Surface treatment composition, method for producing surface treatment composition, surface treatment method, and method for producing semiconductor substrate
By using a surface treatment composition of polymers and chelating agents with specific structural units, the problem of difficult removal of cerium oxide particles and organic residues on the surface of semiconductor substrates after chemical mechanical polishing is solved, achieving higher cleanliness and reliability.
Patent Information
- Application Number
- CN202110890625.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-08-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-08-04
AI Technical Summary
Existing technologies often fail to effectively remove cerium oxide particles and organic residues remaining on the surface of semiconductor substrates after chemical mechanical polishing, leading to reduced reliability of semiconductor devices.
A surface treatment composition containing polymers, chelating agents, and water with specific structural units is used to remove cerium oxide particles and organic residues through chemical interaction and physical adsorption.
It effectively removes cerium oxide particles and organic residues, improving the cleanliness of semiconductor substrates and reducing defects and reliability issues in semiconductor devices.
Smart Images

Figure CN114250124B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a surface treatment composition, a method for producing the surface treatment composition, a surface treatment method, and a method for producing a semiconductor substrate. Background Art
[0002] In recent years, with the multi-layer wiring on the surface of semiconductor substrates, the so-called chemical mechanical polishing (CMP) technology is used when manufacturing semiconductor devices (devices), which polishes the semiconductor substrate to achieve flatness. CMP is a method in which a polishing composition (slurry) containing abrasives such as silicon dioxide, aluminum oxide, cerium oxide, etc., an anticorrosive agent, a surfactant, etc. is used to flatten the surface of a polishing object (polished object) such as a semiconductor substrate. The polishing object (polished object) is a wiring, plug, etc. formed by silicon, polysilicon, silicon oxide film (silicon oxide), silicon nitride, metal, etc.
[0003] A large amount of impurities (defects) remain on the surface of the semiconductor substrate after the CMP process. The impurities include organic substances such as abrasive grains, metals, corrosion inhibitors, and surfactants derived from the polishing composition used in CMP, silicon-containing materials and metals generated by polishing silicon-containing materials, metal wirings, plugs, etc. as polishing objects, and organic substances such as pad scraps generated by various pads.
[0004] If the surface of the semiconductor substrate is contaminated by these impurities, the electrical properties of the semiconductor may be adversely affected, and the reliability of the semiconductor device may be reduced. Therefore, it is desirable to introduce a cleaning process after the CMP process to remove these impurities from the surface of the semiconductor substrate.
[0005] Examples of the cleaning liquid (cleaning composition) used in such a cleaning step include those disclosed in Patent Document 1. Patent Document 1 discloses a slurry composition for chemical mechanical polishing, which contains water, polishing abrasive grains, and one or more water-soluble polymers containing polyvinyl alcohol structural units.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2012-74678 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] When cleaning the polished object, it is desired to further reduce defects.
[0011] Here, the inventors studied the relationship between the types of polished objects and the types of defects. As a result, it was found that cerium oxide particles and organic residues contained in the polishing composition are likely to remain on the surface of the polished object (e.g., a polished semiconductor substrate) containing silicon oxide, silicon nitride, or polycrystalline silicon, and these residues may cause damage to the semiconductor device.
[0012] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a method for sufficiently removing cerium oxide particles and organic residues present on the surface of a polished object.
[0013] Solutions for solving problems
[0014] The present inventors have conducted in-depth research in view of the above-mentioned problems and have found that organic residues existing on the surface of a polished object containing silicon oxide or polycrystalline silicon can be fully removed by using a surface treatment composition containing a polymer having a structural unit represented by the following formula (1), a chelating agent and water, thereby completing the present invention.
[0015]
[0016] In the above formula (1), R 1 is a hydrocarbon group having 1 to 5 carbon atoms, R 2 It is a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms. The chelating agent has at least one of a phosphonic acid group and a carboxylic acid group.
[0017] Effects of the Invention
[0018] According to the present invention, there is provided a means for sufficiently removing cerium oxide particles and organic residues present on the surface of a polished object. DETAILED DESCRIPTION
[0019] The present invention will be described below. However, the present invention is not limited to the following embodiments.
[0020] In the present specification, the expression "(meth)acrylic acid" in the specific name of the compound means "acrylic acid" and "methacrylic acid", and "(meth)acrylate" means "acrylate" and "methacrylate".
[0021] [Organic residue]
[0022] In this specification, the organic residue refers to foreign matter adhering to the surface of the polishing object after polishing, and includes organic substances such as organic low molecular weight compounds and organic high molecular weight compounds, organic salts, and the like.
[0023] Examples of organic residues adhering to the object to be cleaned include pad chips generated from a pad used in the polishing step described below or an arbitrarily provided rinse polishing step, and components derived from additives contained in the polishing composition used in the polishing step or the rinse polishing composition used in the rinse polishing step.
[0024] Organic residues are very different from other foreign matter in color and shape. Therefore, when judging whether a foreign matter is organic residue, it can be determined visually through SEM observation. If necessary, it can also be determined by elemental analysis using an energy dispersive X-ray analyzer (EDX).
[0025] [Polished object]
[0026] In this specification, the polished object to be polished refers to the object to be polished after being polished in the polishing process. The polishing process is not particularly limited, but a CMP process is preferred.
[0027] The surface treatment composition of one embodiment of the present invention is preferably used to reduce cerium oxide (CeO2) particles and organic residues remaining on the surface of a polished object (hereinafter, also referred to as "cleaned object") containing silicon oxide, silicon nitride (hereinafter, also referred to as "SiN") or polycrystalline silicon (hereinafter, also referred to as "Poly-Si"). As the polished object containing silicon oxide, for example, there can be mentioned: TEOS type silicon oxide surface (hereinafter, also referred to as "TEOS") generated using tetraethyl orthosilicate as a precursor, HDP film, USG film, PSG film, BPSG film, RTO film, etc.
[0028] The polished object is preferably a polished semiconductor substrate, more preferably a semiconductor substrate after CMP. The above reason is that, in particular, cerium oxide particles and organic residues may cause damage to semiconductor devices. Therefore, when the polished object is a polished semiconductor substrate, it is necessary to remove cerium oxide particles and organic residues as much as possible as a cleaning process for the semiconductor substrate.
[0029] There are no particular restrictions on the polished object containing silicon oxide, silicon nitride or polycrystalline silicon, and examples thereof include: polished objects formed of silicon oxide, silicon nitride and polycrystalline silicon each separately; polished objects in which materials other than silicon oxide, silicon nitride or polycrystalline silicon are exposed on the surface, etc. Here, as the former, for example, a silicon oxide substrate, a silicon nitride substrate or a polycrystalline silicon substrate as a conductor substrate can be cited. In addition, as for the latter, there are no particular restrictions on materials other than silicon oxide, silicon nitride or polycrystalline silicon, and for example, tungsten can be cited. As specific examples of the above-mentioned polished objects, there can be cited: a polished semiconductor substrate having a structure in which a silicon oxide film, a silicon nitride film or a polycrystalline silicon film is formed on tungsten; a polished semiconductor substrate having a structure in which a tungsten portion, a silicon oxide film, a silicon nitride film and a polycrystalline silicon film are completely exposed, etc.
[0030] Here, from the viewpoint of the effects exerted by the present invention, the polished object according to one embodiment of the present invention preferably contains silicon oxide.
[0031] [Surface treatment composition]
[0032] One embodiment of the present invention is a surface treatment composition for treating the surface of a polished object, the surface treatment composition comprising a polymer having a structural unit represented by the following formula (1), a chelating agent, and water.
