A method for epitaxial filling of silicon carbide trench structure

By using the growth and etching process parameters determined by pre-experiments in the 4H crystalline silicon carbide trench structure to control the deposition and etching rates, efficient trench structure filling is achieved, and the problem of deposition rate affecting trench growth is solved. The occurrence of voids is avoided and the filling rate is improved.

CN114242644BActive Publication Date: 2024-10-25NO 55 INST CHINA ELECTRONIC SCI & TECHNOLOGYGROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111362158.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-17
Publication Date
2024-10-25
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

In the epitaxial process of the 4H crystalline silicon carbide trench structure, the deposition rate can easily affect the trench growth effect, leading to the closure of the trench pits and the occurrence of voids, making it difficult to achieve efficient trench structure filling.

Method used

By using the same growth experimental wafer as the official silicon carbide wafer to be filled for pre-experimentation, the appropriate growth and etching process parameters are determined, the deposition rate at the bottom of the trench and the mesa is controlled, and the epitaxial layer is removed by hydrogen chloride etching to gradually realize the trench structure. Epitaxial filling, and ensure 1.05-1.1 times the filling depth through multiple depositions and etchings.

Benefits of technology

The epitaxial filling rate of the silicon carbide trench structure is improved, the occurrence of voids is avoided, and the filling effect of high aspect ratio is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114242644B_ABST
    Figure CN114242644B_ABST
Patent Text Reader

Abstract

The present invention provides a method for epitaxial filling of a silicon carbide trench structure, comprising the following steps: S1. Experimenting with a growth test piece to determine the epitaxial growth process parameters of a formal piece; S2. Experimenting with an etching test piece to determine the hydrogen chloride etching process parameters; S3. Preparing a silicon carbide formal piece containing a trench structure; S4. Growing according to the growth process parameters determined in step S1; S5. Rapidly reducing the pressure of the reaction chamber after the growth is completed; S6. According to the etching process parameters determined in step S2, introducing hydrogen chloride gas into the reaction chamber for etching; S7. Rapidly reducing the pressure of the reaction chamber after the etching is completed; S8. Repeating steps S4 to S7 until the thickness requirement is met, that is, the epitaxial filling of the trench structure is completed; S9. Polishing to remove the excess epitaxial layer after the cavity is opened and the piece is taken. The present invention improves the accuracy by designing a pre-experiment, greatly increases the epitaxial filling rate of the high aspect ratio trench structure, and avoids the appearance of voids in the trench structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor materials, and in particular relates to an epitaxial filling method for a silicon carbide trench structure. Background Art

[0002] Compared with traditional silicon (Si) materials, 4H-SiC materials have larger bandgap width, higher critical breakdown electric field strength and thermal conductivity and other material properties, which are suitable for the manufacture of high-voltage and high-power power electronic devices. When the blocking voltage of unipolar devices reaches 10kV or even higher, high on-resistance becomes the main factor limiting its application. Superjunction structure (drift layer contains alternating n-type and p-type regions) can improve the trade-off between device withstand voltage and drift layer specific on-resistance.

[0003] The superjunction structure of silicon material can be realized by controlled diffusion of doping sources of different conductivity types in the epitaxial layer. However, unlike silicon material, the diffusion coefficient of doping atoms in 4H-SiC is very low, so it is impossible to realize the SiC superjunction structure by controlled diffusion. The 4H-SiC superjunction structure needs to be manufactured by a multi-step epitaxial method, that is, on the patterned epitaxial layer, that is, on the trench structure, epitaxially grow different conductivity types of external pressure layers, such as epitaxially growing a p-type epitaxial layer in an n-type trench structure or epitaxially growing an n-type epitaxial layer in a p-type trench structure.

[0004] In the trench structure epitaxial process, it is necessary to avoid deposition in areas outside the trench pit, such as mesa deposition, as much as possible. Too fast a mesa deposition rate will lead to the closure of the trench pit, thereby introducing voids. Summary of the invention

[0005] In order to solve the technical problem that the deposition rate of 4H crystalline silicon carbide in the epitaxial process of the trench structure can easily affect the growth effect of the trench pit, the present invention provides a method for epitaxial filling of a silicon carbide trench structure.

