Cathode component for electron beam generation and method for manufacturing the same
By using cathode components with iridium and cerium compounds as the main phase and fabricating single-phase or single-crystal structures through the floating zone method, the shortcomings of existing cathode components in terms of electron emission characteristics and current density have been overcome, and a high-performance electron beam generator has been realized.
Patent Information
- Application Number
- CN202080060617.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-02
- Filing Date
- 2020-08-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-08-28
AI Technical Summary
Existing cathode components for electron beam generation have shortcomings in electron emission characteristics and current density, making it difficult to achieve further high performance.
Using compounds containing iridium and cerium as the main phase or two phases, with the content of by-components controlled below 5% by area, single-phase or single-crystal cathode components are manufactured by the floating zone method to ensure compositional uniformity and consistent crystal orientation.
It achieves excellent electron emission characteristics, can increase the energy of the electron beam, and is suitable for high current density electron beam generating devices.
Smart Images

Figure CN114302983B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a cathode structure for electron beam generation and a method for manufacturing the same. Background Art
[0002] Cathode components (cathode, electron gun) for electron beam generation can be mainly divided into three types according to the principle of electron emission: thermal electron emission, photoelectron emission, and field electron emission. Thermal electron guns that use thermal electron emission are used in various devices and equipment such as electron microscopes and electron beam melting devices. Photoelectron emission type photoelectron guns use the photoelectric effect and are used in low-energy electron beam irradiation devices and non-destructive analysis devices. In addition, field electron emission type components are used in field emission electron microscopes, etc.
[0003] As materials constituting the cathode components for electron beam generation, tungsten (W) and tantalum (Ta) have been used in the past. Recently, lanthanum hexaboride (LaB6) has been used, which can achieve higher current density and longer life than tungsten and tantalum. In addition, it is disclosed in non-patent document 1 that iridium-cerium (Ir-Ce) alloys have less evaporation loss when used at high temperatures than LaB6, and have high durability against corrosive gases. Therefore, if this Ir-Ce alloy is used for the cathode components for electron beam generation, it can be expected to have a longer life.
[0004] In addition to the above-mentioned non-patent document 1, patent documents 1 to 3, non-patent document 2 and non-patent document 3 also report that cathode components made of the above-mentioned Ir-Ce alloy show good properties compared to existing cathode components made of LaB6 and the like, for example, showing excellent performance in low vacuum and corrosive gas atmospheres.
[0005] In addition, it is reported in non-patent document 4 that the work function of Ir-Ce series materials is 2.57 eV (1300K), and Ir-La, Ir-Pr, Ir-Nd, Ir-Sm, etc. also show roughly the same value. In addition, it is reported in the non-patent document 1 that among the cathode materials of Ir-rare earth elements, the cathode materials of Ir-Ce alloy system have a lower evaporation loss rate at the same current density than the cathode materials using La and Pr as other rare earth elements. It is reported in non-patent document 5 that Ir2Ce shows the best characteristics in the composition of iridium-cerium alloys.
[0006] As a method for manufacturing the Ir-Ce alloy used for the cathode component for electron beam generation, the following methods can be listed. First, an arc melting + solidification method is listed in which a metal as a raw material is melted by an arc melting method in an inert gas atmosphere and then solidified. In addition, an arc melting + sintering method is listed in which the solidified material obtained by the arc melting + solidification method is crushed and then the crushed material is sintered. In addition, a mechanical alloying method + sintering method is listed in which the raw material powder is alloyed by a mechanical alloying method and then sintered.
[0007] The arc melting + sintering method is disclosed in Patent Document 4. Specifically, the method discloses a process of preparing a powder having a maximum length of 500 μm or less by melting, mixing and solidifying iridium-cerium raw materials in an inert gas atmosphere by a melting method using a water-cooled copper container as a melting crucible, and then crushing the powder to form the powder under high temperature and high pressure conditions of a temperature of 800° C. to 1500° C. and a pressure of 10 MPa or more, thereby maintaining the homogeneity of the component composition, suppressing the occurrence of defects such as cracks and defects, and achieving a long life of the cathode component.
