Cyclic polymer hydrogenate and method for producing the same, and resin composition
Through the ring-opening polymerization and hydrogenation process of cyclic olefin monomers, the problem of difficult to produce a new structure in the prior art is solved, and the efficient manufacturing of a cyclic polymer hydride with a new structure is achieved for resin combinations. new materials for the substance.
Patent Information
- Application Number
- CN202080061666.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-25
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-09-24
AI Technical Summary
The prior art is difficult to manufacture cyclic polymers with new structures and cannot meet the industrial demand for new polymers.
By opening the ring-open polymerization of the cyclic olefin monomer, the ring-open polymerization step is performed in the presence of the cyclic vinyl ether compound, and the obtained polymer is then hydrogenated to form a cyclic polymer hydride having a novel structure.
The efficient manufacturing of cyclic polymer hydrides with novel structures is achieved, and a new material for resin compositions is provided, and a resin material suitable for various molded bodies is provided.
Smart Images

Figure BDA0003528082350000041 
Figure BDA0003528082350000051 
Figure BDA0003528082350000081
Abstract
Description
Technical Field
[0001] The present invention relates to a hydrogenated cyclic polymer and a method for producing the same, and a resin composition. Background Art
[0002] In order to obtain polymers with industrially useful properties, various methods for producing polymers including the step of subjecting cyclic olefin monomers to ring-opening metathesis polymerization have been studied. For example, in non-patent document 1, as a method for producing cyclic polynorbornene with high regularity of arrangement of repeating units, a method for polymerizing norbornene by stereoselective ring expansion metathesis polymerization (Ring Expansion Metathesis Polymerization: REMP) is disclosed. In addition, in patent document 1, a metathesis polymerization method is disclosed, which includes: a step of activating an organic initiator by exciting a reaction mixture containing a cyclic unsaturated monomer and an organic initiator; and a step of polymerizing a cyclic unsaturated monomer via a four-membered carbocyclic intermediate by the activated organic initiator.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent document 1: International Publication No. 2016 / 036976.
[0006] Non-patent literature
[0007] Non-patent document 1: Stella A. Gonzales et al, "Highly Tactic Cyclic Polynorbornene: Stereoselective Ring Expansion Metathesis Polymerization (REMP) of Norbornene Catalyzed By a New Tethered Tungsten-alkylidene Catalyst", Journal of the American Chemical Society 138(15), April 2016, p.1-51. Summary of the invention
[0008] Problem that the invention aims to solve
[0009] In recent years, polymers having novel structures have been required. Therefore, an object of the present invention is to provide a hydrogenated cyclic polymer having an unprecedented novel structure. Furthermore, an object of the present invention is to provide a resin composition comprising the hydrogenated cyclic polymer having the novel structure.
[0010] Solutions for solving problems
[0011] The present inventors conducted intensive studies to solve the above problems and found that an unprecedented new structure can be created by ring-opening polymerizing a cyclic olefin monomer and then hydrogenating the obtained ring-opening polymer, thereby completing the present invention.
[0012] That is, the object of the present invention is to advantageously solve the above-mentioned problems, and the hydrogenated cyclic polymer of the present invention is characterized in that it is a hydrogenated cyclic polymer containing a cyclic chain composed of repeating units of cyclic olefin ring-opening polymerization units. Such a hydrogenated cyclic polymer has a novel structure.
[0013] In addition, the structure of the hydrogenated cyclic polymer can be analyzed by the method described in Examples of this specification.
[0014] Here, in the hydrogenated cyclic polymer of the present invention, it is preferred that the cyclic chain of the cyclic polymer includes an ether bond.
[0015] In addition, the present invention aims to solve the above-mentioned problems advantageously, and the method for producing a hydrogenated cyclic polymer of the present invention is characterized by comprising: a ring-opening polymerization step of ring-opening polymerization of at least one cyclic olefin monomer in the presence of a cyclic vinyl ether compound to obtain a cyclic polymer including a cyclic chain consisting of repeating units of a cyclic olefin ring-opening polymerization unit; and a hydrogenation step of hydrogenating the cyclic polymer to obtain a hydrogenated cyclic polymer. According to the production method, the hydrogenated cyclic polymer of the present invention can be efficiently produced.
[0016] Here, in the method for producing a hydrogenated cyclic polymer of the present invention, it is preferred that the cyclic chain of the cyclic polymer obtained by the ring-opening polymerization step contains an ether bond.
[0017] Furthermore, an object of the present invention is to advantageously solve the above-mentioned problems. The resin composition of the present invention is characterized by comprising any one of the above-mentioned hydrogenated cyclic polymers.
[0018] Effects of the Invention
[0019] According to the present invention, a hydrogenated cyclic polymer having a novel structure can be provided. In addition, according to the present invention, a resin composition containing the hydrogenated cyclic polymer having a novel structure can be provided. DETAILED DESCRIPTION
[0020] Hereinafter, embodiments of the present invention will be described in detail.
[0021] The cyclic polymer hydrogenate of the present invention is a polymer that can be used as a resin material constituting various molded bodies in various fields. In addition, the cyclic polymer hydrogenate of the present invention is preferably used as a constituent material of the resin composition of the present invention. Furthermore, the cyclic polymer hydrogenate of the present invention can be efficiently produced according to the production method of the cyclic polymer hydrogenate of the present invention.
[0022] (Cyclic polymer hydrogenate)
[0023] The cyclic polymer hydrogenate of the present invention is a hydrogenate of a cyclic polymer containing a cyclic chain consisting of repeating units of cyclic olefin ring-opening polymerization units. Here, in this specification, "cyclic chain" refers to a state in which a polymer chain formed by linking two or more monomers is cyclic. In addition, the cyclic polymer may also have a side chain in addition to the cyclic chain as the main chain. And, the cyclic polymer hydrogenate of the present invention is formed by hydrogenating at least a portion of the carbon-carbon double bonds contained in the cyclic chain and the side chain of the cyclic polymer.
