A sintered iron ore blending method and ore blending system based on wet capacity performance
By calculating the overwet performance index of iron ore raw materials and optimizing the sintering ore distribution plan, the problem of long ore distribution cycle in the existing technology is solved, and the effect of good breathability and fast sintering speed of the material layer is achieved.
Patent Information
- Application Number
- CN202210003205.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-01-04
AI Technical Summary
The existing sintered ore distribution methods do not fully consider the wet capacity of the mixed ore, resulting in a long optimization cycle of the ore distribution process and the inability to quickly guide and optimize the ore distribution plan.
By obtaining the chemical composition and overwet performance data of iron ore raw materials, the dimensionless index is calculated, the overwet performance of mixed ores is simulated, the comprehensive evaluation index is determined, and the ore distribution plan is optimized to improve the breathability and sintering speed of the material layer.
The determination efficiency of the sintering ore distribution plan is significantly improved, and the poor breathability of the sintered material layer caused by the formation of overwet belts is avoided, the sintering speed and productivity are improved, the experimental process is reduced, and manpower, material resources and financial resources are saved.
Smart Images

Figure CN114334034B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sintered iron ore blending, and in particular, to a sintered iron ore blending method based on wet capacity performance. The present invention also relates to a sintered iron ore blending system based on wet capacity performance. Background Art
[0002] my country's steel production process is mainly based on the long process of blast furnace-converter. The smelting charges are mainly sintered ore and pelletized ore with a small amount of lump ore. The proportion of sintered ore is more than 75%. Therefore, the performance of sintered ore will seriously affect the steel production capacity and quality.
[0003] The sintering process is to mix powdered materials (iron ore powder, flux, coke, etc. in a certain proportion) with water, put them into a pelletizer for pelletizing, and then ignite them on a sintering trolley for exhaust sintering. The materials are sintered into blocks under the condition of incomplete melting. During the sintering process, water helps the mixture to granulate, conduct heat, lubricate and assist combustion. The water mainly comes from the physical content of the materials, the water added during mixing and granulating, and the water produced when a small amount of hydrocarbons are burned. During the sintering process, the water in the sintering mixture will be transformed into water vapor as the sintering ignition and combustion zone are formed and moved downward. With the sintering ventilation, the water vapor moves to the lower part of the material layer, and the water vapor temperature gradually decreases. When the water vapor temperature drops below the dew point (60°C), it begins to condense into liquid water. When the liquid water contacts the sintering mixture of the lower material layer, it will first be absorbed by the granulating balls. When the water in the granulating balls reaches a supersaturated state, the remaining water will form flowing free water, begin to fill the pores of the accumulated granulating balls, and move downward along the pores with the ventilation airflow to form an over-wet zone. Since a large amount of free-flowing water occupies part of the pores between the granulating balls, the air permeability of the material layer becomes poor and the sintering speed decreases. In addition, when the strength of some granulating balls is insufficient, when the water in the granulating balls reaches a supersaturated state, under the influence of the ventilation airflow, it is very easy to muddy and form mud, blocking the pores of the material layer, which greatly deteriorates the air permeability of the sintering material layer and has a huge impact on the sintering process.
