Preparation of Growth Catalysts for High Specific Surface Area Carbon Nanotubes
Preparation through co-precipitation reaction of Fe-Co-Mo-Al four-way catalyst solves the problem of quality reduction caused by increasing the number of walls of multi-walled carbon nanotubes, and realizes the production of carbon nanotubes with high specific surface area for use in conductive additives and batteries Conductive agent improves battery performance.
Patent Information
- Application Number
- CN202111554506.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-12-17
AI Technical Summary
During the synthesis process of multi-walled carbon nanotubes, as the number of walls increases, the proportion of disordered graphite increases, resulting in a decrease in quality. It is difficult to effectively increase the specific surface area of carbon nanotubes with existing technology.
The Fe-Co-Mo-Al quaternary carbon nanotube growth catalyst is prepared through the co-precipitation reaction of the metal precursor solution and the precipitant to form carbon nanotubes with a high specific surface area. It does not require high-temperature pretreatment and can be directly used in the chemical vapor phase. deposition.
It achieves the high-yield production of carbon nanotubes with a specific surface area greater than 350m2/g at a lower temperature and in a short time. It has excellent catalytic growth effect and is suitable for polymer conductive additives and lithium-ion battery cathode conductive agents.
Smart Images

Figure CN114308049B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of carbon nanotubes, and in particular to a growth catalyst for preparing carbon nanotubes with high specific surface area. Background Art
[0002] Carbon nanotubes (CNTs) are one-dimensional nanocarbon materials with a hollow tubular structure, composed of carbon atoms arranged in a hexagonal lattice, with a diameter of about 1 to 100 nm and a high aspect ratio. In theory, carbon nanotubes have super tensile strength, excellent thermal conductivity, excellent electrical conductivity and chemical stability. Due to its outstanding physical and chemical properties, CNTs have shown application potential in composite materials, new energy, aerospace, biotechnology, electronics and semiconductors, and have been widely and deeply studied. After years of development, CNTs have been commercially applied in conductive plastics and conductive additives for batteries.
[0003] The main methods for synthesizing CNTs are arc discharge, laser evaporation and chemical vapor deposition. Arc discharge and laser evaporation are not suitable for mass production of CNTs due to cost and equipment limitations. In contrast, chemical vapor deposition has become the main process for large-tonnage carbon nanotube production. The details of chemical vapor deposition are as follows: small organic molecules (such as ethylene, propylene, ethanol, etc.) are catalyzed by transition metal catalysts under high temperature conditions to decompose and deposit solid carbon nanotubes and hydrogen.
[0004] According to the number of tube walls, CNTs can be divided into three types: single-walled CNTs with a diameter of about 1nm; double-walled CNTs with a diameter of about 1.4 to 3nm; and multi-walled CNTs with a diameter of about 5 to 100nm. In the process of synthesizing multi-walled CNTs, the current problem is that as the number of walls of multi-walled carbon nanotubes increases, the proportion of disordered graphite also increases, resulting in a decrease in the quality of multi-walled carbon nanotubes. For this reason, the industry has been working hard to reduce the number of walls of multi-walled CNTs and increase their specific surface area. From the perspective of the preparation process of chemical vapor deposition, transition metal catalysts have an important influence on the growth and structural regulation of CNTs. Therefore, it is necessary to provide a growth catalyst that can increase the specific surface area of carbon nanotubes. Summary of the invention
[0005] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes a growth catalyst capable of increasing the specific surface area of carbon nanotubes.
[0006] In a first aspect of the present application, a carbon nanotube growth catalyst is provided, wherein Fe x Co y Mo z Al indicates that 0.3≤(x+y)≤0.6, 5≤(x+y) / z≤20, and x≤y.