[0033]
[0034] In the above formula (1), R 1 is a hydrocarbon group having 1 to 5 carbon atoms, R 2 It is a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms. The chelating agent has at least one of a phosphonic acid group and a carboxylic acid group.
[0035] The surface treatment composition according to one embodiment of the present invention is particularly preferably used as an organic residue reducing agent for selectively removing cerium oxide particles and organic residues in a surface treatment step.
[0036] The present inventors have estimated the mechanism for solving the above-mentioned problems by the present invention as follows. The surface treatment composition has the following function: each component contained in the surface treatment composition interacts with the surface of the polished object and foreign matter, and as a result of the chemical interaction, the foreign matter on the surface of the polished object is removed or removed more easily.
[0037] The polymer having the structural unit represented by formula (1) can make the surface hydrophilic by physically adsorbing on the hydrophobic wafer surface. The organic residue attached to the wafer is temporarily floated during the process, and then the polymer is adsorbed on the wafer. As a result, the layer formed by the polymer functions as a layer to prevent the organic residue from reattaching, and the organic residue can be easily removed from the wafer.
[0038] A chelating agent having at least one of a phosphonic acid group and a sulfonic acid group can more effectively remove organic residues from a polished object containing silicon oxide (eg, TEOS).
[0039] In addition, the chelating agent having at least one of a phosphonic acid group and a sulfonic acid group can dissolve and remove the cerium oxide particles present on the surface of the polished object. In particular, the chelating agent having a phosphonic acid group has a high function of dissolving the cerium oxide particles.
[0040] If the surface treatment composition contains an ionic dispersant, organic residues can be removed more effectively not only from a polished object containing silicon oxide (for example, TEOS) but also from a polished object containing silicon nitride.
[0041] It should be noted that the above mechanism is based on speculation, and its correctness has no impact on the protection scope of the present invention.
[0042] Hereinafter, each component contained in this surface treatment composition will be described.
[0043] [Polymer having a structural unit represented by formula (1)]
[0044] As R in the above formula (1) 1 Examples of the hydrocarbon group having 1 to 5 carbon atoms include alkyl groups such as methyl, ethyl, and propyl groups; alkenyl groups such as vinyl and propenyl groups; alkynyl groups such as ethynyl and propynyl groups; and cycloalkyl groups such as cyclopentyl groups. Among these, alkyl groups and alkynyl groups are preferred, and hydrocarbon groups having 1 to 3 carbon atoms are more preferred. 1 , more preferably methyl, ethyl and vinyl (vinyl) groups, further preferably methyl and ethyl groups.
[0045] As R in the above formula (1) 2 The hydrocarbon group having 1 to 3 carbon atoms represented by R includes: 1 Among the hydrocarbon groups having 1 to 5 carbon atoms shown in the examples, the hydrocarbon groups having 1 to 3 carbon atoms are as follows. 2 , preferably a hydrogen atom and a methyl group.
[0046] Examples of the unsaturated monomers providing the above structural units include N-vinylacetamide, N-vinylpropionamide, and N-vinylbutyramide, with N-vinylacetamide and N-vinylpropionamide being preferred. The above unsaturated monomers may be used alone or in combination of two or more.
[0047] The weight average molecular weight (Mw) of the polymer is usually 30,000 to 1,000,000, preferably 50,000 to 900,000, and more preferably 50,000 to 100,000. By making the weight average molecular weight (Mw) of the polymer within the above range, the organic residue on the surface of the polishing object after polishing can be more effectively reduced.
[0048] The lower limit of the content of the polymer having the structural unit represented by formula (1) (the total amount in the case of two or more kinds) is not particularly limited, but is preferably 0.02% by mass or more relative to the total amount of the surface treatment composition. If the content is 0.02% by mass or more, the organic residue on the surface of the polished object can be more effectively reduced.
[0049] From the same point of view, the lower limit of the content of the polymer having the structural unit represented by formula (1) is more preferably 0.03% by mass or more, and further preferably 0.05% by mass or more, relative to the total amount of the surface treatment composition. On the other hand, the upper limit of the content of the polymer having the structural unit represented by formula (1) is preferably 1% by mass or less, relative to the total amount of the surface treatment composition. If the content is less than 1% by mass, it becomes easy to remove the polymer having the structural unit represented by formula (1) itself after surface treatment. From the same point of view, the upper limit of the content of the polymer having the structural unit represented by formula (1) is more preferably 0.7% by mass or less, and further preferably 0.5% by mass or less, relative to the total amount of the surface treatment composition.
[0050] The content of the structural unit in the polymer is preferably 30 mol% to 100 mol%, more preferably 50 mol% to 100 mol%, and further preferably 70 mol% to 100 mol%. By making the content of the structural unit within the above range, the organic residue on the surface of the polishing object after polishing can be more effectively reduced.
[0051] [Chelating agent]
[0052] The chelating agent has at least one of a phosphonic acid group and a carboxylic acid group. That is, the chelating agent may have only a phosphonic acid group, may have only a carboxylic acid group, or may have both a phosphonic acid group and a carboxylic acid group.
[0053] The chelating agent plays the following role: by forming complex ions with metal impurities that may be contained in the surface treatment composition and capturing them, the contamination of the polished object caused by the metal impurities can be suppressed. As examples of chelating agents with phosphonic acid groups (hereinafter, also referred to as "phosphonic acid chelating agents"), 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP), nitrilotri(methylenephosphonic acid) (ATMP), ethylenediaminetetra(methylenephosphonic acid) (EDTMP), sodium hexametaphosphate or 2-phosphonobutane-1,2,4-tricarboxylic acid (PBTC) can be cited. As examples of chelating agents with carboxylic acid groups (hereinafter, also referred to as "carboxylic acid chelating agents"), triethylenetetraaminehexaacetic acid (TTHA), ethylenediaminetetraacetic acid (EDTA), diethylenetriaminepentaacetic acid (DTPA), ethylenediamine-N,N'-disuccinic acid (EDDS), succinic acid, glutaric acid, citric acid, and mercaptosuccinic acid can be cited.
[0054] In addition, the phosphonic acid-based chelating agent and the carboxylic acid-based chelating agent are not limited to the above-mentioned ones, and for example, the following examples may be mentioned.
[0055] Examples of phosphonic acid chelating agents include 2-aminoethylphosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, aminotri(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid) (EDTPO), diethylenetriaminepenta(methylenephosphonic acid), ethane-1,1-diphosphonic acid, ethane-1,1,2-triphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, ethane-1-hydroxy-1,1,2-triphosphonic acid, ethane-1,2-dicarboxy-1,2-diphosphonic acid, methanehydroxyphosphonic acid, 2-phosphonobutane-1,2-dicarboxylic acid, 1-phosphonobutane-2,3,4-tricarboxylic acid, and α-methylphosphonosuccinic acid. Among them, preferred examples include EDTPO, diethylenetriaminepenta(methylenephosphonic acid), and diethylenetriaminepentaacetic acid. As particularly preferred phosphonic acid chelating agents, EDTPO and diethylenetriamine penta (methylenephosphonic acid) can be cited. Examples of carboxylic acid chelating agents include: ethylenediaminetetraacetic acid, sodium ethylenediaminetetraacetate, nitrilotriacetic acid, sodium nitrilotriacetate, ammonium nitrilotriacetate, hydroxyethylethylenediaminetriacetic acid, sodium hydroxyethylethylenediaminetriacetate, diethylenetriaminepentaacetic acid, sodium diethylenetriaminepentaacetate, triethylenetetraaminehexaacetic acid, and triethylenetetraaminehexaacetate sodium. The chelating agent can be used alone or in combination of two or more.