[0004] At present, there are many types of iron ores used in sintering production in my country, with different properties and compositions. In traditional sintering ore blending, the chemical element composition and -0.5mm particle size are generally based on certain requirements, and then a preliminary ore blending plan is formulated based on the sintering practice experience of each iron ore raw material. Each ore blending plan is then mixed, pelletized and sintered cup tests are conducted to study and verify the sintering speed and production quality indicators, and finally the optimal ore blending plan is selected and determined. The traditional sintering ore blending plan cannot quickly guide the optimization of ore blending, and the optimization cycle of the ore blending plan is long. Summary of the invention
[0005] The sintered iron ore blending method based on wet capacity performance provided by the present invention solves the technical problems that the wet capacity of the mixed ore is not fully considered in the existing blending process, the ore blending optimization cannot be quickly guided, and the optimization cycle of the ore blending scheme is long.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A sintered iron ore blending method based on wet capacity performance comprises the following steps: S101, obtaining chemical composition data of N kinds of iron ore raw materials in a dried state, and obtaining over-wetting performance data of each kind of iron ore raw material; S102, calculating the dimensionless index Q of the maximum wet capacity of each kind of iron ore raw material according to the over-wetting performance data j , dimensionless exponent V of superhumidification rate j And the dimensionless index W of the migration rate of the wet zone j ; j∈(1, N); S103, according to the chemical composition data of each iron ore raw material and the preset mixed ore composition requirements, at least two iron ore raw materials are simulated and mixed to obtain M simulated ore blending schemes and M simulated target mixed ores, wherein the chemical content of the elements of each simulated target mixed ore meets the preset mixed ore composition requirements; S104, according to the formula The comprehensive evaluation index of the over-humidification performance of each simulated target mixed ore is calculated, where i represents the i-th simulated ore blending scheme; j represents the j-th iron ore raw material in the i-th simulated ore blending scheme, i∈(1, M), j∈(1, N), α ij is the ratio of the jth iron ore raw material in the i-th simulated ore blending scheme, A ij is the weight coefficient corresponding to the dimensionless index of the maximum wet capacity of the jth iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, B ij is the weight coefficient corresponding to the dimensionless index of the overwetting rate of the jth iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, C ij is the weight coefficient corresponding to the dimensionless index of the migration rate of the wet zone of the j-th iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, Q ij V is the dimensionless index of the maximum wet capacity of the jth iron ore raw material in the i-th simulated ore blending scheme, ij W is the dimensionless index of the superwetting rate of the jth iron ore raw material in the i-th simulated ore blending scheme, ij A is the dimensionless index of the migration rate of the over-wet zone of the j-th iron ore raw material in the i-th simulated ore blending scheme, ij +B ij +C ij =1; S105, determining a simulated ore blending scheme whose value of the comprehensive evaluation index of over-humidity performance meets the preset conditions as a guiding mixed ore blending scheme.
[0008] Furthermore, A ij =0.65, B ij =0.5, C ij =-0.15.
[0009] Furthermore, in step S101, "obtaining the over-wetting performance data of each type of iron ore raw material" specifically includes: piling each type of iron ore raw material into a cylinder or a regular polygon, wherein the stacking height of the iron ore raw material is H (cm), and the stacking cross-sectional area is S (m 2 ); obtain the dry material mass M (g) of the accumulated iron ore raw material, introduce water vapor into the accumulated iron ore raw material and obtain the time t (s) for the iron ore raw material to reach the maximum water absorption, and obtain the maximum water content m (g) of the accumulated iron ore raw material.
[0010] Further, each type of iron ore raw material is piled up into a vertically placed cylinder, the pile height H of the iron ore raw material is 15 to 25 cm, and the pile cross-sectional radius of the iron ore raw material is 6 to 14 cm.
[0011] Furthermore, using the formula The dimensionless index Q of the maximum wet capacity of each iron ore raw material is calculated j .
[0012] Furthermore, using the formula The dimensionless index V of the superwetting rate of the first group of iron ore raw materials was calculated j .
[0013] Furthermore, using the formula The migration rate W of the wet zone of the first group of iron ore raw materials is calculated j .
[0014] Furthermore, the preset mixed ore composition requirements include: TFe of the preset mixed ore i The range of % is ≥57%; the SiO 2i % range is 4.5% to 5.0%; the MgO of the preset blended ore i % ranges from 0% to 0.5%; the preset Al2O 3i % ranges from 1% to 2%; the preset mixed ore P i The % range is 40% to 60%.
[0015] Furthermore, step S105 specifically includes: determining a simulated ore blending scheme with a maximum value of the comprehensive evaluation index of the over-humidification performance as a guiding mixed ore blending scheme.
[0016] The present invention also provides a sintered iron ore blending system based on wet capacity performance, comprising a chemical composition analysis device for obtaining chemical composition data of N types of iron ore raw materials in a dried state; an over-moisture performance detection device for obtaining over-moisture performance data of each type of iron ore raw material; a calculator device, the calculator device comprising a memory, a processor, and a computer program stored in the memory and executable on the processor, and the processor implements the above-mentioned sintered iron ore blending method based on wet capacity performance when executing the computer program.
