Method for producing resin composition

Nanoparticles are uniformly dispersed in the resin material through stirring mixing and high-speed centrifugation technology, which solves the problem of poor dispersion of nanoparticles in the resin material and improves the performance and stability of the composite material.

CN114316518BActive Publication Date: 2024-10-18TAIWAN SOKOU INDS KOFUN YUUGENKOUSHI
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202210009146.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-06
Publication Date
2024-10-18
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

It is difficult to uniformly disperse nanoparticles in resin materials with existing technology, leading to degradation of material properties and brittle fracture. In addition, residual solvents in traditional methods lead to hole defects and reduce material performance.

Method used

By mixing nanoparticles, micron inorganic particles and resin, combined with high-speed centrifugation technology, a uniformly dispersed resin composition is formed, which reduces the agglomeration of nanoparticles and improves dispersibility.

Benefits of technology

It achieves uniform dispersion of nanoparticles, reduces stress concentration defects, improves the mechanical and electrical properties of composite materials, and enhances the strength and stability of the resin composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114316518B_ABST
    Figure CN114316518B_ABST
Patent Text Reader

Abstract

A method for manufacturing a resin composition comprises the following operations: stirring and mixing nanoparticle fillers, micron inorganic particles and resin to form a mixture; centrifuging the mixture at high speed to form an upper mixed liquid and a lower mixed liquid; and taking out the upper mixed liquid to obtain a resin composition. This method can make the nanoparticle fillers uniformly dispersed in the resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing a resin composition. Background Art

[0002] High-performance resin compositions are widely used in adhesives, electronic instruments, aerospace, coatings, electronic and electrical insulation materials, and advanced composite materials. After curing, high-performance resin compositions form a three-dimensional network structure with a high cross-linking density, which can significantly improve the strength, rigidity, modulus, hardness, and heat resistance of the resin material. However, the material will also be inherently brittle due to the high cross-linking density, and it is easy to cause brittle fracture under the action of hard force during use, thereby limiting its application. One of the toughening methods is to introduce nanoparticles with special modified functionalization on the surface to achieve toughening.

[0003] However, since nanoparticles have the characteristic of high surface energy and are very easy to agglomerate, it is difficult to evenly disperse the nanometer size of the nanoparticles themselves in the resin composition, and it is impossible to give play to its nanoparticle characteristics. The dispersibility of nanoparticles inside the resin material has a great relationship with the properties of the enhancement, and the better the dispersibility of nanoparticles, the better the effect of the enhancement. If the nanoparticles have poor dispersibility, not only there is no enhancement effect, but the properties may be decreased on the contrary, such as the agglomeration defects formed by the poor dispersion of nanoparticles inside the resin material, resulting in stress concentration areas and strength reduction.

[0004] Many of the current methods for dispersing nanoparticles use solvents to dissolve the resin composition, and then use ultrasonic dispersers to disperse it, and then remove the solvent. However, the final resin composition will have residual solvent, causing the formation of voids in high-performance composite materials and reducing performance. Using only a high-speed mixer to stir the nanoparticles cannot fully disperse the nanoparticles, and the problem of nanoparticle agglomeration in the resin formula still exists. Summary of the invention

[0005] According to various embodiments of the present invention, a method for manufacturing a resin composition is provided, comprising stirring and mixing nanoparticle filler, micron inorganic particles and resin to form a mixture; centrifuging the mixture at high speed to form an upper mixed liquid and a lower mixed liquid; and taking out the upper mixed liquid to obtain a resin composition.

[0006] According to some embodiments of the present invention, the nanoparticle filler includes nano-silicon dioxide, nano-silver, nano-calcium carbonate, nano-kaolin, nano-titanium dioxide, nano-carbon fiber or a combination thereof.

[0007] According to certain embodiments of the present invention, the nanoparticle filler has a particle size of about 5 nm to 250 nm.

[0008] According to certain embodiments of the present invention, the nanoparticle filler has a weight percentage of about 0.1-10%.

[0009] According to some embodiments of the present invention, the micron inorganic particles include zirconium dioxide, titanium dioxide, micron glass beads or a combination thereof.

[0010] According to some embodiments of the present invention, the micron inorganic particles have a particle size of about 2 μm-200 μm.

[0011] According to certain embodiments of the present invention, the micron inorganic particles have a weight percentage of about 0.1-30%.

[0012] According to some embodiments of the present invention, the resin includes phenolic resin, urea formaldehyde resin, melamine resin, epoxy resin, vinyl ester, unsaturated polyester, polyurethane resin, silicone resin, acrylic acid ester or a combination thereof.

