Ore dressing method for extracting high-purity silicon powder from quartz tailings
Through the pre-slurrying-desliming-grinding-classification-regrinding-magnetic separation process combined with multi-stage dehydration and magnetic separation technology, the complexity of impurities and resource utilization problems in quartz tail mud are solved, and the production of high-purity silicon powder is realized. Deep purification reduces production costs and environmental pollution, and improves product quality and whiteness.
Patent Information
- Application Number
- CN202210022942.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-01-10
AI Technical Summary
The existing quartz tail mud purification technology has complex processes, high production costs, environmental pollution, and inability to effectively remove impurities, which limits the development and utilization of high-purity silica powder in quartz tail mud, resulting in resource waste and environmental pollution.
It adopts pre-slurrying-desliming-grinding-classification-regrinding-magnetic separation process, combined with multi-stage dehydration and multi-stage magnetic separation technology, and achieves high-quality through high-frequency vibration dehydration, disc vacuum filtration and superconducting magnetic separation. Deep purification of pure silicon powder reduces production costs and environmental pollution.
Efficient extraction of high-purity silica powder is achieved. The product whiteness reaches 95.1%, the grade reaches 99.49wt%, the iron content is reduced to 0.0078wt%, and there is no secondary pollution. The production process is environmentally friendly and low-cost, and solves the problem of impurities affecting the quality of silica powder. problem.
Smart Images

Figure CN114273075B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for extracting high-purity silicon micropowder from quartz tailings, and belongs to the technical field of mineral processing. Background Art
[0002] Quartz is a common non-metallic mineral resource. Quartz powder can be purified and processed to obtain high-purity silicon micropowder. Thanks to its very stable physical and chemical properties, it can not only be widely used in traditional industries such as metallurgy, plates, coatings, etc., but also has an irreplaceable position and role in high-tech industries such as aerospace, solar energy, chips, etc.
[0003] Siliceous resources and quartz tailings contain high levels of impurities such as aluminum, iron, and mud (mainly clay). Due to their insufficient purity, they cannot be effectively developed and utilized and can only be used in low-end industries. They have low economic value or are even abandoned due to their lack of economic value, resulting in excessive accumulation and causing huge pollution and safety hazards to the surrounding environment.
[0004] The domestic quartz tailings purification technology started late and developed slowly. The high-purity quartz sand purification technology mainly adopts the acid washing process, and the silicon micropowder product purification technology generally adopts the "magnetic separation-flotation-acid washing" process. The process is complex, the production cost is high, and it pollutes the environment. In addition, impurities such as "yellow skin" and "black spots" in the silicon micropowder cannot be effectively removed, which has become a technical "bottleneck" problem in the industry. It has always restricted the development of the quartz tailings deep processing industry, resulting in a large number of valuable non-metallic minerals in the quartz tailings cannot be effectively recovered and utilized in a timely manner. Summary of the invention
[0005] The present invention aims to provide a physical beneficiation method suitable for extracting high-purity silicon micropowder from quartz tailings with a large mud content and high impurities such as iron, potassium, sodium, calcium, magnesium, aluminum and organic carbon. The beneficiation method has low production cost, no environmental pollution and no tailing in the entire production process.