[0056] [Water-soluble polymer having a structural unit derived from glycerol]
[0057] The surface treatment composition of one embodiment of the present invention may contain a water-soluble polymer having a structural unit derived from glycerin.
[0058] Preferred examples of water-soluble polymers having structural units derived from glycerol include: at least one selected from the group consisting of polyglycerol (see the following formula (2)), polyglycerol alkyl (C10-14) esters, polyglycerol alkyl (C10-14) ethers, ethylene oxide-modified polyglycerol, sulfonic acid-modified polyglycerol (for example, see the following formulas (3) and (4)), and phosphonic acid-modified polyglycerol (for example, see the following formulas (5) and (6)).
[0059]
[0060] In the above formulae (2) to (6), m and n each independently represent the number of repeating units, and in the above formulae (3) to (6), M each independently represents a hydrogen atom, Na, K or NH4 + .
[0061] It should be noted that the multiple M's in the above formulas (3) to (6) may be the same or different. For example, the n M's in the above formula (3) may all be Na, or may be hydrogen atoms, Na, K and NH4. + In addition, for example, the m M in the above formula (4) may all be Na, or may be a hydrogen atom, Na, K and NH4 + A combination of 2 or more.
[0062] The water-soluble polymers having a structural unit derived from glycerol described above may be used alone or in combination of two or more.
[0063] The content (concentration) of the water-soluble polymer having a structural unit derived from glycerol (the total amount in the case of two or more kinds) is not particularly limited, but is preferably 0.02% by mass or more relative to the total amount of the surface treatment composition. If the content of the water-soluble polymer having a structural unit derived from glycerol is 0.02% by mass or more, the effect of the present invention is improved.
[0064] From the same point of view, the content (concentration) of the water-soluble polymer having a structural unit derived from glycerol is more preferably 0.03% by mass or more, and further preferably 0.05% by mass or more, relative to the total amount of the surface treatment composition. In addition, the content (concentration) of the water-soluble polymer having a structural unit derived from glycerol is preferably 1% by mass or less, relative to the total amount of the surface treatment composition. If the content (concentration) of the water-soluble polymer having a structural unit derived from glycerol is less than 1% by mass, it becomes easy to remove the water-soluble polymer having a structural unit derived from glycerol itself after surface treatment. From the same point of view, the content (concentration) of the water-soluble polymer having a structural unit derived from glycerol is more preferably 0.7% by mass or less, and further preferably 0.5% by mass or less, relative to the total amount of the surface treatment composition.
[0065] The weight average molecular weight (Mw) of the water-soluble polymer having a structural unit derived from glycerol is preferably 1000 or more. If the weight average molecular weight is 1000 or more, the effect of removing foreign matter is further improved. It is speculated that the above reason is that the coverage of the water-soluble polymer having a structural unit derived from glycerol when covering the cleaning object and foreign matter becomes better, and the removal effect of foreign matter from the surface of the cleaning object or the inhibition effect of foreign matter on the re-attachment of the cleaning object surface is further improved. From the same point of view, the weight average molecular weight is more preferably 3000 or more, and more preferably 8000 or more. In addition, the upper limit of the weight average molecular weight of the water-soluble polymer having a structural unit derived from glycerol is not particularly limited, preferably 1000000 or less, more preferably 100000 or less, and more preferably 50000 or less. The weight average molecular weight can be determined by gel permeation chromatography (GPC) using a GPC apparatus (manufactured by Shimadzu Corporation, model: Prominence+ELSD detector (ELSD-LTII)) etc., by conversion to polyethylene glycol. Specifically, it can be measured by the method described in the Examples.
[0066] The water-soluble polymer having a structural unit derived from glycerol may be a commercially available product or a synthetic product. The production method for the synthesis is not particularly limited, and a known polymerization method may be used.
[0067] [acid]
[0068] The surface treatment composition of one embodiment of the present invention may contain an acid. It should be noted that in this specification, the ionic dispersant described below is considered to be an acid different from the additive described herein. The acid is mainly added for the purpose of adjusting the pH of the surface treatment composition.
[0069] In addition, it is speculated that the acid plays a role in making the surface of the polished object or the surface of the foreign matter positively charged when the polished object contains silicon oxide, silicon nitride or polycrystalline silicon. Therefore, when the surface treatment composition is used for foreign matter or cleaning object having the property of making the surface treatment composition positively charged, the addition of acid can further promote the electrostatic repulsion effect, and the removal effect of foreign matter generated by the surface treatment composition is further improved.
[0070] As the acid, any one of an inorganic acid or an organic acid can be used. As the inorganic acid, there is no particular limitation, and examples thereof include sulfuric acid, nitric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. As the organic acid, there is no particular limitation, and examples thereof include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and carboxylic acids such as lactic acid, and methanesulfonic acid, ethanesulfonic acid, and isethionic acid.
[0071] Among them, maleic acid or nitric acid is more preferred from the viewpoint of further improving the effect of positively charging the surface of the polished object and the surface of foreign matter and improving the removability of foreign matter.
[0072] In addition, the acid can be used individually or in combination of 2 or more types.
[0073] The content of the acid is preferably 0.01% by mass or more relative to the total amount of the surface treatment composition. If the content of the acid is 0.01% by mass or more, the effect of removing foreign matter is further improved. It is speculated that the above reason is because the effect of making the surface of the polished object and the surface of the foreign matter with positive charge becomes better. From the same point of view, the content of the acid is preferably 0.02% by mass or more, and more preferably 0.03% by mass or more relative to the total amount of the surface treatment composition. In addition, the content of the acid is preferably 5% by mass or less relative to the total amount of the surface treatment composition. If the content of the acid is 5% by mass or less, it is preferred from the perspective of cost reduction. From the same point of view, the content of the acid is more preferably 3% by mass or less, and more preferably 1% by mass or less relative to the total amount of the surface treatment composition.
[0074] [Dispersion medium]
[0075] The surface treatment composition of one aspect of the present invention must contain water as a dispersion medium (solvent). The dispersion medium has the function of dispersing or dissolving each component. The dispersion medium is more preferably only water. In addition, for the dispersion or dissolution of each component, the dispersion medium can be a mixed solvent of water and an organic solvent. In the above case, as the organic solvent used, it can be cited: organic solvents mixed with water, i.e., acetone, acetonitrile, ethanol, methanol, isopropanol, glycerol, ethylene glycol, propylene glycol, etc. In addition, these organic solvents can be used without mixing with water, and each component is dispersed or dissolved and then mixed with water. These organic solvents can be used alone or in combination of two or more.
[0076] From the viewpoint of contamination of the object to be cleaned and interference with the action of other components, water preferably contains as few impurities as possible. For example, water having a total content of transition metal ions of 100 ppb or less is preferred. Here, the purity of water can be improved by, for example, removing impurity ions using an ion exchange resin, removing foreign matter using a filter, distillation, and the like. Specifically, as water, for example, deionized water (ion exchange water), pure water, ultrapure water, distilled water, and the like are preferably used.
[0077] [pH]
[0078] The pH of the surface treatment composition of one embodiment of the present invention can exceed 5, but is preferably below 5. If the pH is below 5, when the surface treatment composition is used for foreign matter or a cleaning object having a property of causing the surface treatment composition to be positively charged, the surface of the cleaning object or the surface of the foreign matter can be more reliably positively charged, and a higher foreign matter removal effect can be obtained by electrostatic repulsion. If the pH exceeds 5, it becomes difficult to obtain a foreign matter removal effect under specific conditions (for example, as shown in Example 10 described later, a polished silicon nitride substrate). The pH is more preferably below 4, further preferably below 3, and further preferably below 3 (for example 2.5). In addition, the pH of the surface treatment composition is preferably above 1. If the pH is above 1, costs can be further reduced.