[0013] According to some embodiments of the present invention, the stirring and mixing comprises stirring at a temperature of about 20-160° C. and a stirring speed of about 100-5000 rpm for about 0.5-15 hours.

[0014] According to some embodiments of the present invention, the stirring and mixing comprises stirring and evacuating at a vacuum degree of about 0.01-100 Torr and a stirring speed of 50-5000 rpm for about 0.1-2 hours.

[0015] According to some embodiments of the present invention, high-speed centrifugation of the mixture comprises centrifuging at a speed of about 5000-150000 rpm for about 0.1-5 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Aspects of the present disclosure will be fully understood from the following detailed description when read with the accompanying drawings.

[0017] Figure 1 The present invention is a flowchart of a method for manufacturing a resin composition according to some embodiments of the present invention. DETAILED DESCRIPTION

[0018] The following will disclose multiple embodiments of the present invention with the accompanying drawings. For the purpose of clear description, many practical details will be described together in the following description. However, it should be understood that these practical details should not be used to limit the present invention.

[0019] Although a series of operations or steps are used below to illustrate the method disclosed herein, the order shown in these operations or steps should not be construed as a limitation of the present invention. For example, certain operations or steps can be performed in different orders and / or simultaneously with other steps. In addition, it is not necessary to perform all the operations, steps and / or features illustrated to implement the embodiments of the present invention. In addition, each operation or step described herein may include several sub-steps or actions.

[0020] Figure 1 1 is a flow chart of a method for manufacturing a resin composition according to various embodiments of the present invention. Figure 1 As shown, method 100 includes operation 110 , operation 120 , and operation 130 .

[0021] Please refer to Figure 1 In operation 110 of method 100, the nanoparticle filler, the micron inorganic particles and the resin are stirred and mixed to form a mixture. In some embodiments, the stirring and mixing of the nanoparticle filler, the micron inorganic particles and the resin comprises adding the nanoparticle filler, the micron inorganic particles and the resin into a high-speed mixer. For example, the high-speed mixer can be a planetary mixer.

[0022] In some embodiments, the nanoparticle filler includes nano silicon dioxide, nano silver, nano calcium carbonate, nano kaolin, nano titanium dioxide, nano carbon fiber or a combination thereof. In some embodiments, the nanoparticle filler has a particle size of about 5nm-250nm. The nanoparticle filler with a particle size within this range can effectively enhance the performance of the resin composition, such as mechanical properties, heat resistance, etc. For example, the particle size of the nanoparticle filler can be about 10, 20, 30, 50, 70, 100, 115, 135, 155, 175, 195, 200, 210, 220, 230, 240 or 245nm. In some embodiments, the nanoparticle filler has a weight percentage of about 0.1-10%. For example, the weight percentage of the nanoparticle filler can be about 1, 3, 5, 7 or 9%. Adding the nanoparticle filler of this weight percentage range can enhance the mechanical, electrical and other properties of the resin composition.

[0023] In some embodiments, the micron inorganic particles include zirconium dioxide, titanium dioxide, micron glass beads or a combination thereof. The micron inorganic particles can be used as a medium to further disperse the nanoparticle filler in the resin by the shear force and impact force of the rotation and collision generated by the mechanical external force. In some embodiments, the micron inorganic particles have a particle size of about 2μm-200μm. For example, the particle size of the micron inorganic particles can be about 3, 5, 7, 10, 30, 50, 70, 90, 110, 130, 150, 170, or 190μm. In detail, the micron inorganic particles with too large particle size cannot effectively collide and shear to disperse the nanoparticle filler, and the too small micron inorganic particles are less likely to be separated from the mixture (including resin, nanoparticle filler) in the subsequent process. In some embodiments, the micron inorganic particles have a weight percentage of about 0.1-30%. For example, the weight percentage of the micron inorganic particles can be about 0.5, 1, 5, 10, 15, 20, or 25%. Using too many micron inorganic particles will make it difficult to remove the upper mixed solution after the subsequent centrifugation operation, while using too few micron inorganic particles will not generate sufficient collision and shear force, resulting in reduced effect and longer time when dispersing the nanoparticles.

[0024] In some embodiments, the resin may be a thermosetting resin. In some embodiments, the resin includes phenol formaldehyde resin (PF), urea-formaldehyde resin (UF), melamine resin, epoxy resin (EP), vinyl ester resin (VE), unsaturated polyester resin (UP), polyurethane resin (PU), silicone resin, acrylic resin or a combination thereof. In some embodiments, other additives such as curing agents, accelerators, etc. may also be added to the resin.