[0024] <Ring Chain>
[0025] Here, as described above, the cyclic chain is composed of repeating units of cyclic olefin ring-opening polymerization units. More specifically, the cyclic chain preferably contains only cyclic olefin ring-opening polymerization units as repeating units.
[0026] <<Cyclic olefin ring-opening polymerization unit>>
[0027] The cyclic olefin monomer that can be used to form the cyclic olefin ring-opening polymerization unit is not particularly limited, and examples thereof include monomers having a norbornene skeleton (hereinafter referred to as "norbornene-based monomers") and monocyclic cyclic olefin monomers, etc. The monomers may be used alone or in combination of two or more.
[0028] -Norbornene-based monomers-
[0029] Here, examples of the norbornene-based monomers include norbornene; norbornene-based monomers not having a ring condensed with a norbornene ring (hereinafter, sometimes referred to as “norbornene-based monomers not forming a condensed ring”); and norbornene-based monomers having a ring condensed with a norbornene ring (hereinafter, sometimes referred to as “norbornene-based monomers forming a condensed ring”).
[0030] Examples of the norbornene monomers that do not form a condensed ring include norbornenes having an alkyl group such as 5-methyl norbornene, 5-ethyl norbornene, 5-butyl norbornene, 5-hexyl norbornene, 5-decyl norbornene, 5-cyclohexyl norbornene, and 5-cyclopentyl norbornene; norbornenes having an alkenyl group such as 5-ethylidene norbornene, 5-vinyl norbornene, 5-propenyl norbornene, 5-cyclohexenyl norbornene, and 5-cyclopentenyl norbornene; norbornenes having an aromatic ring such as 5-phenyl norbornene; 5-methoxycarbonyl norbornene, 5-ethyl norbornene, 5-cyclohexenyl norbornene, and 5-cyclopentenyl norbornene; Norbornenes having a polar group containing an oxygen atom such as oxycarbonyl norbornene, 5-methyl-5-methoxycarbonyl norbornene, 5-methyl-5-ethoxycarbonyl norbornene, norbornene-2-methylpropionate, norbornene-2-methyloctanoate, 5-hydroxymethyl norbornene, 5,6-di(hydroxymethyl)norbornene, 5,5-di(hydroxymethyl)norbornene, 5-hydroxyisopropyl norbornene, 5,6-dicarboxynorbornene, 5-methoxycarbonyl-6-carboxynorbornene; norbornenes having a polar group containing a nitrogen atom such as 5-cyano norbornene, etc. These may be used alone or in combination of two or more.
[0031] Examples of the norbornene-based monomer that forms a condensed ring include monomers represented by the following formulae (I) and (II).
[0032] [Chemical formula 1]
[0033]
[0034] In the above formula (I), R 1 and R 2 Each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom (excluding a substituent belonging to a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent), and may be combined to form a ring. 3 It is a divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent.
[0035] [Chemical formula 2]
[0036]
[0037] In the above formula (II), R 4 , R 5 , R 6 , R 7Each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom (excluding a substituent belonging to a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent), R 4 and R 6 They may also combine to form a ring. m is 1 or 2.
[0038] Examples of the monomer represented by the formula (I) include dicyclopentadiene, methyldicyclopentadiene, dimethyldicyclopentadiene, tricyclo[5.2.1.0 2,6 ]Deca-8-ene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]tetradeca-3,5,7,12-tetraene (also known as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene), tetracyclo[10.2.1.0 2,11 .0 4,9 ] Pentadeca-4,6,8,13-tetraene (also called 1,4-methano-1,4,4a,9,9a,10-hexahydroanthracene). These may be used alone or in combination of two or more.
[0039] Examples of the monomer represented by the formula (II) include tetracyclododecenes in which m is 1 and hexacycloheptadecenes in which m is 2.
[0040] Examples of the tetracyclododecenes (m=1) include tetracyclododecene; tetracyclododecene having an alkyl group, such as 8-methyltetracyclododecene, 8-ethyltetracyclododecene, 8-cyclohexyltetracyclododecene, and 8-cyclopentyltetracyclododecene; tetracyclododecene having a double bond outside the ring, such as 8-methylenetetracyclododecene, 8-ethyltetracyclododecene, 8-vinyltetracyclododecene, 8-propenyltetracyclododecene, 8-cyclohexenyltetracyclododecene, and 8-cyclopentenyltetracyclododecene; tetracyclododecene having an aromatic ring, such as 8-phenyltetracyclododecene; and 8-methoxycarbonyltetracyclododecene. Tetracyclododecenes having a substituent containing an oxygen atom, such as 8-methyl-8-methoxycarbonyltetracyclododecene, 8-hydroxymethyltetracyclododecene, 8-carboxytetracyclododecene, tetracyclododecene-8,9-dicarboxylic acid, and tetracyclododecene-8,9-dicarboxylic anhydride; tetracyclododecenes having a substituent containing a nitrogen atom, such as 8-cyanotetracyclododecene and tetracyclododecene-8,9-dicarboxylic acid imide; tetracyclododecenes having a substituent containing a halogen atom, such as 8-chlorotetracyclododecene; tetracyclododecenes having a substituent containing a silicon atom, such as 8-trimethoxysilyltetracyclododecene, etc. These may be used alone or in combination of two or more.
[0041] Examples of the hexacycloheptadecene (m=2) include hexacycloheptadecene; hexacycloheptadecene having an alkyl group, such as 12-methylhexacycloheptadecene, 12-ethylhexacycloheptadecene, 12-cyclohexylhexacycloheptadecene, and 12-cyclopentylhexacycloheptadecene; hexacycloheptadecene having a double bond outside the ring, such as 12-methylenehexacycloheptadecene, 12-ethylhexacycloheptadecene, 12-vinylhexacycloheptadecene, 12-propenylhexacycloheptadecene, 12-cyclohexenylhexacycloheptadecene, and 12-cyclopentenylhexacycloheptadecene; hexacycloheptadecene having an aromatic ring, such as 12-phenylhexacycloheptadecene; and 12-methoxycarbonylhexacycloheptadecene. Hexacycloheptadecene having a substituent containing an oxygen atom, such as 12-methyl-12-methoxycarbonylhexacycloheptadecene, 12-hydroxymethylhexacycloheptadecene, 12-carboxyhexacycloheptadecene, hexacycloheptadecene-12,13-dicarboxylic acid, and hexacycloheptadecene-12,13-dicarboxylic anhydride; hexacycloheptadecene having a substituent containing a nitrogen atom, such as 12-cyanohexacycloheptadecene and hexacycloheptadecene-12,13-dicarboxylic acid imide; hexacycloheptadecene having a substituent containing a halogen atom, such as 12-chlorohexacycloheptadecene; hexacycloheptadecene having a substituent containing a silicon atom, such as 12-trimethoxysilylhexacycloheptadecene, and the like.
