LED chip and preparation method thereof

By forming an annealing layer on the epitaxial structure of the GaN-based LED chip and injecting electrons, the problem of uneven distribution of electrons and holes is solved, the luminescence efficiency and efficiency stability under large currents are improved, and more efficient photoelectric performance is achieved.

CN114242860BActive Publication Date: 2024-11-26JIANGSU INST OF ADVANCED SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111618418.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-27
Publication Date
2024-11-26
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

Traditional GaN-based LED chips have a fast electron mobility and high free electron concentration, resulting in uneven distribution of electrons and holes, which reduces the luminous efficiency, especially under large currents, which is serious in the phenomenon of rapid efficiency drop.

Method used

An annealing layer is formed on the epitaxial structure, and annealing treatment allows the annealing layer to inject electrons into the epitaxial structure to improve the hole concentration, improve the distribution unevenness of electrons and holes, and improve the radiation recombination efficiency.

Benefits of technology

It effectively improves the luminous efficiency and radiation recombination efficiency of LED chips, improves the efficiency drop effect under large currents, and improves the overall photoelectric performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114242860B_ABST
    Figure CN114242860B_ABST
Patent Text Reader

Abstract

The invention discloses an LED chip and a preparation method thereof. The preparation method of the LED chip comprises: providing a substrate; providing a substrate; forming an epitaxial structure and an annealing layer; the epitaxial structure is located on the upper surface of the substrate, the annealing layer is located on the upper surface of the epitaxial structure, and the annealing layer exposes the epitaxial structure; forming a first electrode on the upper surface of the annealing layer and the exposed epitaxial structure, and the annealing layer injects electrons into the epitaxial structure during annealing treatment to increase the hole concentration in the epitaxial structure, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under large current.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor optoelectronic devices, and in particular to an LED chip and a preparation method thereof. Background Art

[0002] GaN-based light-emitting diode (LED) is a semiconductor light-emitting device with the advantages of long life, low energy consumption, small size and high reliability. It has become the most promising lighting source and an important trend in leading lighting technology. However, there are still problems with low luminous intensity and efficiency. Further improving the luminous intensity and light efficiency of LED is the goal of the development of LED lighting technology.

[0003] Traditional GaN-based LED chips have a faster electron mobility than holes, and the concentration of free electrons is higher than that of holes. In addition, the p-type layer at the top of the chip is difficult to obtain a high hole concentration due to the passivation effect of hydrogen atoms, which easily leads to uneven distribution of electrons and holes in the multi-quantum well (MQW) light-emitting layer. The holes are concentrated in the MQW layer closer to the p-type layer, and gradually decay in the n-type direction, which is not conducive to the recombination of electrons and holes, thereby reducing the luminous efficiency of the LED chip. Summary of the invention

[0004] Based on this, it is necessary to provide an LED chip and a preparation method thereof to address the problems in the above-mentioned background technology. During the annealing process, the annealing layer formed on the epitaxial structure injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure.

[0005] In order to solve the above technical problems, the first aspect of the present application provides a method for preparing an LED chip, comprising:

[0006] providing a substrate;

[0007] forming an epitaxial structure and an annealing layer, wherein the epitaxial structure is located on the upper surface of the substrate, the annealing layer is located on the upper surface of the epitaxial structure, and the annealing layer exposes the epitaxial structure; during the annealing process, the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure;

[0008] A first electrode is formed on the upper surface of the annealing layer and the exposed epitaxial structure.

[0009] In the preparation method of the LED chip provided in the above embodiment, a substrate, an epitaxial structure, an annealing layer and a first electrode are arranged in sequence from bottom to top, and the first electrode is located on the upper surface of the annealing layer and the exposed epitaxial structure; the obtained structure formed as above is annealed so that the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under large current.

[0010] In one embodiment, after forming the first electrode on the upper surface of the annealing layer and the exposed epitaxial structure, the method further comprises:

[0011] applying a current to the first electrode and performing the annealing treatment on the obtained structure;

[0012] The applied current is 1 mA-40 mA; the temperature of the annealing treatment is 150° C.-450° C.; the time of the annealing treatment is 5 min-50 min; and the atmosphere of the annealing treatment includes a nitrogen atmosphere and / or an oxygen atmosphere.

[0013] In one embodiment, the base includes a substrate, a buffer layer, a non-doped layer and an N-type semiconductor layer stacked in sequence from bottom to top; the forming of the epitaxial structure and the annealing layer includes:

[0014] forming a light-emitting material layer on the upper surface of the substrate;

[0015] forming a P-type nitride stacked material layer on the upper surface of the light emitting material layer;

[0016] forming an annealing material layer on the upper surface of the P-type nitride stacked material layer;

[0017] Sequentially etching and removing a portion of the annealing material layer, a portion of the P-type nitride stacked material layer, and a portion of the light-emitting material layer to expose the N-type semiconductor layer, and forming a light-emitting layer, a P-type nitride stacked layer, and an annealing layer stacked sequentially from bottom to top, wherein the light-emitting layer and the P-type nitride stacked layer together constitute the epitaxial structure;

[0018] After forming the annealing layer, the method further includes: forming a second electrode on the exposed upper surface of the N-type semiconductor layer.

[0019] In one embodiment, forming a P-type nitride stacked material layer on the upper surface of the light emitting material layer includes:

[0020] forming a first P-type nitride material layer on the upper surface of the light emitting material layer;

[0021] forming a P-type nitride barrier material layer on the upper surface of the first P-type nitride material layer;

[0022] forming a non-doped nitride material layer on the upper surface of the P-type nitride barrier material layer;

[0023] forming a second P-type nitride material layer on the upper surface of the undoped nitride material layer;

[0024] After etching the portion of the P-type nitride stack material layer, a first P-type nitride layer, a P-type nitride barrier layer, an undoped nitride layer and a second P-type nitride layer are formed which are stacked in sequence from bottom to top. The first P-type nitride layer, the P-type nitride barrier layer, the undoped nitride layer and the second P-type nitride layer together constitute the P-type nitride stack.

[0025] In one embodiment, the second P-type nitride layer contains a magnesium-hydrogen complex; the annealing layer injects electrons into the second P-type nitride layer, and the electrons capture magnesium-hydrogen bonds to decompose to form hydrogen ions, thereby increasing the hole concentration in the second P-type nitride layer.

[0026] In one embodiment, after forming the annealing layer, the method further comprises:

[0027] The annealing layer is etched to have an opening in the annealing layer, wherein the opening exposes the upper surface of the epitaxial structure.