[0025] In some embodiments, after the nanoparticle filler, micron inorganic particles, and resin are added to the high-speed stirrer, they can be stirred and mixed for about 0.5-15 hours at a temperature of about 20-160° C. and a stirring speed of about 100-5000 rpm. For example, the stirring temperature can be about 25, 30, 50, 70, 90, 100, 120, or 140° C. In some embodiments, the nanoparticle filler, micron inorganic particles, and resin can be heated and stirred (for example, heated to 130° C.) to improve fluidity. In other embodiments, resins with good fluidity themselves, such as low molecular weight liquid epoxy resins, epoxy resin solvent solution formulations, aqueous modified polyurethane resin aqueous solution formulations, vinyl ester resins with reactive diluents, unsaturated polyester resins with reactive diluents, etc., still have obvious fluidity that can be observed by the naked eye after being mixed with nanoparticle fillers and micron inorganic particles, and do not need to be heated.

[0026] In some embodiments, after the above stirring and mixing, the mixture may be stirred and evacuated for about 0.1-2 hours at a vacuum degree of about 0.01-100 Torr and a stirring speed of 50-5000 rpm to form a mixture. In some embodiments, the temperature during the evacuation may be maintained at or lower than the temperature of the previous stirring and mixing (i.e., 20-160° C.).

[0027] Please continue to refer to Figure 1 In operation 120 of method 100, the mixture is centrifuged at high speed to form an upper mixed solution and a lower mixed solution. In some embodiments, the high-speed centrifugation of the mixture comprises centrifuging at a centrifugal speed of about 5000-150000 rpm for about 0.5-5 hours. Specifically, after the mixture formed in operation 110 is centrifuged at high speed, the micron inorganic particles can be centrifuged to the lower layer of the container, while the nanoparticle filler is in the upper layer of the container. That is, the lower mixed solution contains micron inorganic particles, and the upper mixed solution contains nanoparticle filler.

[0028] Please refer to Figure 1 , in operation 130 of method 100, the upper mixed liquid is taken out to obtain a resin composition. Through the stirring and dispersing method of the above operation, the nanoparticle filler can be fully and evenly dispersed in the resin. In other words, the resin composition contains uniformly dispersed nanoparticle fillers. This resin composition can be further formed into a composite material in a subsequent process (for example, curing). The composite material with nanoparticles uniformly dispersed therein can reduce the stress concentration defects caused by the presence of undispersed nanoparticle fillers and pores compounded inside the material. Therefore, the performance of the composite material, for example, electrical performance, mechanical performance, etc., can be enhanced.

[0029] The following examples are used to describe the specific aspects of the present invention in detail and enable those skilled in the art to implement the present invention. However, the following examples should not be used to limit the present invention.

[0030] Example 1

[0031] Add nano silicon dioxide particles with an average particle size of about 20 nm, micron zirconium dioxide particles with an average particle size of about 3 μm and liquid epoxy resin into a planetary mixer. Mix and homogenize at a revolution of 1200 rpm, a rotation of 1080 rpm, a temperature of 120° C., a vacuum degree of about 0.5 Torr, and a time of 1 hour to obtain a mixed mother solution of epoxy resin after particle dispersion. The weight percentage of nano silicon dioxide particles is 4%, and the weight percentage of micron zirconium dioxide particles is 10%.

[0032] The low viscosity epoxy resin mixed mother liquor was transferred into a centrifuge for high speed centrifugation at a speed of 80,000 rpm for 10 minutes to obtain a mixture of nano-silicon dioxide particles and epoxy resin uniformly dispersed in the upper layer and micron zirconium dioxide particles obtained by centrifugation in the lower layer.

[0033] The upper mixed liquid is taken out to obtain a resin composition in which nano-silicon dioxide particles and epoxy resin are evenly dispersed.

[0034] Example 2

[0035] Nano silver particles with an average particle size of about 75 nm, micron titanium dioxide particles with an average particle size of about 5 μm, and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of the nano silver particles is 3%, and the weight percentage of the micron titanium dioxide particles is 15%. The blending and homogenizing stirring time is about 1 hour, the stirring temperature is about 120° C., the vacuum degree is about 0.5 Torr, the revolution stirring speed is about 1500 rpm, and the rotation stirring speed is about 1350 rpm.