[0008] In recent years, as shown in Non-Patent Document 6, a technique for producing a single crystal solidified material of an Ir—Ce alloy using a quadruple arc furnace has been proposed.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: U.S. Patent No. 5773922
[0012] Patent Document 2: Japanese Patent Application No. 2002-527855
[0013] Patent Document 3: Japanese Patent Application Publication No. 2002-260520
[0014] Patent Document 4: Japanese Patent Application Publication No. 2015-198034
[0015] Non-patent literature
[0016] Non-patent document 1: G. Kuznetsov, "High temperature cathodes for high current density", Nuclear Instruments and Methods in Physics Research A340, 1994, pp. 204-208
[0017] Non-patent document 2: T. Natsui, M. Yoshida, et al., "High Charge Low Emittance RFGun for SUPERKEKB", Proc. IPAC, 2012, pp. 1533-1535
[0018] Non-patent document 3: GI Kuznetsov, "IrCe Cathode For EBIS", J. Physics: Conference Series 2, 2004, pp. 35-41
[0019] Non-patent literature 4: SERozhkov, OKKulashev, and LIDashevskaya, "WORKFUNCTION OF IRIDIUM ALLOYS WITH LANTHANUM, CERIUM, PRASEODYMIUM, NEODYMIUM, ANDSAMARIUM", Brief messages, Received 1967, pp.936-937
[0020] Non-patent document 5: D. Satoh et al., "High performance of iridium-cerium photocathode for SuperKEKB electron injector", Proceedings of PASJ2017, WEP106 (2017)
[0021] Non-patent document 6: H. Sugawara et al., "Single crystal growth and electrical properties of CeRh2 and CeIr2", J. Phys. Soc. Jpn. 63, pp. 1502-1507 (1994)
[0022] In the arc melting + solidification method, defects and cracks are easily generated during solidification. The sintered material obtained by the arc melting + sintering method or the mechanical alloying method + sintering method shown in Patent Document 4 is denser than the solidified material, and can suppress the occurrence of defects such as cracks and defects, and can achieve a longer life. However, in recent years, it is required to further improve the electron emission characteristics, especially to achieve a cathode component for electron beam generation that can further increase the current density. Summary of the invention
[0023] Technical issues to be solved by the invention
[0024] The present invention is proposed in view of this situation, and its purpose is to provide a cathode component for electron beam generation with excellent electron emission characteristics and high performance such as increased electron beam energy, and a practical size and a manufacturing method thereof. Hereinafter, the cathode component for electron beam generation of the present invention is referred to as "cathode component" for short.
[0025] Technical means to solve problems
[0026] A first aspect of the present invention is a cathode member for electron beam generation, wherein:
[0027] A single phase or two phases of a compound containing iridium and cerium accounts for more than 95% by area,
[0028] The total content of metallic iridium and one or more accessory components in oxides of one or more elements selected from iridium and cerium is 5 area % or less.
[0029] A second aspect of the present invention is the cathode member for electron beam generation according to the first aspect, wherein the compound containing iridium and cerium is a compound selected from the group consisting of Ir2Ce, Ir3Ce, Ir7Ce2 and Ir5Ce2.
[0030] A third aspect of the present invention is the cathode member for electron beam generation according to the first or second aspect, wherein the size of the subcomponent is 50 μm or less in terms of an equivalent circle diameter.
[0031] Aspect 4 of the present invention is the cathode component for electron beam generation according to aspect 2 or 3, wherein a single phase of Ir2Ce, Ir3Ce, Ir7Ce2 or Ir5Ce2 occupies 95% by area or more.
[0032] Aspect 5 of the present invention is the cathode member for electron beam generation according to aspect 2 or 3, wherein two phases of Ir2Ce and Ir3Ce, Ir2Ce and Ir7Ce2, or Ir7Ce2 and Ir3Ce account for 95% by area or more.
[0033] Mode 6 of the present invention is a cathode component for electron beam generation according to Mode 1, wherein the compound containing iridium and cerium contains a single phase of Ir2Ce, Ir3 Ce, Ir7Ce2 or Ir5Ce2, and does not include metallic iridium and oxides of one or more elements among iridium and cerium.
[0034] A seventh aspect of the present invention is the cathode member for electron beam generation according to any one of aspects 1 to 6, wherein the single-phase crystal structure is unidirectional solidification or single crystal.
[0035] Aspect 8 of the present invention is a method for manufacturing a cathode member for electron beam generation according to any one of aspects 1 to 7, comprising the following steps:
[0036] A melting step of melting a metallic cerium raw material and a metallic iridium raw material to obtain a smelted material;
[0037] A pulverizing step of pulverizing the smelted material to obtain a pulverized product;
[0038] A sintering step of sintering the crushed product of the molten material at a temperature of 1400 to 1600° C. and a pressure of 25 to 50 MPa to obtain a sintered material for crystal production;
[0039] A crystal production process is provided for producing a compound crystal containing iridium and cerium by a floating zone method using the crystal production sintered material.