[0079] The pH value of the surface treatment composition can be confirmed using a pH meter (manufactured by Horiba, Ltd., product name: LAQUA (registered trademark)).
[0080] When adjusting the pH value, components other than the surface treatment composition of one embodiment of the present invention may become the cause of foreign matter, so it is desirable not to add them as much as possible. Thus, the surface treatment composition is preferably prepared only by the above-mentioned water-soluble polymer having a structural unit derived from glycerol, acid, water, and an ionic dispersant added as needed. However, in the case where it is difficult to obtain the desired pH only by these, other additives such as any alkali that can be added (such as ammonia) can be used to adjust within the scope of not hindering the effect of the present invention.
[0081] [Ionic dispersants]
[0082] The surface treatment composition of one embodiment of the present invention preferably further comprises an ionic dispersant. The ionic dispersant is beneficial for removing foreign matter generated by the surface treatment composition. Thus, the surface treatment composition comprising the ionic dispersant can fully remove foreign matter (including impurities such as organic residues) remaining on the surface of the polished object during the surface treatment (cleaning, etc.) of the polished object.
[0083] Examples of ionic dispersants include: polymer compounds having sulfonic acid (salt) groups; polymer compounds having phosphate (salt) groups; polymer compounds having phosphonic acid (salt) groups; polymer compounds having carboxylic acid (salt) groups; water-soluble polymers containing nitrogen atoms such as polyvinyl pyrrolidone (PVP), polyvinyl imidazole (PVI), polyvinyl carbazole, polyvinyl caprolactam, polyvinyl piperidine, polyacryloyl morpholine (PACMO); polyvinyl alcohol (PVA); hydroxyethyl cellulose (HEC), etc.
[0084] Among them, the polymer compound having a sulfonic acid (salt) group is preferred. The polymer compound having a sulfonic acid (salt) group is described below.
[0085] <Polymer compound having sulfonic acid (salt) group>
[0086] The above-mentioned ionic dispersant of the surface treatment composition of one embodiment of the present invention is preferably a polymer compound having a sulfonic acid (salt) group. The polymer compound having a sulfonic acid (salt) group (also referred to as "sulfonic acid group-containing polymer" in this specification) is more likely to be more conducive to removing foreign matter generated by the surface treatment composition. Therefore, the surface treatment composition containing the above-mentioned sulfonic acid group-containing polymer has the effect of more easily removing foreign matter (including impurities such as organic residues) remaining on the surface of the polished polishing object during the surface treatment (cleaning, etc.) of the polished polishing object.
[0087] The sulfonic acid group-containing polymer can form micelles due to the affinity of the part other than the sulfonic acid (salt) group (i.e., the polymer chain part of the sulfonic acid group-containing polymer) with foreign matter (especially hydrophobic components). It is believed that the micelles are dissolved or dispersed in the surface treatment composition, so that foreign matter as a hydrophobic component can also be effectively removed.
[0088] In addition, under acidic conditions, when the surface of the ground object to be polished is cationic, the sulfonic acid group anionizes, thereby becoming easily adsorbed on the surface of the ground object to be polished. As a result, it is believed that the above-mentioned sulfonic acid group-containing polymer is covered on the surface of the ground object to be polished. On the other hand, the sulfonic acid group of the sulfonic acid group-containing polymer is easily adsorbed on the residual foreign matter (especially the material that is easy to be cationic), so the surface of the foreign matter becomes anionic. Thus, the foreign matter whose surface becomes anionic and the anionized sulfonic acid group of the sulfonic acid group-containing polymer adsorbed on the surface of the ground object to be polished repel electrostatically. In addition, when the foreign matter is anionic, the foreign matter itself and the anionized sulfonic acid group present on the ground object to be polished repel electrostatically. Therefore, it is believed that by utilizing such electrostatic repulsion, foreign matter can be effectively removed.
[0089] It is further speculated that when the ground object is not easy to be charged, foreign matter is removed by a mechanism different from the above. It is believed that first, for the hydrophobic ground object, foreign matter (especially hydrophobic components) is in a state of easy attachment due to hydrophobic interaction. Here, the polymer chain part (hydrophobic structural part) of the sulfonic acid group-containing polymer is oriented toward the surface side of the ground object due to its hydrophobicity, and on the other hand, the anionized sulfonic acid group as a hydrophilic structural part is oriented to the opposite side of the surface side of the ground object. It is speculated that the surface of the ground object becomes covered with anionized sulfonic acid groups and becomes hydrophilic. As a result, it is believed that it becomes difficult for foreign matter (especially hydrophobic components) to interact hydrophobically with the ground object, and the attachment of foreign matter is suppressed.
[0090] Furthermore, the polymer having the structural unit represented by the above formula (1), the water-soluble polymer having the structural unit derived from glycerol, and the sulfonic acid group-containing polymer adsorbed on the surface of the polished object can be easily removed by further washing with water or the like.
[0091] It should be noted that, in this specification, "sulfonic acid (salt) group" refers to a sulfonic acid group (-SO3H)) or a group of its salt (-SO3M 2 Here, M 2 is an organic or inorganic cation).
[0092] The sulfonic acid group-containing polymer is not particularly limited as long as it has a plurality of sulfonic acid (salt) groups, and known compounds can be used. Examples of sulfonic acid group-containing polymers include polymer compounds obtained by sulfonating a polymer compound that will serve as a base, polymer compounds obtained by (co)polymerizing a monomer having a sulfonic acid (salt) group, and the like.
[0093] More specifically, sulfonic acid (salt) group-containing polyvinyl alcohol (sulfonic acid modified polyvinyl alcohol), polystyrene sulfonic acid, sodium polystyrene sulfonate and other sulfonic acid (salt) group-containing polystyrenes, sulfonic acid (salt) group-containing polyvinyl acetate (sulfonic acid modified polyvinyl acetate), sulfonic acid (salt) group-containing polyesters, copolymers of (meth) acrylic acid-sulfonic acid (salt) group-containing monomers and copolymers of (meth) acrylic acid-sulfonic acid (salt) group-containing monomers, etc. It should be noted that in this specification, the expression "(meth) acrylic acid" in the specific name of the compound refers to "acrylic acid" and "methacrylic acid", and "(meth) acrylate" refers to "acrylate" and "methacrylate". The above-mentioned sulfonic acid group-containing polymers can be used alone or in combination of two or more. At least a part of the sulfonic acid groups possessed by these polymers can be in the form of salts. As examples of salts, alkali metal salts such as sodium salts and potassium salts, salts of Group 2 elements such as calcium salts and magnesium salts, amine salts, ammonium salts, etc. can be cited. In particular, when the object to be polished is a semiconductor substrate after a CMP process, an ammonium salt is preferred from the viewpoint of removing as much metal as possible from the surface of the substrate.
[0094] When the sulfonic acid group-containing polymer is a sulfonic acid group-containing polyvinyl alcohol, the saponification degree is preferably 80% or more, more preferably 85% or more (the upper limit is 100%) from the viewpoint of solubility.
[0095] In the present invention, the weight average molecular weight of the sulfonic acid group-containing polymer is preferably 1000 or more. If the weight average molecular weight is 1000 or more, the effect of removing foreign matter is further improved. It is speculated that the above reason is that the covering property when covering the polished polishing object and foreign matter becomes better, and the removal effect of foreign matter from the surface of the cleaning object or the re-attachment inhibition effect of organic residues on the surface of the polished polishing object is further improved. From the same viewpoint, the weight average molecular weight is more preferably 2000 or more, and more preferably 8000 or more.