[0036] The low viscosity epoxy resin mixed mother liquor was transferred into a centrifuge for high speed centrifugation at a speed of 70,000 rpm for 10 minutes to obtain a mixed solution in which nano silver particles and epoxy resin were evenly dispersed on the upper layer and micronized titanium dioxide particles were centrifuged on the lower layer.

[0037] The upper mixed solution is taken out to obtain a resin composition in which nano silver particles and epoxy resin are evenly dispersed.

[0038] Example 3

[0039] Nano-silicon dioxide particles with an average particle size of about 20 nm, micron-zirconium dioxide particles with an average particle size of about 3 μm, and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of nano-silicon dioxide particles is 4%, and the weight percentage of micron-zirconium dioxide particles is 20%. The blending and homogenizing stirring time is 1 hour, the stirring temperature is 120° C., the vacuum degree is about 0.5 Torr, the revolution stirring speed is about 1200 rpm, and the rotation stirring speed is about 1080 rpm.

[0040] The low viscosity epoxy resin mixed mother liquor was transferred into a centrifuge for high speed centrifugation at a speed of 80,000 rpm for 10 minutes to obtain a mixture of nano-silicon dioxide particles and epoxy resin uniformly dispersed in the upper layer and micron zirconium dioxide particles obtained by centrifugation in the lower layer.

[0041] The upper mixed liquid is taken out to obtain a resin composition in which nano-silicon dioxide particles and epoxy resin are evenly dispersed.

[0042] Example 4

[0043] Nano silver particles with an average particle size of about 75 nm, micron titanium dioxide particles with an average particle size of about 5 μm and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a particle-dispersed epoxy resin mixed mother liquor, wherein the weight percentage of the nano silver particles is 3%, and the weight percentage of the micron titanium dioxide particles is 25%. The blending and homogenizing stirring time is 1 hour, the stirring temperature is 120° C., the vacuum degree is about 0.5 Torr, the revolution stirring speed is 1500 rpm, and the rotation stirring speed is 1350 rpm.

[0044] The low viscosity epoxy resin mixed mother liquor was transferred into a centrifuge for high speed centrifugation at a speed of 70,000 rpm for 10 minutes to obtain a mixed solution in which nano silver particles and epoxy resin were evenly dispersed on the upper layer and micronized titanium dioxide particles were centrifuged on the lower layer.

[0045] The upper mixed solution is taken out to obtain a resin composition in which nano silver particles and epoxy resin are evenly dispersed.

[0046] Example 5

[0047] Nano-silicon dioxide particles with an average particle size of about 20 nm, micron-zirconium dioxide particles with an average particle size of about 3 μm and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of nano-silicon dioxide particles is 1% and the weight percentage of micron-zirconium dioxide particles is 20%. The blending and homogenizing stirring time is 1 hour, the stirring temperature is 120° C., the vacuum degree is about 0.5 Torr, the revolution stirring speed is 1200 rpm, and the rotation stirring speed is 1080 rpm.

[0048] The low viscosity epoxy resin mixed mother liquor was transferred into a centrifuge for high speed centrifugation at a speed of 80,000 rpm for 10 minutes to obtain a mixture of nano-silicon dioxide particles and epoxy resin uniformly dispersed in the upper layer and micron zirconium dioxide particles obtained by centrifugation in the lower layer.

[0049] The upper mixed liquid is taken out to obtain a resin composition in which nano-silicon dioxide particles and epoxy resin are evenly dispersed.

[0050] Example 6

[0051] Nano-silicon dioxide particles with an average particle size of about 20 nm, micron-zirconium dioxide particles with an average particle size of about 3 μm, and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of nano-silicon dioxide particles is 8%, and the weight percentage of micron-zirconium dioxide particles is 20%. The blending and homogenizing stirring time is 1 hour, the stirring temperature is 120° C., the vacuum degree is about 0.5 Torr, the revolution stirring speed is 1200 rpm, and the rotation stirring speed is 1080 rpm.

[0052] The low viscosity epoxy resin mixed mother liquor was transferred into a centrifuge for high speed centrifugation at a speed of 80,000 rpm for 10 minutes to obtain a mixture of nano-silicon dioxide particles and epoxy resin uniformly dispersed in the upper layer and micron zirconium dioxide particles obtained by centrifugation in the lower layer.

[0053] The upper mixed liquid is taken out to obtain a resin composition in which nano-silicon dioxide particles and epoxy resin are evenly dispersed.