[0042] Among these, as the norbornene-based monomer, norbornene, dicyclopentadiene, and tetracyclododecene are preferred.
[0043] -Monocyclic cycloolefin monomers-
[0044] Examples of the monocyclic cycloolefin monomer include cyclopentene, cyclohexene, and cycloheptane. Among them, cyclopentene is preferred as the monocyclic cycloolefin monomer.
[0045] Furthermore, in the hydrogenated cyclic polymer of the present invention, it is preferred that the cyclic chain contain an ether bond. More specifically, it is preferred that the cyclic chain contain one ether bond.
[0046] <Hydrogenation rate>
[0047] The hydrogenation rate of the hydrogenated cyclic polymer of the present invention (the ratio of hydrogenated carbon-carbon double bonds to all carbon-carbon double bonds contained in the cyclic polymer as a precursor) is usually 90% or more, preferably 95% or more, and more preferably 99% or more. The hydrogenation rate (molar basis) of the hydrogenated cyclic polymer can be determined by measuring 1 confirmed by H-NMR.
[0048] In addition, the hydrogenation rate of the cyclic polymer hydrogenate can be adjusted by, for example, changing the conditions of the hydrogenation reaction.
[0049] <Weight Average Molecular Weight>
[0050] The weight average molecular weight of the hydrogenated cyclic polymer of the present invention is preferably 3,000 or more, more preferably 5,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less.
[0051] The weight average molecular weight of the hydrogenated cyclic polymer can be adjusted by, for example, changing the method for producing the hydrogenated cyclic polymer, for example, by changing the type and / or amount of the cyclic vinyl ether compound and catalyst added when preparing the cyclic polymer as a precursor of the hydrogenated cyclic polymer.
[0052] <Metal Content>
[0053] In the cyclic polymer hydride of the present invention, the metal content is preferably less than 10ppm, more preferably less than 5ppm, based on the total mass of the cyclic polymer hydride. As a metal, at least one selected from Ru, Mo, W and Ni can be cited. In addition, when the cyclic polymer hydride contains multiple metals, it is preferred that their total content is less than the above-mentioned upper limit. These metals come from the catalyst components that can be used arbitrarily when synthesizing the cyclic polymer as a precursor of the cyclic polymer hydride and / or when hydrogenating the cyclic polymer, and sometimes remain in the cyclic polymer hydride. In the cyclic polymer hydride of the present invention, if the metal content is less than the above-mentioned upper limit, high transparency can be obtained. In addition, the metal content in the cyclic polymer hydride can be obtained by inductively coupled plasma (ICP) emission spectrometry.
[0054] (Method for producing hydrogenated cyclic polymer)
[0055] The method for producing a cyclic polymer hydrogenate of the present invention is characterized by comprising: a ring-opening polymerization step of ring-opening polymerization of at least one cyclic olefin monomer in the presence of a cyclic vinyl ether compound to obtain a cyclic polymer comprising a cyclic chain consisting of repeating units of cyclic olefin ring-opening polymerization units; and a hydrogenation step of hydrogenating the cyclic polymer to obtain a cyclic polymer hydrogenate. According to the production method, the cyclic polymer hydrogenate of the present invention can be produced efficiently. In addition, after the hydrogenation step, post-treatment can be performed as needed.
[0056] <Ring-opening polymerization step>
[0057] In the ring-opening polymerization step, at least one cyclic olefin monomer is ring-opening polymerized in the presence of a cyclic vinyl ether compound to obtain a cyclic polymer containing a cyclic chain consisting of repeating units of cyclic olefin ring-opening polymerization units. More specifically, in the presence of a cyclic vinyl ether compound, a monomer composition containing at least one of the above-mentioned cyclic olefin monomers is ring-opening polymerized. In addition, in the ring-opening polymerization step, a catalyst can be added to the polymerization system. In addition, the ring-opening polymerization step can be carried out without a solvent or in the presence of a solvent.
[0058] <<Cyclic Vinyl Ether>>
[0059] The cyclic vinyl ether compound is a component that can function as a polymerization initiator in the ring-opening polymerization step. Examples of the cyclic vinyl ether compound include compounds represented by the following general formula (X).
[0060] [Chemical formula 3]
[0061]
[0062] In the above general formula (X), R and R' form a ring structure or one of R' and R" forms a ring structure with R'". Here, in the above general formula (X), R to R'" can each independently be a substituted or unsubstituted alkyl group having 12 or less carbon atoms, a trialkylsilyl group (wherein each alkyl group is each independently an alkyl group having 3 or less carbon atoms), or a substituted or unsubstituted alkoxy group having 12 or less carbon atoms.
[0063] Specifically, as the cyclic vinyl ether compound, for example, 2,3-dihydrofuran and its derivatives, 3,4-dihydro-2H-pyran and its derivatives, 1-(trimethylsilyloxy)cyclohexene and its derivatives, 1-(trimethylsilyloxy)cyclopentene and its derivatives, 1-methoxycyclooctene and its derivatives, 2,3,4,5-tetrahydrofuran and its derivatives, Tetrahydrooxepine and its derivatives, etc. Among them, 3,4-dihydro-2-methoxy-2H-pyran and 3,4-dihydro-2-ethoxy-2H-pyran, which are derivatives of 3,4-dihydro-2H-pyran, are preferred from the viewpoint of improving the yield.