[0096] In addition, the weight average molecular weight of the sulfonic acid group-containing polymer is preferably 100,000 or less. If the weight average molecular weight is 100,000 or less, the removal effect of foreign matter is further improved. It is speculated that the above reason is because the removability of the sulfonic acid group-containing polymer after the cleaning process becomes better. From the same point of view, the weight average molecular weight is more preferably 50,000 or less, and further preferably 40,000 or less.
[0097] The weight average molecular weight can be measured by gel permeation chromatography (GPC), and specifically, can be measured by the method described in Examples.
[0098] As the sulfonic acid group-containing polymer, commercially available products can be used, for example, GOHSENX (registered trademark) L-3226 and GOHSENX (registered trademark) CKS-50 manufactured by Nippon Synthetic Chemical Industry Co., Ltd., ARON (registered trademark) A-6012, A-6016A, and A-6020 manufactured by Toagosei Co., Ltd., and PolyNASS (registered trademark) PS-1 manufactured by Tosoh Organic Chemical Co., Ltd. can be used.
[0099] The content (concentration) of the sulfonic acid group-containing polymer relative to the total amount of the surface treatment composition is preferably 0.001% by mass or more. If the content of the sulfonic acid group-containing polymer is 0.001% by mass or more, the removal effect of foreign matter is further improved. It is speculated that the above reason is that when the sulfonic acid group-containing polymer covers the polished polishing object and foreign matter, it can cover more area. As a result, foreign matter, in particular, becomes easy to form micelles, and therefore, the removal effect of foreign matter produced by the dissolution / dispersion of the micelles is improved. In addition, it is speculated that this is because the electrostatic adsorption or repulsion effect can be more strongly reflected by increasing the number of sulfonic acid (salt) groups. From the same point of view, the content (concentration) of the sulfonic acid group-containing polymer relative to the total amount of the surface treatment composition is more preferably 0.003% by mass or more, and further preferably 0.005% by mass or more. In addition, the content (concentration) of the sulfonic acid group-containing polymer relative to the total amount of the surface treatment composition is preferably 0.5% by mass or less. If the content (concentration) of the sulfonic acid group-containing polymer is 0.5% by mass or less, the removal effect of foreign matter is further improved. The above reason is presumably because the removability of the sulfonic acid group-containing polymer itself after the cleaning step becomes better. From the same viewpoint, the content of the sulfonic acid group-containing polymer is more preferably 0.2 mass % or less, further preferably 0.1 mass % or less, and particularly preferably 0.05 mass % or less relative to the total amount of the surface treatment composition.
[0100] In addition, in this specification, a "polymer compound" refers to a compound having a weight average molecular weight of 1,000 or more.
[0101] [Other additives]
[0102] The surface treatment composition of one embodiment of the present invention contains other additives in any ratio as required within the range that does not hinder the effect of the present invention. However, components other than the essential components of the surface treatment composition of one embodiment of the present invention may become the cause of foreign matter, and therefore, it is desired not to add them as much as possible. Therefore, it is preferred that the components other than the essential components are added in as little amount as possible, and more preferably not contained. As other additives, for example, abrasives, alkalis, preservatives, dissolved gases, reducing agents, oxidants and alkanolamines can be cited. Among them, in order to further improve the foreign matter removal effect, the surface treatment composition preferably does not substantially contain abrasives. Here, "substantially does not contain abrasives" refers to the situation where the content of abrasives relative to the entire surface treatment composition is less than 0.01% by mass.
[0103] The amount of the foreign matter (organic residue) is a value measured by the method described in the examples after the surface treatment is performed by the method described in the examples.
[0104] [Method for producing surface treatment composition]
[0105] The method for producing the surface treatment composition is not particularly limited. For example, a polymer having a structural unit shown in the above formula (1), a chelating agent containing at least one of a phosphonic acid group and a sulfonic acid group, and water are mixed to produce the surface treatment composition. That is, according to another embodiment of the present invention, a method for producing the surface treatment composition is also provided, which comprises: mixing a polymer having a structural unit shown in the above formula (1), a chelating agent containing at least one of a phosphonic acid group and a sulfonic acid group, and water. The type and amount of the polymer having the structural unit shown in the above formula (1) are as described above. Furthermore, in the method for producing the surface treatment composition of one embodiment of the present invention, the above-mentioned ionic dispersant, the above-mentioned water-soluble polymer having a structural unit derived from glycerol (glycerol-based water-soluble polymer), other additives, a dispersion medium other than water, etc. can be further mixed as needed. Their types, amounts, etc. are as described above.
[0106] There is no particular restriction on the order and method of adding the above-mentioned components. The above-mentioned materials can be added simultaneously or separately, or in stages or continuously. In addition, there is no particular restriction on the mixing method, and a known method can be used. Preferably, the method for producing the above-mentioned surface treatment composition comprises the following steps: sequentially adding a water-soluble polymer having a structural unit derived from glycerol, an acid, water and an ionic dispersant added as needed, and stirring in water. In addition, the method for producing the above-mentioned surface treatment composition may also include the following steps: measuring the pH of the surface treatment composition and adjusting it so that the pH is below 5.
[0107] [Surface treatment method]
[0108] Another embodiment of the present invention is a surface treatment method, which comprises the following steps: using the surface treatment composition to perform surface treatment on a polished object. In this specification, the surface treatment method refers to a method for reducing foreign matter on the surface of the polished object, which is a method for cleaning in a broad sense.
[0109] According to a surface treatment method of one embodiment of the present invention, foreign matter remaining on the surface of a polished object can be fully removed. That is, according to another embodiment of the present invention, a method for reducing foreign matter on the surface of a polished object is provided, which uses the above-mentioned surface treatment composition to perform surface treatment on the polished object.
[0110] The surface treatment method according to one embodiment of the present invention is performed by a method in which the surface treatment composition of the present invention is brought into direct contact with a polished object.
[0111] As the surface treatment method, mainly (I) a method using a rinsing and grinding treatment and (II) a method using a cleaning treatment can be cited. That is, the surface treatment of one embodiment of the present invention is preferably carried out by rinsing and grinding or cleaning. The rinsing and grinding treatment and the cleaning treatment are carried out to remove foreign matter (particles, metal pollution, organic residues, gasket chips, etc.) on the surface of the ground object to be ground and obtain a clean surface. The above (I) and (II) are described below.
[0112] (I) Rinsing and grinding
[0113] The surface treatment composition of the present invention can be suitable for flushing and grinding treatment. The flushing and grinding treatment is carried out as follows: After the final grinding (finishing grinding) of the grinding object, it is carried out on a grinding plate (drum, platen) equipped with a grinding pad for the purpose of removing foreign matter on the surface of the grinding object. At this time, the flushing and grinding treatment is carried out by directly contacting the surface treatment composition of the present invention with the ground grinding object. As a result, the foreign matter on the surface of the ground grinding object is removed by the friction force (physical effect) generated by the grinding pad and the chemical effect generated by the surface treatment composition. Among the foreign matter, particles and organic residues are particularly easily removed by physical action. Therefore, in the flushing and grinding treatment, the friction with the grinding pad on the grinding plate (drum) is utilized to effectively remove particles and organic residues.
[0114] Specifically, the rinse polishing treatment can be carried out as follows: the surface of the polished object after the polishing process is placed on a polishing plate (roller) of a polishing device, the polishing pad is brought into contact with the polished semiconductor substrate, and a surface treatment composition (rinsing polishing composition) is supplied to the contact portion while the polished object and the polishing pad are made to slide relative to each other.