[0006] The present invention adopts the following technical solution:

[0007] A method for epitaxial filling of a silicon carbide trench structure comprises the following steps:

[0008] S1. Use the same growth test piece as the silicon carbide formal piece to be filled in the trench structure to conduct experiments, determine the epitaxial growth process parameters of the formal piece, and obtain the epitaxial deposition rate G of the trench table under this condition. R_mt and the epitaxial deposition rate G at the bottom of the trench R_tb ;

[0009] S2. Use the etching test piece with the same groove structure and the same deposition thickness as the growth test piece in S1 to conduct experiments, determine the hydrogen chloride etching process parameters, including the etching pressure of the reaction chamber and the ratio of chloride to hydrogen, and obtain the etching rate E of the groove table under this condition. R_mt and the etching rate E at the bottom of the trench R_tb ;

[0010] S3. placing the formal silicon carbide sheet containing the groove structure on a graphite susceptor in the reaction chamber of the epitaxial system, and adjusting the growth process parameters determined in step S1;

[0011] S4. A silicon source and a carbon source are introduced into the reaction chamber, and an n-type or p-type doping source is introduced according to the doping type different from that of the trench structure layer, and epitaxial growth is started according to the growth process parameters determined in step S1, wherein the growth time is t epi , the deposition thickness at the bottom of the groove is G R_tb ·t epi , the deposition thickness at the bottom of the groove is controlled to be ≤3μm by controlling the growth time;

[0012] S5. After the growth is completed, the silicon source and the carbon source are turned off, the hydrogen flow rate is kept constant, and the pressure of the reaction chamber is quickly reduced;

[0013] S6. According to the etching process parameters determined in step S2, hydrogen chloride gas is introduced into the reaction chamber, and the epitaxial layer on the trench structure table is removed by hydrogen chloride-assisted hydrogen etching, while improving the surface quality of the epitaxial layer inside and outside the trench. The etching time is t etch =(G R_mt ·t epi ) / E R_mt ;

[0014] S7. Turn off the hydrogen chloride gas, keep the hydrogen flow rate unchanged, and quickly reduce the pressure in the reaction chamber;

[0015] S8. Repeat steps S4 to S7 n times until n×(G R_tb ·t epi -E R_tb ·t etch ) is greater than the trench depth of the silicon carbide formal wafer, that is, the epitaxial filling of the trench structure is completed;

[0016] S9. After opening the cavity and taking out the wafer, polish and remove the excess epitaxial layer.

[0017] Furthermore, the epitaxial growth process parameters of the formal wafer in step S1 include hydrogen flow rate, reaction chamber growth pressure, growth temperature, silicon-hydrogen ratio and carbon-silicon ratio.

[0018] Furthermore, in step S1, an experiment is performed using a growth experimental sheet with the same trench structure as the silicon carbide formal sheet to be filled to determine the epitaxial growth process parameters of the formal sheet, including the following steps:

[0019] S11. Prepare a test piece having the same groove structure as the formal piece to be filled;

[0020] S12. The experimental piece is placed on a graphite susceptor in the reaction chamber of the epitaxial system; the reaction chamber gas is replaced multiple times with argon gas, hydrogen is introduced into the reaction chamber, and the hydrogen flow rate is gradually increased to 60-120 L / min. Hydrogen or argon gas is used as a flotation gas to drive the graphite susceptor to rotate, the reaction chamber pressure is set to 200-400 mbar, and the reaction chamber is gradually heated to a growth temperature of 1600-1700°C;

[0021] S13. A silicon source and a carbon source are introduced into the reaction chamber, the silicon-hydrogen ratio is controlled to be less than 0.08%, the carbon-silicon ratio is controlled to be 0.6 to 1.3, and an n-type or p-type doping source is introduced according to the doping type different from that of the trench structure layer to start epitaxial growth, and the growth time is t1;

[0022] S14. After the growth is completed, the growth source and the doping source are turned off, the temperature of the reaction chamber is cooled to room temperature in a hydrogen atmosphere, and then the hydrogen is discharged, and the gas in the reaction chamber is replaced multiple times by argon gas, and finally the reaction chamber pressure is inflated to atmospheric pressure with argon gas, and the cavity is opened to take out the slice;