[0006] The present invention is achieved in that:
[0007] A method for extracting high-purity silicon micropowder from quartz tailings. The quartz tailings are first screened by a vibrating screener to remove coarse particles and impurities. Materials larger than 0.12 mm are stored separately for further treatment. Materials with a particle size smaller than 0.12 mm enter the secondary mixing tank for slurry adjustment. After slurry adjustment, they are pumped to a separation tower for three desliming operations: the overflow of the primary separation tower is discharged into a sedimentation tank, the bottom flow enters the secondary separation tower for secondary desliming after slurry adjustment in the mixing tank, the overflow of the secondary separation tower is discharged into a sedimentation tank, the bottom flow enters the tertiary separation tower for tertiary desliming after slurry adjustment in the mixing tank, the bottom flow of the tertiary separation tower is pumped to a high-frequency vibration dewatering screen for dehydration, the products on the screen are stored in a raw material finished product warehouse, the materials under the high-frequency vibration dewatering screen and the overflow mixture of the first three separation towers are discharged into a sedimentation tank, and the overflow of the sedimentation tank can be reused as return water in the mineral processing process;
[0008] After desludging, the quartz fine mud product is fed to the belt conveyor by the belt feeder, and then sent to the ball mill ore feeding trolley by the belt conveyor and enters the ball mill. The ball mill grinding product is discharged into the pump pool, and the slurry is sent to the hydrocyclone group for classification through the slurry pump. The fineness of the classified overflow product is controlled at -0.043mm, accounting for 95~98wt%. The cyclone sedimentation is fed into the continuous ball mill for grinding treatment. The whole process constitutes a closed-loop circulation process of grinding and classification. The overflow of the cyclone is fed to the high-frequency vibration deslagging screen, and the screened product is sent to the magnetic separation operation through the slurry pump;
[0009] The magnetic separation equipment uses a superconducting magnetic separator for separation. The overflow product of the cyclone classification is sent to the magnetic separator through a slurry pump for a magnetic separation operation to obtain a primary magnetic separation concentrate and a primary magnetic separation tailings; the magnetic separation concentrate is slurried and then enters a secondary magnetic separation operation to obtain a secondary magnetic separation concentrate and a secondary magnetic separation tailings; the secondary magnetic separation concentrate is slurried and then enters a tertiary magnetic separation operation to finally obtain a tertiary magnetic separation concentrate product (i.e., a low-iron, high-purity silicon micropowder product) and a tertiary magnetic separation tailings product. The first three magnetic separation tailings products are combined into medium ore products (i.e., high-iron, high-silicon products);
[0010] After three magnetic separations, the concentrate product is dehydrated in two stages by a concentration tower and a disc vacuum filter to obtain a high-purity silicon micropowder concentrate with a moisture content of 10~15wt%. After being dried by a disc continuous drying equipment, a high-purity silicon micropowder product with a moisture content of about 1wt% is finally obtained.
[0011] Aochuang Wanhe (Shenzhen) Technology Co., Ltd. (China-Australia Silicon Innovation Team) organized core scientific researchers to study quartz tailings resources in Zhanjiang, Guangdong, Ji'an, Jiangxi, and Huaihua, Hunan. They conducted field research and sampling on site to fully understand the local quartz ore structure, mineral types and occurrence states, mineral co-existence and mosaic relationships, particle size distribution, migration and distribution of valuable components and impurities in the process of mineral processing and enrichment, and the degree of monomer dissociation under different particle size conditions. Based on the research results of process mineralogy properties, they conducted small and pilot tests on quartz tailings deep purification technology research and development, such as desludging, separation of potassium, sodium, calcium, aluminum, and iron impurity components, removal of organic carbon, iron removal, grinding fineness, and fine mud sedimentation separation, and formed a pre-slurrying-desludging-grinding-classification-regrinding-magnetic separation process for quartz tailings, and achieved success. At present, the invention has been tested by a 500 kg material expansion continuity test, which verifies the stability, continuity, and reliability of the mineral processing process. The present invention is mainly aimed at the treatment process of fine-grained tailings generated in the process of producing glass sand, fine mud generated in the process of marble processing, potassium-sodium feldspar, kaolin and other fine muds. The various process methods of the present invention are conventional and easy to implement in industrial production. The pre-slurry adjustment-demuding-grinding-classification-regrinding-magnetic separation process is used to deeply purify high-purity silicon micropowder. Compared with the traditional process, it reduces the production cost, simplifies the production process, and the production process is chemically pollution-free and environmentally friendly. The present invention is based on solving the problems of large mud content in quartz tailings, complex impurity components, and organic carbon affecting the quality and whiteness of silicon micropowder products. The production process is simpler than the traditional process, the production cost is low, there is no secondary pollution, and it is easy to implement in production.