[0115] The rinsing and polishing process can be performed using any one of a single-sided polishing device and a double-sided polishing device. In addition, the above-mentioned polishing device is preferably provided with a discharge nozzle for rinsing the polishing composition on the basis of a discharge nozzle for the polishing composition. The operating conditions during the rinsing and polishing process of the polishing device are not particularly limited and can be appropriately set for those skilled in the art.
[0116] (II) Cleaning
[0117] The surface treatment composition of the present invention can be suitable for cleaning treatment. The cleaning treatment is carried out as follows: after the final grinding (finishing grinding) of the grinding object, or after the above-mentioned rinsing and grinding treatment, it is carried out for the purpose of removing foreign matter on the surface of the grinding object. It should be noted that the cleaning treatment and the above-mentioned rinsing and grinding treatment can be classified according to the place where these treatments are carried out, and the cleaning treatment is a surface treatment carried out after the ground grinding object is removed from the grinding plate (drum). During the cleaning treatment, the surface treatment composition of the present invention can also be brought into direct contact with the ground grinding object to remove foreign matter on the surface of the object.
[0118] As an example of a method for performing a cleaning treatment, the following methods can be cited: method (i), while the polished polishing object is held, a cleaning brush is brought into contact with one or both surfaces of the polished polishing object, and the surface of the polished polishing object is scrubbed with the cleaning brush while supplying a surface treatment composition to the contact portion; method (ii), immersing the polished polishing object in the surface treatment composition, and performing ultrasonic treatment and stirring (immersion method); etc. In the above methods, foreign matter on the surface of the polishing object is removed by the friction force generated by the cleaning brush or the mechanical force generated by the ultrasonic treatment and stirring, and the chemical action generated by the surface treatment composition.
[0119] In the above method (i), there is no particular limitation on the method by which the surface treatment composition (cleaning composition) contacts the polished object, and examples include: a rotating method in which the polished object is rotated at high speed while the surface treatment composition flows from a nozzle onto the object; a spraying method in which the surface treatment composition is sprayed onto the object and cleaned; etc.
[0120] From the viewpoint of achieving more effective contamination removal in a short time, the cleaning treatment is preferably performed by a rotary method or a spray method, and more preferably by a rotary method.
[0121] As devices for performing such cleaning treatment, there are the following devices: an intermittent cleaning device that simultaneously performs surface treatment on a plurality of polished objects stored in a box; a single-wafer cleaning device that mounts a single polished object on a holder and performs surface treatment, etc. From the viewpoint of shortening the cleaning time, etc., the method using the single-wafer cleaning device is preferred.
[0122] Further, as a device for performing a cleaning process, a grinding device can be cited: it has a cleaning device for scrubbing the ground object with a cleaning brush after removing the ground object from a grinding plate (drum). By using such a grinding device, the cleaning process of the ground object can be performed more effectively.
[0123] As such a polishing device, a general polishing device having a holder for holding the polished object, a motor capable of changing the rotation speed, a cleaning brush, etc. can be used. As the polishing device, any one of a single-sided polishing device or a double-sided polishing device can be used. It should be noted that, when a rinse polishing process is performed after the CMP process, it is more effective and preferred to perform the cleaning process using the same device as the polishing device used in the rinse polishing process.
[0124] There is no particular limitation on the cleaning brush, but a brush made of resin is preferably used. The material of the resin brush is not particularly limited, but for example, PVA (polyvinyl alcohol) is preferably used. Moreover, a sponge made of PVA is particularly preferably used as the cleaning brush.
[0125] There is no particular restriction on the cleaning conditions either, and they can be appropriately set according to the type of the cleaning object and the type and amount of the organic residue to be removed. For example, it is preferred that the rotation speed of the cleaning brush is more than 10rpm and less than 200rpm, the rotation speed of the cleaning object is more than 10rpm and less than 100rpm, and the pressure (grinding pressure) applied to the cleaning object is more than 0.5psi and less than 10psi. There is no particular restriction on the method of supplying the surface treatment composition to the cleaning brush, for example, a method (casting) of continuously supplying with a pump etc. can be adopted. There is no restriction on its supply amount, and the surface of the cleaning brush and the cleaning object is preferably always covered by the surface treatment composition, and preferably more than 10mL / minute and less than 5000mL / minute. There is no particular restriction on the cleaning time either, and for the process of using the surface treatment composition of one mode of the present invention, it is preferably more than 5 seconds and less than 180 seconds. If it is such a range, foreign matter can be removed more effectively.
[0126] The temperature of the surface treatment composition during cleaning is not particularly limited, and may be generally room temperature (25° C.), or may be heated to about 40° C. to 70° C. within a range that does not impair performance.
[0127] In the above method (ii), the conditions of the cleaning method by immersion are not particularly limited, and a known method can be adopted.
[0128] Before, after, or during the cleaning treatment by the above-mentioned methods (i) and (ii), cleaning with water may be performed.
[0129] In addition, the polished object (cleaning object) after cleaning is preferably, utilizes a rotary dryer etc., the water droplets attached to the surface are shaken off and dried. In addition, the surface of the cleaning object can also be dried by air blowing.
[0130] [Method for manufacturing semiconductor substrate]
[0131] The surface treatment method of one embodiment of the present invention can be applied when the polished object is a polished semiconductor substrate. That is, according to another embodiment of the present invention, a method for manufacturing a semiconductor substrate is provided, wherein the polished object is a polished semiconductor substrate, and the method comprises the following steps: using the above-mentioned surface treatment composition to perform surface treatment on the polished semiconductor substrate.
[0132] The details of the semiconductor substrate to which the above-mentioned manufacturing method is applied are as described in the description of the polished object which has been surface-treated with the above-mentioned surface treatment composition.
[0133] In addition, as a manufacturing method for a semiconductor substrate, as long as it includes a surface treatment composition using one mode of the present invention, the process (surface treatment process) of surface treatment of the surface of the ground semiconductor substrate is not particularly limited. As the above-mentioned manufacturing method, for example, the following method can be cited: having a grinding process and a cleaning process for forming a ground semiconductor substrate. In addition, as another example, the following method can be cited: on the basis of the grinding process and the cleaning process, a rinsing grinding process is provided between the grinding process and the cleaning process. Below, these various processes are described.
[0134] <Grinding process>
[0135] The polishing step that may be included in the method for manufacturing a semiconductor substrate is a step of polishing the semiconductor substrate to form a polished semiconductor substrate.
[0136] The polishing process is not particularly limited as long as it is a process for polishing the semiconductor substrate, and a chemical mechanical polishing (CMP) process is preferred. In addition, the polishing process may be a polishing process consisting of a single process or a polishing process consisting of multiple processes. As a polishing process consisting of multiple processes, for example, there can be cited: a process of performing a finishing polishing process after a pre-polishing process (rough polishing process); a process of performing a second polishing process once or twice or more after a first polishing process, and then performing a finishing polishing process; etc. The surface treatment process using the surface treatment composition of the present invention is preferably performed after the above-mentioned finishing polishing process.
[0137] As the grinding composition, known grinding compositions can be suitably used according to the characteristics of the semiconductor substrate. As the grinding composition, there is no particular limitation, and for example, a grinding composition comprising abrasive grains, an acid salt, a dispersion medium and an acid can be preferably used. As a specific example of the above-mentioned grinding composition, a grinding composition comprising cerium oxide, polyacrylic acid, water and maleic acid can be cited.
[0138] As the grinding device, a general grinding device having a support for holding the grinding object and a motor capable of changing the rotation speed, etc., and a grinding plate capable of adhering a grinding pad (grinding cloth) can be used. As the grinding device, any one of a single-sided grinding device or a double-sided grinding device can be used.