[0028] The annealing layer includes an N-type nitride layer, and forming a first electrode on the upper surface of the annealing layer and the exposed epitaxial structure includes:

[0029] A first N-type electrode is formed on the upper surface of the annealing layer, and a first P-type electrode is formed in the opening, wherein the first P-type electrode and the first N-type electrode together constitute the first electrode.

[0030] A second aspect of the present application provides an LED chip, comprising:

[0031] substrate;

[0032] an epitaxial structure, located on the upper surface of the substrate;

[0033] An annealing layer is located on the upper surface of the epitaxial structure, and the annealing layer exposes the epitaxial structure; during the annealing process, the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure;

[0034] The first electrode is located on the upper surface of the annealing layer and on the exposed epitaxial structure.

[0035] In one embodiment, the epitaxial structure includes a light-emitting layer and a P-type nitride stack stacked in sequence from bottom to top; the P-type nitride stack includes a first P-type nitride layer, a P-type nitride barrier layer, an undoped nitride layer and a second P-type nitride layer stacked in sequence from bottom to top.

[0036] In one embodiment, the second P-type nitride layer contains a magnesium-hydrogen complex; the annealing layer injects electrons into the second P-type nitride layer, and the electrons capture magnesium-hydrogen bonds to decompose to form hydrogen ions, thereby increasing the hole concentration in the second P-type nitride layer.

[0037] In one embodiment, the first electrode includes a first N-type electrode and a first P-type electrode, the first N-type electrode is located on the upper surface of the annealing layer; the annealing layer has an opening, the opening exposes the second insertion layer; the first P-type electrode is located in the opening;

[0038] Wherein, the base comprises a substrate, a buffer layer, a non-doped layer and an N-type semiconductor layer stacked in sequence from bottom to top;

[0039] The LED chip further includes: a second electrode located on the upper surface of the N-type semiconductor layer.

[0040] In the LED chip provided in the above embodiment, a substrate, an epitaxial structure, an annealing layer and a first electrode are sequentially arranged, and the first electrode is located on the upper surface of the annealing layer and the exposed epitaxial structure; the obtained structure formed as above is annealed so that the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under large current.

[0041] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, drawings of other embodiments can be obtained based on these drawings without paying any creative work.

[0043] Figure 1 A schematic diagram of a process for preparing a semiconductor structure provided in an embodiment of the present application;

[0044] Figure 2 A schematic diagram of the structure of a substrate, a multi-layer material layer forming an epitaxial structure, and an annealed material layer provided in one embodiment of the present application;

[0045] Figure 3 A schematic diagram of a structure obtained after forming an epitaxial structure and an annealing layer provided in an embodiment of the present application;

[0046] Figure 4 A schematic diagram of a structure obtained by forming an opening provided in an embodiment of the present application;

[0047] Figure 5 A schematic diagram of a structure obtained after forming a first electrode and a second electrode provided in an embodiment of the present application;

[0048] Figure 6 A schematic structural diagram of a substrate, a multi-layer material layer forming an epitaxial structure, and an annealed material layer provided in another embodiment of the present application;

[0049] Figure 7 A schematic diagram of a structure obtained after forming an epitaxial structure and an annealing layer provided in another embodiment of the present application;

[0050] Figure 8 A schematic structural diagram of a structure obtained after forming a first electrode and a second electrode provided in another embodiment of the present application;

[0051] Fig. 9 A schematic structural diagram of a substrate, a multi-layer material layer forming an epitaxial structure, and an annealed material layer provided in another embodiment of the present application;

[0052] Fig.10 A schematic diagram of a structure obtained after forming an epitaxial structure and an annealing layer provided in another embodiment of the present application;

[0053] Fig.11 This is a schematic diagram of a structure obtained after forming a first electrode and a second electrode in another embodiment of the present application. Explanation of reference numerals: 10, base; 11, substrate; 12, buffer layer; 13, non-doped layer; 14, N-type semiconductor layer;

[0054] 20. epitaxial structure; 21. light-emitting layer; 211. light-emitting material layer; 22. first P-type nitride layer; 221. first P-type nitride material layer; 23. P-type nitride barrier layer; 231. P-type nitride barrier material layer; 24. undoped nitride layer; 241. undoped nitride layer; 25. second P-type nitride layer; 251. second P-type nitride material layer; 26. P-type nitride stack; 261. P-type nitride stack material layer;

[0055] 30. annealing layer; 31. annealing material layer; 311. opening;

[0056] 40. first electrode; 41. first N-type electrode; 42. first P-type electrode;

[0057] 50. a second electrode;

[0058] 60. Transparent conductive layer. DETAILED DESCRIPTION

[0059] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0060] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0061] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present application, the first element, component, region, layer or part discussed below can be represented as a second element, component, region, layer or part.

[0062] Spatially relative terms such as "under," "below," "below," "under," "above," "above," etc., may be used herein for ease of description to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that in addition to the orientations shown in the figures, the spatially relative terms are intended to include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, then the elements or features described as "under other elements" or "under" or "under" will be oriented as "on" the other elements or features. Therefore, the exemplary terms "under" and "under" may include both upper and lower orientations. The device may be oriented otherwise (rotated 90 degrees or other orientations) and the spatial descriptors used herein are interpreted accordingly.

[0063] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0064] Embodiments of the application are described herein with reference to cross-sectional views that are schematic diagrams of ideal embodiments (and intermediate structures) of the application. Thus, variations from the shapes shown due to, for example, manufacturing techniques and / or tolerances can be expected. Therefore, embodiments of the application should not be limited to the specific shapes of the zones shown herein, but rather include shape deviations due to, for example, manufacturing, and the zones shown in the figures are schematic in nature, and their shapes are not intended to display the actual shapes of the zones of the device and are not intended to limit the scope of the application.

[0065] The existing LED chip structure generally includes a buffer layer, an undoped GaN layer, an n-type doped layer, a multi-quantum well layer (MQW), an electron blocking layer, and a p-type layer. There are two problems: 1. Since the mobility of electrons is faster than that of holes, and the concentration of free electrons is higher than that of holes, and it is difficult to obtain a high hole concentration due to the passivation of H atoms in the p-type layer, it is easy to cause uneven distribution of electrons and holes in the MQW. Holes are concentrated in the MQW close to the p-type layer, and gradually decay in the n-type direction, which is not conducive to the recombination of electrons and holes; 2. Due to the high electron concentration and fast migration, electrons are easy to overflow into the p-type layer and recombine with ionized holes in the p-type layer, reducing the ionization efficiency of holes and generating non-radiative recombination, reducing the injection efficiency of holes and causing a sudden drop in luminous efficiency, which is more serious under high current working conditions.