[0017] The present invention has the following beneficial effects:
[0018] The sintered iron ore blending method based on wet capacity performance of the present invention obtains chemical composition data of N iron ore raw materials in a drying state, and simulates and mixes at least two iron ore raw materials according to the chemical composition data of each iron ore raw material and the preset mixed ore composition requirements to obtain M kinds of simulated blending schemes and M kinds of simulated target mixed ores, wherein the chemical content of the elements of each simulated target mixed ore meets the preset mixed ore composition requirements, and preliminary blending is guided according to the preset mixed ore composition requirements so that the chemical content of the simulated target mixed ore meets the basic requirements; when the chemical content of the simulated target mixed ore meets the basic requirements, quantitative analysis and comparison of the over-wetting performance of various simulated target mixed ores are performed to determine whether the value of the comprehensive evaluation index of the over-wetting performance meets the preset conditions The simulated ore blending scheme corresponding to the simulated target mixed ore of the piece is used as the guiding mixed ore blending scheme, and then guides the raw tea blending, so that the simulated target mixed ore has the advantages of good material layer permeability, fast sintering speed and high sintering productivity during the sintering process; compared with the determination of the traditional sintering ore blending scheme, in the ore blending process, in addition to considering that the chemical composition of the simulated target mixed ore meets the sintering requirements, the present invention also comprehensively considers the over-wetting performance of the simulated target mixed ore in advance, which can avoid the poor air permeability of the sintering material layer caused by the rapid formation of the over-wet zone and the large thickness of the over-wet zone during the sintering process, which in turn leads to a decrease in the sintering rate and low sintering production efficiency. It saves a lot of sintering cup experimental processes, saves a lot of manpower, material and financial resources, and greatly improves the efficiency of determining the sintering ore blending scheme.
[0019] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0021] Figure 1 It is a flow chart of a sintered iron ore blending method based on wet capacity performance according to a preferred embodiment of the present invention;
[0022] Figure 2 It is a schematic structural diagram of the over-humidity performance detection device in the present invention. DETAILED DESCRIPTION
[0023] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. However, the present invention can be implemented in many different ways as defined and covered below.
[0024] Figure 1 It is a flow chart of a sintered iron ore blending method based on wet capacity performance according to a preferred embodiment of the present invention; Figure 2 It is a schematic structural diagram of the over-humidity performance detection device in the present invention.
[0025] like Figure 1 As shown, the sintered iron ore blending method based on wet capacity performance of this embodiment includes the following steps: S101, obtaining chemical composition data of N kinds of iron ore raw materials in a dried state, and obtaining over-wetting performance data of each kind of iron ore raw material; S102, calculating the dimensionless index Q of the maximum wet capacity of each kind of iron ore raw material according to the over-wetting performance data j , dimensionless exponent V of superhumidification rate j And the dimensionless index W of the migration rate of the wet zone j ; Wherein, j∈(1, N); S103, according to the chemical composition data of each iron ore raw material and the preset mixed ore composition requirements, at least two iron ore raw materials are simulated and mixed to obtain M simulated ore blending schemes and M simulated target mixed ores, wherein the chemical content of the elements of each simulated target mixed ore meets the preset mixed ore composition requirements; S104, according to the formula The comprehensive evaluation index of the over-humidification performance of each simulated target mixed ore is calculated, where i represents the i-th simulated ore blending scheme; j represents the j-th iron ore raw material in the i-th simulated ore blending scheme, i∈(1, M), j∈(1, N), α ij is the ratio of the jth iron ore raw material in the i-th simulated ore blending scheme, A ij is the weight coefficient corresponding to the dimensionless index of the maximum wet capacity of the jth iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, B ij is the weight coefficient corresponding to the dimensionless index of the overwetting rate of the jth iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, C ij is the weight coefficient corresponding to the dimensionless index of the migration rate of the wet zone of the j-th iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, Q ij V is the dimensionless index of the maximum wet capacity of the jth iron ore raw material in the i-th simulated ore blending scheme, ijW is the dimensionless index of the superwetting rate of the jth iron ore raw material in the i-th simulated ore blending scheme, ij A is the dimensionless index of the migration rate of the over-wet zone of the j-th iron ore raw material in the i-th simulated ore blending scheme, ij +B ij +C ij =1; S105, determining a simulated ore blending scheme whose value of the comprehensive evaluation index of over-humidity performance meets the preset conditions as a guiding mixed ore blending scheme.