[0139] As the polishing pad, general nonwoven fabric, polyurethane, porous fluororesin, etc. can be used without particular limitation. The polishing pad is preferably provided with grooves for retaining the polishing liquid.
[0140] There is no particular restriction on the grinding conditions, for example, the rotation speed of the grinding plate and the rotation speed of the head (carrier) are preferably more than 10rpm and less than 100rpm, and the pressure (grinding pressure) applied to the grinding object is preferably more than 0.5psi and less than 10psi. There is no particular restriction on the method of supplying the grinding composition to the grinding pad, for example, a method (casting) of continuously supplying with a pump etc. can be adopted. There is no restriction on its supply amount, and the surface of the preferred grinding pad is always covered with the grinding composition, and preferably more than 10mL / minute and less than 5000mL / minute. There is no particular restriction on the grinding time, and for the process using the grinding composition, it is preferably more than 5 seconds and less than 180 seconds.
[0141] <Surface treatment process>
[0142] The surface treatment step is a step of reducing foreign matter on the surface of the polished object using the surface treatment composition of the present invention. In the method for manufacturing a semiconductor substrate, a cleaning step as a surface treatment step may be performed after the rinsing and polishing step, or only the rinsing and polishing step or only the cleaning step may be performed.
[0143] (Rinsing and grinding process)
[0144] The rinsing and polishing step can be provided between the polishing step and the cleaning step in the method for manufacturing a semiconductor substrate. The rinsing and polishing step is a step for reducing foreign matter on the surface of the polished object (polished semiconductor substrate) by using a surface treatment method (rinsing and polishing treatment method) of one embodiment of the present invention.
[0145] Regarding the polishing apparatus, polishing pad and other equipment, and polishing conditions, the same equipment and conditions as those in the above-mentioned polishing step can be applied except that the surface treatment composition of the present invention is supplied instead of the polishing composition.
[0146] The details of the rinsing and polishing method used in the rinsing and polishing step are as described in the description of the above rinsing and polishing process.
[0147] (Cleaning process)
[0148] The cleaning step can be provided after the grinding step or after the rinse grinding step in the method for manufacturing a semiconductor substrate. The cleaning step is a step for reducing foreign matter on the surface of the polished object (polished semiconductor substrate) by using a surface treatment method (cleaning method) of one embodiment of the present invention.
[0149] The details of the cleaning method used in the cleaning step are as described in the description of the above cleaning method.
[0150] Example
[0151] The present invention is further described in detail using the following examples and comparative examples. However, the technical scope of the present invention should not be limited to the following examples. It should be noted that, unless otherwise specified, "%" and "parts" refer to "mass %" and "mass parts", respectively. In addition, in the following examples, unless otherwise specified, the operation is carried out under the conditions of room temperature (25°C) / relative humidity 40 to 50%RH.
[0152] The weight average molecular weight of each polymer compound refers to a value of a weight average molecular weight (in terms of polyethylene glycol) measured by gel permeation chromatography (GPC), and more specifically, the measurement was performed using the following apparatus and conditions.
[0153] GPC device: manufactured by Shimadzu Corporation
[0154] Model: Prominence+ELSD detector (ELSD-LTII)
[0155] Column: VP-ODS (manufactured by Shimadzu Corporation)
[0156] Mobile phase A: MeOH
[0157] B: 1% acetic acid aqueous solution
[0158] Flow rate: 1mL / min
[0159] Detector: ELSD temp.40℃、Gain 8、N2GAS 350kPa
[0160] Column oven temperature: 40°C
[0161] Injection volume: 40μL
[0162] <Preparation of surface treatment composition>
[0163] [Example 1: Preparation of surface treatment composition (A-1)]
[0164] The entire composition was set to 100 parts by mass, 0.1 parts by mass of poly-N-vinylacetamide (weight average molecular weight (Mw): 50,000; the structural unit represented by formula (1) was 100 mol%), 0.01 parts by mass of polystyrene sulfonic acid-acrylic acid copolymer (weight average molecular weight (Mw): 10,000) as an ionic dispersant, and 0.2 parts by mass of 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP) as a chelating agent were mixed with water (deionized water), and nitric acid was added as a pH adjuster in an amount to give a pH of 3.0 to prepare a surface treatment composition (A-1). The pH of the surface treatment composition (A-1) (liquid temperature: 25° C.) was measured using a pH meter (manufactured by Horiba, Ltd., product name: LAQUA (registered trademark)).
[0165] [Examples 2 to 28 and Comparative Examples 1 to 3: Preparation of surface treatment compositions (A-2) to (A-28) and (a-1) to (a-3)]
[0166] Each surface treatment composition was prepared in the same manner as in Example 1 except that the pH of each surface treatment composition was adjusted to the pH shown in Table 1 using each component having the type, molecular weight and content shown in Table 1. In Table 1, "-" means that the component was not used.
[0167] In Table 1, PSS-PA stands for "polystyrene sulfonic acid-acrylic acid copolymer". In Table 1, PNVA stands for "poly-N-vinylacetamide".
[0168] It should be noted that the total number of phosphonic acid groups and carboxylic acid groups of the chelating agent according to the embodiment of the present invention is 2 or more. The chelating agents used in Examples 1 to 28 all meet this condition. On the other hand, the phosphoric acid and acetic acid used in Comparative Examples 1 and 2 do not meet this condition and are not chelating agents. In Comparative Example 3, not only is no chelating agent added, but phosphoric acid and acetic acid are also not added.
[0169] <Evaluation>
[0170] <Preparation of polished object (surface treatment object)>
[0171] A polished TEOS substrate, a polished silicon nitride substrate, a polished polysilicon substrate and a polished bare silicon substrate which have been polished through the following chemical mechanical polishing (CMP) process or a polished TEOS substrate, a polished silicon nitride substrate, a polished polysilicon substrate and a polished bare silicon substrate which have been further treated through the following rinsing process as needed are prepared as surface treatment objects.
[0172] [CMP process]
[0173] For the TEOS substrate, silicon nitride substrate, and polycrystalline silicon substrate as semiconductor substrates, polishing was performed under the following conditions using polishing composition M (composition: cerium oxide, primary particle size 60nm, secondary particle size 100nm) 1% by mass, 30% by mass maleic acid aqueous solution 0.18% by mass, polyacrylic acid (molecular weight: 6000) 0.25% by mass, solvent: water). Here, the TEOS substrate, silicon nitride substrate, polycrystalline silicon substrate, and polished bare silicon substrate used 300 mm wafers.
[0174] (Grinding device and grinding conditions)
[0175] Grinding device: FREX 300E manufactured by Ebara Manufacturing Co., Ltd.
[0176] Polishing pad: Fujibo Co., Ltd. soft pad H800
[0177] Grinding pressure: 2.0 psi (1 psi = 6894.76 Pa, the same below)
[0178] Grinding plate speed: 90rpm
[0179] Head speed: 90rpm
[0180] Supply of polishing composition: Pouring
[0181] Polishing composition supply amount: 200 mL / min
[0182] Grinding time: 60 seconds
[0183] [Rinsing and polishing process]
[0184] For the polished TEOS substrate, the polished silicon nitride substrate, the polished polysilicon substrate and the polished bare silicon substrate polished by the above CMP process, each polished substrate is removed from the polishing plate (drum). Then, in the same polishing device, each polished substrate is mounted on another polishing plate (drum), and the surface of each substrate is rinsed and polished with each prepared surface treatment composition under the following conditions.
[0185] (Grinding device and grinding conditions)
[0186] Grinding device: FREX 300E manufactured by Ebara Manufacturing Co., Ltd.