[0066] In one embodiment of the present application, Figure 1 As shown, a method for preparing an LED chip is provided, comprising the following steps:

[0067] Step S10: providing a substrate;

[0068] Step S20: forming an epitaxial structure and an annealing layer, wherein the epitaxial structure is located on the upper surface of the substrate, the annealing layer is located on the upper surface of the epitaxial structure, and the annealing layer exposes the epitaxial structure; during the annealing process, the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure;

[0069] Step S30: forming a first electrode on the upper surface of the annealing layer and the exposed epitaxial structure.

[0070] In the preparation method of the LED chip provided in the above embodiment, a substrate, an epitaxial structure, an annealing layer and a first electrode are arranged in sequence from bottom to top, and the first electrode is located on the upper surface of the annealing layer and the exposed epitaxial structure; the obtained structure formed as above is annealed so that the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under large current.

[0071] The substrate, epitaxial structure, and annealing layer proposed in the embodiments of the present application can all be deposited using Metal-organic Chemical Vapor Deposition (MOCVD) technology, but this is of course not limited to this, and other thin film deposition technologies may also be used.

[0072] In one embodiment, Figure 2As shown, the base 10 provided in step S10 includes a substrate 11 , a buffer layer 12 , a non-doped layer 13 and an N-type semiconductor layer 14 stacked sequentially from bottom to top.

[0073] In one embodiment, the epitaxial structure 20 and the substrate 10 are in a mesa structure, and the epitaxial structure 20 exposes the substrate 10 (eg Figure 3 shown).

[0074] As an example, the substrate 11 includes but is not limited to any one or more combinations of a sapphire substrate, a silicon carbide substrate, a gallium nitride substrate, a gallium oxide substrate, a zinc oxide substrate or an aluminum nitride substrate; after the substrate 11 is formed, the surface of the substrate 11 is cleaned in a hydrogen atmosphere at a temperature of 1200° C., and the cleaning time can be 5 minutes.

[0075] As an example, the buffer layer 12 includes a low-temperature grown nitride layer, and the thickness of the buffer layer 12 is 10nm-100nm; for example, the thickness of the buffer layer 12 is 10nm, 50nm, 80nm or 100nm, etc. Specifically, the buffer layer 12 can be a non-doped GaN layer, the Ga source required for growth is a trimethyl gallium (TMG) source, the growth atmosphere is a H2 atmosphere, the growth temperature is 600°C, and the growth pressure is 650mbar.

[0076] As an example, the non-doped layer 13 includes a non-doped nitride layer, and the thickness of the non-doped layer 13 is 1um-5um; for example, the thickness of the non-doped layer 13 is 1um, 2um, 3um or 5um, etc. The non-doped layer 13 can be a non-doped GaN layer, the Ga source required for growth is a TMG source, the growth atmosphere is a H2 atmosphere, the growth temperature is 1215°C, and the growth pressure is 300mbar.

[0077] As an example, the N-type semiconductor layer 14 includes an N-type nitride layer, and the thickness of the N-type semiconductor layer 14 is 2.0 μm-5 μm; for example, the thickness of the N-type semiconductor layer 14 is 2.0 μm, 2.5 μm or 5.0 μm, etc. The N-type semiconductor layer 14 can be an N-type doped GaN layer, and the dopant can be Si, and the doping concentration of Si is 5×10 18 cm -3 The Ga source required for growth is TMG source, the growth atmosphere is H2 atmosphere, the growth temperature is 1210℃, and the growth pressure is 150mbar.

[0078] In one embodiment, after step S30: forming a first electrode on the upper surface of the annealing layer and the exposed epitaxial structure, the method further comprises:

[0079] Step S40: applying a current to the first electrode and performing an annealing process on the obtained structure;

[0080] The applied current is 1 mA-40 mA; the annealing temperature is 150° C.-450° C.; the annealing time is 5 min-50 min; and the annealing atmosphere includes a nitrogen atmosphere and / or an oxygen atmosphere.

[0081] It should be noted that the obtained structure mentioned in step S40 may include a substrate, an epitaxial structure, an annealing layer, a first electrode and a second electrode.

[0082] As an example, to ensure that the obtained structure is processed in a pure nitrogen and / or pure oxygen atmosphere, the obtained structure is placed on a heating table in a glove box for annealing. Optionally, the applied current is 1 mA, 10 mA, 20 mA or 40 mA, etc.; the annealing temperature is 150° C., 300° C. or 450° C., etc.; the annealing time is 5 min, 25 min or 50 min, etc.

[0083] The formation of the epitaxial structure, the annealing layer and the first electrode is described from the following three embodiments:

[0084] In one embodiment, step S20: forming an epitaxial structure and an annealing layer, comprises the following steps:

[0085] Step S21: forming a light emitting material layer 211 on the upper surface of the substrate 10;

[0086] Step S22: forming a P-type nitride stacked material layer 261 on the upper surface of the light emitting material layer 211;

[0087] Step S23: forming an annealing material layer 31 on the upper surface of the P-type nitride stacked material layer 261, such as Figure 2 As shown;

[0088] Step S24: etching and removing part of the annealing material layer 31, part of the P-type nitride stacked material layer 261 and part of the light-emitting material layer 211 in sequence to expose the N-type semiconductor layer 14, and forming a light-emitting layer 21, a P-type nitride stacked layer 26 and an annealing layer 30 stacked in sequence from bottom to top, wherein the light-emitting layer and the P-type nitride stacked layer 26 together constitute the epitaxial structure 20, as shown in FIG. Figure 3 shown.

[0089] In one embodiment, if Figure 2 As shown, step S22: forming a P-type nitride stacked material layer on the upper surface of the light-emitting material layer, comprising the following steps:

[0090] Step S221a: forming a first P-type nitride material layer 221 on the upper surface of the light emitting material layer 211;

[0091] Step S222a: forming a P-type nitride barrier material layer 231 on the upper surface of the first P-type nitride material layer 221;

[0092] Step S223a: forming a non-doped nitride material layer 241 on the upper surface of the P-type nitride barrier material layer 231;

[0093] Step S224 a : forming a second P-type nitride material layer 251 on the upper surface of the undoped nitride material layer 241 .