[0040] A ninth aspect of the present invention is a method for manufacturing a cathode member for electron beam generation according to the eighth aspect, wherein:
[0041] After the crystal production step, the process further includes: a crystal crushing step of crushing the crystal to obtain a crushed product;
[0042] A sintering step is performed in which the crushed product of the crystal is sintered at a temperature of 1400 to 1600° C. and a pressure of 25 to 50 MPa to obtain a sintered product.
[0043] Effects of the Invention
[0044] According to the present invention, it is possible to provide a cathode member for electron beam generation having excellent electron emission characteristics and capable of realizing high performance in terms of increased energy of electron beams and having a practical size, and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a photograph of the appearance of a crystal (cathode member) obtained in Examples.
[0046] Figure 2 This is a scanning electron microscope observation photograph (magnification 100 times) of a crystal (cathode member) in the example.
[0047] Figure 3 This is a scanning electron microscope observation photograph (magnification 10000 times) of the crystal (cathode member) in the example.
[0048] Figure 4 It is a figure which shows the EDX analysis result of the crystal (cathode member) in Example.
[0049] Figure 5 This is a photograph showing the EBSD analysis range of the crystal (cathode member) in the example.
[0050] Figure 6 It is a figure which shows the EBSD analysis result of the crystal (cathode member) in Example.
[0051] Figure 7 is a powder X-ray diffraction (XRD) pattern of the crystal (cathode member) in the example.
[0052] Figure 8 This is a scanning electron microscope observation photograph (magnification 500 times) of the crystal (cathode member) in the example. DETAILED DESCRIPTION
[0053] The inventors of the present invention have made intensive research on the use of Ir-Ce materials to achieve excellent electron emission characteristics, that is, to further increase the current density, and as a result, to achieve a high-performance, practical-sized cathode component for electron beam generation and a method for manufacturing the same, with the use of Ir-Ce materials as a prerequisite. As a result, it was found that as long as a single phase or two phases of a compound containing iridium and cerium account for more than 95 area %. In addition, the present invention can achieve a cathode component having the above-mentioned structure, and the total content of one or more secondary components in the oxide of metal iridium and one or more elements of iridium and cerium is less than 5 area %. In addition, the present invention also found that as a method for manufacturing a cathode component, if a crystal containing a compound of iridium and cerium is prepared by a floating zone method as a prerequisite, and a raw material for the floating zone method is prepared by the method of the present invention, a cathode component with a practical size, suppressed defects, excellent electron emission characteristics, and high-performance that can increase the energy of the electron beam can be obtained. The following is described in order from the cathode component for electron beam generation of the present invention.
[0054] First, the cathode component of the present invention is mainly composed of a compound containing iridium and cerium. As the compound containing iridium and cerium, in order from low to high Ce concentration added to Ir, Ir5 Ce, Ir7Ce2, Ir3 Ce, Ir2Ce, Ir4Ce5, Ir3 Ce5, Ir3 Ce7, IrCe3, and IrCe4 can be listed. Among them, it is preferred to select one or more from Ir2Ce, Ir3 Ce, Ir7Ce2, and Ir5 Ce, which have high melting points and are suitable for cathode components for electron beam generation that are easily formed into high-temperature atmospheres. Among these four compounds, Ir2Ce is most preferred because the higher the thermodynamic stability and the higher the Ce concentration, the better the electron emission characteristics.
[0055] Therefore, when the compound containing iridium and cerium constituting the cathode member is a single phase, the compound containing iridium and cerium is preferably Ir2Ce, Ir3Ce, Ir7Ce2 or Ir5Ce2, and most preferably Ir2Ce. In addition, when the compound containing iridium and cerium constituting the cathode member is a two-phase, the compound containing iridium and cerium is preferably two compounds selected from the group consisting of Ir2Ce, Ir3Ce, Ir7Ce2 and Ir5Ce2, and more preferably a combination of Ir2Ce and Ir3Ce, Ir2Ce and Ir7Ce2, or Ir7Ce2 and Ir3Ce.