[0007] The carbon nanotube growth catalyst according to the embodiment of the present application has at least the following beneficial effects:
[0008] The Fe-Co-Mo-Al quaternary carbon nanotube growth catalyst provided in the embodiment of the present invention comprises multiple components of iron, cobalt, molybdenum and aluminum. The catalyst can be used directly without high-temperature pretreatment. When the catalyst is used for chemical vapor deposition, a carbon nanotube with a specific surface area of more than 350m can be produced at a high rate. 2 / g of carbon nanotubes, with excellent catalytic growth effect, and has great application prospects in the preparation of carbon nanotubes.
[0009] In a second aspect of the present application, a method for preparing a carbon nanotube growth catalyst is provided, the preparation method comprising the following steps:
[0010] Providing a metal precursor solution, the metal precursor solution comprising an iron source, a cobalt source, a molybdenum source and an aluminum source in a stoichiometric ratio, wherein the stoichiometric ratio is as follows: taking the molar amount of aluminum as 1, the molar amount of iron as x, the molar amount of cobalt as y, the molar amount of molybdenum as z, 0.3≤(x+y)≤0.6, 5≤(x+y) / z≤20, and x≤y;
[0011] The metal precursor solution and the precipitant are mixed and reacted, and the precipitate is collected to obtain a carbon nanotube growth catalyst.
[0012] The metal precursor solution refers to a raw material solution including the metal elements required for the carbon nanotube growth catalyst, including Fe x Co y Mo z The precursor solution is mixed with a precipitant to produce a coprecipitation reaction, wherein the metal elements are hydrolyzed to form a precipitate, thereby obtaining a carbon nanotube growth catalyst. The precipitant refers to a precipitant that can be optionally coprecipitated with the above-mentioned metal precursor solution, including but not limited to at least one of ammonia water, ammonium carbonate, ammonium bicarbonate, urea, ammonium fluoride, etc.
[0013] It can be seen that the preparation method of the carbon nanotube growth catalyst provided in the embodiment of the present application uses a multi-component containing iron, cobalt, molybdenum and aluminum as raw materials, and can be prepared without adding additional chelating agents and surfactants. The process is simpler and is conducive to large-scale production. The prepared growth catalyst can achieve high yield production of carbon nanotubes with a large specific surface area.
[0014] It is understandable that the metal source and the precipitant undergo a precipitation reaction, and hydroxide is directly formed. Considering the chemical vapor deposition process of carbon nanotube preparation, the five-element metal hydroxide can actually be calcined and reduced under high temperature conditions of vapor deposition to form a mixture or alloy of five-element metal elements to participate in the catalytic reaction. Therefore, the calcination and reduction steps can be omitted or retained in the preparation process of the catalyst. If the calcination and reduction steps need to be retained, the calcination can be carried out at 400-800°C, and further calcined at 400-700°C, 500-700°C, and 600-700°C.
[0015] In some embodiments of the present application, 0.3≤(x+y)≤0.5, or 0.375≤(x+y)≤0.6, or 0.375≤(x+y)≤0.5.
[0016] In some embodiments of the present application, 5≤(x+y) / z≤15, or 8≤(x+y) / z≤12, or (x+y) / z is approximately 10.
[0017] It will be appreciated that the above requirements for the stoichiometric ratio of x and y, and the stoichiometric ratio of x, y and z may be arbitrarily combined therein.
[0018] In some embodiments of the present application, the iron source, the cobalt source and the aluminum source are independently selected from nitrates, sulfates, chlorides and acetates.
[0019] In some embodiments of the present application, the molybdenum source is a molybdate, including but not limited to at least one of ammonium molybdate and ammonium heptamolybdate.
[0020] In some embodiments of the present application, the precipitant is selected from at least one of ammonium carbonate, ammonium bicarbonate and ammonia water.
[0021] In some embodiments of the present application, the concentration of the precipitant is 1 to 4 mol / Kg.
[0022] In some embodiments of the present application, the reaction temperature after adding the precipitant is 20-100°C, preferably, the reaction temperature is 20-80°C, 30-60°C.
[0023] In some embodiments of the present application, the method for collecting the precipitate is to filter the precipitate and then dry it at a temperature of 80 to 200°C.