[0094] Specifically, after etching part of the P-type nitride stack material layer 261, a first P-type nitride layer 22, a P-type nitride barrier layer 23, an undoped nitride layer 24 and a second P-type nitride layer 25 are formed which are stacked in sequence from bottom to top. The first P-type nitride layer 22, the P-type nitride barrier layer 23, the undoped nitride layer 24 and the second P-type nitride layer 25 together constitute a P-type nitride stack 26.

[0095] As an example, inductively coupled plasma (ICP) technology can be used to etch part of the annealed material layer 31, part of the second P-type nitride material layer 251, part of the undoped nitride material layer 241, part of the P-type nitride barrier material layer 231, part of the first P-type nitride material layer 221 and part of the light-emitting material layer 211.

[0096] As an example, the light-emitting material layer 211 is a nitride quantum well layer and a nitride quantum barrier layer with 1-30 periodic cycles of repeated structures, the thickness of the nitride quantum well layer is 1-15nm, and the thickness of the quantum barrier layer is 3-20nm; for example, the thickness of the nitride quantum well layer is 1nm, 3nm or 15nm, etc.; the thickness of the quantum barrier layer is 3nm, 11nm or 20nm, etc. The nitride quantum well layer includes an InGaN layer, the growth temperature is 850°C, the growth pressure is 300mbar, the Ga source required for growth is a TEGa source, and the In source required for growth is a TMIn source; the nitride quantum barrier layer includes a GaN layer, the growth temperature is 950°C, the growth pressure is 400mbar, and the Ga source required for growth is a TEGa source.

[0097] Optionally, there are 10 pairs of nitride quantum well layers and nitride quantum barrier layers in total.

[0098] Optionally, the In component in the light-emitting layer 21 may be changed to achieve a light-emitting band of the LED chip within the wavelength range from ultraviolet to green light.

[0099] As an example, the first P-type nitride material layer 221 includes a low-temperature grown P-type GaN layer, and the thickness of the P-type GaN layer is 20nm-200nm; for example, the thickness of the P-type GaN layer is 20nm, 50nm or 200nm, etc. The P-type doping material is magnesium, and the magnesium doping concentration is 2×10 19 cm -3 The Ga source required for growth is TMG source, the growth atmosphere is switched to H2 atmosphere, and the growth temperature is 1100℃.

[0100] As an example, the P-type nitride barrier material layer 231 includes a P-type doped AlGaN layer, and the thickness of the P-type nitride barrier material layer 231 is 10nm-150nm; for example, the thickness of the P-type nitride barrier material layer 231 is 10nm, 100nm or 150nm, etc. The Ga source required for growth is a TMG source, the Al source is a TMAl source, the growth atmosphere is an N2 atmosphere, the growth temperature is 1000°C, and the growth pressure is 150mbar.

[0101] As an example, the non-doped nitride material layer 241 includes a non-doped GaN layer, and the thickness of the non-doped nitride material layer 241 is 10nm-100nm, for example, the thickness of the non-doped nitride material layer 241 is 10nm, 15nm or 100nm, etc. The Ga source required for growth is a TMG source, the growth atmosphere is switched to a H2 atmosphere, the growth temperature is 1100°C, and the growth pressure is 500mbar.

[0102] In one embodiment, the second P-type nitride layer 25 contains a magnesium-hydrogen complex; the annealing layer 30 injects electrons into the second P-type nitride layer 25, and the electrons capture the magnesium-hydrogen bonds to decompose to form hydrogen ions, thereby improving the P-type nitride doping activation efficiency, greatly improving the hole concentration of the second P-type nitride layer 25, and improving the hole injection of the LED chip, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the hole ionization efficiency and radiation recombination efficiency, and improving the efficiency drop effect under large current.

[0103] As an example, the thickness of the second P-type nitride layer 25 is 30nm-300nm; for example, the thickness of the second P-type nitride layer 25 is 30nm, 45nm or 300nm, etc. The second P-type nitride layer 25 can be a P-type GaN layer, the P-type doping material is magnesium, and the magnesium doping concentration is 5×10 19 cm -3 The Ga source required for growth is TMG source, the growth atmosphere is switched to H2 atmosphere, the growth temperature is 1100℃, and the growth pressure is 500mbar.

[0104] As an example, the thickness of the annealed material layer 31 is 1 nm-150 nm, for example, the thickness of the annealed material layer 31 is 1 nm, 50 nm or 150 nm, etc. The annealed material layer 31 includes an N-type GaN layer, and the dopant is Si, and the doping concentration of Si is 5×10 18 cm -3 The Ga source required for growth is TMG source, the growth atmosphere is H2 atmosphere, the growth temperature is 1210℃, and the growth pressure is 150mbar.

[0105] In one embodiment, after forming the annealing layer 30, step S20 further includes:

[0106] Step S201: Etching the annealing layer 30 to form an opening 311 in the annealing layer 30. The opening 311 exposes the upper surface of the epitaxial structure 20. Figure 4 shown.

[0107] In one embodiment, if Figure 5 As shown, the annealing layer includes an N-type nitride layer, and step S30: forming a first electrode 40 on the upper surface of the annealing layer 30 and the exposed epitaxial structure 20 includes:

[0108] Step S31 a : forming a first N-type electrode 41 on the upper surface of the annealing layer 30 , and forming a first P-type electrode 42 in the opening 311 . The first P-type electrode 42 and the first N-type electrode 41 together constitute the first electrode 40 .

[0109] Specifically, the opening 311 exposes the upper surface of the second P-type nitride layer 25 , and the first P-type electrode 42 is formed on the portion of the upper surface of the second P-type nitride layer 25 exposed by the opening 311 .

[0110] In one embodiment, please continue to refer to Figure 5 , Figure 8 as well as Fig.11 , step S20: after forming the annealing layer 30, further comprising:

[0111] Step S202 : forming a second electrode 50 on the exposed upper surface of the N-type semiconductor layer 14 .

[0112] As an example, the second electrode 50 includes an N-type electrode; the first electrode 40 and the second electrode 50 can be prepared simultaneously or in separate steps; the material of the first electrode 40 includes a single layer or a multilayer combination of metals Cr, Al, Au, Pt, Pd, Ti, Ta, and Ni; the material of the second electrode 50 includes a single layer or a multilayer combination of metals Cr, Al, Au, Pt, Pd, Ti, Ta, and Ni; the material of the first electrode 40 and the material of the second electrode 50 can be the same or different.