[0064] <<Catalyst>>
[0065] As a catalyst that can be added to the polymerization system in the ring-opening polymerization step, a photoredox catalyst can be preferably used. Here, the photoredox catalyst refers to a compound that can generate free radicals when irradiated with light in the ultraviolet visible light region, such as visible light with a wavelength of 425 nm. As a photoredox catalyst that can be preferably used in the ring-opening polymerization step, for example, pyranose described in International Publication No. 2016 / 036976 can be cited. Salt and acridine In particular, pyranose can be preferably used as a photoredox catalyst in the ring-opening polymerization step. Salt. As pyran Salts include pyranose represented by the following formula (III): Salt.
[0066] [Chemical formula 4]
[0067]
[0068] In formula (III), R 8 Each independently represents hydrogen, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group. - represents a monovalent anion. In addition, the alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, or the aryl group may have a substituent.
[0069] Among them, multiple R 8 All are methoxy, X - For BF4 - , that is, the pyran represented by formula (III) The salt is 2,4,6-tri(4-methoxyphenyl)pyran Tetrafluoroborate.
[0070] In addition, the catalyst used in the ring-opening polymerization step preferably contains no metal.
[0071] <<Solvents>>
[0072] The ring-opening polymerization step is preferably carried out in a solvent, particularly an organic solvent, from the viewpoint of being able to well control the reaction.
[0073] The organic solvent used is not particularly limited as long as it can dissolve or disperse the obtained cyclic polymer therein and is inactive in the polymerization reaction. Specifically, examples include: aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; alicyclic hydrocarbon solvents such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, ethylcyclohexane, diethylcyclohexane, decahydronaphthalene, bicycloheptane, tricyclodecane, hexahydroindene, cyclohexane, and cyclooctane; aromatic hydrocarbon solvents such as benzene, toluene, and xylene (o-xylene, m-xylene, and p-xylene); halogenated aliphatic hydrocarbon solvents such as dichloromethane, chloroform, 1,2-dichloroethane, and 1,1,2,2-tetrachloroethane; halogenated aromatic hydrocarbon solvents such as chlorobenzene and dichlorobenzene; nitrogen-containing hydrocarbon solvents such as nitromethane, nitrobenzene, and acetonitrile; ether solvents such as diethyl ether and tetrahydrofuran; aromatic ether solvents such as anisole and phenethyl ether, etc. The solvent may be used alone or in combination of two or more. Furthermore, as the solvent, a halogenated aliphatic hydrocarbon solvent is particularly preferred.
[0074] In addition, the conditions of the ring-opening polymerization (the amount of each component used, the polymerization time and the polymerization temperature, etc.) are not particularly limited and can be appropriately set according to the physical properties of the desired cyclic polymer and the cyclic polymer hydrogenate. In addition, the cyclic polymer obtained in the ring-opening polymerization step can be recovered from the reaction solution and supplied to the hydrogenation reaction, or the reaction solution containing the cyclic polymer can be directly supplied to the hydrogenation step.
[0075] <<Ring-opening polymerization route>>
[0076] In one example, when a photoredox catalyst is used as a catalyst and 3,4-dihydro-2H-pyran which is a vinyl ether compound is used as a polymerization initiator, the ring-opening polymerization reaction is presumed to proceed along the following route.
[0077] [Chemical formula 5]
[0078]
[0079] First, for example, the above-mentioned pyran A photoredox catalyst such as a salt is excited by light irradiation and becomes capable of functioning as an electronic oxidant (not shown in the route). Then, 3,4-dihydro-2H-pyran is electronically oxidized by the electronic oxidant ((1) in the route) to become a radical cation ((2) in the route). In this way, the radical cation forms a four-membered ring structure with the cyclic olefin monomer present in the polymerization system to generate a radical cation intermediate ((3) in the route). The radical cation intermediate (3) thus generated undergoes a ring-opening metathesis reaction, and the resulting intermediate becomes a further radical cation ((4) in the route). The further radical cation (4) extends the cyclic chain of the cyclic polymer by sequentially reacting with n cyclic olefin monomers present in the polymerization system ((5) in the route). Then, the polymerization reaction is terminated by stopping the light irradiation, whereby the radical cation is electronically reduced ((6) in the route). As a result of this ring-opening polymerization reaction, a cyclic polymer having a vinyl ether bond in the cyclic chain is produced. The vinyl ether bond is derived from 3,4-dihydro-2H-pyran ((7) in the scheme) as a polymerization initiator.
[0080] <<Hydrogenation process>>
[0081] In the hydrogenation step, the cyclic polymer obtained through the above-mentioned ring-opening polymerization step is hydrogenated to obtain a hydride of the cyclic polymer. More specifically, in the hydrogenation step, at least a portion of the carbon-carbon double bonds of the cyclic chain of the cyclic polymer and the carbon-carbon double bonds including these when the cyclic polymer has carbon-carbon double bonds in addition to the cyclic chain are hydrogenated. In addition, in the hydrogenation step, it is preferred that the hydrogenation rate (molar basis) in the obtained hydride is 90% or more, preferably 95% or more, and preferably 99% or more. In addition, in the hydrogenation step, when the carbon-carbon double bonds of the vinyl ether bonds from the polymerization initiator contained in the cyclic polymer obtained through the above-mentioned ring-opening polymerization step are hydrogenated, the obtained hydride will contain a structural unit having an ether bond represented by "-COC-".
[0082] Here, in the hydrogenation step, the carbon-carbon double bonds present in the cyclic polymer can be hydrogenated by (a) adding a hydrogenating agent to the system containing the cyclic polymer obtained in the above step, followed by heating to react (hydrogen transfer type hydrogenation reaction), or (b) adding a hydrogenation catalyst, followed by adding hydrogen to react (catalytic hydrogenation reaction), without particular limitation.
[0083] The hydrogenating agent used in the above-mentioned (a) hydrogen transfer type hydrogenation reaction is not particularly limited, and any hydrogenating agent can be used as long as it can hydrogenate the carbon-carbon double bonds present in the cyclic polymer, and examples thereof include hydrazine and p-toluenesulfonyl hydrazide.