[0026] The sintered iron ore blending method based on wet capacity performance of the present invention obtains chemical composition data of N iron ore raw materials in a drying state, and simulates and mixes at least two iron ore raw materials according to the chemical composition data of each iron ore raw material and the preset mixed ore composition requirements to obtain M kinds of simulated blending schemes and M kinds of simulated target mixed ores, wherein the chemical content of the elements of each simulated target mixed ore meets the preset mixed ore composition requirements, and preliminary blending is guided according to the preset mixed ore composition requirements so that the chemical content of the simulated target mixed ore meets the basic requirements; when the chemical content of the simulated target mixed ore meets the basic requirements, quantitative analysis and comparison of the over-wetting performance of various simulated target mixed ores are performed to determine whether the value of the comprehensive evaluation index of the over-wetting performance meets the preset conditions The simulated ore blending scheme corresponding to the simulated target mixed ore of the piece is used as the guiding mixed ore blending scheme, and then guides the raw tea blending, so that the simulated target mixed ore has the advantages of good material layer permeability, fast sintering speed and high sintering productivity during the sintering process; compared with the determination of the traditional sintering ore blending scheme, in the ore blending process, in addition to considering that the chemical composition of the simulated target mixed ore meets the sintering requirements, the present invention also comprehensively considers the over-wetting performance of the simulated target mixed ore in advance, which can avoid the poor air permeability of the sintering material layer caused by the rapid formation of the over-wet zone and the large thickness of the over-wet zone during the sintering process, which in turn leads to a decrease in the sintering rate and low sintering production efficiency. It saves a lot of sintering cup experimental processes, saves a lot of manpower, material and financial resources, and greatly improves the efficiency of determining the sintering ore blending scheme.
[0027] Optionally, in order to improve the accuracy of the analysis, each type of iron ore raw material is sampled and dried using a dichotomy method; in the present invention, the over-wetting performance of the iron ore raw material can be detected by capillary water, or by an over-wetting performance detection device.
[0028] Furthermore, in order to accurately obtain the comprehensive evaluation index of the over-humidification performance of the simulated target mixed ore, A ij =0.65, B ij =0.5, C ij =-0.15. Optionally, in other embodiments, it can also be A ij =0.60, B ij =0.55, C ij=-0.15, as long as A ij +B ij +C ij =1.
[0029] It can be understood that each iron ore raw material is subjected to chemical analysis to obtain the chemical composition data of each iron ore raw material; each iron ore raw material is subjected to overwetting performance testing to obtain the dimensionless index q of the maximum wet capacity of each iron ore raw material and the dimensionless index v1 / (m 2 ﹒ s) and the dimensionless exponent w of the migration rate of the super-wet zone.
[0030] Furthermore, in step S101, "obtaining the over-wetting performance data of each type of iron ore raw material" specifically includes: piling each type of iron ore raw material into a cylinder or a regular polygon, wherein the stacking height of the iron ore raw material is H (cm), and the stacking cross-sectional area is S (m 2 ); obtain the dry material mass M (g) of the accumulated iron ore raw material, introduce water vapor into the accumulated iron ore raw material and obtain the time t (s) for the iron ore raw material to reach the maximum water absorption, and obtain the maximum water content m (g) of the accumulated iron ore raw material. It can be understood that when the over-humidity performance test of the iron ore raw material is carried out, the iron ore raw material is placed in the over-humidity performance test device for testing. Please refer to Figure 2In the present invention, an over-humidity performance detection device detects the over-humidity performance of iron ore raw materials. The over-humidity performance detection device includes a steam supply unit, a material holding unit, a water collection unit, a weighing unit, a pressure testing unit and a negative pressure suction unit. The material holding unit is provided with a receiving cavity for receiving materials. The steam supply unit, the water collection unit, the pressure testing unit and the negative pressure suction unit are all sealed and connected with the material holding unit. The steam supply unit is used to transport water vapor from the top of the material holding unit to the receiving cavity. The water collection unit is used to collect condensed water in the receiving cavity from the bottom of the material holding unit. The weighing unit is used to weigh the material holding unit. The pressure testing unit is used to measure the pressure of the receiving cavity. The negative pressure suction unit is used to extract the airflow in the receiving cavity from the bottom of the material holding unit. The steam supply unit is used to transport water vapor to the top of the material holding unit and into the accommodating cavity. The water vapor condenses when it encounters the low-temperature material in the material holding unit, and the material begins to absorb water and gradually becomes over-humidified. This process completely and accurately simulates the over-humidification zone