[0187] Polishing pad: Fujibo Co., Ltd. soft pad H800
[0188] Grinding pressure: 1.0 psi (1 psi = 6894.76 Pa, the same below)
[0189] Grinding plate speed: 60rpm
[0190] Head speed: 60rpm
[0191] Supply of polishing composition: Pouring
[0192] Polishing composition supply amount: 300 mL / min
[0193] Grinding time: 60 seconds
[0194] (Water washing process)
[0195] Each of the rinse-polished substrates obtained above was rinsed and polished, and then cleaned for 60 seconds in a cleaning section while dripping deionized water (DIW) with a PVA brush, and then dried for 30 seconds using a spin dryer.
[0196] <Evaluation>
[0197] The following items were measured and evaluated for each substrate after the water washing step obtained above. The evaluation results are shown in Table 2.
[0198] [Determination of Ce dissolution amount]
[0199] In order to evaluate the removal performance of cerium oxide, the Ce dissolution amount was measured for each substrate. The greater the Ce dissolution amount, the higher the removal performance of the cerium oxide particles. The method for measuring the Ce dissolution amount is as follows.
[0200] The sample used for evaluation was composed of 1 part by mass of cerium oxide particles (particle size: 60 nm), a chelating agent, and a sample adjusted to pH 3.5 with a pH adjuster.
[0201] The prepared sample solution was stirred at 500 rpm for 2 hours at room temperature and pressure. Then, about 35 g was taken in a centrifugal separation vial and centrifuged at 20,000 rpm for 2 hours (Avanti HP-301, manufactured by Beckman Coulter). Then, the supernatant was taken and filtered with a filter having a pore size of 0.1 μm. 10 mL of the filtered solution was diluted to 5 times and measured by ICP.
[0202] [Determination of total number of defects]
[0203] The number of defects of the surface-treated TEOS substrate (0.037 μm or more), silicon nitride substrate (0.038 μm or more), polysilicon substrate (0.057 μm or more), and polished bare silicon substrate (0.060 μm or more) obtained after the water washing step was measured. The number of defects was measured using a wafer defect inspection device SP-5 manufactured by KLA TENCOR. The measurement was performed as follows: the portion remaining after removing a 3 mm wide portion (a portion from 0 mm to 3 mm wide when the outer peripheral end is 0 mm) from the outer peripheral end of each substrate surface after surface treatment was measured.
[0204] [Measurement of the number of pit defects on Si]
[0205] For the bare silicon substrate after the above surface treatment, the number of dent defects was measured by SEM observation using FE-SEM (SU-8000) of Hitachi High-Tech Co., Ltd. In the SEM observation, the number of dents was visually confirmed within the measurement range of 1.0kV 8.0mm×50.0k SE (UL) magnification. Dents with a diameter of 50-100nm were defined as dent defects. It should be noted that the average number of dents on Si observed in 30 fields of view was 10 or less, which was considered good.
[0206] [Evaluation of the number of organic residues]
[0207] The polished object after the above-mentioned surface treatment was observed by SEM using Review SEM RS6000 manufactured by Hitachi, Ltd. to measure the amount of organic residues. First, in the SEM observation, 100 defects existing in the remaining portion after removing a portion with a width of 3 mm from the outer peripheral edge of one side of the polished object were sampled. Next, the organic residues were visually determined from the 100 sampled defects under SEM observation, and the number of organic residues was confirmed, thereby calculating the ratio (%) of organic residues in the defects. Then, in the evaluation of the above-mentioned total number of defects, the total number of defects (pieces) of TEOS substrates (above 0.037μm), silicon nitride substrates (above 0.038μm), polycrystalline silicon substrates (above 0.057μm) and polished bare silicon substrates (above 0.060μm) measured by SP-5 manufactured by KLA TENCOR Corporation, and the product of the ratio (%) of organic residues in the defects calculated based on the above-mentioned SEM observation results are calculated as the number of organic residues (pieces).
[0208] It should be noted that the ratio (%) of organic residues in defects is 10% for TEOS substrates, 10% for silicon nitride (SiN) substrates, 90% for polycrystalline silicon substrates, and 90% for polished bare silicon substrates. In addition, the criteria for judging whether the number of organic residues has been reduced are 15,000 or less for TEOS substrates, 3,000 or less for silicon nitride substrates, 5,000 or less for polycrystalline silicon substrates, and 5,000 or less for bare silicon substrates, and these are recorded as good.
[0209] Table 2 below shows the evaluation results of organic residues in each surface treatment composition when a polished TEOS substrate, a polished silicon nitride substrate, and a polished polysilicon substrate were used as the surface treatment object.
[0210] [Table 1]
[0211]
[0212] [Table 2]
[0213]
[0214] As is clear from Tables 1 and 2, the surface treatment composition of the example can reduce the amount of organic residue on the surface of the cerium oxide particles and the polished object, as compared with the surface treatment composition of the comparative example.
[0215] Specifically, it is found that the surface treatment compositions of Examples 1 to 28 containing a chelating agent having a total of 2 or more phosphonic acid groups and carboxylic acid groups can remove cerium oxide and reduce organic residues on the polished TEOS substrate surface compared to the surface treatment compositions of Comparative Examples 1 to 3.
[0216] In addition, it can be seen that the surface treatment compositions of Examples 1 to 6 and 15 to 20 containing a phosphonic acid chelating agent can more effectively remove cerium oxide particles and can also more effectively reduce organic residues on the surface of the polished TEOS substrate. In addition, it can be seen that the surface treatment compositions of Examples 1 to 6 and 15 to 20 can also reduce the number of pit defects on Si.
[0217] In addition, it was found that the surface treatment compositions of Examples 1 to 14 containing polystyrene sulfonic acid-acrylic acid copolymers can reduce organic residues not only on the polished TEOS substrate surface but also on the polished silicon nitride substrate surface.
Claims
1. A surface treatment composition, which is a surface treatment composition for treating the surface of a polished object, comprising: A polymer having a structural unit represented by the following formula (1), Chelating agents, and water, In the formula (1), R 1 is a hydrocarbon group having 1 to 5 carbon atoms, R 2 is a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, The chelating agent is a compound having a phosphonic acid group.
2. The surface treatment composition according to claim 1, wherein In the chelating agent, the total number of the phosphonic acid group and the carboxylic acid group is 2 or more. The surface treatment composition according to claim 1 or 2, which has a pH of 5 or less. The surface treatment composition according to claim 1 or 2, which has a pH of 3 or less. The surface treatment composition according to claim 1 or 2, further comprising an ionic dispersant.
6. The surface treatment composition according to claim 5, wherein The ionic dispersant is a polymer compound having a sulfonic acid (salt) group.
7. The surface treatment composition according to claim 1 or 2, which does not substantially contain abrasive particles.
8. The surface treatment composition according to claim 1 or 2, wherein The polished object includes silicon oxide.
9. The surface treatment composition according to claim 6, wherein The polished object includes silicon nitride.
10. A method for producing a surface treatment composition, comprising the steps of: mixing a polymer having a structural unit represented by the following formula (1), a chelating agent and water; In the formula (1), R 1 is a hydrocarbon group having 1 to 5 carbon atoms, R 2 is a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, The chelating agent is a compound having a phosphonic acid group.
11. A surface treatment method, comprising treating a polished object with the surface treatment composition according to any one of claims 1 to 9 to reduce organic residues on the surface of the polished object.
12. The surface treatment method according to claim 11, wherein: The surface treatment includes rinsing, grinding or cleaning.
13. A method for manufacturing a semiconductor substrate, comprising the following surface treatment step: reducing organic residues on the surface of a polishing object after polishing by the surface treatment method according to claim 11 or 12, The polished object is a polished semiconductor substrate.