[0054] Example 7

[0055] Nano-silicon dioxide particles with an average particle size of about 130 nm, micron glass beads with an average particle size of about 100 μm, and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of nano-silicon dioxide particles is 0.5%, and the weight percentage of micron glass beads is 5%. The blending and homogenizing stirring time is 1 hour, the stirring temperature is 120° C., the vacuum degree is about 0.5 Torr, the revolution stirring speed is 1200 rpm, and the rotation stirring speed is 1080 rpm.

[0056] The low viscosity epoxy resin mixed mother liquor was transferred into a centrifuge for high speed centrifugation at 80000 rpm for 10 minutes to obtain an upper layer of a mixed liquid in which nano-silica particles and epoxy resin were evenly dispersed, and a lower layer of micron glass bead particles were obtained by centrifugation.

[0057] The upper mixed liquid is taken out to obtain a resin composition in which nano-silicon dioxide particles and epoxy resin are evenly dispersed.

[0058] Comparative Example 1

[0059] Nano-silica particles with an average particle size of about 20 nm and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of the nano-silica particles is 4%, the blending and homogenizing stirring time is 1 hour, the stirring temperature is 120°C, the vacuum degree is about 0.5 Torr, and the stirring speed is 1200 rpm.

[0060] The low-viscosity epoxy resin mixed mother liquor after the particles are dispersed is transferred into a centrifuge for high-speed centrifugation, wherein the centrifugal speed is 80,000 rpm and the centrifugal time is 10 minutes.

[0061] The centrifuged mixed solution of nano-silicon dioxide particles and epoxy resin is taken out.

[0062] Comparative Example 2

[0063] Nanosilver particles with an average particle size of about 75 nm and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of the nanosilver particles is 3%, the blending and homogenizing stirring time is 1 hour, the stirring temperature is 120° C., the vacuum degree is about 0.5 Torr, and the stirring speed is 1500 rpm.

[0064] The low-viscosity epoxy resin mixed mother liquor after the particles are dispersed is transferred into a centrifuge for high-speed centrifugation, wherein the centrifugal speed is 70,000 rpm and the centrifugal time is 10 minutes.

[0065] The centrifuged mixed solution of the nano-silver particles and the epoxy resin is taken out.

[0066] Comparative Example 3

[0067] Nano-silica particles with an average particle size of about 130 nm and liquid epoxy resin are added to a planetary mixer for blending and homogenizing to obtain a mixed epoxy resin mother liquor after particle dispersion, wherein the weight percentage of nano-silica particles is 0.5%, the blending and homogenizing stirring time is 1 hour, the stirring temperature is 120°C, the vacuum degree is about 0.5 Torr, and the stirring speed is 1200 rpm.

[0068] The low-viscosity epoxy resin mixed mother liquor after the particles are dispersed is transferred into a centrifuge for high-speed centrifugation, wherein the centrifugal speed is 80,000 rpm and the centrifugal time is 10 minutes.

[0069] The centrifuged mixed solution of nano-silicon dioxide particles and epoxy resin is taken out.

[0070] Comparative Example 4

[0071] The liquid epoxy resin was added into a planetary mixer for stirring, and then transferred into a centrifuge for high-speed centrifugation, wherein the stirring time was 1 hour, the stirring temperature was 120°C, the vacuum degree was about 0.5 Torr, the stirring speed was 1200 rpm, the centrifugal speed was 70000 rpm, and the centrifugal time was 10 minutes.

[0072] In the following examples, the epoxy equivalent of the epoxy resin used in Examples 1-7 and Comparative Examples 1-3 was calculated, mixed with the same equivalent of etheramine curing agent and poured into the mold. After that, the mold was moved to an oven and heated to 60°C for curing to prepare a resin nanocomposite plate. After that, the resin nanocomposite plate was CNC cut into a resin nanocomposite standard test piece for various performance tests, including bending strength, bending modulus, dispersion rate, etc. The test results are shown in Table 1 below.

[0073] Table 1

[0074]

[0075] The bending strength in Table 1 is tested according to the ASTM D790 standard. The specimens made according to the standard are bent with a three-point bending fixture, and the maximum yield stress is taken as the strength (MPa). The strength test instrument is a German ZwickRoell universal material testing machine.

[0076] The bending modulus is tested according to the ASTM D790 standard. The specimen made in accordance with the standard is bent with a three-point bending fixture, and the elastic limit internal stress and strain are calculated (MPa). The modulus measurement instrument is a German ZwickRoell universal material testing machine.

[0077] The dispersion rate was observed by scanning electron microscope (SEM) and the size of nanofiller agglomeration was calibrated by software. The imaging observation instrument was Hitachi FE-SEM from Japan.

