The large-particle metal powder produced in the gas atomization process is crushed and ground by using the high processing efficiency of the powder stirring mill for small-particle powders to obtain qualified metal powders, thereby reducing the repeated melting and processing of large-particle powders that do not meet the standards by the atomization method, saving a lot of manpower and material resources. Moreover, the whole process is designed as an integrated process, and the efficiency of metal powder preparation is significantly improved, which effectively improves the yield rate of metal powders and reduces production costs.

[0049] Example 2

[0050] A powder mixing mill comprises a motor, a reducer and a barrel, wherein the motor, the reducer and the barrel are all mounted on a fixed bracket, and the reducer is connected to the motor through a coupling. Figure 2 As shown, the reducer is connected to the rotating main shaft 6 in the cylinder, and an agitator 7, an outlet grid and a stirring medium are arranged in the cylinder. The agitator 7 and the outlet grid are synchronously installed on the rotating main shaft 6. The stirring medium corresponds to the agitator 7 and the outlet grid respectively. The volume of the stirring medium accounts for 18% to 22% of the internal volume of the cylinder. The stirring medium includes ball milling steel balls, and the diameter of the ball milling steel balls is 12 mm.

[0051] When metal powder stirring and grinding is required, the metal powder to be ground is placed in the cylinder, the motor is turned on, the rotation speed is adjusted, the rotating spindle 6 starts to rotate, driving the agitator 7 and the outlet grid to rotate, so that the stirring medium in the cylinder and the metal powder are fully ground, thereby achieving the grinding of large-particle-size metal powder and obtaining metal powder of a suitable particle size suitable for 3D printing.

[0052] It is worth noting that, in this embodiment, the motor provides power to the entire equipment; the reducer is connected to the motor through a torque limiting coupling to achieve the purpose of reducing the rotation speed and increasing the torque; the outlet grid and the agitator are coaxially installed to separate the grinding medium and the ultrafine powder; the fixed bracket is an integrated interconnecting design to provide support for the motor, the reducer, and the cylinder.

[0053] It is worth noting that, in this embodiment, the ball mill steel balls collide randomly in the powder stirring mill, and the ratio of all the steel balls to the volume of the cylinder is 18% to 22%, which can fully grind the metal powder and improve the grinding quality.

[0054] Example 3

[0055] A method for preparing powder for 3D printing, comprising the following steps:

[0056] S1. Smelting and preparing metal bar material 1 for gas atomization processing.

[0057] S2. Atomize and powder the metal rod 1 prepared in step S1 using gas atomization powder making technology to obtain atomized metal powder 4.

[0058] S3, collecting the metal powder obtained by atomization powder making in step S2.

[0059] S4. Screening the metal powder collected in step S3 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulating it.

[0060] S5, adding the metal powder with a particle size larger than the appropriate particle size screened out in step S4 into a powder stirring mill for grinding.

[0061] S6. Collect and sieve the metal powder ground in step S5 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulate it, and repeatedly grind the metal powder with a particle size larger than the suitable particle size.

[0062] In application, the metal powder for 3D printing with suitable particle size obtained in step S3 and the metal powder for 3D printing with suitable particle size obtained in step S6 both meet actual needs. This embodiment can be based on gas atomization powder making technology, and obtain partially qualified metal powder by screening the metal powder prepared by gas atomization powder making technology, and then use a powder stirring mill to circulate and grind the large-particle metal powder obtained by screening. Taking advantage of the high processing efficiency of the powder stirring mill for small-particle powder, the large-particle metal powder produced in the gas atomization process is crushed and ground to obtain qualified metal powder, reducing the repeated melting and processing of large-particle powder that does not meet the standards by the atomization method, saving a lot of manpower and material resources. In addition, the entire process is designed as an integrated process, and the efficiency of metal powder preparation is significantly improved, effectively improving the yield of metal powder and reducing production costs.