[0024] In a third aspect of the present application, a method for preparing carbon nanotubes is provided, the method comprising the following steps:
[0025] In a protective atmosphere, a carbon source is chemically vapor deposited under the action of a metal catalyst to obtain carbon nanotubes. The metal catalyst is the aforementioned carbon nanotube growth catalyst, or the carbon nanotube growth catalyst prepared by the aforementioned preparation method.
[0026] In some embodiments of the present application, the carbon source is an optional carbon source substance participating in the reaction in the form of a reaction gas, including but not limited to hydrocarbons in the gas phase at room temperature, such as at least one of methane, ethane, ethylene, propane, propylene, acetylene, etc. In some preferred embodiments, the carbon source is selected from ethylene or propylene. It is understood that other commonly used carbon sources such as ethanol, acetone, dimethyl ether, etc. can also be used as the carbon source required in the preparation process.
[0027] In some embodiments of the present application, the reaction temperature of chemical vapor deposition is 600-700° C., more preferably 630-650° C.; the reaction time of chemical vapor deposition is 10-30 minutes, more preferably 15-20 minutes.
[0028] In some embodiments of the present application, the protective atmosphere refers to the use of inert gas or nitrogen or the like for protection to isolate air, oxygen, etc. to avoid affecting the growth of carbon nanotubes.
[0029] In a fourth aspect of the present application, a carbon nanotube is provided, wherein the carbon nanotube is prepared by the above-mentioned preparation method. The carbon nanotube prepared by the above-mentioned method has a diameter of at least 350 m 2 / g BET specific surface area, the aggregation morphology of carbon nanotubes under microscope is entangled. Based on the high specific surface area of the carbon nanotubes, its performance in all aspects is also more excellent.
[0030] The fifth aspect of the present application provides a composition, which includes the aforementioned carbon nanotubes. The composition is formed by using the carbon nanotubes as a main raw material or additive component, including but not limited to conductive paste, additives, lubricants, etc.
[0031] The present application is directed to a four-component carbon nanotube growth catalyst and a catalyst having a specific surface area greater than 350 m 2 / g of entangled carbon nanotubes. By optimizing the ratio of the components of the Fe-Co-Mo-Al catalyst, as well as the growth time and temperature of the carbon nanotubes, the carbon nanotubes with large specific surface area can be prepared with a high yield and used as polymer conductive additives and positive electrode conductive agents for lithium-ion batteries.
[0032] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a scanning electron microscope image of the carbon nanotubes grown at 620° C. for 10 minutes in Example 1 of the present invention.
[0034] Figure 2This is a scanning electron microscope image of carbon nanotubes grown at 640° C. for 10 minutes in Example 2 of the present invention.
[0035] Figure 3 This is a transmission electron microscope image of carbon nanotubes grown at 640° C. for 10 minutes in Example 2 of the present invention. DETAILED DESCRIPTION
[0036] The following will clearly and completely describe the concept of the present application and the technical effects produced in combination with the embodiments, so as to fully understand the purpose, features and effects of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of them. Based on the embodiments of the present application, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present application.
[0037] The embodiments of the present application are described in detail below. The described embodiments are exemplary and are only used to explain the present application, and should not be understood as limiting the present application.
[0038] In the description of this application, the meaning of "several" is more than one, the meaning of "many" is more than two, the meaning of "greater than", "less than", "exceed" etc. is understood as not including the number itself, and the meaning of "above", "below", "within" etc. is understood as including the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing the technical features, and cannot be understood as indicating or implying the relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features. The meaning of "approximately" can be understood as fluctuating within the range of ±20%, ±15%, ±10%, ±8%, ±5%, ±3%, ±2%, ±1%, ±0.5%, ±0.2%, ±0.1% of the point value.