formation process in the iron ore sintering process. After the material is completely over-humidified, the excess condensed water is collected by the water body collection unit. After the value weighed by the weighing unit is stable, the material reaches the maximum wet capacity, and the maximum water content is obtained by weighing the weighing unit. The negative pressure change in the accommodating cavity is recorded by the pressure test sheet, and the air is exhausted by the negative pressure suction unit. At the same time, the change process of the moisture content and negative pressure in the material with time is recorded, so as to facilitate the preparation of the material wet capacity-time curve, the material layer negative pressure-time curve, and the wet capacity-material layer negative pressure curve under the specified water vapor flow rate and normal pressure state. The maximum wet capacity, over-humidification rate, over-humidification zone migration rate, etc. of the material are calculated by measuring the maximum water absorption, the time when the maximum water absorption is reached, the material layer height, the dry material mass and other data, and the over-humidification performance of the iron ore raw material is measured in the simulated sintering environment with high measurement accuracy.
[0031] Understandably, please refer again Figure 2The steam supply unit, the water collection unit, the pressure testing unit and the negative pressure suction unit are all sealed and connected to the material holding unit and are all connected to the accommodating cavity; the steam supply unit includes a constant temperature steam generator, a slow cooling gas mixing tank and a steam delivery pipe, the input end of the slow cooling gas mixing tank is connected to the output end of the constant temperature steam generator, the output end of the slow cooling gas mixing tank is connected to the input end of the steam delivery pipe, and the output end of the steam delivery pipe passes through the top wall of the material holding unit and extends into the accommodating cavity; the steam delivery pipe includes a first steam pipeline, an insulation belt, an insulation temperature controller, a steam valve, a buffer cylinder and a steam supply pipe. and a second steam pipe, the input end of the first steam pipe is connected to the output end of the slow cooling mixing tank, the output end of the first steam pipe is connected to the input end of the buffer cylinder through a steam valve, the output end of the buffer cylinder is connected to the input end of the second steam pipe, the output end of the second steam pipe passes through the top wall of the material holding unit and extends into the accommodating cavity, the insulation belt is wrapped on the first steam pipe, and the insulation temperature controller is electrically connected to the insulation belt; the water collection unit includes a collection cylinder and a collection pipe, the first end of the collection pipe is connected to the bottom of the accommodating cavity, and the second end of the collection pipe is connected to the collection cylinder. It can be understood that in the present application, the collection cylinder is sealed and connected to the accommodating chamber through the collection pipe, thereby preventing the collection cylinder from leaking and affecting the pressure of the accommodating cavity; the collection cylinder is arranged below the material holding unit, and the second end of the collection pipe is arranged to tilt downward. It can be understood that in order to facilitate the collection of condensed water and gravity water generated during the over-humidification process, the second end of the collection tube is arranged to be tilted downward; the weighing unit includes an electronic balance, the material holding unit is placed on the electronic balance, and / or the pressure testing unit includes a negative pressure display, and the input end of the negative pressure display is connected to the accommodating cavity; the negative pressure suction unit includes a suction pipe, a suction flowmeter, a suction valve and a negative pressure fan, the input end of the suction pipe is connected to the accommodating cavity from the bottom of the material holding unit, the output end of the suction pipe is connected to the first end of the suction flowmeter, and the second end of the suction flowmeter is connected to the negative pressure fan through the suction valve; the material holding unit includes a cup body with an opening at the top and a cup cover for sealing the opening, and a accommodating cavity is provided in the cup body. The material holding unit also includes an active clip for fixing the cup cover and the cup body; the cup body includes a material cup and a cup seat, the material cup is detachably arranged on the cup seat, the material cup is provided with a material cavity which penetrates the material cup along the height direction of the material cup, the bottom of the material cup is provided with a filter screen for covering the material cavity, the cup seat is provided with a water vapor cavity with a top opening, the material cup is pressed onto the cup seat and communicates with the material cavity and the water vapor cavity to form a accommodating cavity, the steam providing unit is used to transport water vapor from the top of the material holding unit into the material cavity, the water body collecting unit is used to collect condensed water in the water vapor cavity from the bottom of the material holding unit, the pressure testing unit is used to measure the pressure of the water vapor cavity, and the negative pressure suction unit is used to extract the airflow in the water vapor cavity from the bottom of the material holding unit.