[0063] It is worth noting that, in this embodiment, a powder stirring mill used in step S6 is also provided, comprising a motor, a reducer and a barrel, the motor, the reducer and the barrel are all mounted on a fixed bracket, and the reducer is connected to the motor through a coupling, such as Figure 3 As shown, the reducer is connected to the rotating main shaft 6 in the cylinder, a feed port 5 and a discharge port 8 are provided on the cylinder, an agitator 7, an outlet grid and a stirring medium are provided in the cylinder, the agitator 7 and the outlet grid are synchronously installed on the rotating main shaft 6, the stirring medium corresponds to the agitator 7 and the outlet grid respectively, the volume of the stirring medium accounts for 18% to 22% of the internal volume of the cylinder, and the stirring medium includes ball milling steel balls, and the diameter of the ball milling steel balls is 12 mm.

[0064] When metal powder stirring and grinding is required, the metal powder to be ground is placed in the cylinder, the motor is turned on, the rotation speed is adjusted, the rotating spindle 6 starts to rotate, driving the agitator 7 and the outlet grid to rotate, so that the stirring medium in the cylinder and the metal powder are fully ground, thereby achieving the grinding of large-particle-size metal powder and obtaining metal powder of a suitable particle size suitable for 3D printing.

[0065] It is worth noting that, in this embodiment, the motor provides power to the entire equipment; the reducer is connected to the motor through a torque limiting coupling to achieve the purpose of reducing the rotation speed and increasing the torque; the outlet grid and the agitator are coaxially installed to separate the grinding medium and the ultrafine powder; the fixed bracket is an integrated interconnecting design to provide support for the motor, the reducer, and the cylinder.

[0066] It is worth noting that, in this embodiment, the ball mill steel balls collide randomly in the powder stirring mill, and the ratio of all the steel balls to the volume of the cylinder is 18% to 22%, which can fully grind the metal powder and improve the grinding quality.

[0067] Example 4

[0068] A method for preparing powder for 3D printing, comprising the following steps:

[0069] S1, smelting and preparing the metal bar 1 for gas atomization processing. Specifically, the following steps are included: Y1, using the raw material of the metal bar 1 to perform electric arc furnace steelmaking, adopting refining and vacuum degassing treatment; pouring the solution of the metal bar 1 obtained in step Y1 into the mold, cooling and forming, and then performing fine processing to obtain the metal bar 1. The metal bar 1 is refined and vacuum degassed to reduce the residual gas in the molten steel, improve the performance of the metal bar 1 after forming, and the surface of the metal bar 1 is finely processed to remove the oxide layer and debris on the surface of the metal bar 1.

[0070] S2, using gas atomization powder making technology to atomize and powder the metal bar material 1 prepared in step S1 to obtain atomized metal powder 4. Specifically, the following steps are included:

[0071] T1. Atomize and powder the metal bar 1 using the crucible-free electrode induction melting gas atomization technology, and perform vacuum treatment in the atomization equipment and introduce inert gas. Figure 1 As shown, the electrode induction melting gas atomization technology is used to atomize and powder the metal bar 1. The surface of the metal bar 1 melts during the rotation process, which correspondingly reduces the diameter of the metal bar 1. The centrifugal force during the rotation of the metal bar 1 is too large, which causes the metal liquid flow to deviate from the axis and then deviate from the atomization area. The stability of the gas atomization powder making process of the metal bar 1 is ensured. The inert gas can protect the entire atomization powder making process and ensure the stability of the metal particles made after atomization.

[0072] It is worth noting that in this embodiment, the vacuum degree in the atomization device after the vacuum treatment in step T1 is ≤1×10 -1 Pa, after vacuum treatment, the oxygen content in the atomizing powder making equipment is reduced, reducing the possibility of oxidation reaction of the molten droplets of the metal rod 1, preliminarily ensuring the yield of the metal powder obtained by the atomizing powder making equipment, and preparing for the subsequent filling of inert gas. Subsequently, an inert gas such as argon with a purity of 99.9% is introduced into the atomizing powder making equipment to further ensure the stability of the molten droplets of the metal rod 1 in the atomizing powder making equipment, thereby ensuring the yield of the metal powder obtained by the atomizing powder making equipment.