[0023] S15. After slicing the experimental piece, analyze its cross section to obtain the epitaxial deposition thickness δ on the groove table surface. mt , and the epitaxial deposition thickness δ at the bottom of the trench tb , according to the growth time t1, the trench terrace epitaxial deposition rate G is obtained R_mt =δ mt / t1, epitaxial deposition rate G at the bottom of the trench R_tb =δ tb / t1;

[0024] S16. When G R_mt / G R_tb ≤0.5, the process parameters in steps S12 and S13 are used as the epitaxial growth process parameters of the formal wafer; when G R_mt / G R_tb >0.5, increase the pressure in the reaction chamber and repeat steps S12 to S15 until G is satisfied. R_mt / G R_tb ≤0.5, and the process parameters at this time are used as the epitaxial growth process parameters of the formal wafer.

[0025] Further, in step S2, an etching test piece having the same groove structure and the same deposition thickness as the growth test piece obtained in S1 is used to conduct an experiment to determine the hydrogen chloride etching process parameters, including the following steps:

[0026] S21. The etching test piece is placed on a graphite base in the reaction chamber, and the epitaxial deposition thickness of the groove table of the etching test piece is δ ′ mt , the epitaxial deposition thickness at the bottom of the trench is δ t ′ b ; Use argon to replace the reaction chamber gas multiple times, set the reaction chamber etching pressure to 80-400 mbar, adjust the process parameters to the same as step S1 except for the pressure, and use hydrogen or argon as the flotation gas to drive the graphite base to rotate;

[0027] S22. Hydrogen chloride gas is introduced into the reaction chamber, the chlorine-hydrogen ratio is controlled to be ≥1%, and hydrogen etching is started for a time of t2;

[0028] S23. After the etching is completed, the hydrogen chloride is turned off, and the temperature of the reaction chamber is cooled to room temperature in a hydrogen atmosphere. After the temperature of the reaction chamber reaches room temperature, the hydrogen is discharged, and the gas in the reaction chamber is replaced several times by argon gas. Finally, the reaction chamber pressure is inflated to atmospheric pressure with argon gas, and the cavity is opened to take the film;

[0029] S24. Analyze its cross section to obtain the epitaxial deposition thickness δ on the trench table ′ mt_E , and the epitaxial deposition thickness δ at the bottom of the trench t ′ b_E , under the corresponding conditions, the trench terrace etching rate E R_mt =(δ ′ mt -δ ′ mt_E ) / t2, the etching rate E at the bottom of the trench R_tb =(δ t ′ b -δ t ′ b_E ) / t2;

[0030] S25.When E R_mt / E R_tb ≥2, the reaction chamber pressure in step S21 and the chlorine-hydrogen ratio in step S22 are used as the etching process parameters for the formal wafer; when E R_mt / E R_tb <2, modify the reaction chamber pressure and repeat steps S21 to S24 until E is satisfied. R_mt / ER_tb ≥2, the reaction chamber pressure and chlorine-hydrogen ratio at this time are used as the etching process parameters for the formal wafer.

[0031] Furthermore, in step S3, argon is first used to replace the reaction chamber gas multiple times, and then hydrogen is introduced into the reaction chamber according to the growth process parameters determined in step S1 and the flow rate is gradually increased to the hydrogen flow rate determined in step S1, the reaction chamber is gradually heated to the growth temperature determined in step S1, and hydrogen or argon is used as a flotation gas to drive the graphite base to rotate.

[0032] Furthermore, in step S8, n×(G R_tb ·t epi -E R_tb ·t etch ) is 1.05-1.1 times the groove depth of the silicon carbide formal sheet.

[0033] Furthermore, step S9 of opening a cavity and taking out a wafer includes: closing the growth source and the doping source, cooling the temperature of the reaction chamber to room temperature in a hydrogen atmosphere, exhausting the hydrogen after the temperature of the reaction chamber reaches room temperature, replacing the gas in the reaction chamber with argon for multiple times, and finally inflating the reaction chamber pressure to atmospheric pressure with argon before opening the cavity and taking out the wafer.