[0056] The cathode component for electron beam generation of the present invention can fully exert excellent electron emission characteristics by containing 95% by area or more of the single phase or two phases of the compound containing iridium and cerium (Ir-Ce compound). The proportion of the single phase or two phases of the compound containing iridium and cerium in the entire cathode component is preferably 98% by area or more, more preferably 99.945% by area or more, further preferably 99.99% by area or more, and further preferably 99.999% by area or more.
[0057] The ratio of the single phase or two phases of the compound containing iridium and cerium can be evaluated by microscopic observation photos or X-ray diffraction as shown in the examples described later. In microscopic observation, the difference in phase can be judged due to the difference in contrast, and the area ratio of the single phase or two phases of the compound containing iridium and cerium in the entire field of view can be obtained. In addition, by performing EDX analysis (energy dispersive X-ray analysis, Energy dispersive X-ray spectrometry), the components of the phase can be identified. In addition, peak separation can be performed in the X-ray diffraction method for quantitative evaluation.
[0058] The cathode component of the present invention may also contain substances other than the above-mentioned Ir-Ce compound within the range that does not hinder the electron emission characteristics. The substance may include one or more secondary components of metal iridium and oxides of one or more elements among iridium and cerium. The proportion of the secondary components is preferably 5 area% or less (including 0 area%) in total. From the perspective of achieving more preferred electron emission characteristics, the proportion of the above-mentioned secondary components is more preferably 3 area% or less, and most preferably 0 area%. In other words, it does not include: metal iridium; and oxides of one or more elements among iridium and cerium.
[0059] When the auxiliary component is included, it is preferred that the size of the auxiliary component is less than 50 μm in terms of equivalent circle diameter, since it is easier to ensure good electron emission characteristics. In other words, when observing by the method described in the embodiments described later, it is preferred that the size of the largest auxiliary component observed in the observation field is suppressed to less than 50 μm in terms of equivalent circle diameter. The size of the oxide is more preferably less than 30 μm in terms of equivalent circle diameter, and further preferably less than 15 μm in terms of equivalent circle diameter. The size of the auxiliary component is obtained by the method described in the embodiments described later.
[0060] The cathode component of the present invention preferably contains a single phase of Ir2Ce, Ir3Ce, Ir7Ce2 or Ir5Ce2, in other words, the entire structure of the cathode component is occupied by the single phase, and does not contain metal iridium, and oxides of one or more elements among iridium and cerium. More preferably, it contains a single phase of Ir2Ce, and does not contain metal iridium, and oxides of one or more elements among iridium and cerium.
[0061] The cathode component of the present invention is preferably a single-phase crystal structure that is unidirectionally solidified or single crystal. By making the composition uniform and the crystal orientation uniform in one direction to homogenize the crystal structure, it is possible to further improve the electron emission characteristics. The cathode component of the present invention is more preferably a single-phase and single crystal of the compound containing iridium and cerium (preferably Ir2Ce, Ir3Ce, Ir7Ce2 or Ir5Ce2, particularly preferably Ir2Ce).
[0062] The cathode component of the present invention has a shape in which the maximum equivalent circular diameter of a cross section perpendicular to the long axis direction can be 5 mm or more. It is more suitable for applications such as electron beam welding machines that require high current density. Specifically, it can be used as a cathode component with higher heat resistance. The maximum equivalent circular diameter is more preferably 7 mm or more, and further preferably 10 mm or more. If the cathode component is manufactured by the floating zone method, the long axis direction is the same as the growth direction of the crystals by the floating zone method. In addition, if the shape of the cathode component is a sphere with an uncertain long axis direction, the long axis direction can be in any direction.
[0063] [Manufacturing method]
[0064] Next, the manufacturing method of the cathode component is described. The manufacturing method of the cathode component for electron beam generation of the present invention comprises the following steps:
[0065] A melting step of melting a metallic cerium raw material and a metallic iridium raw material to obtain a smelted material;
[0066] A pulverizing step of pulverizing the smelted material to obtain a pulverized product;
[0067] A sintering step of sintering the pulverized material in a high temperature and high pressure atmosphere to obtain a sintered material;
[0068] A crystal production process is to produce a crystal containing a compound of iridium and cerium by a floating zone method using the sintered material.
[0069] Hereinafter, each step of the production method of the present invention will be described. Hereinafter, the floating zone method is referred to as the "FZ method".