[0084] In addition, the hydrogenation catalyst used in the above-mentioned (b) catalytic hydrogenation reaction is not particularly limited, and a catalyst commonly used in the hydrogenation reaction of olefin compounds can be used. For example, cobalt acetate and triethylaluminum, nickel acetylacetonate and triisobutylaluminum, dichlorotitanocene and n-butyllithium, dichlorozirconocene and sec-butyllithium, tetrabutoxytitanate and dimethylmagnesium, etc., which are Ziegler catalysts composed of a combination of a transition metal compound and an alkali metal compound; dichlorotri(triphenylphosphine)rhodium, RuHCl(CO)(PPh3)3, RuHCl(CO)[P(p-Me-Ph)3]3, RuHCl(CO)(PCy3)2, RuHCl(CO)[P(n-Bu)3]3, RuHCl(CO)[P(i-Pr)3]2, RuH2(CO)(PPh3)3, RuH2(CO)[P(p- Homogeneous catalysts such as precious metal complex catalysts composed of ruthenium compounds such as RuH2(CO)(PPh3)3, RuH2(CO)(PCy3)3, RuH2(CO)[P(n-Bu)3]3, RuH(OCOCH3)(CO)(PPh3)2, RuH(OCOPh)(CO)(PPh3)2, RuH(OCOPh-CH3)(CO)(PPh3)2, RuH(OCOPh-OCH3)(CO)(PPh3)2, RuH(OCOPh)(CO)(PCy3)2; supported heterogeneous catalysts in which metals such as nickel, palladium, platinum, rhodium and ruthenium are supported on carriers such as carbon, silica, diatomaceous earth, alumina, and titanium oxide.
[0085] The hydrogenation catalyst may be used alone or in combination of two or more. In addition, as the hydrogenation catalyst, a supported heterogeneous catalyst is preferred because the hydrogenation catalyst can be easily removed by filtering the reaction solution after the hydrogenation reaction.
[0086] Specific preferred supported heterogeneous catalysts include combinations of nickel / silica, nickel / diatomaceous earth, nickel / alumina, palladium / carbon, palladium / silica, palladium / diatomaceous earth, palladium / alumina and the like.
[0087] <<Conditions of Hydrogenation Process>>
[0088] The conditions for the hydrogenation reaction (the amounts of the hydrogenating agent and hydrogenation catalyst used, the reaction time, the reaction temperature, and the hydrogen pressure during the catalytic hydrogenation reaction according to (b) above) are not particularly limited and can be appropriately set according to the desired physical properties of the hydrogenated cyclic polymer (e.g., hydrogenation rate).
[0089] The solvent used in the hydrogenation step is not particularly limited, and for example, the solvents listed as the solvents (particularly, organic solvents) that can be used in the above-mentioned ring-opening polymerization step can be used.
[0090] <Post-processing process>
[0091] After the above-mentioned ring-opening polymerization step and hydrogenation step, a post-treatment step can be performed as needed. In the post-treatment step, the reaction solution containing the cyclic polymer hydrogenate obtained in the above-mentioned hydrogenation step is treated by a coagulation drying method or a direct drying method using a thin film dryer, etc., thereby the target cyclic polymer hydrogenate can be well separated. In addition, the cyclic polymer hydrogenate can usually be obtained alone in a powdery or granular form.
[0092] (Resin composition)
[0093] The resin composition of the present invention contains the hydrogenated cyclic polymer of the present invention and can optionally contain known additives. Furthermore, the resin composition of the present invention can be advantageously used as a material for a molded article because it contains the hydrogenated cyclic polymer of the present invention.
[0094] Known additives are not particularly limited, and examples thereof include: polymers (thermoplastic elastomers, etc.) other than the cyclic polymer hydrogenate of the present invention, fillers, antioxidants, mold release agents, flame retardants, antibacterial agents, wood powder, coupling agents, plasticizers, colorants, lubricants, silicone oils, foaming agents, surfactants, light stabilizers, dispersing aids, heat stabilizers, ultraviolet absorbers, antistatic agents, dispersants, chlorine traps, crystal nucleating agents, antifogging agents, organic fillers, neutralizers, decomposers, metal passivators, and anti-pollution agents. These additives may be used alone or in combination of two or more.
[0095] In addition, the method for producing the resin composition is not particularly limited. For example, there can be mentioned a method of obtaining a granular resin composition by kneading a cyclic polymer hydrogenate and an additive added as required; a method of mixing a cyclic polymer hydrogenate and an additive added as required in a suitable solvent and removing the solvent to obtain a resin composition.
[0096] Example
[0097] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples. In the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.
[0098] In the Examples and Comparative Examples, the hydrogenation rate and weight average molecular weight of the obtained products were measured by the following methods. In addition, in the Examples and Comparative Examples, the analysis of the obtained products and the measurement of the metal content were performed by the following methods.
[0099] <Weight Average Molecular Weight>
[0100] The weight average molecular weight of the hydrogenated cyclic polymer was measured as a standard polystyrene conversion value obtained by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent. As a measuring apparatus, HLC8320GPC (manufactured by Tosoh Corporation) was used.
[0101] The sample was prepared by dissolving the measurement sample in tetrahydrofuran at room temperature so that the sample concentration became 1 mg / ml.
[0102] Four TSKgel Super Multipore HZ-H (manufactured by Tosoh Corporation) were connected in series as a column, and the measurement was performed under the conditions of a flow rate of 0.35 ml / min, an injection volume of 50 μl, and a column temperature of 40°C.
[0103] <Hydrogenation rate>
[0104] according to 1 More specifically, the ring-opening polymer obtained through the ring-opening polymerization step and the ring-opening polymer hydrogenated product obtained through the hydrogenation step were respectively subjected to 1 The amount of carbon-carbon double bonds contained in each ring-opening polymer (molar basis) was determined by H-NMR measurement, and the ratio (%) of the amount of carbon-carbon double bonds contained in the hydrogenated ring-opening polymer to the amount of carbon-carbon double bonds contained in the ring-opening polymer as 100% was calculated.