[0012] The characteristics and advantages of the present invention are as follows:
[0013] 1. Fine mud separation process: In view of the fine particle size and high mud content of this type of tailings, this process adopts a pre-multi-stage pulping, coarse and fine slurry separation, separation tower and cyclone combined desludging and tailings discarding process;
[0014] 2. Dehydration equipment configuration: high-frequency vibrating screen is used to dehydrate the desludging product, disc vacuum filter is used to dehydrate high-purity silicon powder and iron slag, and automatic diaphragm plate and frame filter press is used to dehydrate overflow fine particles. The equipment process configuration has low energy consumption and obvious dehydration effect;
[0015] 3. Grinding-classification closed-loop process: It solves the problems of over-crushing of useful minerals and poor monomer dissociation, effectively removes organic carbon, and improves the quality and whiteness of silicon micropowder. The whiteness of the product reaches 95.1 and the grade reaches 99.49wt%;
[0016] 4. Multi-stage superconducting magnetic separation process: The three-stage series magnetic separation process is adopted to effectively reduce the iron content in silicon micropowder, and the product purity is effectively improved. The iron content in high-purity silicon micropowder is reduced from 0.030wt% to 0.0078wt%;
[0017] 5. Through the organic combination of the various processes in the above process, the quartz tailings with high mud content and multiple impurities such as potassium, sodium, calcium, magnesium, titanium and iron are deeply purified, and SiO2: 99.49wt%, K2O, Na2O, MgO, TiO2 are all less than 0.010wt%, and Fe2O3 is 0.0078wt%. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 A schematic diagram of the process flow of the present invention is shown;
[0019] Figure 2 Draw a table showing the test results of the raw ore of quartz tailings samples from Yilong Mining Company in Zhanjiang City, Guangdong Province;
[0020] Figure 3 A table showing the test results of mineral processing technology indicators obtained by using the present invention on the quartz tailings sample ore of Yilong Mining Company in Zhanjiang City, Guangdong Province. DETAILED DESCRIPTION
[0021] Taking the purification of high-purity silicon powder from quartz tailings of Yilong Minerals Company in Zhanjiang City, Guangdong Province as an example, the test results of the original ore of the sample are shown in Figure 2 :
[0022] The conclusion of the sample mineral identification is as follows:
[0023] (1) The main component is SiO2, the main impurity elements are Al2O3, K2O, Na2O, CaO, MgO, TiO2 and Fe2O3, and the main impurity components are mica, etc.;
[0024] (2) The product particle size is relatively fine: -0.12~+0.043 mm accounts for 50wt%, -0.043~+0.020 mm accounts for 33wt%, and -0.020 mm accounts for 17wt%.
[0025] The quartz tailings sample adopts the following process flow, and the obtained mineral processing process indicators are shown in Figure 3 :
[0026] The process is as follows:
[0027] 1. Feeding: The raw materials are fed into a mixing barrel with a diameter of Φ1m through a feeder for slurry adjustment, and the concentration is controlled at 25~30wt%. The slurry is pumped by a diaphragm pump to another mixing barrel with a diameter of Φ1m for mixing, and then pumped into a separation tower by a vertical sand pump for desludging;
[0028] 2. Mud and sand separation: Under a certain pressure, the slurry is separated by a special separation device (a separation tower with a diameter of Φ1 meter). The overflow of the separation tower is the tailings product, and the bottom flow of the separation tower is the desludging product. The desludging product is slurried to a concentration of 25~30wt%. After two desludgings in the separation tower, the final sorted coarse concentrate product is obtained;
[0029] 3. Dehydration of coarse concentrate: Use high-frequency vibrating fine screen to dehydrate the sorted coarse concentrate to obtain the coarse concentrate product after dehydration, with a moisture content of 10~15wt%;
[0030] 4. Grinding-classification cycle: The dehydrated materials are fed into the Φ1200×1420mm continuous ball mill in batches for grinding. The grinding products are controlled and classified by a Φ200mm hydrocyclone. The particle size range of the classified overflow products is controlled to be -0.074mm, accounting for 95~98wt%. The classified sand is returned to the ball mill for regrinding.