[0032] It can be understood that the material holding unit is a detachable structure, the cup seat and the material cup are detachably arranged, and the material cup and the cup cover are detachably arranged; the cross-section of the material cup is S (m), and the height of the material cup is H (cm).
[0033] The device for measuring the over-humidification performance of sintered iron ore raw materials of the present application comprises the following steps when used specifically: loading the material to be measured into a dry material cup, placing the material cup containing the material on the cup holder, sealing the cup cover on the top opening of the material cup and fastening it with a movable snap fastener; after the electronic balance indication is stable, clear the balance; turn on the constant temperature steam generator, set the flow rate according to actual needs, such as 10ml / min, turn on the insulation temperature controller, and set the insulation temperature to ℃ under a standard atmospheric pressure; after the steam generation is stable, turn on the negative pressure fan, adjust the relief valve so that the exhaust negative pressure meets the requirements, and start timing at the same time; as the steam continues to condense in the material, the indication of the electronic balance gradually changes, and the change of the electronic balance indication over time is recorded online, and the negative pressure indication on the negative pressure display is recorded at the same time; when the electronic balance indication is stable again, turn off the negative pressure fan, close the regulating relief valve, close the steam valve, close the constant temperature steam generator, and when no condensate flows out of the collecting pipe, record the electronic balance indication m.
[0034] Further, each type of iron ore raw material is piled up into a vertically placed cylinder, the pile height H of the iron ore raw material is 15 to 25 cm, and the pile cross-sectional radius of the iron ore raw material is 6 to 14 cm.
[0035] Furthermore, using the formula The dimensionless index Q of the maximum wet capacity of each iron ore raw material is calculated j , using the formula The dimensionless index V of the superwetting rate of the first group of iron ore raw materials was calculated j , using the formula The migration rate W of the wet zone of the first group of iron ore raw materials is calculated j .
[0036] Further, please refer to Table 1, and design a preliminary simulation ore blending scheme according to the requirements of the total iron content, SiO2 content, MgO content, Al2O3 content and the proportion of -0.5 mm particle size of the preset mixed ore, and obtain i kinds of simulated ore blending schemes. The calculation method of the total iron content, SiO2 content, MgO content, Al2O3 content and -0.5m particle size proportion of each simulated target mixed ore in the i kinds of simulated ore blending schemes is as follows: Among them, TFe i % is the total iron content of the simulated target mixed ore of the ith simulated ore blending scheme, α ij TFe is the mass ratio of the jth iron ore raw material in the i-th simulated ore blending scheme; ij% is the total iron content of the jth iron ore raw material of the simulated target mixed ore in the i-th simulated ore blending scheme; In the formula, SiO 2i % is the SiO2 content of the simulated target mixed ore of the i-th simulated ore blending scheme; α ij is the mass ratio of the jth iron ore raw material in the i-th simulated ore blending scheme; SiO 2ij % is the SiO2 content of the jth iron ore raw material in the simulated target mixed ore in the i-th simulated ore blending scheme; In the formula, MgO i % is the MgO content of the simulated target mixed ore of the i-th simulated ore blending scheme; α ij is the mass ratio of the jth iron ore raw material in the i-th simulated ore blending scheme; MgO ij % is the MgO content of the jth iron ore raw material in the simulated target mixed ore in the i-th simulated ore blending scheme; In the formula, Al2O 3i % is the Al2O3 content of the simulated target mixed ore of the i-th simulated ore blending scheme; α ij is the mass ratio of the jth iron ore raw material in the i-th simulated ore blending scheme; Al2O 3ij % is the Al2O3 content of the jth iron ore raw material of the simulated target mixed ore in the i-th simulated ore blending scheme; Where P i % is the -0.5mm particle size content of the simulated target mixed ore of the ith simulated ore blending scheme; α ij is the mass ratio of the jth iron ore raw material in the i-th simulated ore blending scheme; P ij % is the -0.5 mm particle size content of the jth iron ore raw material in the simulated target mixed ore in the i-th simulated ore blending scheme; the mass ratio of n iron ore raw materials in the i-th preliminary simulated ore blending scheme is α ij After the above formula is introduced, the following conditions must be met: TFe of the simulated target mixed ore i % range is ≥55%; the SiO 2i % ranges from 4.0% to 6.0%; MgO of the simulated target blended ore i % ranges from 0% to 2%; the Al2O 3i % ranges from 0% to 3%; P of the simulated target mixed ore i The % range is from 20% to 80%.