[0039] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0040] Example 1
[0041] This embodiment provides a Fe-Co-Mo-Al quaternary carbon nanotube growth catalyst, and the preparation method thereof is as follows:
[0042] (1) Dissolve Fe(NO3)3·9H2O, Co(NO3)2·6H2O and Al(NO3)3·9H2O in deionized water to prepare a 1 mol / kg solution. 24 ·4H2O is dissolved in deionized water to make a 0.1 mol / Kg solution for later use. Take (NH4)2CO3 and dissolve it in deionized water to make a 2 mol / Kg solution for later use.
[0043] (2) According to the stoichiometric ratio of the element molar ratio of Fe:Co:Mo:Al=0.25:0.25:0.05:1, 20 g, 20 g, 40 g and 80 g of Fe, Co, Mo and Al precursor solutions were respectively measured and mixed to obtain a metal precursor solution.
[0044] (3) Add 200 mL of deionized water and 150 g of the prepared (NH4)2CO3 solution to a 2 L three-necked flask, stir, heat to 45 ° C, and slowly drip the metal precursor solution. Continue stirring for half an hour after the addition is completed, and the final pH is 8-8.5 measured with pH test paper. Filter the precipitate, do not need to wash with deionized water, put it in a 120 ° C drying oven for 24 hours, and grind the dried product into fine powder to obtain Fe-Co-Mo-Al quaternary carbon nanotube growth catalyst.
[0045] This embodiment also provides a carbon nanotube, and the preparation method of the carbon nanotube is as follows:
[0046] The carbon nanotube growth experiment was carried out in a horizontal fixed-bed quartz reactor. The carbon nanotube growth catalyst prepared in this example was taken and evenly placed in a quartz boat, and then the quartz boat was pushed into the constant temperature zone of the tube furnace. The temperature was raised to the reaction temperature under a nitrogen atmosphere, and then ethylene was introduced as a carbon source. After a period of reaction, the introduction of ethylene was stopped, and the temperature was lowered to room temperature under a nitrogen atmosphere, the carbon nanotubes were taken out, the weight was weighed, the ratio was calculated, and the specific surface area was measured by the BET method.
[0047] According to the above preparation method, different reaction temperatures and reaction times are used, and the test results of the carbon nanotubes finally prepared are shown in Table 1:
[0048] Table 1. Carbon nanotube production rate and specific surface area results under different experimental conditions in Example 1
[0049] Experiment No. Reaction temperature / ℃ Reaction time / min Production rate <![CDATA[Specific surface area / (m 2 / g)]]> 1 600 10 14 344 2 610 10 16 352 3 620 10 19 362 4 620 15 24 351 5 630 10 22 356 6 640 10 25 355 7 660 10 35 345
[0050] Wherein, production rate = (total weight of CNT after reaction - weight of catalyst before reaction) / weight of catalyst before reaction;
[0051] The specific surface area of CNT is measured by the BET method. A larger BET specific surface area indicates that the CNT has a smaller diameter. When used as a conductive additive, CNT with a large specific surface area is added in a smaller amount.
[0052] refer to Figure 1 , is an electron microscope image of the carbon nanotubes grown at a reaction temperature of 620° C. for 10 minutes in the above table. It can be seen from the image that the carbon nanotubes prepared in the embodiment of the present application have an obvious "entangled" secondary aggregation morphology.
[0053] Referring to the test results in Table 1, within the reaction temperature range of 610-640°C, a specific surface area greater than 350 m 2 / g of CNT. On the other hand, by comparing its growth rate, it can be found that with the increase of temperature, the growth rate of CNT gradually increases; at the same time, after 10 minutes of reaction time, the carbon nanotube can reach a growth rate of 25.