[0078] Please refer to Table 1. The resin nanocomposite prepared by Example 1 has a 10.3% higher flexural strength and a 17.6% higher flexural modulus than the resin material prepared by Comparative Example 4. The resin nanocomposite prepared by Example 2 has a 8.9% higher flexural strength and a 13.9% higher flexural modulus than the resin material prepared by Comparative Example 4. The resin nanocomposite prepared by Example 3 has a 11.8% higher flexural strength and a 18.5% higher flexural modulus than the resin material prepared by Comparative Example 4. The resin nanocomposite prepared by Example 4 has a 9.3% higher flexural strength and a 14.3% higher flexural modulus than the resin material prepared by Comparative Example 4. The resin nanocomposite prepared by Example 5 has a 7.6% higher flexural strength and a 5.2% higher flexural modulus than the resin material prepared by Comparative Example 4. The resin nanocomposite prepared by Example 6 has a 5.8% higher flexural strength and a 17.1% higher flexural modulus than the resin material prepared by Comparative Example 4. Compared with the resin material prepared in Comparative Example 4, the flexural strength of the resin nanocomposite prepared in Example 7 is increased by 7.5%, and the flexural modulus is increased by 4.5%.

[0079] The resin nanocomposite prepared by Example 1 has a 9.3% higher flexural strength and a 4.9% higher flexural modulus than the resin nanocomposite prepared by Comparative Example 1. The resin nanocomposite prepared by Example 2 has a 6.6% higher flexural strength and a 3.9% higher flexural modulus than the resin nanocomposite prepared by Comparative Example 2.

[0080] In addition, according to Table 1, the agglomeration size of the resin nanocomposites prepared by Examples 1-7 is significantly smaller than the agglomeration size of the resin nanocomposites prepared by Comparative Examples 1-3.

[0081] As described above, according to an embodiment of the present invention, a method for manufacturing a resin composition is provided. This method can effectively and evenly disperse the nanoparticle filler in the resin, and reduce the stress concentration defects of the composite material formed after curing due to the presence of undispersed nanoparticle filler inside the composite material. Therefore, the mechanical properties and stability of the resin composition and the composite material can be improved.

[0082] Although the present invention has been disclosed in the above embodiments, it is not intended to limit the present invention. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims.

[0083]

Explanation of symbols

[0084] 100: Method

[0085] 110: Steps

[0086] 120: Steps

[0087] 130: Steps.

Claims

1. A method for producing a resin composition, characterized in that: include: Stirring and mixing nanoparticle filler, micron inorganic particles and resin to form a mixture, wherein the micron inorganic particles have a weight percentage of 0.1-30%, the micron inorganic particles include zirconium dioxide, titanium dioxide, micron glass beads or a combination thereof, the micron inorganic particles have a particle size of 2 μm-200 μm, the nanoparticle filler has a particle size of 5 nm-250 nm, and the nanoparticle filler includes nano silicon dioxide, nano silver, nano calcium carbonate, nano kaolin, nano titanium dioxide, nano carbon fiber or a combination thereof; Centrifuging the mixture at high speed to form an upper mixed solution including the nanoparticle filler and a lower mixed solution including the micron inorganic particles, wherein the high-speed centrifugation of the mixture comprises a centrifugal speed of 5000-150000 rpm and a centrifugal time of 0.1-5 hours; and The upper mixed liquid is taken out to obtain the resin composition.

2. The method according to claim 1, characterized in that The nanoparticle filler has a weight percentage of 0.1-10%.

3. The method according to claim 1, characterized in that The resin includes phenolic resin, urea formaldehyde resin, melamine resin, epoxy resin, vinyl ester resin, unsaturated polyester resin, polyurethane resin, silicone resin, acrylic resin or a combination thereof.

4. The method according to claim 1, characterized in that: The stirring and mixing comprises stirring at a temperature of 20-160° C. and a stirring speed of 100-5000 rpm for 0.5-15 hours.

Citation Information

Patent Citations

  • Preparation method of micro / nano inorganic particle / epoxy resin ternary composites

    CN103865234A

  • Epoxy resin composition for insulator, preparation method and use thereof

    CN104327456A

  • Electrical insulating epoxy resin composition and preparation method thereof

    CN104479294A

  • Centrifugal manufacturing method for dielectric functional gradient insulator

    CN105542399A

  • Grain depot sealed heat insulation window capable of achieving remote opening and closing

    CN108678590A