[0073] T2, turn on the atomization equipment, energize the induction coil 2, and the metal bar 1 rotates, and the metal bar 1 starts to descend. Figure 1 As shown, after the atomization equipment is turned on and the induction coil 2 is energized, the metal bar 1 rotates, and the rotation speed is controlled at 20r / min. At the same time, the metal bar 1 begins to descend, and the descending speed is 100mm / min.

[0074] It is worth noting that, in this embodiment, the metal bar 1 is H13, which is made of the following raw materials by mass fraction: 0.36% C, 1.02% Si, 0.35% Mn, 5.17% Cr, 1.33% Mo, 0.95% V, and the rest is Fe. The length of the metal bar 1 is 300 mm, and the diameter of the metal bar 1 is 50 mm. The longer length of the metal bar 1 can speed up the speed of the metal bar in the descending process, reduce the segregation of alloy components caused by the long existence time of the molten metal state, and ensure the quality of the metal powder obtained by the gas atomization powder making technology.

[0075] T3, the high-pressure inert gas 3 sprayed from the atomizing nozzle breaks up and atomizes the molten metal droplets, and the powder particles produced by atomization cool and solidify into the collection bin. Figure 1 As shown, the atomizing nozzle is a free-falling nozzle. The atomizing pressure has an important influence on the distribution of metal powder particles. The flow rate of high-pressure inert gas 3 is 800m 3 / h, the high-pressure inert gas can atomize the molten metal droplets, and then the atomized metal powder 4 condenses and falls into the collection bin.

[0076] S3, collecting the metal powder obtained by atomization powder making in step S2. Specifically, the metal powder in the collection bin is collected under the protection of an inert gas such as argon gas with a purity of 99.9%.

[0077] S4, sieving the metal powder collected in step S3 to obtain metal powder of suitable particle size for 3D printing and encapsulating it. Specifically, using a sieve with a mesh size of 240 to sieve the collected metal powder, collecting the metal powder under the sieve and vacuum encapsulating it to obtain the first metal powder that meets the requirements for 3D printing.

[0078] S5, adding the metal powder with a particle size larger than the appropriate particle size screened out in step S4 into a powder stirring mill for grinding. Adding the metal powder with a particle size larger than 240 mesh screened out into a powder stirring mill, and fully grinding the metal powder by utilizing the high processing efficiency of the powder stirring mill for small particle powders.

[0079] It is worth noting that the rotation speed of the powder stirring mill is 200 r / min, the single grinding time of the powder stirring mill is 10 min, and inert gas is introduced during the grinding process of the powder stirring mill.

[0080] S6, collecting the metal powder ground in step S5 and sieving it, obtaining metal powder for 3D printing with a suitable particle size and encapsulating it, and repeatedly grinding the metal powder with a particle size larger than the suitable particle size that is screened out. After grinding the metal powder using a powder stirring mill, a batch of metal powders that meet the requirements and a batch of metal powders with a particle size larger than 240 mesh can be obtained through a 240-mesh screen, and the metal powders that meet the requirements are vacuum packaged, and the metal powders with a particle size larger than 240 mesh are put into the powder stirring mill again for repeated grinding. By multiple screening and repeated grinding, more metal powders that meet the requirements can be obtained.

[0081] It is worth noting that, in this embodiment, Figure 2 As shown, the powder stirring mill used in step S5 includes a power assembly, a fixed support, a barrel and a stirring assembly, the power assembly is connected to the rotating main shaft 6 in the barrel, the barrel and the power assembly are installed on the fixed support, the stirring assembly is located in the barrel and is coaxially arranged with the barrel and the stirring assembly is arranged on the rotating main shaft 6, as shown in FIG. Figure 3 As shown, the cylinder is provided with a feed port 5 and a discharge port 8, and the grinding medium provided in the cylinder corresponds to the stirring assembly. When the metal powder needs to be ground, the metal powder is put into the cylinder through the feed port 5, the power assembly is started, the rotating main shaft 6 starts to rotate, and the stirring assembly is driven to rotate. Driven by the stirring assembly, the grinding medium and the metal powder are fully ground, and the rotation grinding and extrusion crushing are performed. After the grinding is completed, the vent is filled with high-pressure inert gas, and the metal powder is blown out of the discharge port 8 of the powder stirring mill by the high-pressure gas. After the metal powder is collected, it is packaged by vacuum sealing.