[0105] <Analysis of Products>
[0106] First, the obtained ring-opening polymer was used as a measurement sample. 1 H-NMR measurement. This measurement is used to determine whether the sample has a structure containing a cyclic olefin ring-opening polymerization unit and a vinyl ether portion as a repeating unit. Next, a time-of-flight mass spectrometer (MALDI (Matrix Assisted Laser Desorption / Ionization)-TOF (Time of Flight)-MS (Mass Spectrometer)) is used to measure the absolute molecular weight of the sample. When it is confirmed that the molecular weight of the mass peak of each polymer chain contained in the sample is (multiple of the molecular weight of the repeating unit) + (molecular weight of the polymerization initiator), the sample is identified as a cyclic polymer.
[0107] Next, the ring-opening polymer hydrogenated product obtained by hydrogenating the ring-opening polymer was used as a measurement sample. 1H-NMR measurement. This measurement is used to determine whether the measurement sample has a structure containing a cyclic olefin ring-opening polymerization hydride unit and an ether portion as a repeating unit. Next, the absolute molecular weight of the measurement sample is measured using a time-of-flight mass spectrometer. When it is confirmed that the molecular weight of the mass peak of each polymer chain contained in the measurement sample is (multiple of the molecular weight of the hydride of the repeating unit) + (molecular weight of the hydride of the polymerization initiator), the measurement sample is identified as a cyclic polymer.
[0108] In Example 5 in which a polymer having a relatively high molecular weight was obtained, in addition to the above analysis, analysis was performed using gel permeation chromatography-multiangle laser light scattering (GPC-MALLS), and it was confirmed that a cyclic polymer was obtained.
[0109] <Metal Content of Product>
[0110] Furthermore, the total content (ppm; hydride mass basis) of Ru, Mo, W and Ni was determined by inductively coupled plasma (ICP) emission spectrometry using the cyclic polymer hydride obtained in the examples as a measurement sample. The total content was confirmed to be 5 ppm or less in all the examples.
[0111] (Example 1)
[0112] <Ring-opening polymerization step>
[0113] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 34.6 mg of 3,4-dihydro-2H-pyran as a cyclic vinyl ether compound as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.01 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 9100. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 3,4-dihydro-2H-pyran as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of 3,4-dihydro-2H-pyran as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0114] <Hydrogenation process>
[0115] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0116] <Post-processing process>
[0117] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was 99% or more. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and that the vinyl group of 3,4-dihydro-2H-pyran as a polymerization initiator was hydrogenated and maintained an ether site. Next, the absolute molecular weight of the ring-opening polymer hydrogenate as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenate of norbornene as a cyclic olefin monomer) + (molecular weight of the hydrogenate of 3,4-dihydro-2H-pyran as a polymerization initiator). From these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0118] (Example 2)
[0119] <Ring-opening polymerization step>
[0120] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 36.1 mg of 2,3-dihydrofuran as a cyclic vinyl ether compound as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.01 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 10200. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 2,3-dihydrofuran as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of 2,3-dihydrofuran as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0121] <Hydrogenation process>
[0122] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0123] <Post-processing process>
[0124] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was 99% or more. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate of a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and that the vinyl group of 2,3-dihydrofuran as a polymerization initiator was hydrogenated and maintained an ether site. Next, the absolute molecular weight of the ring-opening polymer hydrogenate as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenate of norbornene as a cyclic olefin monomer) + (molecular weight of the hydrogenate of 2,3-dihydrofuran as a polymerization initiator). From these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0125] (Example 3)
[0126] <Ring-opening polymerization step>
[0127] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 35.2 mg of 3,4-dihydro-2-methoxy-2H-pyran, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.25 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 14700. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 3,4-dihydro-2-methoxy-2H-pyran as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of 3,4-dihydro-2-methoxy-2H-pyran as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0128] <Hydrogenation process>
[0129] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0130] <Post-processing process>
[0131] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was 99% or more. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and that the vinyl group of 3,4-dihydro-2-methoxy-2H-pyran as a polymerization initiator was hydrogenated and maintained an ether site. Next, the absolute molecular weight of the ring-opening polymer hydrogenate as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenate of norbornene as a cyclic olefin monomer) + (molecular weight of the hydrogenate of 3,4-dihydro-2-methoxy-2H-pyran as a polymerization initiator). From these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0132] (Example 4)
[0133] <Ring-opening polymerization step>
[0134] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 32.9 mg of 3,4-dihydro-2-ethoxy-2H-pyran, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.36 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 10600. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0135] <Hydrogenation process>
[0136] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0137] <Post-processing process>
[0138] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was 99% or more. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and that the vinyl group of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator was hydrogenated and the ether portion was retained. Next, the absolute molecular weight of the ring-opening polymer hydrogenate as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenate of norbornene as a cyclic olefin monomer) + (molecular weight of the hydrogenate of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator). From these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0139] (Example 5)
[0140] <Ring-opening polymerization step>
[0141] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 1.65 mg of 3,4-dihydro-2-ethoxy-2H-pyran, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.36 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 113,000. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator. Next, the obtained ring-opening polymer was compared with a linear polynorbornene using GPC-MALLS, and it was confirmed that the obtained ring-opening polymer was cyclic. Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0142] <Hydrogenation process>
[0143] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0144] <Post-processing process>
[0145] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was more than 99%. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of cyclic olefins, and that the vinyl group of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator was hydrogenated and maintained the ether portion. Next, using GPC-MALLS, the obtained ring-opening polymer hydrogenate was compared with the linear polynorbornene hydrogenate, and it was confirmed that the obtained ring-opening polymer hydrogenate was cyclic. Based on these results, it was confirmed that the ring-opening polymer hydrogenate obtained in this process was a cyclic polymer.