[0070] In the method of the present invention, the crystal is produced by the floating zone (FZ) method as described above. In the existing FZ method, the raw material rod used as the raw material has fine pores, or there are deviations in pore distribution and sintering density, which makes the supply of raw materials in the FZ method unstable, the component composition is easily uneven, and it is difficult to obtain crystals with consistent directions.
[0071] In the present invention, raw materials for the FZ method, i.e., raw material rods and seed materials, are prepared as follows. The homogeneous and high-sintered density sintered material prepared as follows is used as the raw material rods and seed materials in the FZ method, thereby obtaining a desired high-quality crystal with homogeneous component composition, preferably a unidirectional solidified material or a single crystal.
[0072] [Production of sintered material for crystal production]
[0073] (Melting process)
[0074] First, prepare a metal cerium raw material and a metal iridium raw material. These raw materials sold on the market can also be directly used for melting. In the present invention, since the impurities can be removed by the FZ method, the impurity concentration of oxygen and the like in the smelting material and sintered material used for the FZ method is not important. However, the raw materials can also be pre-treated in the following manner before melting as needed. As the pre-treatment of the raw materials, for example, mechanically removing the altered parts such as the oxide film present in the metal cerium raw material can be cited. Specifically, for example, using a metal file, a router, a grinder, a shear, etc., grinding the above-mentioned altered parts for removal.
[0075] After mechanical removal, pickling and water washing can also be performed. The acid used for pickling has no particular problem as long as it can remove the above-mentioned surface deterioration layer. For example, it can be immersed in an acid aqueous solution such as a nitric acid aqueous solution (normal temperature) in which nitric acid is diluted with water at a ratio of nitric acid: water (volume ratio) = 1:6. It is preferred that after pickling, water washing is performed to remove the acid attached to the cerium.
[0076] The form of the metallic iridium raw material is not important. As shown in the examples described below, powdered metallic iridium may be used. When powdered iridium is used, a material having an average particle size in the range of 45 to 90 μm may be used.
[0077] The above-mentioned metal cerium raw material and metal iridium raw material are mixed and melted in an inert gas atmosphere. Examples of the melting method include plasma arc melting and cold crucible induction melting. From the viewpoint of preventing oxidation of the ingot, the plasma arc melting method using high-purity Ar gas is preferred. After the melt mixing, for example, it is poured into a mold to solidify, and an Ir-Ce alloy ingot can be obtained as a smelting material.
[0078] (Melt material crushing process)
[0079] The molten material is crushed. The molten material may be cut into the size of the raw material for crushing by mechanical processing as needed. In addition, the altered part of the raw material for crushing may be removed by grinding treatment or the like as needed before crushing. Since the raw material contains a large amount of cerium as an active element, the atmosphere for crushing is not in the air atmosphere, but preferably in an inert gas atmosphere such as argon. The method of crushing is not particularly limited, and for example, crushing can be performed by crushing in a glove box filled with an inert gas.
[0080] The size of the pulverized product is preferably in the range of 45 to 90 μm, for example, in the average particle size. For example, in the FZ method described later, in order to produce a crystal of a compound containing iridium and cerium having a size and composition that satisfies the embodiment of the present invention, it is preferred to use a dense raw material rod, and in order to obtain the dense raw material rod, it is preferred to finely pulverize the above-mentioned molten material. However, if the above-mentioned molten material is pulverized too finely, the raw material is easily oxidized, so the size of the pulverized product is preferably within the range of the above-mentioned average particle size.
[0081] (Sintering process of pulverized product of molten material)
[0082] The crushed material is filled into a sintering mold, and a sintered material for crystal production can be manufactured by spark plasma sintering in an inert atmosphere such as argon, such as a raw material rod and a seed material for FZ method. The conditions of the spark plasma sintering method are preferably a temperature of 1400 to 1600°C and a pressure of 25 to 50 MPa. More preferably, the temperature is 1500 to 1550°C and the pressure is 45 to 50 MPa. The sintering can also be performed by hot pressing sintering, instead of the spark plasma sintering method.
[0083] [Crystal production process]
[0084] In an embodiment of the present invention, a raw material rod obtained from the sintered material and a seed material are used to produce a crystal containing a compound of iridium and cerium by the FZ method. In this method, since a crucible is not used, there is no worry that impurities will be mixed from the crucible. In addition, a high temperature can be reached without relying on the heat-resistant temperature of the crucible.