[0082] Furthermore, the power assembly includes a motor and a reducer located on a fixed bracket, the reducer is connected to the motor through a coupling, and the reducer is connected to the rotating main shaft 6; the stirring assembly includes an agitator 7 and an outlet grille, and the agitator 7 and the outlet grille are synchronously installed on the rotating main shaft 6; the volume of the stirring medium accounts for 18% of the internal volume of the cylinder, and the stirring medium includes ball milling steel balls, and the diameter of the ball milling steel balls is 12 mm.

[0083] It is worth noting that, in this embodiment, the motor provides power to the entire equipment; the reducer is connected to the motor through a torque limiting coupling to achieve the purpose of reducing the rotation speed and increasing the torque; the outlet grid and the agitator are coaxially installed to separate the grinding medium and the ultrafine powder; the fixed bracket is an integrated interconnecting design to provide support for the motor, the reducer, and the cylinder.

[0084] It is worth noting that, in this embodiment, the ball mill steel balls collide randomly in the powder stirring mill, and the ratio of all the steel balls to the volume of the cylinder is 18%, which can fully grind the metal powder and improve the grinding quality.

[0085] Example 5

[0086] A method for preparing powder for 3D printing, comprising the following steps:

[0087] S1, smelting and preparing the metal bar 1 for gas atomization processing. Specifically, the following steps are included: Y1, using the raw material of the metal bar 1 to perform electric arc furnace steelmaking, adopting refining and vacuum degassing treatment; pouring the solution of the metal bar 1 obtained in step Y1 into a mold, cooling and forming it, and then performing fine processing to obtain the metal bar 1.

[0088] S2, using gas atomization powder making technology to atomize and powder the metal bar material 1 prepared in step S1 to obtain atomized metal powder 4. Specifically, the following steps are included:

[0089] T1. A crucible-free electrode induction melting gas atomization technology is used to atomize and powder the metal bar material 1, and a vacuum treatment is performed in the atomization equipment and an inert gas is introduced.

[0090] It is worth noting that in this embodiment, the vacuum degree in the atomization device after the vacuum treatment in step T1 is ≤1×10 -1 Pa, an inert gas such as argon with a purity of 99.9% is introduced into the powder making equipment.

[0091] T2, turn on the atomization equipment, energize the induction coil 2, and the metal bar 1 rotates, and the metal bar 1 starts to descend. Figure 1 As shown, after the atomization equipment is turned on and the induction coil 2 is energized, the metal bar 1 rotates, and the rotation speed is controlled at 30r / min. At the same time, the metal bar 1 begins to descend, and the descending speed is 110mm / min.

[0092] It is worth noting that, in this embodiment, the metal bar 1 is H13, which is made of the following raw materials by mass fraction: 0.36% C, 1.02% Si, 0.35% Mn, 5.17% Cr, 1.33% Mo, 0.95% V, and the rest is Fe. The length of the metal bar 1 is 330 mm, and the diameter of the metal bar 1 is 55 mm.

[0093] T3, the high-pressure inert gas 3 sprayed from the atomizing nozzle breaks up and atomizes the molten metal droplets, and the powder particles produced by atomization cool and solidify into the collection bin. Figure 1 As shown, the atomizing nozzle is a free-falling nozzle, and the flow rate of the high-pressure inert gas 3 is 1000m 3 / h.

[0094] S3, collecting the metal powder obtained by atomization powder making in step S2. Specifically, the metal powder in the collection bin is collected under the protection of an inert gas such as argon gas with a purity of 99.9%.

[0095] S4, sieving the metal powder collected in step S3 to obtain metal powder with a suitable particle size for 3D printing and encapsulating it. Specifically, using a sieve with a mesh size of 300 to sieve the collected metal powder, collecting the metal powder under the sieve and vacuum encapsulating it to obtain the first metal powder that meets the requirements for 3D printing.