[0034] Furthermore, in step S9, after the cavity is opened and the wafer is taken out, the redundant epitaxial layer is removed by chemical mechanical polishing.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The present invention designs a preliminary experiment and uses an experimental piece with the same trench structure as the silicon carbide to be filled to conduct the preliminary experiment. After obtaining suitable growth parameters, the growth and etching of the formal piece are carried out, which can improve the accuracy. Compared with the conventional silicon carbide (SiC) based epitaxial process, the epitaxial filling rate of the high aspect ratio trench structure is greatly increased, and the occurrence of voids in the trench structure is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematic diagram of the epitaxial filling process of the trench structure.

[0038] Figure 2 Schematic diagram of the epitaxial growth rate and etching rate at the bottom of the trench and on the trench terrace as the pressure of the reaction chamber changes.

[0039] Figure 3 1 is a cross-sectional scanning electron microscope scanning result of the trench structure grown in the embodiment. DETAILED DESCRIPTION

[0040] The present invention is further described below in conjunction with examples. The examples are only used to illustrate the present invention and do not constitute a limitation on the scope of the claims. Other alternative means that can be thought of by those skilled in the art are all within the scope of the claims of the present invention.

[0041] Embodiment 1,

[0042] A method for epitaxial filling of a silicon carbide trench structure, such as Figure 1 As shown, the following steps are included:

[0043] S1. Use the same growth test piece as the silicon carbide formal piece to be filled with trench structure to conduct experiments, determine the epitaxial growth process parameters of the formal piece, including hydrogen flow rate, reaction chamber growth pressure, growth temperature, silicon-hydrogen ratio and carbon-silicon ratio, and obtain the epitaxial deposition rate G of the trench table under this condition R_mt and the epitaxial deposition rate G at the bottom of the trench R_tb , including the following steps:

[0044] S11. Prepare a test piece having the same groove structure as the formal piece to be filled;

[0045] S12. The experimental piece is placed on a graphite susceptor in the reaction chamber of the epitaxial system; the reaction chamber gas is replaced multiple times with argon gas, hydrogen is introduced into the reaction chamber, and the hydrogen flow rate is gradually increased to 60-120 L / min. Hydrogen or argon gas is used as a flotation gas to drive the graphite susceptor to rotate, the reaction chamber pressure is set to 200-400 mbar, and the reaction chamber is gradually heated to a growth temperature of 1600-1700°C;

[0046] S13. A silicon source and a carbon source are introduced into the reaction chamber, the silicon-hydrogen ratio is controlled to be less than 0.08%, the carbon-silicon ratio is controlled to be 0.6 to 1.3, and an n-type or p-type doping source is introduced according to the doping type different from that of the trench structure layer to start epitaxial growth, and the growth time is t1;

[0047] S14. After the growth is completed, the growth source and the doping source are turned off, the temperature of the reaction chamber is cooled to room temperature in a hydrogen atmosphere, and then the hydrogen is discharged, and the gas in the reaction chamber is replaced multiple times by argon gas, and finally the reaction chamber pressure is inflated to atmospheric pressure with argon gas, and the cavity is opened to take out the slice;

[0048] S15. After slicing the experimental piece, analyze its cross section to obtain the epitaxial deposition thickness δ on the groove table surface. mt , and the epitaxial deposition thickness δ at the bottom of the trench tb , according to the growth time t1, the trench terrace epitaxial deposition rate G is obtained R_mt =δ mt / t1, epitaxial deposition rate G at the bottom of the trench R_tb =δ tb / t1;

[0049] S16.According to Figure 2 (a) shows the relationship between the epitaxial growth rate and the reaction chamber pressure. R_mt / G R_tb ≤0.5, the process parameters in steps S12 and S13 are used as the epitaxial growth process parameters of the formal wafer; when G R_mt / G R_tb >0.5, increase the pressure in the reaction chamber and repeat steps S12 to S15 until G is satisfied. R_mt / G R_tb ≤0.5, and the process parameters at this time are used as the epitaxial growth process parameters of the formal wafer.