[0085] As the FZ method, both high frequency heating and concentrated light heating can be used. As raw materials, there are two modes: a mode in which a seed material is set on the raw material rod together with the raw material rod to control the orientation, and a mode in which only the raw material rod is used without setting the seed material. Hereinafter, as the FZ method, a method of making a crystal by concentrated light heating using a raw material rod and a seed material is described as an example.
[0086] As an apparatus for implementing the FZ method, a focused heating floating zone (FZ) culture apparatus equipped with a xenon lamp can be cited. On the upper and lower axes of the apparatus, the raw material rod and the seed material are respectively fixed via a fixture, and an inert gas is introduced into the FZ culture apparatus. As an inert gas, for example, a high-purity argon gas is introduced at a flow rate of 1 to 10 L / min. The seed material and its peripheral parts are melted by focused heating to form an initial molten zone, thereby cultivating a single crystal at a culture speed of 0.1 to 50 mm / hr or performing unidirectional solidification, thereby obtaining a crystal. In addition, the rotation speed of the upper and lower axes can be 1 to 100 rpm.
[0087] If necessary, the crystals may be crushed and then sintered as described below. This method can provide a cathode member having a higher strength and capable of being used for a longer period of time.
[0088] [Crystal crushing process]
[0089] The crystal obtained by the crystal production step is crushed to obtain a crushed product of the crystal. Since the raw material contains a large amount of cerium as an active element, the crushing atmosphere should not be in the air atmosphere, but preferably in an inert gas atmosphere such as argon. The crushing method is not particularly limited, and for example, crushing in a glove box filled with an inert gas can be cited. The particle size of the crushed product is preferably in the range of 45 to 90 μm, for example, an average particle size.
[0090] [Sintering step of crushed crystal]
[0091] The crushed crystal is sintered in a high temperature and high pressure atmosphere to obtain a sintered product. The crushed product can be filled into a sintering mold, and a sintered material can be produced by a spark plasma sintering method in an inert atmosphere such as argon. The conditions of the spark plasma sintering method are preferably a temperature of 1400 to 1600° C. and a pressure of 25 to 50 MPa. The sintering can also be performed by a hot press sintering method instead of the spark plasma sintering method.
[0092] After the crystal is produced or after the pulverized product of the crystal is sintered, it may be subjected to machining or the like to obtain a shape of a cathode member as required.
[0093] Example
[0094] The following examples are given to more specifically illustrate the embodiments of the present invention. The present invention is not limited to the following examples, and can be appropriately modified and implemented within the scope of the above and below-mentioned purposes, and these are all included in the technical scope of the present invention.
[0095] 1. Preparation of sintered material for crystal production
[0096] As a raw material for crystal production used in the FZ method, a seed crystal material and a raw material rod are produced in the following manner.
[0097] 1-1. Preparation of smelting materials (ingots)
[0098] In the manufacture of molten materials for cathode components for electron beam generation, commercially available metal cerium (purity 3N) and high-purity iridium powder (purity of about 3N) stored in oil are used. First, the inventors of the present invention grind the surface of the metal cerium raw material using a router to remove the altered parts such as the oxide film. Thereafter, an acid pickling treatment is performed. In the acid pickling treatment, the cerium raw material after the surface grinding is immersed in a nitric acid aqueous solution diluted with nitric acid: water (volume ratio) = 1:6 to remove the residual oxide film, etc. In the said immersion, the metal cerium with a diameter of about several mm is immersed for several seconds each. After the acid pickling treatment, the acid attached to the cerium raw material is removed by water washing with pure water to prepare the metal cerium raw material.
[0099] The pre-treated metallic cerium raw material and the iridium powder are mixed in such a way that the cerium content in the total raw material is 26.7% by mass and the balance is iridium, melted by a plasma arc melting method using high-purity Ar gas, and poured into a mold to obtain an ingot (melting material) of an iridium-cerium alloy.
[0100] 1-2. Crushing process of molten material and sintering process of crushed material
[0101] The ingot is cut into pieces with a diameter of 10 mm and a length of 2 to 3 mm by mechanical processing, and the processed surface is ground to remove the surface oxide film and the deteriorated layer. Then, the ingot is manually crushed in an inert gas atmosphere to obtain fine powder with an average particle size of 45 μm to 90 μm.
[0102] Next, the fine powder is filled into a graphite mold and spark plasma sintered at a temperature of 1400-1600°C and a pressure of 25-50 MPa to obtain a sintered material with a diameter of 8 mm or more. Thereafter, the surface is ground to obtain a seed material and a raw material rod.