[0096] S5, adding the metal powder with a particle size larger than the appropriate particle size screened out in step S4 into a powder stirring mill for grinding. Adding the metal powder with a particle size larger than 300 mesh screened out into a powder stirring mill, and fully grinding the metal powder by utilizing the high processing efficiency of the powder stirring mill for small particle powders.

[0097] It is worth noting that the rotation speed of the powder stirring mill is 220 r / min, the single grinding time of the powder stirring mill is 12 min, and inert gas is introduced during the grinding process of the powder stirring mill.

[0098] S6. Collect and sieve the metal powder ground in step S5 to obtain metal powder with a suitable particle size for 3D printing and package it, and repeatedly grind the metal powder with a particle size larger than the suitable particle size.

[0099] It is worth noting that, in this embodiment, Figure 2 As shown, the structure of the powder stirring mill used in step S5 is the same as that of the powder stirring mill in Example 4, and will not be repeated here.

[0100] Example 6

[0101] A method for preparing powder for 3D printing, comprising the following steps:

[0102] S1, smelting and preparing the metal bar 1 for gas atomization processing. Specifically, the following steps are included: Y1, using the raw material of the metal bar 1 to perform electric arc furnace steelmaking, adopting refining and vacuum degassing treatment; pouring the solution of the metal bar 1 obtained in step Y1 into a mold, cooling and forming it, and then performing fine processing to obtain the metal bar 1.

[0103] S2, using gas atomization powder making technology to atomize and powder the metal bar material 1 prepared in step S1 to obtain atomized metal powder 4. Specifically, the following steps are included:

[0104] T1. A crucible-free electrode induction melting gas atomization technology is used to atomize and powder the metal bar material 1, and a vacuum treatment is performed in the atomization equipment and an inert gas is introduced.

[0105] It is worth noting that in this embodiment, the vacuum degree in the atomization device after the vacuum treatment in step T1 is ≤1×10 -1 Pa, an inert gas such as argon with a purity of 99.9% is introduced into the powder making equipment.

[0106] T2, turn on the atomization equipment, energize the induction coil 2, and the metal bar 1 rotates, and the metal bar 1 starts to descend. Figure 1 As shown, after the atomization equipment is turned on and the induction coil 2 is energized, the metal bar 1 rotates, and the rotation speed is controlled at 40r / min. At the same time, the metal bar 1 begins to descend, and the descending speed is 120mm / min.

[0107] It is worth noting that, in this embodiment, the metal bar 1 is H13, which is made of the following raw materials by mass fraction: 0.36% C, 1.02% Si, 0.35% Mn, 5.17% Cr, 1.33% Mo, 0.95% V, and the rest is Fe. The length of the metal bar 1 is 360 mm, and the diameter of the metal bar 1 is 60 mm.

[0108] T3, the high-pressure inert gas 3 sprayed from the atomizing nozzle breaks up and atomizes the molten metal droplets, and the powder particles produced by atomization cool and solidify into the collection bin. Figure 1 As shown, the atomizing nozzle is a free-falling nozzle, and the flow rate of the high-pressure inert gas 3 is 1200m 3 / h.

[0109] S3, collecting the metal powder obtained by atomization powder making in step S2. Specifically, the metal powder in the collection bin is collected under the protection of an inert gas such as argon gas with a purity of 99.9%.

[0110] S4, sieving the metal powder collected in step S3 to obtain metal powder of suitable particle size for 3D printing and encapsulating it. Specifically, using a sieve with a mesh size of 350 to sieve the collected metal powder, collecting the metal powder under the sieve and vacuum encapsulating it to obtain the first metal powder that meets the requirements for 3D printing.

[0111] S5, adding the metal powder with a particle size larger than the appropriate particle size screened out in step S4 into a powder stirring mill for grinding. Adding the metal powder with a particle size larger than 350 mesh screened out into a powder stirring mill, and fully grinding the metal powder by utilizing the high processing efficiency of the powder stirring mill for small particle powders.