[0050] S2. Use the etching test piece with the same groove structure and the same deposition thickness as the growth test piece in S1 to conduct experiments, determine the hydrogen chloride etching process parameters, including the etching pressure of the reaction chamber and the ratio of chloride to hydrogen, and obtain the etching rate E of the groove table under this condition. R_mt and the etching rate E at the bottom of the trench R_tb ;

[0051] S21. The etching test piece is placed on a graphite base in the reaction chamber, and the epitaxial deposition thickness of the groove table of the etching test piece is δ ′ mt , the epitaxial deposition thickness at the bottom of the trench is δ t ′ b ; Use argon to replace the reaction chamber gas multiple times, set the reaction chamber etching pressure to 80-400 mbar, adjust the process parameters to the same as step S1 except for the pressure, and use hydrogen or argon as the flotation gas to drive the graphite base to rotate;

[0052] S22. Hydrogen chloride gas is introduced into the reaction chamber, the chlorine-hydrogen ratio is controlled to be ≥1%, and hydrogen etching is started for a time of t2;

[0053] S23. After the etching is completed, the hydrogen chloride is turned off, and the temperature of the reaction chamber is cooled to room temperature in a hydrogen atmosphere. After the temperature of the reaction chamber reaches room temperature, the hydrogen is discharged, and the gas in the reaction chamber is replaced several times by argon gas. Finally, the reaction chamber pressure is inflated to atmospheric pressure with argon gas, and the cavity is opened to take the film;

[0054] S24. Analyze its cross section to obtain the epitaxial deposition thickness δ on the trench table ′ mt_E , and the epitaxial deposition thickness δ at the bottom of the trench t ′ b_E , under the corresponding conditions, the trench terrace etching rate E R_mt =(δ ′ mt-δ ′ mt_E ) / t2, the etching rate E at the bottom of the trench R_tb =(δ t ′ b -δ t ′ b_E ) / t2;

[0055] S25.According to Figure 2 (b) shows the relationship between the etching rate and the reaction chamber pressure. R_mt / E R_tb ≥2, the reaction chamber pressure in step S21 and the chlorine-hydrogen ratio in step S22 are used as the etching process parameters for the formal wafer; when E R_mt / E R_tb <2, modify the reaction chamber pressure and repeat steps S21 to S24 until E is satisfied. R_mt / E R_tb ≥2, the reaction chamber pressure and chlorine-hydrogen ratio at this time are used as the etching process parameters for the formal wafer.

[0056] S3. placing the grooved silicon carbide wafer on the graphite susceptor in the reaction chamber of the epitaxial system, replacing the reaction chamber gas with argon gas for multiple times, and then introducing hydrogen into the reaction chamber according to the growth process parameters determined in step S1 and gradually increasing the flow rate to the hydrogen flow rate determined in step S1, gradually heating the reaction chamber to the growth temperature determined in step S1, and using hydrogen or argon as a flotation gas to drive the graphite susceptor to rotate;

[0057] S4. A silicon source and a carbon source are introduced into the reaction chamber, and an n-type or p-type doping source is introduced according to the doping type different from that of the trench structure layer, and epitaxial growth is started according to the growth process parameters determined in step S1, wherein the growth time is t epi , the deposition thickness at the bottom of the groove is G R_tb ·t epi , the deposition thickness at the bottom of the groove is controlled to be ≤3μm by controlling the growth time;

[0058] S5. After the growth is completed, the silicon source and the carbon source are turned off, the hydrogen flow rate is kept constant, and the pressure of the reaction chamber is quickly reduced;

[0059] S6. According to the etching process parameters determined in step S2, hydrogen chloride gas is introduced into the reaction chamber, and the epitaxial layer on the trench structure table is removed by hydrogen chloride-assisted hydrogen etching, while improving the surface quality of the epitaxial layer inside and outside the trench. The etching time is t etch =(G R_mt ·t epi ) / E R_mt ;

[0060] S7. Turn off the hydrogen chloride gas, keep the hydrogen flow rate unchanged, and quickly reduce the pressure in the reaction chamber;

[0061] S8. Repeat steps S4 to S7 n times until n×(G R_tb ·t epi -E R_yb ·t etch ) is greater than the trench depth of the silicon carbide formal sheet, that is, the epitaxial filling of the trench structure is completed; in step S8, n×(G R_tb ·t epi -E R_tb ·t etch ) is 1.05-1.1 times the groove depth of the silicon carbide formal sheet; multiple deposition and etching such as Figure 1 As shown in (a)-(e), after multiple deposition and etching, the filling reaches 1.05-1.1 times the depth of the trench, completing the trench deep pit filling.