[0113] In one embodiment, Figure 5 , Figure 8 and Fig.11 As shown, before forming the first electrode 40 and the second electrode 50 , a step of forming a transparent conductive layer 60 is further included, and the first electrode 40 is located on the upper surface of the transparent conductive layer 60 .

[0114] As an example, the transparent conductive layer 60 includes an indium tin oxide material (ITO), and the thickness of the transparent conductive layer 60 is 50 nm-250 nm; for example, the thickness of the transparent conductive layer 60 is 50 nm, 150 nm, or 250 nm, etc.

[0115] In another embodiment, if Figure 6 As shown, step S22: forming a P-type nitride stacked material layer on the upper surface of the light-emitting material layer, comprising the following steps:

[0116] Step S221b: forming a first P-type nitride material layer 221 on the upper surface of the light emitting material layer 211;

[0117] Step S222b: forming a non-doped nitride material layer 241 on the upper surface of the first P-type nitride material layer 221;

[0118] Step S223b: forming a P-type nitride barrier material layer 231 on the upper surface of the first P-type nitride material layer 221;

[0119] Step S224 b : forming a second P-type nitride material layer 251 on the upper surface of the P-type nitride barrier material layer 231 .

[0120] Specifically, after etching a portion of the P-type nitride stack material layer 261, the annealing material layer 31 and the second P-type nitride material layer 251 are etched to expose the P-type nitride barrier material layer 231, and form a first P-type nitride layer 22, a non-doped nitride layer 24, a P-type nitride barrier layer 23 and a second P-type nitride layer 25 stacked in sequence from bottom to top. The first P-type nitride layer 22, the non-doped nitride layer 24, the P-type nitride barrier layer 23 and the second P-type nitride layer 25 together constitute a P-type nitride stack 26, as shown in FIG. Figure 7 shown.

[0121] Regarding the preparation methods of the light-emitting material layer 211, the first P-type nitride material layer 221, the undoped nitride material layer 241, the P-type nitride barrier material layer 231, the second P-type nitride material layer 251 and the annealing material layer 31, please refer to the above text and will not be repeated here.

[0122] In another embodiment, if Figure 8 As shown, step S30: forming a first electrode 40 on the upper surface of the annealing layer 30 and the exposed epitaxial structure 20, including:

[0123] Step S31b: forming a first N-type electrode 41 on the upper surface of the annealing layer, and forming a first P-type electrode 42 on the upper surface of the P-type nitride barrier layer 23, the first P-type electrode 42 being located on opposite sides of the second P-type nitride layer 25 and the annealing layer 30; the first N-type electrode 41 and the first P-type electrode 42 together constitute the first electrode 40.

[0124] In yet another embodiment, Fig. 9 As shown, step S22: forming a P-type nitride stacked material layer on the upper surface of the light-emitting material layer, comprising the following steps:

[0125] Step S221c: forming a non-doped nitride material layer 241 on the upper surface of the light emitting material layer 211;

[0126] Step S222c: forming a first P-type nitride material layer 221 on the upper surface of the undoped nitride material layer 241;

[0127] Step S223c: forming a P-type nitride barrier material layer 231 on the upper surface of the first P-type nitride material layer 221;

[0128] Step S224 c : forming a second P-type nitride material layer 251 on the upper surface of the P-type nitride barrier material layer 231 .

[0129] Specifically, after etching a portion of the P-type nitride stack material layer 261, the annealed material layer 31, the second P-type nitride material layer 251 and the P-type nitride barrier material layer 231 are etched to expose the first P-type nitride material layer 221, and form a non-doped nitride layer 24, a first P-type nitride layer 22, a P-type nitride barrier layer 23 and a second P-type nitride layer 25 stacked in sequence from bottom to top, and the non-doped nitride layer 24, the first P-type nitride layer 22, the P-type nitride barrier layer 23 and the second P-type nitride layer 25 together constitute a P-type nitride stack 26, as shown in FIG. Fig.10 shown.

[0130] Regarding the specific preparation methods of the light-emitting material layer 211, the undoped nitride material layer 241, the first P-type nitride material layer 221, the P-type nitride barrier material layer 231, the second P-type nitride material layer 251 and the annealing material layer, please refer to the above text and will not be repeated here.

[0131] In yet another embodiment, Fig.11 As shown, step S30: forming a first electrode 40 on the upper surface of the annealing layer 30 and the exposed epitaxial structure 20, including:

[0132] Step S31c: forming a first N-type electrode 41 on the upper surface of the annealing layer 30, and forming a first P-type electrode 42 on the upper surface of the first P-type nitride layer 22, the first P-type electrode 42 being located on opposite sides of the annealing layer 30, the second P-type nitride layer 25 and the P-type nitride barrier layer 23; the first N-type electrode 41 and the first P-type electrode 42 together constitute the first electrode 40.

[0133] In one embodiment of the present application, an LED chip is further proposed, which includes: a substrate 10; an epitaxial structure 20, which is located on the upper surface of the substrate 10; an annealing layer 30, which is located on the upper surface of the epitaxial structure 20, and the annealing layer 30 exposes the epitaxial structure 20; the annealing layer 30 injects electrons into the epitaxial structure 20 during the annealing process to increase the hole concentration in the epitaxial structure 20; and a first electrode 40, which is located on the upper surface of the annealing layer 30 and on the exposed epitaxial structure 20.

[0134] In the LED chip provided in the above embodiment, a substrate, an epitaxial structure, an annealing layer and a first electrode are sequentially arranged, and the first electrode is located on the upper surface of the annealing layer and the exposed epitaxial structure; the obtained structure formed as above is annealed so that the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under large current.

[0135] In one embodiment, the base 10 includes a substrate 11 , a buffer layer 12 , a non-doped layer 13 , and an N-type semiconductor layer 14 stacked sequentially from bottom to top.

[0136] In one embodiment, the first electrode 40 includes a first P-type electrode 42 and a first N-type electrode 41 ; the first N-type electrode 41 is located on the upper surface of the annealing layer 30 .

[0137] In one embodiment, the epitaxial structure 20 includes a light-emitting layer 21 and a P-type nitride layer 26 stacked sequentially from bottom to top; the P-type nitride layer 26 includes a first P-type nitride layer 22, a P-type nitride barrier layer 23, an undoped nitride layer 24, and a second P-type nitride layer 25 stacked sequentially from bottom to top.