[0146] (Example 6)
[0147] <Ring-opening polymerization step>
[0148] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 3.9 mg of 1-(trimethylsiloxy)cyclohexene, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation with an LED lamp (wavelength 425 nm) was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.28 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 13200. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 1-(trimethylsiloxy)cyclohexene as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of 1-(trimethylsiloxy)cyclohexene as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0149] <Hydrogenation process>
[0150] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0151] <Post-processing process>
[0152] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was 99% or more. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and that the vinyl group of 1-(trimethylsiloxy)cyclohexene as a polymerization initiator was hydrogenated and maintained an ether site. Next, the absolute molecular weight of the ring-opening polymer hydrogenate as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenate of norbornene as a cyclic olefin monomer) + (molecular weight of the hydrogenate of 1-(trimethylsiloxy)cyclohexene as a polymerization initiator). From these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0153] (Example 7)
[0154] <Ring-opening polymerization step>
[0155] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 3.5 mg of 1-(trimethylsiloxy)cyclopentene, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation with an LED lamp (wavelength 425 nm) was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.41 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 11,000. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 1-(trimethylsiloxy)cyclopentene as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of 1-(trimethylsiloxy)cyclopentene as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0156] <Hydrogenation process>
[0157] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0158] <Post-processing process>
[0159] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was 99% or more. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and that the vinyl group of 1-(trimethylsiloxy)cyclopentene as a polymerization initiator was hydrogenated and maintained an ether site. Next, the absolute molecular weight of the ring-opening polymer hydrogenate as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenate of norbornene as a cyclic olefin monomer) + (molecular weight of the hydrogenate of 1-(trimethylsiloxy)cyclopentene as a polymerization initiator). From these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0160] (Example 8)
[0161] <Ring-opening polymerization step>
[0162] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 3.2 mg of 1-(methoxy)cyclooctene, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation with an LED lamp (wavelength 425 nm) was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.75 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 9400. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 1-(methoxy)cyclooctene as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of 1-(methoxy)cyclooctene as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0163] <Hydrogenation process>
[0164] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0165] <Post-processing process>
[0166] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was 99% or more. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and that the vinyl group of 1-(methoxy)cyclooctene as a polymerization initiator was hydrogenated and maintained an ether site. Next, the absolute molecular weight of the ring-opening polymer hydrogenate as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenate of norbornene as a cyclic olefin monomer) + (molecular weight of the hydrogenate of 1-(methoxy)cyclooctene as a polymerization initiator). From these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0167] (Example 9)
[0168] <Ring-opening polymerization step>
[0169] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of norbornene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 2.2 mg of 2,3,4,5-tetrahydrofuran (2,3,4,5-tetrahydrofuran) as a polymerization initiator was added. After stirring, light irradiation with an LED lamp (wavelength 425nm) was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction solution containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.75g. The weight-average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 9400. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure containing a cyclic olefin ring-opening polymerization unit formed by the ring-opening polymerization of cyclic olefins, and retained 2,3,4,5-tetrahydro Next, the absolute molecular weight of the ring-opening polymer as the measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiples of the molecular weight of norbornene as a cyclic olefin monomer) + (multiples of the molecular weight of 2,3,4,5-tetrahydrofuran as a polymerization initiator) Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0170] <Hydrogenation process>
[0171] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0172] <Post-processing process>
[0173] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was more than 99%. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by the ring-opening polymerization of cyclic olefins, and that 2,3,4,5-tetrahydro The vinyl group of heptane was hydrogenated while maintaining the ether part. Next, the absolute molecular weight of the hydrogenated ring-opening polymer as the measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenated norbornene as a cyclic olefin monomer) + (multiple of the molecular weight of the hydrogenated 2,3,4,5-tetrahydrofuran as a polymerization initiator). Based on these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0174] (Example 10)
[0175] <Ring-opening polymerization step>
[0176] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of dicyclopentadiene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 32.9 mg of 3,4-dihydro-2-ethoxy-2H-pyran, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.36 g. The weight average molecular weight of the obtained ring-opening polymer was measured as described above, and the result was 4300. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of dicyclopentadiene as a cyclic olefin monomer) + (molecular weight of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0177] <Hydrogenation process>
[0178] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0179] <Post-processing process>
[0180] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was more than 99%. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by the ring-opening polymerization of cyclic olefins, and that the vinyl group of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator was hydrogenated and maintained the ether portion. Next, the absolute molecular weight of the hydrogenated ring-opening polymer as the measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenated dicyclopentadiene as the cyclic olefin monomer) + (molecular weight of the hydrogenated 3,4-dihydro-2-ethoxy-2H-pyran as the polymerization initiator). Based on these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0181] (Example 11)
[0182] <Ring-opening polymerization step>
[0183] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were added and stirred. Next, a solution obtained by dissolving 1.0 g of norbornene and 0.75 g of dicyclopentadiene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 32.9 mg of 3,4-dihydro-2-ethoxy-2H-pyran, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.36 g. The weight average molecular weight of the obtained ring-opening polymer was measured as above, and the result was 5900. The obtained ring-opening polymer was subjected to <Product Analysis> as above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (the sum of the multiples of the molecular weight of norbornene as a cyclic olefin monomer and the multiples of the molecular weight of dicyclopentadiene) + (the molecular weight of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0184] <Hydrogenation process>
[0185] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0186] <Post-processing process>
[0187] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was more than 99%. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by the ring-opening polymerization of cyclic olefins, and that the vinyl group of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator was hydrogenated and maintained the ether portion. Next, the absolute molecular weight of the hydrogenated ring-opening polymer as the measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (the sum of the multiples of the molecular weight of the hydrogenated norbornene and the molecular weight of the hydrogenated dicyclopentadiene) + (the molecular weight of the hydrogenated 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator). Based on these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0188] (Example 12)
[0189] <Ring-opening polymerization step>
[0190] 5 mg of pyranose as a photoredox catalyst was added to a glass reactor equipped with a stirrer. 2,4,6-Tris(4-methoxyphenyl)pyran Tetrafluoroborate and 5 ml of dichloromethane as a solvent were stirred. Next, a solution obtained by dissolving 1.75 g of tetracyclododecene as a cyclic olefin monomer in 1.75 g of dichloromethane as a solvent was added and stirred. Next, 32.9 mg of 3,4-dihydro-2-ethoxy-2H-pyran, a cyclic vinyl ether compound, as a polymerization initiator was added, and after stirring, light irradiation (wavelength 425 nm) with an LED lamp was started to initiate the ring-opening metathesis polymerization reaction. After reacting at room temperature for 15 hours, a large amount of acetone was injected into the polymerization reaction liquid containing the ring-opening polymer as the reaction product to condense the precipitate, and the condensate containing the ring-opening polymer was filtered out. After washing the filtrate with methanol, it was dried under reduced pressure at 40°C for 24 hours. The yield of the obtained ring-opening polymer was 0.11 g. The weight average molecular weight of the obtained ring-opening polymer was measured as above, and the result was 3200. The obtained ring-opening polymer was subjected to <Product Analysis> as above. As a result, it was identified that the obtained ring-opening polymer had a structure including a cyclic olefin ring-opening polymerization unit formed by ring-opening polymerization of a cyclic olefin, and maintained the vinyl ether portion of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiples of the molecular weight of tetracyclododecene as a cyclic olefin monomer) + (molecular weight of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator). Based on these results, it was confirmed that the ring-opening polymer obtained in this step was a cyclic polymer.