[0062] S9. Turn off the growth source and doping source, cool the reaction chamber to room temperature in a hydrogen atmosphere, exhaust the hydrogen after the reaction chamber reaches room temperature, replace the gas in the reaction chamber multiple times with argon, and finally inflate the reaction chamber to atmospheric pressure with argon. Then open the cavity and take out the wafer. Then remove the excess epitaxial layer by chemical mechanical polishing. As shown in Figure (f), the final step is to remove the excess deposition.

[0063] The SEM image of the silicon carbide structure obtained by the final growth and filling is shown in Figure 3 As shown, the accuracy is high, no voids occur, and there is a significant improvement.

[0064] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for epitaxial filling of a silicon carbide trench structure, characterized in that: The following steps are involved: S1. Use the same growth test piece as the silicon carbide formal piece to be filled in the trench structure to conduct experiments, determine the epitaxial growth process parameters of the formal piece, and obtain the epitaxial deposition rate of the trench table under this condition and the epitaxial deposition rate at the bottom of the trench , wherein determining the epitaxial growth process parameters of the formal slice includes the following steps: S11. Prepare a test piece having the same groove structure as the formal piece to be filled; S12. The experimental piece is placed on a graphite susceptor in a reaction chamber of an epitaxial system; the reaction chamber gas is replaced multiple times with argon gas, hydrogen is introduced into the reaction chamber, and the hydrogen flow rate is gradually increased to 60-120 L / min. Hydrogen or argon gas is used as a flotation gas to drive the graphite susceptor to rotate, the reaction chamber pressure is set to 200-400 mbar, and the reaction chamber is gradually heated to a growth temperature of 1600-1700°C; S13. A silicon source and a carbon source are introduced into the reaction chamber, the silicon-hydrogen ratio is controlled to be less than 0.08%, the carbon-silicon ratio is controlled to be 0.6-1.3, and an n-type or p-type doping source is introduced according to the doping type different from that of the trench structure layer to start epitaxial growth, and the growth time is t1; S14. After the growth is completed, the growth source and the doping source are turned off, the temperature of the reaction chamber is cooled to room temperature in a hydrogen atmosphere, and then the hydrogen is discharged, and the gas in the reaction chamber is replaced multiple times by argon gas, and finally the reaction chamber pressure is inflated to atmospheric pressure with argon gas, and the cavity is opened to take out the slice; S15. After slicing the experimental piece, analyze its cross section to obtain the epitaxial deposition thickness on the groove table , and the thickness of the epitaxial deposition at the bottom of the trench , according to the growth time t1, the epitaxial deposition rate of the trench terrace is obtained , epitaxial deposition rate at the bottom of the trench ; S16. When When , the process parameters in steps S12 and S13 are used as the epitaxial growth process parameters of the formal wafer; when When the pressure in the reaction chamber is increased, steps S12 to S15 are repeated until the pressure is satisfied. , the process parameters at this time are used as the epitaxial growth process parameters of the formal wafer; S2. Use the same trench structure and deposition thickness of the growth test piece in S1 to conduct experiments, determine the hydrogen chloride etching process parameters, including the reaction chamber etching pressure and the chlorine-hydrogen ratio, and obtain the etching rate of the trench table under these conditions. and the etching rate at the bottom of the trench ; S3. placing the formal silicon carbide sheet containing the groove structure on a graphite susceptor in the reaction chamber of the epitaxial system, and adjusting the growth process parameters determined in step S1; S4. A silicon source and a carbon source are introduced into the reaction chamber, and an n-type or p-type doping source is introduced according to the doping type different from that of the trench structure layer, and epitaxial growth is started according to the growth process parameters determined in step S1, wherein the growth time is , the deposition thickness at the bottom of the trench is , the deposition thickness at the bottom of the groove is controlled to be ≤3 μm by controlling the growth time; S5. After the growth is completed, the silicon source and the carbon source are turned off, the hydrogen flow rate is kept constant, and the pressure of the reaction chamber is quickly reduced; S6. According to the etching process parameters determined in step S2, hydrogen chloride gas is introduced into the reaction chamber to remove the epitaxial layer on the trench structure table surface by hydrogen chloride-assisted hydrogen etching, while improving the surface quality of the epitaxial layer inside and outside the trench. The etching time is ; S7. Turn off the hydrogen chloride gas, keep the hydrogen flow rate unchanged, and quickly reduce the pressure in the reaction chamber; S8. Repeat steps S4 to S7n times until The trench depth is greater than that of the silicon carbide formal wafer, that is, the epitaxial filling of the trench structure is completed; S9. After opening the cavity and taking out the wafer, polish and remove the excess epitaxial layer.