[0138] Specifically, the annealing layer 30 has an opening 311 , and the opening 311 exposes the second P-type nitride layer 25 ; the first P-type electrode 42 is located in the opening 311 .

[0139] In another embodiment, the epitaxial structure 20 includes a light-emitting layer 21 and a P-type nitride layer 26 stacked sequentially from bottom to top; the P-type nitride layer 26 includes a first P-type nitride layer 22, an undoped nitride layer 24, a P-type nitride barrier layer 23 and a second P-type nitride layer 25 stacked sequentially from bottom to top.

[0140] Specifically, the first P-type electrode 42 is located on the upper surface of the P-type nitride barrier layer 23 , and is located on two opposite sides of the second P-type nitride layer 25 and the annealing layer 30 .

[0141] In another embodiment, the epitaxial structure 20 includes a light-emitting layer 21 and a P-type nitride layer 26 stacked sequentially from bottom to top; the P-type nitride layer 26 includes an undoped nitride layer 24, a first P-type nitride layer 22, a P-type nitride barrier layer 23 and a second P-type nitride layer 25 stacked sequentially from bottom to top.

[0142] As an example, the first P-type electrode 42 is located on the upper surface of the first P-type nitride layer 22 and on two opposite sides of the annealing layer 30 , the second P-type nitride layer 25 and the P-type nitride barrier layer 23 .

[0143] In one embodiment, the second P-type nitride layer 25 contains a magnesium-hydrogen complex; the annealing layer 30 injects electrons into the second P-type nitride layer 25 , and the electrons capture magnesium-hydrogen bonds to decompose to form hydrogen ions, thereby increasing the hole concentration in the second P-type nitride layer 25 .

[0144] In one embodiment, the semiconductor structure further includes a second electrode 50 , and the second electrode 50 is located on the upper surface of the N-type semiconductor layer 14 .

[0145] In one embodiment, the semiconductor structure further includes a transparent conductive layer 60 ; the first electrode 40 is located on the upper surface of the transparent conductive layer 60 .

[0146] The following specific examples adopt the preparation method of the present invention to prepare Figure 5 The chip has a chip size of 1530; the substrate 11 is a sapphire substrate; the buffer layer 12 is a non-doped gallium nitride with a thickness of 20 nm; the non-doped layer 13 is a non-doped GaN with a thickness of 2 μm; the N-type semiconductor layer is an N-type doped GaN layer, and the doping concentration of Si is 5×10 18 cm -3 The light-emitting material layer 211 is an InGaN quantum well layer and a GaN quantum barrier layer that are repeated in 10 cycles. The thickness of the InGaN quantum well is 3 nm, and the thickness of the GaN quantum barrier is 11 nm. The first P-type nitride material layer 221 is a P-type GaN layer with a thickness of 50 nm and a magnesium doping concentration of 2×10 19 cm -3The P-type nitride barrier material layer 231 is a P-type doped AlGaN layer with a thickness of 100 nm and a magnesium doping concentration of 6×10 19 cm -3 The non-doped nitride material layer 241 is a non-doped GaN layer with a thickness of 15 nm, the second P-type nitride layer 25 is a P-type GaN layer with a thickness of 45 nm, and the magnesium doping concentration is 5×10 19 cm -3 The annealed material layer 31 is an N-type GaN layer with a thickness of 50 nm and a Si doping concentration of 5×10 18 cm -3 .

[0147] Example 1

[0148] For the above structure, the annealing layer thickness is 50 nm, and the annealing time is 20 min under the conditions of applying 20 mA current and 300° C.

[0149] Comparative Example 1

[0150] Different from Example 1, Comparative Example 1 does not have an annealing material layer 31 and a first electrode 40, and adopts conventional furnace annealing at a temperature of 300°C for 20 minutes.

[0151] Comparative Example 2

[0152] Different from Example 1, Comparative Example 2 does not have an annealing material layer 31 and a first electrode 40, and adopts conventional furnace annealing at a temperature of 100°C for 20 minutes.

[0153] Comparative Example 3

[0154] Different from Example 1, Comparative Example 3 does not have an annealing material layer 31 and a first electrode 40, and adopts conventional furnace annealing at a temperature of 450°C for 20 minutes.

[0155] Comparative Example 4

[0156] Different from Example 1, Comparative Example 4 does not have an annealing material layer 31 and a first electrode 40, and adopts conventional furnace annealing at a temperature of 750°C for 20 minutes.

[0157] Comparative Example 5

[0158] The difference between Comparative Example 5 and Example 1 is that the annealing material layer 31 is a p-type GaN layer with a thickness of 50 nm.

[0159] Comparative Example 6

[0160] The difference with respect to the first embodiment is that the annealing material layer 31 is a non-doped GaN layer with a thickness of 50 nm.

[0161] Comparative Example 7

[0162] Comparative Example 7 is different from Comparative Example 5 in that the annealing temperature is 450°C.

[0163] Comparative Example 8

[0164] Comparative Example 8 is different from Comparative Example 5 in that the annealing temperature is 750°C.

[0165] The test data of Example 1 and Comparative Examples 1-8 are shown in the following table:

[0166]

[0167] Compared with conventional chips annealed in a conventional high-temperature annealing furnace, Example 1 of the present invention has higher brightness and lower voltage. Therefore, it can be seen from the above test data that the chip of the embodiment of the present invention injects electrons into the epitaxial structure 20 through the annealing layer 30 during annealing to increase the hole concentration in the epitaxial structure 20, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under large current.

[0168] In addition, it can be seen from the data that the annealing material layer 31 and the first electrode 40 are not set, and when the conventional chip annealing temperature is lower than 450°C, the chip does not emit light, and high temperature (≥450°C) is required to anneal the chip to activate the p-type doping in the epitaxial structure. Therefore, compared with conventional chip processes, the present invention greatly reduces the annealing temperature of the second P-type nitride layer 25, reduces the damage to the quality of the light-emitting area caused by high-temperature annealing, and improves the photoelectric performance of the LED chip.

[0169] Furthermore, it can be seen from the data that the annealing layer 30 using a p-type GaN layer or a non-doped GaN layer cannot achieve the effect of the embodiments of the present invention. In embodiments 7 and 8, increasing the annealing temperature of the annealing layer 30 can ultimately only achieve performance that is basically equivalent to that of a conventional chip process. Therefore, the chip of the embodiment of the present invention injects electrons into the epitaxial structure 20 through the annealing layer 30 during annealing to increase the hole concentration in the epitaxial structure 20, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under high current.