[0112] It is worth noting that the rotation speed of the powder stirring mill is 240 r / min, the single grinding time of the powder stirring mill is 15 min, and inert gas is introduced during the grinding process of the powder stirring mill.

[0113] S6. Collect and sieve the metal powder ground in step S5 to obtain metal powder with a suitable particle size for 3D printing and package it, and repeatedly grind the metal powder with a particle size larger than the suitable particle size.

[0114] It is worth noting that, in this embodiment, Figure 2 As shown, the structure of the powder stirring mill used in step S5 is the same as that of the powder stirring mill in Example 4, and will not be repeated here.

[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing powder for 3D printing, characterized in that: The following steps are involved: S1, smelting and preparing metal bars (1) for gas atomization processing; S2, using gas atomization powder making technology to atomize and powder the metal rod material (1) prepared in step S1 to obtain atomized metal powder (4); S3, collecting the metal powder obtained by atomization powder making in step S2; S4, sieving the metal powder collected in step S3 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulating it; S5, adding the metal powder with a particle size larger than the appropriate particle size screened out in step S4 into a powder stirring mill for grinding; S6, collecting and sieving the metal powder ground in step S5 to obtain metal powder with a suitable particle size suitable for 3D printing and encapsulating it, and repeatedly grinding the metal powder with a particle size larger than the suitable particle size; The metal bar (1) is H13 steel, the length of the metal bar (1) is 300-360 mm, and the diameter of the metal bar (1) is 50-60 mm; The step S2 specifically includes: T1. Atomize and powderize the metal bar (1) using a crucible-free electrode induction melting gas atomization technology. The atomization equipment is vacuum treated and an inert gas is introduced. The vacuum degree in the atomization equipment after vacuum treatment is ≤1×10 -1 Pa; T2, the atomizing device is turned on, the induction coil (2) is energized, the metal bar (1) rotates, and the metal bar (1) begins to descend. The rotation speed of the metal bar (1) is 20-40 r / min, and the descending speed is 100-120 mm / min; T3, the high-pressure inert gas (3) sprayed from the atomizing nozzle breaks up and atomizes the molten metal droplets, and the powder particles produced by atomization cool and solidify into the collection bin; the flow rate of the high-pressure inert gas (3) is 800~1200m 3 / h; The powder stirring mill in step S5 comprises a power assembly, a fixed support, a barrel and a stirring assembly, wherein the power assembly is connected to a rotating main shaft (6) in the barrel, the barrel and the power assembly are mounted on the fixed support, the stirring assembly is located in the barrel and is coaxially arranged with the barrel and is arranged on the rotating main shaft (6), the barrel is provided with a feed inlet (5) and a discharge outlet (8), and the stirring medium arranged in the barrel corresponds to the stirring assembly; the volume of the stirring medium accounts for 18% to 22% of the internal volume of the barrel, the stirring medium is a ball milling steel ball, and the diameter of the ball milling steel ball is 12 mm.

2. The method for preparing powder for 3D printing according to claim 1, characterized in that: The mesh size of the sieve used for metal powder screening in step S4 and step S6 is 240-350 meshes.

3. The method for preparing powder for 3D printing according to claim 1, characterized in that: The power assembly comprises a motor and a reducer located on a fixed bracket, the reducer being connected to the motor via a coupling, and the reducer being connected to a rotating main shaft (6); the stirring assembly comprises a stirrer (7) and an outlet grille, the stirrer (7) and the outlet grille being synchronously mounted on the rotating main shaft (6).

4. The method for preparing powder for 3D printing according to any one of claims 1 to 3, characterized in that: The rotation speed of the powder stirring mill is 200-240 r / min, the single grinding time of the powder stirring mill is 10-15 min, and inert gas is introduced during the grinding process of the powder stirring mill.

5. The method for preparing powder for 3D printing according to claim 1, characterized in that: The step S1 specifically includes: Y1. Using the raw material of the metal bar (1) to carry out electric arc furnace steelmaking, adopting refining and vacuum degassing treatment; Y2. Pour the solution of the metal bar (1) obtained in step Y1 into a mold, cool and shape it, and then perform fine processing to obtain the metal bar (1).