2. The method for epitaxial filling of a silicon carbide trench structure according to claim 1, characterized in that: The epitaxial growth process parameters of the formal wafer in step S1 include hydrogen flow rate, reaction chamber growth pressure, growth temperature, silicon-hydrogen ratio and carbon-silicon ratio.

3. The method for epitaxial filling of a silicon carbide trench structure according to claim 1, characterized in that: In step S2, an etching test piece having the same groove structure and the same deposition thickness as the growth test piece obtained in step S1 is used to conduct an experiment to determine the hydrogen chloride etching process parameters, including the following steps: S21. The etching test piece is placed on a graphite base in the reaction chamber, and the epitaxial deposition thickness of the groove table of the etching test piece is , the epitaxial deposition thickness at the bottom of the trench ; Use argon to replace the reaction chamber gas multiple times, set the reaction chamber etching pressure to 80~400mbar, adjust the process parameters to the same as step S1 except for the pressure, and use hydrogen or argon as the flotation gas to drive the graphite base to rotate; S22. Hydrogen chloride gas is introduced into the reaction chamber, the chlorine-hydrogen ratio is controlled to be ≥1%, and hydrogen etching is started for a time of t2; S23. After the etching is completed, the hydrogen chloride is turned off, and the temperature of the reaction chamber is cooled to room temperature in a hydrogen atmosphere. After the temperature of the reaction chamber reaches room temperature, the hydrogen is discharged, and the gas in the reaction chamber is replaced several times by argon gas. Finally, the reaction chamber pressure is inflated to atmospheric pressure with argon gas, and the cavity is opened to take the film; S24. Analyze its cross section to obtain the epitaxial deposition thickness on the trench terrace , and the thickness of the epitaxial deposition at the bottom of the trench , under the corresponding conditions, the trench terrace etching rate , the etching rate at the bottom of the trench ; S25. When When , the reaction chamber pressure in step S21 and the chlorine-hydrogen ratio in step S22 are used as the etching process parameters of the formal wafer; when When the pressure in the reaction chamber is modified, steps S21 to S24 are repeated until the pressure is satisfied. At this time, the reaction chamber pressure and the chlorine-hydrogen ratio are used as the etching process parameters for the formal wafer.

4. The method for epitaxial filling of a silicon carbide trench structure according to claim 1, characterized in that: In step S3, argon is first used to replace the reaction chamber gas multiple times, and then hydrogen is introduced into the reaction chamber according to the growth process parameters determined in step S1 and the flow rate is gradually increased to the hydrogen flow rate determined in step S1, the reaction chamber is gradually heated to the growth temperature determined in step S1, and hydrogen or argon is used as a flotation gas to drive the graphite base to rotate.

5. The method for epitaxial filling of a silicon carbide trench structure according to claim 1, characterized in that: In step S8 The value is 1.05-1.1 times the groove depth of the silicon carbide formal sheet.

6. The method for epitaxial filling of a silicon carbide trench structure according to claim 1, characterized in that: Step S9 includes: closing the growth source and the doping source, cooling the reaction chamber temperature to room temperature in a hydrogen atmosphere, exhausting the hydrogen after the reaction chamber temperature reaches room temperature, replacing the gas in the reaction chamber with argon gas for multiple times, and finally inflating the reaction chamber pressure to atmospheric pressure with argon gas before opening the cavity and taking the film.

7. The method for epitaxial filling of a silicon carbide trench structure according to claim 1, characterized in that: In step S9, after the cavity is opened and the wafer is taken out, the excess epitaxial layer is removed by chemical mechanical polishing.