[0170] Example 2

[0171] The difference between Example 2 and Example 1 is that the annealing time is 5 minutes.

[0172] Example 3

[0173] The difference between Example 3 and Example 1 is that the annealing time is 50 minutes.

[0174] Example 4

[0175] The difference between Example 4 and Example 1 is that the annealing time is 60 minutes.

[0176] Example 5

[0177] The difference between Example 5 and Example 1 is that the annealing time is 1 min.

[0178] Keeping the annealing temperature at 300°C unchanged and changing the annealing time, the test data of Example 2, Example 3, Example 4 and Example 5 are as follows:

[0179] Annealing 300℃ Annealing time (min) Voltage (VF) Brightness(mW) droop(%) Example 1 20min 3.10 242 40.1% Example 2 5min 3.12 238 43.4% Example 3 50min 3.11 240 42.2% Example 4 60min 3.13 235 46.2% Example 5 1min 3.14 232 46.9%

[0180] In the annealing time range of 5min-60min, the test voltage, brightness and efficiency drop droop performance of the LED chip of the present invention are improved. It can be found that the best performance is obtained by annealing at 300°C for 20min in Example 1. If the annealing time is too low, electrons cannot be effectively injected into the epitaxial structure 20 to increase the hole concentration in the epitaxial structure 20. If the annealing time is too long, various performances show a downward trend. This may be because if the annealing time is too long, electrons are injected into the epitaxial structure 20 to form a new donor structure to compensate for the hole concentration.

[0181] Example 6

[0182] The difference from Example 1 is that the annealing temperature is 150°C.

[0183] Example 7

[0184] The difference from Example 1 is that the annealing temperature is 450°C.

[0185] Example 8

[0186] The difference from Example 1 is that the annealing temperature is 500°C.

[0187] Example 9

[0188] The difference from Example 1 is that the annealing temperature is 100°C.

[0189] The test data of Example 6, Example 7, Example 8 and Example 9 are as follows:

[0190] Annealing 20min Annealing temperature(℃) Voltage (VF) Brightness(mW) droop(%) Example 1 300 3.10 242 40.1% Example 6 150 3.12 239 40.9% Example 7 450 3.11 240 41.2% Example 8 500 3.13 235 46.7% Example 9 100 3.14 232 47.0%

[0191] It can be seen from the data that within the annealing temperature range of 150°C-300°C, the test voltage, brightness and efficiency drop performance of the LED chip of the present invention are all improved. It can be found that the best performance is obtained by annealing at 300°C for 20 minutes in Example 1. If the annealing temperature is too low, electrons cannot be effectively injected into the epitaxial structure 20 to increase the hole concentration in the epitaxial structure 20. If the annealing temperature is too high, various performances show a downward trend. This may be because the annealing time is too long and electrons are injected into the epitaxial structure 20 to form a new donor structure to compensate for the hole concentration.

[0192] Example 10

[0193] The difference between Example 10 and Example 1 is that the annealing temperature and annealing time are 450° C. and 5 min, respectively.

[0194] Embodiment 11

[0195] The difference between Example 11 and Example 1 is that the annealing temperature and annealing time are 150° C. and 50 min, respectively.

[0196] The test data of Example 10 and Example 11 are as follows:

[0197] Annealing time (min) & temperature (℃) Voltage (VF) Brightness(mW) droop(%) Example 1 20min&300℃ 3.10 242 40.1% Example 10 5min&450℃ 3.11 241 40.9% Embodiment 11 50min%150℃ 3.11 243 40.2%

[0198] It can be seen from the data that, compared with Example 1, annealing for 5 minutes and 50 minutes, respectively, at 450°C and 150°C, can achieve performance substantially equivalent to that of Example 1, that is, the annealing time is inversely correlated with the annealing temperature, and the annealing time is reduced while the annealing temperature is increased, while the performance equivalent to that of Example 1 can be achieved. Therefore, the present invention can match the annealing time and the annealing temperature, effectively forming the injection of electrons into the epitaxial structure 20 to increase the hole concentration in the epitaxial structure 20, thereby improving the uneven distribution of electrons and holes, avoiding the problem of electrons spilling into the epitaxial structure due to high electron concentration and fast migration, improving the ionization efficiency and radiation recombination efficiency of holes, and improving the efficiency drop effect under high current.

[0199] Example 12

[0200] The difference between Example 12 and Example 1 is that the thickness of the annealing layer is 1 nm.

[0201] Example 13

[0202] The difference between Example 13 and Example 1 is that the thickness of the annealing layer is 150 nm.

[0203] Embodiment 14

[0204] The difference between Example 14 and Example 1 is that the thickness of the annealing layer is 1 nm and the annealing temperature is 100°C.

[0205] Embodiment 15

[0206] The difference between Example 15 and Example 1 is that the thickness of the annealing layer is 1 nm and the annealing time is 5 min.

[0207] Example 16

[0208] The difference between Example 16 and Example 1 is that the annealing layer thickness is 150 nm, the annealing time is 5 min, and the annealing temperature is 450° C.

[0209] Embodiment 17

[0210] The difference between Example 17 and Example 1 is that the annealing layer thickness is 150 nm, the annealing time is 50 min, and the annealing temperature is 150° C.

[0211] Example 12, Example 13, Example 14, Example 15, Example 16 and Example 17 mainly compare the differences in the thickness of the annealing layer, the annealing time and the annealing temperature. The test data of Example 12, Example 13, Example 14, Example 15, Example 16 and Example 17 are as follows:

[0212] Annealing layer thickness (nm) Annealing time (min) & temperature (℃) Voltage (VF) Brightness(mW) droop(%) Example 1 50 20min&300℃ 3.10 242 40.1% Example 12 1 20min&300℃ 3.13 238 43.9% Example 13 150 20min&300℃ 3.13 239 42.5% Embodiment 14 1 20min&100℃ 3.11 243 40.8% Embodiment 15 1 5min&300℃ 3.10 243 40.6% Example 16 150 5min&450℃ 3.10 241 40.5% Embodiment 17 150 50min&150℃ 3.11 243 40.2%

[0213] It can be seen from the data that the annealing layer 30 is relatively thin, and the annealing temperature or annealing time can be reduced to achieve the same effect as in Example 1. The annealing layer 30 is relatively thick, and the annealing temperature or annealing time can be increased to achieve the same effect as in Example 1.