[0054] The specific surface area of CNT is directly related to the number of walls and diameter. The fewer walls, the larger the specific surface area. The number of walls and diameter are related to the particle size of the catalyst active component particles. The smaller the particle size, the fewer CNT walls, the smaller the diameter, and the larger the specific surface area. The initial particle size of the catalyst active component particles is determined by the catalyst preparation method, but in the process of preparing CNT by chemical vapor deposition, its particle size will gradually grow as the reaction proceeds at a higher reaction temperature, resulting in an increase in the number of CNT walls and a larger diameter until the catalyst is deactivated; lowering the reaction temperature can slow down the growth of catalyst particles, but the contradiction is that lowering the reaction temperature will cause the CNT growth rate to slow down and reduce production efficiency. The catalyst prepared in this embodiment can achieve a growth rate of about 25 at a lower temperature and in a shorter time, while maintaining a high specific surface area of CNT.
[0055] Example 2
[0056] This embodiment provides a Fe—Co—Mo—Al quaternary carbon nanotube growth catalyst. The catalyst preparation method is the same as that in Embodiment 1, and the element molar ratio is Fe:Co:Mo:Al=0.125:0.25:0.0375:1.
[0057] The experimental results of carbon nanotubes prepared by the preparation method in Example 1 using the above carbon nanotube growth catalyst at different reaction temperatures and reaction times are shown in Table 2:
[0058] Table 2. Carbon nanotube production rate and specific surface area results under different experimental conditions in Example 2
[0059] Experiment No. Reaction temperature / ℃ Reaction time / min Production rate <![CDATA[Specific surface area / (m 2 / g)]]> 1 620 10 8.5 368 2 630 10 11 368 3 640 10 12 374 4 650 10 13 374 5 660 10 17 369 6 700 10 23 347
[0060] refer to Figure 2 and Figure 3 , respectively, are the scanning electron microscope and transmission electron microscope images of carbon nanotubes grown at 640℃ for 10 minutes. Figure 2 It can be seen that the carbon nanotubes prepared in this embodiment are also "entangled" carbon nanotubes. Figure 3 The diameter of the carbon nanotubes prepared in Example 2 of the present application is 10 to 20 nm, and the multi-layer structure can be clearly seen. It is a typical multi-walled carbon nanotube with more than 8 walls.
[0061] Combining the test results of Table 2 and Table 1, compared with Example 1, after increasing the proportion of Co element, the production rate decreased, but the specific surface area of the obtained CNT reached 370m 2 / g or so.
[0062] Comparative Example 1
[0063] This comparative example provides a Fe—Co—Mo—Al quaternary carbon nanotube growth catalyst, which is different from Example 1 in that the molar ratio of elements is Fe:Co:Mo:Al=0.25:0.125:0.0375:1.
[0064] The experimental results of carbon nanotubes prepared by the preparation method in Example 1 using the above carbon nanotube growth catalyst at different reaction temperatures and reaction times are shown in Table 3:
[0065] Table 3. Carbon nanotube production rate and specific surface area results under different experimental conditions in Comparative Example 1
[0066]
[0067]
[0068] Compared with Example 2, the molar ratio of Fe and Co in Comparative Example 1 was changed so that the ratio of Fe was greater than that of Co. The specific surface area of the CNTs finally prepared was lower, decreasing by 50-70 m 2 / g.
[0069] Comparative Example 2
[0070] This comparative example provides a Fe—Co—Mn—Mo—Al five-component carbon nanotube growth catalyst, which differs from Example 1 in that the molar ratio of elements is Fe:Co:Mn:Mo:Al=0.3:0.3:0.09:0.06:1.
[0071] The experimental results of carbon nanotubes prepared by the preparation method in Example 1 using the above carbon nanotube growth catalyst at different reaction temperatures and reaction times are shown in Table 4:
[0072] Table 4. Carbon nanotube production rate and specific surface area results under different experimental conditions in Comparative Example 2
[0073] Experiment No. Reaction temperature / ℃ Reaction time / min Production rate <![CDATA[Specific surface area / (m 2 / g)]]> 1 620 10 13 303 2 640 10 20 300 3 660 10 17 279
[0074] Compared with Example 1, Comparative Example 2 adds an additional Mn element, but the specific surface area of carbon nanotubes prepared by this catalyst under the same conditions is still only 300m 2 / g is even insufficient, and the decline is obvious.