[0037] According to the above principles, i kinds of simulated ore blending schemes are obtained, and the proportion of each iron ore raw material in each simulated ore blending scheme is:
[0038] Iron ore raw materials The first type of iron ore raw material Second type of iron ore raw material …… The jth iron ore raw material Simulation ore matching scheme 1 <![CDATA[α 11 ]]> <![CDATA[α 12 ]]> …… <![CDATA[α 1j ]]> Simulation ore allocation plan 2 <![CDATA[α 21 ]]> <![CDATA[α 22 ]]> …… <![CDATA[α 2j ]]> …… …… …… …… …… Simulation of ore matching plan <![CDATA[α 11 ]]> <![CDATA[α 12 ]]> …… <![CDATA[α 1j ]]>
[0039] Table 1
[0040] Furthermore, the preset mixed ore composition requirements include: TFe of the preset mixed ore i The range of % is ≥57%; the SiO 2i % range is 4.5% to 5.0%; the MgO of the preset blended ore i % ranges from 0% to 0.5%; the preset Al2O 3i % ranges from 1% to 2%; the preset mixed ore P i The % range is 40% to 60%.
[0041] Furthermore, step S105 specifically includes: determining a simulated ore blending scheme with a maximum value of the comprehensive evaluation index of the over-humidification performance as a guiding mixed ore blending scheme.
[0042] In the present invention, preliminary ore blending is carried out according to the guidance of the chemical content of the simulated target mixed ore, so that the chemical content of the simulated target mixed ore meets the basic requirements; when the chemical content of the simulated target mixed ore meets the basic requirements, quantitative analysis and comparison of the over-wetting performance of various simulated target mixed ores are carried out, and a simulated ore blending scheme of the simulated target mixed ore with good over-wetting performance is selected as a reference scheme, and then the ore blending is guided, so that the simulated target mixed ore has the advantages of good air permeability of the material layer, fast sintering speed and high sintering productivity during the sintering process; compared with the determination of the traditional sintering ore blending scheme, in addition to considering whether the chemical composition of the mixed ore meets the sintering requirements during the ore blending process, the present invention also comprehensively considers the over-wetting performance of the ore blending scheme in advance, and selects a simulated ore blending scheme with a high comprehensive evaluation index of the over-wetting performance for sintering practice, which can avoid the problem of poor air permeability of the sintering material layer caused by fast formation of over-wetting zone and large thickness of over-wetting zone during the sintering process, thereby reducing the sintering rate and low sintering production efficiency, eliminating a large number of sintering cup experimental processes, saving a large amount of manpower, material and financial resources, and greatly improving the efficiency of determining the sintering ore blending scheme.
[0043] The present invention also provides a sintered iron ore blending system based on wet capacity performance, comprising a chemical composition analysis device for obtaining chemical composition data of N types of iron ore raw materials in a dried state; an over-moisture performance detection device for obtaining over-moisture performance data of each type of iron ore raw material; a calculator device, the calculator device comprising a memory, a processor, and a computer program stored in the memory and executable on the processor, and the processor implements the above-mentioned sintered iron ore blending method based on wet capacity performance when executing the computer program.