[0103] 2. Crystal production process
[0104] A single crystal is grown or solidified in one direction using a focused heating floating zone (FZ) culture device equipped with a xenon lamp. Specifically, the raw material rod and the seed material are fixed to the upper and lower axes of the FZ culture device via a fixture. Then, high-purity argon gas is introduced into the FZ culture device at a flow rate of 5L / min. After that, the seed material and its surrounding parts are melted by focused heating to form an initial melting zone, and then the single crystal is grown or solidified in one direction at a culture speed of 10mm / hr to obtain a crystal. In addition, the rotation speed of the upper and lower axes is 20ppm.
[0105] Figure 1 The appearance of the obtained crystal (cathode member) is shown in FIG. Figure 1 In the figure, the left direction of the photo indicates the growth direction of the crystal. The maximum equivalent circle diameter of the cross section of the crystal obtained in this embodiment, which is perpendicular to the long axis direction corresponding to the growth direction of the crystal, is 8 mm. This size is much larger than the diameter of the crystal of 4 mm shown in non-patent document 6. This is a size that can be tolerated in practical applications such as electron beam welding machines that require high current density, and specifically, it is a size that can be used as a cathode member without heat resistance problems.
[0106] Next, the structure observation, EBSD (Electron Back Scatter Diffraction Pattern) analysis, and powder X-ray diffraction (XRD) analysis of the obtained crystal (cathode member) were performed as follows.
[0107] 4. Observation of the structure of cathode components
[0108] Observation was performed using a scanning electron microscope (SEM). The reason for the observation using SEM is that in powder X-ray diffraction (XRD) analysis, if the heterophase or impurity phase is minute compared to the main phase (main crystalline phase), these cannot be detected. In the above observation, a scanning electron microscope (SEM) was used to photograph the three central fields of view of the cathode component at a magnification of 100 times and 10,000 times. The SEM observation photographs at a magnification of 100 times and 10,000 times are shown in FIG. Figure 2 , Figure 3 In this embodiment, Figure 3 EDX analysis of the symbol A and symbol B at each position. The results are shown in Figure 4 In (a) and (b).
[0109] according to Figure 4 As a result, Ir and Ce were detected at both position A (white part) and position B (gray part), and there was no difference in the analysis results between the two. Figure 3 , but these are not grain boundaries. Figures 2 to 4 As a result, in the cathode member according to the embodiment of the present invention, no non-uniformity in component composition was observed.
[0110] In this embodiment, according to the above SEM observation photos and the above Figure 4 In the EDX analysis results, no secondary components such as oxides with an equivalent circle diameter of 50 μm or less and pure Ir phase were observed, but the single phase of Ir2Ce occupied the surface. In other words, in this embodiment, the single phase of Ir2Ce occupied more than 95% by area.
[0111] 5. EBSD analysis
[0112] In order to confirm whether the crystal orientation of the cathode component is consistent, EBSD (Electron Back Scatter Diffraction pattern) analysis is performed. In the SEM-EBSD method, the sample placed in the barrel of the FE-SEM is irradiated with an electron beam, and the diffraction pattern of the electron backscatter is input into the EBSD device. The crystal orientation analysis is performed while scanning the sample surface at equal intervals. In this way, the EBSP of each point is obtained and its index is calibrated to obtain the crystal orientation of the electron beam irradiated portion. The measuring surface is set to ND (Normal Direction), the pull-up direction is set to RD (Reference Direction), and the normal direction is set to TD (Transverse Direction). In this embodiment, Figure 5 The portion surrounded by the dotted line in the microscope photograph shown (approximately 150 μm×approximately 150 μm) was measured with a distance (step length) of 0.5 μm between crystal orientation measurement points, and then crystal orientation analysis was performed using version 5 of OIM manufactured by TSL as orientation analysis software.
[0113] The results obtained from the above analysis are shown in Figure 6 (a) to (d). Figure 6 (a) is the IQ distribution diagram, Figure 6 (b) to (d) are diagrams showing the crystal orientation distributions of ND, RD, and TD, respectively. Figure 6 (b) to (d) are respectively indicated by light blue, pink, and green in the analysis. However, in the present embodiment, in the analysis results indicated by color or black and white, it is sufficient to determine whether it is a single color indicating a single crystal.