[0191] <Hydrogenation process>
[0192] Next, 0.1 g of the ring-opening polymer (i.e., cyclic polymer) obtained in the ring-opening polymerization step and 0.8 g of p-toluenesulfonyl hydrazide as a hydrogenating agent were added to a glass reactor equipped with a stirrer. Then, 30 ml of p-xylene as a solvent was added, and a hydrogenation reaction was carried out at 125° C. for 5 hours to obtain a hydrogenation reaction liquid containing a ring-opening polymer hydrogenate (i.e., a cyclic polymer hydrogenate).
[0193] <Post-processing process>
[0194] The hydrogenation reaction liquid was injected into a large amount of acetone to completely precipitate the ring-opening polymer hydrogenate obtained through the hydrogenation process, and filtered and washed. Thereafter, the filtered and washed product was dried under reduced pressure at 40°C for 24 hours. The hydrogenation rate of the obtained ring-opening polymer hydrogenate was measured as described above, and the result was more than 99%. The obtained ring-opening polymer hydrogenate was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer hydrogenate had a structure of a hydrogenate containing a cyclic olefin ring-opening polymerization unit formed by the ring-opening polymerization of cyclic olefins, and that the vinyl group of 3,4-dihydro-2-ethoxy-2H-pyran as a polymerization initiator was hydrogenated and maintained the ether portion. Next, the absolute molecular weight of the hydrogenated ring-opening polymer as the measurement sample was measured using a time-of-flight mass spectrometer, and it was confirmed that the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of the hydrogenated tetracyclododecene as the cyclic olefin monomer) + (molecular weight of the hydrogenated 3,4-dihydro-2-ethoxy-2H-pyran as the polymerization initiator). Based on these results, it was confirmed that the hydrogenated ring-opening polymer obtained in this step was a cyclic polymer.
[0195] (Comparative Example 1)
[0196] As a polymerization initiator, 8.85 g of ethyl propene ether as a linear vinyl ether compound was added instead of the cyclic vinyl ether compound. The same method as in Example 1 was used to carry out the ring-opening polymerization step, the hydrogenation step and the post-treatment step. The yield of the ring-opening polymer obtained in the ring-opening polymerization step was 1.0 g. In addition, according to the results of the above measurement, the weight average molecular weight of the ring-opening polymer obtained in the ring-opening polymerization step was 44,000. The obtained ring-opening polymer was subjected to <Product Analysis> as described above. As a result, it was identified that the obtained ring-opening polymer had a structure containing a cyclic olefin ring-opening polymerization unit formed by the ring-opening polymerization of cyclic olefins, and maintained the vinyl ether part of ethyl propene ether as a polymerization initiator. Next, the absolute molecular weight of the ring-opening polymer as a measurement sample was measured using a time-of-flight mass spectrometer, and the molecular weight of the mass peak of each polymer chain was (multiple of the molecular weight of norbornene as a cyclic olefin monomer) + (molecular weight of ethyl propene ether as a polymerization initiator), and it was confirmed to be a chain polymer. Furthermore, the hydrogenation rate of the hydrogenated product obtained through the hydrogenation step and the post-treatment step was 99% or more. In addition, the solid content obtained by pressure drying in the post-treatment step did not contain a cyclic polymer hydrogenate, and the proportion of the cyclic polymer hydrogenate was 0%.
[0197] According to Examples 1 to 12, hydrogenated cyclic polymers including a cyclic chain composed of repeating units of cyclic olefin ring-opening polymerization units were obtained.
[0198] Furthermore, from Comparative Example 1, it is understood that when a linear vinyl ether compound is used as a polymerization initiator instead of a cyclic vinyl ether compound, a hydrogenated cyclic polymer cannot be obtained.
[0199] Industrial Applicability
[0200] According to the present invention, a hydrogenated cyclic polymer having a novel structure can be provided. In addition, according to the present invention, a resin composition containing the hydrogenated cyclic polymer having a novel structure can be provided.
Claims
1. A hydrogenated product of a cyclic polymer comprising a cyclic chain composed of repeating units of a cyclic olefin ring-opening polymerization unit, wherein the cyclic chain of the cyclic polymer comprises one ether bond.
2. A method for producing a cyclic polymer hydrogenate, the method comprising: a ring-opening polymerization step of ring-opening polymerizing at least one cyclic olefin monomer in the presence of a cyclic vinyl ether compound to obtain a cyclic polymer comprising a cyclic chain consisting of repeating units of cyclic olefin ring-opening polymerization units; as well as The hydrogenation step is to hydrogenate the cyclic polymer to obtain a hydrogenated product of the cyclic polymer.
3. The method for producing a hydrogenated cyclic polymer according to claim 2, wherein: The cyclic chain of the cyclic polymer obtained by the ring-opening polymerization step includes an ether bond. A resin composition comprising the hydride according to claim 1.