[0214] When the annealing layer 30 is relatively thin, the test data of excessively increasing the annealing time and the annealing temperature is relatively poor. The possible reason is that the electrons in the annealing layer 30 are injected into the epitaxial structure 20 to form a new donor structure compensation. When the annealing layer 30 is relatively thick, the hole concentration is not increased by the annealing time or the annealing temperature is not increased enough, and the test data is relatively poor. The possible reason is that the electrons in the annealing layer 30 are injected into the epitaxial structure 20 relatively little, and the effect of the present invention cannot be achieved.

[0215] Please note that the above embodiments are for illustrative purposes only and are not meant to limit the present application. It should also be noted that, according to the actual process, for chips that are smaller or larger than the chip of the present embodiment, the annealing time and annealing temperature can also be matched to obtain LED chips with excellent performance.

[0216] It should be understood that, unless otherwise specified herein, the execution of the steps described is not strictly limited in order, and the steps may be executed in other orders. Moreover, at least a portion of the steps described may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times, and the execution order of these sub-steps or stages is not necessarily sequential, but may be executed in turn or alternately with other steps or at least a portion of the sub-steps or stages of other steps.

[0217] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0218] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0219] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing an LED chip, characterized in that: include: providing a substrate; forming an epitaxial structure and an annealing layer, wherein the epitaxial structure is located on the upper surface of the substrate, the annealing layer is located on the upper surface of the epitaxial structure, and the annealing layer exposes the epitaxial structure; during the annealing process, the annealing layer injects electrons into the epitaxial structure to increase the hole concentration in the epitaxial structure; forming a first electrode on the upper surface of the annealing layer and the exposed epitaxial structure; applying a current to the first electrode and performing the annealing treatment on the obtained structure; The applied current is 1 mA-40 mA; the temperature of the annealing treatment is 150° C.-450° C.; the time of the annealing treatment is 5 min-50 min; and the atmosphere of the annealing treatment includes a nitrogen atmosphere and / or an oxygen atmosphere.

2. The method for preparing an LED chip according to claim 1, characterized in that: The base comprises a substrate, a buffer layer, a non-doped layer and an N-type semiconductor layer stacked in sequence from bottom to top; the forming of the epitaxial structure and the annealing layer comprises: forming a light-emitting material layer on the upper surface of the substrate; forming a P-type nitride stacked material layer on the upper surface of the light emitting material layer; forming an annealing material layer on the upper surface of the P-type nitride stacked material layer; Sequentially etching and removing a portion of the annealing material layer, a portion of the P-type nitride stacked material layer, and a portion of the light-emitting material layer to expose the N-type semiconductor layer, and forming a light-emitting layer, a P-type nitride stacked layer, and an annealing layer stacked sequentially from bottom to top, wherein the light-emitting layer and the P-type nitride stacked layer together constitute the epitaxial structure; After forming the annealing layer, the method further includes: forming a second electrode on the exposed upper surface of the N-type semiconductor layer.

3. The method for preparing an LED chip according to claim 2, characterized in that: The forming of a P-type nitride stacked material layer on the upper surface of the light emitting material layer comprises: forming a first P-type nitride material layer on the upper surface of the light emitting material layer; forming a P-type nitride barrier material layer on the upper surface of the first P-type nitride material layer; forming a non-doped nitride material layer on the upper surface of the P-type nitride barrier material layer; forming a second P-type nitride material layer on the upper surface of the undoped nitride material layer; After etching the portion of the P-type nitride stack material layer, a first P-type nitride layer, a P-type nitride barrier layer, an undoped nitride layer and a second P-type nitride layer are formed which are stacked in sequence from bottom to top. The first P-type nitride layer, the P-type nitride barrier layer, the undoped nitride layer and the second P-type nitride layer together constitute the P-type nitride stack.

4. The method for preparing an LED chip according to claim 3, characterized in that: The second P-type nitride layer contains a magnesium-hydrogen complex; the annealing layer injects electrons into the second P-type nitride layer, and the electrons capture magnesium-hydrogen bonds to decompose and form hydrogen ions, thereby increasing the hole concentration in the second P-type nitride layer.

5. The method for preparing an LED chip according to claim 1, characterized in that: After the annealing layer is formed, the method further comprises: Etching the annealing layer to form an opening in the annealing layer, wherein the opening exposes the upper surface of the epitaxial structure; The annealing layer includes an N-type nitride layer, and forming a first electrode on the upper surface of the annealing layer and the exposed epitaxial structure includes: A first N-type electrode is formed on the upper surface of the annealing layer, and a first P-type electrode is formed in the opening, wherein the first P-type electrode and the first N-type electrode together constitute the first electrode.

6. An LED chip, characterized in that: include: substrate; an epitaxial structure, located on the upper surface of the substrate; An annealing layer, located on the upper surface of the epitaxial structure, wherein the annealing layer exposes the epitaxial structure; The annealing layer injects electrons into the epitaxial structure during annealing to increase the hole concentration in the epitaxial structure; A first electrode is located on the upper surface of the annealing layer and the exposed epitaxial structure; applying a current to the first electrode and performing the annealing treatment on the obtained structure; The applied current is 1 mA-40 mA; the temperature of the annealing treatment is 150° C.-450° C.; the time of the annealing treatment is 5 min-50 min; and the atmosphere of the annealing treatment includes a nitrogen atmosphere and / or an oxygen atmosphere.

7. The LED chip according to claim 6, characterized in that: The epitaxial structure includes a light-emitting layer and a P-type nitride stack stacked in sequence from bottom to top; the P-type nitride stack includes a first P-type nitride layer, a P-type nitride barrier layer, an undoped nitride layer and a second P-type nitride layer stacked in sequence from bottom to top.

8. The LED chip according to claim 7, characterized in that: The second P-type nitride layer contains a magnesium-hydrogen complex; the annealing layer injects electrons into the second P-type nitride layer, and the electrons capture magnesium-hydrogen bonds to decompose and form hydrogen ions, thereby increasing the hole concentration in the second P-type nitride layer.

9. The LED chip according to claim 7, characterized in that: The first electrode includes a first N-type electrode and a first P-type electrode, the first N-type electrode is located on the upper surface of the annealing layer; the annealing layer has an opening, the opening exposes the upper surface of the second P-type nitride layer; the first P-type electrode is located in the opening; Wherein, the base comprises a substrate, a buffer layer, a non-doped layer and an N-type semiconductor layer stacked in sequence from bottom to top; The LED chip further includes: a second electrode located on the upper surface of the N-type semiconductor layer.