[0114] Due to this Figure 6 Each of the photos (b) to (d) is monochrome, in other words, the EBSD patterns are the same, so it can be confirmed that the cathode component is a single crystal. The uniform crystal orientation of the cathode component helps to generate high-quality electron beams, and further helps to exert excellent electron emission characteristics. In addition, Figure 6The black dots shown in (b) to (d) have no influence on the inverse pole figure orientation distribution (IPF) and IQ distribution, and are considered to have no correlation with the crystal orientation and subcomponents.
[0115] In addition, powder X-ray diffraction (XRD) analysis was performed on the central portion of the obtained cathode member to confirm whether the desired iridium-cerium alloy could be obtained. The results are shown in Figure 7 In. By Figure 7 It can be seen that a single phase of Ir2Ce can be obtained.
[0116] For reference, in this embodiment, the FZ method is a high-frequency method, but other methods can also be used to obtain crystals in the same way as the above method. In the high-frequency method, a high-frequency oscillator is used to generate high frequencies in the induction heating coil to heat the raw material rod and melt it to produce crystals. The SEM observation results (magnification 500 times) are shown in Figure 8 In. Also in Figure 8 In the figure, the black dots and black lines have nothing to do with the original material. Figure 8 In the experiment, the grains were extended to form a columnar structure, and it was confirmed that a unidirectionally solidified material could be obtained.
[0117] When an Ir2Ce single crystal is produced using a four-arc furnace as shown in non-patent document 6 and its cross section is confirmed using a scanning electron microscope, large voids can be confirmed. In contrast, the crystal obtained in this embodiment has no voids, as shown in the above-mentioned SEM observation photograph.
[0118] As shown above, in this embodiment, the secondary components are fully suppressed, and the crystal is homogenized, and in particular, a single-phase, single-crystal or unidirectionally solidified crystal can be obtained. In such a crystal, impurities that hinder the electron emission characteristics of the cathode component, the unevenness of the component composition, and the diversity of the crystal are suppressed, so if used for a cathode component for electron beam generation, it is possible to achieve a cathode component for electron beam generation with excellent electron emission characteristics.
[0119] This application claims priority based on Japanese Patent Application No. 2019-159587 filed on September 2, 2019. Japanese Patent Application No. 2019-159587 is incorporated herein by reference.
[0120] Industrial Applicability
[0121] The cathode member for electron beam generation of the present invention can be used as a core part of an electron beam generator such as a general-purpose analysis device, and can also be used for plasma jet acceleration in electron beam melting devices, accelerators, artificial satellites, and the like.
Claims
1. A cathode member for generating an electron beam, in, The single phase containing the compound of iridium and cerium occupies more than 95% by area, The total content of metallic iridium and one or more accessory components in the oxide of one or more elements selected from iridium and cerium is 5 area % or less, The compound comprising iridium and cerium is Ir 2 Ce、Ir 3 Ce、Ir 7 Ce 2 or Ir 5 Ce compounds, The crystal structure of the single phase is a single crystal, Wherein, the compound containing iridium and cerium is prepared by a floating zone method, The maximum equivalent circle diameter of the cross section perpendicular to the long axis direction which is the same as the growth direction of the crystal by the floating zone method is 5 mm or more.
2. The cathode member for electron beam generation according to claim 1, in, The size of the subcomponent is 50 μm or less in terms of circle equivalent diameter.
3. The cathode member for electron beam generation according to claim 1, in, The compound comprising iridium and cerium comprises Ir 2 Ce、Ir 3 Ce、Ir 7 Ce 2 or Ir 5 The single phase of Ce does not contain metal iridium and oxides of one or more elements among iridium and cerium.
4. A method for manufacturing a cathode member for electron beam generation, which is the method for manufacturing a cathode member for electron beam generation according to claim 1 or 2, in, Including the following processes: A melting step of melting a metallic cerium raw material and a metallic iridium raw material to obtain a smelted material; A pulverizing step of pulverizing the smelted material to obtain a pulverized product; A sintering step of sintering the crushed product of the molten material at a temperature of 1400 to 1600° C. and a pressure of 25 to 50 MPa to obtain a sintered material for crystal production; A crystal production process is to produce a crystal containing a compound of iridium and cerium by a floating zone method using the sintered material for crystal production.
Citation Information
Patent Citations
Fluid flow inlet
EP1062017A1
Metal cathode and heat radiating cathode structural body having the same
JP2002260520A
Cathode material for electron beam device and manufacturing method thereof
JP2002527855A
Cathode member for electron beam generation and method for manufacturing the same