[0075] Comparative Example 3
[0076] This comparative example provides a Fe—Co—Mo—Al quaternary carbon nanotube growth catalyst, which is different from Example 1 in that the molar ratio of elements is Fe:Co:Mo:Al=0.125:0.125:0.025:1.
[0077] The experimental results of carbon nanotubes prepared by the preparation method in Example 1 using the above carbon nanotube growth catalyst at different reaction temperatures and reaction times are shown in Table 5:
[0078] Table 5. Carbon nanotube production rate and specific surface area results under different experimental conditions in Comparative Example 3
[0079] Experiment No. Reaction temperature / ℃ Reaction time / min Production rate <![CDATA[Specific surface area / (m 2 / g)]]> 1 620 10 3.2 300 2 640 10 4 318 3 660 10 5.4 316 4 680 10 4.9 290
[0080] Compared with Example 1, the content of Fe and Co in the catalyst of this comparative example is greatly reduced, and the CNT finally obtained is still only 300m 2 / g, which cannot meet the quality requirements for high-quality multi-walled carbon nanotubes.
[0081] Based on the test results of the above examples and comparative examples, it can be seen that the carbon nanotube growth catalyst disclosed in the examples of the present application is composed of Fe x Co y Mo z The catalyst can be prepared by coprecipitation reaction of metal precursor solution and alkaline solution. When the ratio of each element satisfies the conditions of 0.3≤(x+y)≤0.6, 5≤(x+y) / z≤20, and x≤y, the specific surface area of carbon nanotubes prepared by chemical vapor deposition using the catalyst prepared by the above catalyst preparation method can reach 350m 2 / g or more, the carbon nanotubes belong to entangled carbon nanotubes. Such high specific surface area carbon nanotubes can be used as polymer conductive additives and positive electrode conductive agents for lithium ion batteries, thereby improving battery performance.
[0082] The present application is described in detail above in conjunction with the embodiments, but the present application is not limited to the above embodiments, and various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present application. In addition, the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
Claims
1. A method for preparing a carbon nanotube growth catalyst, characterized in that: Here are the steps: Providing a metal precursor solution, wherein the metal precursor solution is composed of an iron source, a cobalt source, a molybdenum source and an aluminum source in a stoichiometric ratio, wherein the stoichiometric ratio is as follows: taking the molar amount of aluminum as 1, the molar amount of iron as x, the molar amount of cobalt as y, the molar amount of molybdenum as z, 0.3≤(x+y)≤0.6, 5≤(x+y) / z≤20, and x≤y; Mixing the metal precursor solution with a precipitant to react, collecting the precipitate, and obtaining the carbon nanotube growth catalyst; The reaction temperature after adding the precipitant is 20 to 100°C; The method for collecting the precipitate is to filter the precipitate and then dry it at a temperature of 80 to 200°C.
2. The preparation method according to claim 1, characterized in that: The precipitant is selected from at least one of ammonium carbonate, ammonium bicarbonate and ammonia water.
3. The preparation method according to claim 1, characterized in that: The iron source, cobalt source and aluminum source are independently selected from nitrates, sulfates, chlorides and acetates.
4. The preparation method according to claim 1, characterized in that: The molybdenum source is molybdate.
5. A carbon nanotube growth catalyst, characterized in that: Fe x Co y Mo z Al represents, 0.3≤(x+y)≤0.6, 5≤(x+y) / z≤20, and x≤y; prepared by the preparation method according to any one of claims 1 to 4.
6. A method for preparing carbon nanotubes, characterized in that: The following steps are involved: Under a protective atmosphere, a carbon source is subjected to chemical vapor deposition under the action of a metal catalyst to obtain the carbon nanotubes. The metal catalyst is the carbon nanotube growth catalyst according to claim 5, or the carbon nanotube growth catalyst obtained by the preparation method according to any one of claims 1 to 4.