[0031] 5. Multi-stage magnetic separation: The cyclone overflow is subjected to three-stage series magnetic separation using a superconducting magnetic separator of model ACWHSL-500GG to obtain magnetically separated concentrate products (low iron and high purity silicon powder 1) and magnetically separated tailings products (high iron and high silicon powder 2);
[0032] 6. Filtration: Use a disc vacuum dehydrator to dehydrate the magnetic separation concentrate product to obtain a high-purity silicon micropowder concentrate product with a moisture content of 10~15wt%; the tailings from each stage of magnetic separation are combined into a middling product and dehydrated using a vacuum disc filter to obtain a high iron and high silicon product with a moisture content of 10~15wt%; the filtrate is discharged into a sedimentation tank, and a flocculant is added to clarify it. The supernatant can be used as mineral processing return water;
[0033] 7. Drying: The high-purity silicon micropowder concentrate is dried and dried by a disc continuous dryer to obtain a high-purity silicon micropowder product with a moisture content of less than 1wt%.
[0034] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art of the present invention, several equivalent substitutions or obvious modifications can be made without departing from the concept of the present invention. All equivalent changes made according to the structure, shape, and principle of the present invention should be deemed to belong to the protection scope of the present invention.
Claims
1. Extraction of high-purity silicon powder from quartz tailings It is characterized in that include: (1) Tailing mud generated in the process of mineral processing - 0.120mm, not only limited to the quartz tailing mud generated in the process of glass sand production, but also applicable to the purifying method of potassium, sodium, calcium, magnesium and aluminum non-metallic mineral products from the tailing mud generated in the process of marble, feldspar, carbonate rock, kaolin and mica mineral processing; (2) The quartz tailings are washed with water to remove a large amount of ore mud and clay; (3) Washed sludge and clay are collected in a concentration tank, and the supernatant is returned to the beneficiation process as backwater. The bottom flow is filtered and stored in the tailings bin; (4) Grinding the desludging product and controlling the fineness of the grinding product by classification; (5) The classified products are subjected to magnetic separation to obtain a magnetic separation concentrate product; after filtration, a high-purity silicon micropowder concentrate with a moisture content of 10-15wt% is obtained; (6) The high-purity silicon micropowder concentrate is dried to produce a high-purity silicon micropowder product, the moisture content of which is less than 1wt%; The equipment used in the water washing and desludging process in step (2) is a separation tower and a hydrocyclone; In step (4), the grinding process adopts a closed-circuit grinding-classification process, the grinding concentration is controlled at 75-80wt% by mass, the grinding equipment adopts a continuous ball mill, the liner adopts a high-aluminum alloy material with an aluminum content of 92-95wt%, and the grinding medium adopts a high-aluminum alloy material with an aluminum content of 92-95wt%; the classification equipment adopts a hydrocyclone, and the fineness of the classified product is controlled at -0.043mm particle size accounting for 95-98wt%.
2. The method for extracting high-purity silicon powder from quartz tailings according to claim 1, It is characterized in that The non-metallic mineral products in step (1) include: kaolin concentrate, alumina concentrate, potassium feldspar, sodium feldspar concentrate and mica concentrate.
3. The method for extracting high-purity silicon powder from quartz tailings according to claim 1, It is characterized in that In step (3), the filtering equipment adopts an automatic diaphragm plate and frame filter press.
4. The method for extracting high-purity silicon powder from quartz tailings according to claim 1, It is characterized in that In step (5), the magnetic separation process adopts a three-stage selection process. The magnetic concentrate is filtered to produce a high-purity silicon micropowder product, and the magnetic tailings are filtered to produce a high-iron and high-silicon product. The three-stage magnetic selection equipment adopts a superconducting magnetic separator.
5. The ore dressing method for extracting high-purity silicon powder from quartz tailings according to claim 1, It is characterized in that In step (6), the drying equipment is a disc-type continuous dryer.
6. The ore dressing method for extracting high-purity silicon powder from quartz tailings according to claim 4, It is characterized in that The filtration equipment for magnetic tailings and magnetic concentrate products adopts disc vacuum dehydrator.
7. The method for extracting high-purity silicon powder from quartz tailings according to any one of claims 1 to 6, It is characterized in that The obtained high-purity silicon micropowder product has a silicon dioxide content of 99.30-99.50wt%, a ferric oxide content of 0.0078-0.013wt%, a natural whiteness of 90-96, and a burnt whiteness of 95-98.
Citation Information
Cited By
Method for preparing silica powder based on chlorinated waste brine quenching slag
CN121020594A