[0044] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for blending sintered iron ore based on wettability, characterized in that: The steps include: S101, obtaining chemical composition data of N kinds of iron ore raw materials in a drying state, and obtaining over-humidification performance data of each of the iron ore raw materials; “Obtaining the over-wetting performance data of each of the iron ore raw materials” specifically includes: Each of the iron ore raw materials is piled up into a cylinder or a regular polygon, wherein the pile height of the iron ore raw materials is H (cm) and the pile cross-sectional area is S (m 2 ); Obtaining the dry material mass M (g) of the accumulated iron ore raw material, introducing water vapor into the accumulated iron ore raw material and obtaining the time t (s) for the iron ore raw material to reach the maximum water absorption, and obtaining the maximum water content m (g) of the accumulated iron ore raw material; S102, calculating the dimensionless index Q of the maximum moisture capacity of each type of the iron ore raw material according to the over-wetting performance data j , dimensionless index V of superhumidification rate j And the dimensionless index W of the migration rate of the wet zone j ; where j∈(1,N); S103, according to the chemical composition data of each of the iron ore raw materials and the preset mixed ore composition requirements, simulate mixing at least two of the iron ore raw materials to obtain M simulated ore blending schemes and M simulated target mixed ores, wherein the chemical content of the elements of each of the simulated target mixed ores meets the preset mixed ore composition requirements; S104, according to the formula The comprehensive evaluation index of the over-humidification performance of each simulated target mixed ore is calculated, where i represents the i-th simulated ore blending scheme; j represents the j-th iron ore raw material in the i-th simulated ore blending scheme, i∈(1,M), j∈(1,N), α ij is the ratio of the jth iron ore raw material in the i-th simulated ore blending scheme, A ij is the weight coefficient corresponding to the dimensionless index of the maximum wet capacity of the jth iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, B ij is the weight coefficient corresponding to the dimensionless index of the overwetting rate of the jth iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, C ij is the weight coefficient corresponding to the dimensionless index of the migration rate of the wet zone of the j-th iron ore raw material in the i-th simulated ore blending scheme and the permeability of the material layer, Q ij V is the dimensionless index of the maximum wet capacity of the jth iron ore raw material in the i-th simulated ore blending scheme, ij W is the dimensionless index of the superwetting rate of the jth iron ore raw material in the i-th simulated ore blending scheme, ij A is the dimensionless index of the migration rate of the over-wet zone of the j-th iron ore raw material in the i-th simulated ore blending scheme, ij+ B ij+ C ij =1; Using formula The dimensionless index Q of the maximum wet capacity of each iron ore raw material is calculated as follows: j ; Using formula The dimensionless index V of the superwetting rate of the first group of iron ore raw materials was calculated j ; Using formula The migration rate W of the wet zone of the first group of iron ore raw materials is calculated j ; S105, determining the simulated ore blending scheme whose value of the comprehensive evaluation index of over-humidification performance meets the preset conditions as a guiding mixed ore blending scheme.
2. The sintered iron ore blending method based on wet capacity performance according to claim 1, characterized in that: A ij =0.65,B ij =0.5,C ij =-0.15。 3. The sintered iron ore blending method based on wet capacity performance according to claim 1, characterized in that: Each of the iron ore raw materials is piled up into a vertically placed cylinder, the pile height H of the iron ore raw materials is 15 to 25 cm, and the pile cross-sectional radius of the iron ore raw materials is 6 to 14 cm.
4. The sintered iron ore blending method based on wet capacity performance according to claim 1, characterized in that: The preset mixed ore composition requirements include: The TFe of the preset mixed ore i The range of % was ≥57%; The preset mixed ore SiO 2i % ranged from 4.5% to 5.0%; The MgO content of the preset mixed ore i % ranges from 0% to 0.5%; The Al2O 3i % ranges from 1% to 2%; The P of the preset mixed ore i % ranges from 40% to 60%.
5. The sintered iron ore blending method based on wet capacity performance according to claim 1, characterized in that: The step S105 specifically includes: The simulated ore blending scheme with the largest value of the comprehensive evaluation index of over-humidification performance is determined as a guiding mixed ore blending scheme.
6. A sintered iron ore blending system based on wet capacity performance, characterized in that: It includes a chemical composition analysis device for obtaining chemical composition data of N kinds of iron ore raw materials in a drying state; An over-humidity performance detection device, used to obtain over-humidity performance data of each of the iron ore raw materials; A computer device, the computer device comprising a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor implements the sintered iron ore blending method based on wettability as described in any one of claims 1 to 5 when executing the computer program.