Generation and use of dynamic state diagrams when growing single crystal silicon ingots

By introducing dynamic state charts and control units into the ingot growth system, the problem of difficulty in monitoring and controlling growth parameters in the continuous Chuklasky process is solved, and rapid adjustment of ingot growth parameters and improved system stability are achieved.

CN114341407BActive Publication Date: 2024-11-15GLOBALWAFERS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080061399.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-29
Filing Date
2020-07-28
Publication Date
2024-11-15
Estimated Expiration
2040-07-28

AI Technical Summary

Technical Problem

In the continuous Chuklasky process, the growth parameters of single crystal silicon ingots are difficult to monitor and control, resulting in difficult to maintain the system equilibrium state and affecting the quality of the ingot.

Method used

An ingot growth system containing a control unit of a processor and memory is designed, which can monitor and adjust multiple growth parameters in real time, and provides visual output through dynamic state charts to help operators quickly understand and adjust ingot growth parameters.

Benefits of technology

Through the use of dynamic state charts, operators can quickly access and adjust ingot growth parameters, improving the quality of ingots and the stability of the system, and simplifying the ingot growth process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114341407B_ABST
    Figure CN114341407B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for growing a single crystal silicon ingot. A dynamic state chart that monitors multiple ingot growth parameters can be generated and used during the manufacture of a single crystal silicon ingot. In some embodiments, the dynamic state chart is a dynamic pie chart having multiple sections, wherein each section monitors an ingot growth parameter.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 879,829, filed on July 29, 2019, the entirety of which is incorporated herein by reference. Technical Field

[0003] The field of the present disclosure relates to methods for growing single crystal silicon ingots, and in particular, to the generation and use of dynamic state diagrams that monitor multiple ingot growth parameters. Background Art

[0004] Single crystal silicon ingots may be grown in a Czochralski process in which an ingot is pulled from a silicon melt within an ingot puller system. The grown single crystal ingot involves several growth parameters that are monitored to ensure successful growth (e.g., to achieve a target ingot diameter without forming dislocations in the ingot). This is particularly true for a continuous Czochralski process in which the ingot is continuously grown by adding silicon to the melt during ingot growth. Continuous Czochralski is particularly sensitive to changes in various ingot growth parameters and difficult to control. Small changes in one parameter can cascade to other parameters, which can cause the system to lose its equilibrium state.

[0005] There is a need for systems and methods that allow monitoring and / or control of various ingot growth parameters and / or provide a visual output of the parameters that is easily accessible to an operator and provides a simple visual overview of the ingot growth system.

[0006] This section is intended to introduce the reader to various aspects of the art that may be related to the various aspects of the present disclosure described and / or claimed below. It is believed that this discussion is helpful in providing the reader with background information to facilitate a better understanding of the various aspects of the present disclosure. Therefore, it should be understood that these statements should be read in this sense and not as an admission of prior art. Summary of the invention

[0007] One aspect of the present disclosure relates to a method for growing a single crystal silicon ingot in a Czochralski process. A silicon melt is prepared in a crucible. A single crystal silicon ingot is extracted from the melt. A plurality of growth parameters associated with the growth of the single crystal silicon ingot are provided. A dynamic state diagram containing a visual representation of the growth parameters is provided.

[0008] Another aspect of the present disclosure relates to an ingot growth system for manufacturing a single crystal silicon ingot. The system includes a growth chamber and a crucible disposed in the growth chamber. The crucible is configured to hold a melt including molten silicon. The system includes an ingot pulling mechanism for extracting an ingot from the melt. The system includes a control unit including a processor and a memory. The memory stores instructions that, when executed by the processor, cause the processor to determine a plurality of growth parameters associated with the growth of the single crystal silicon ingot and provide a dynamic state chart including a visual representation of the growth parameters to a user.

[0009] There are various improvements to the features set forth with respect to the above-mentioned aspects of the present disclosure. Likewise, further features may also be incorporated into the above-mentioned aspects of the present disclosure. These improvements and additional features may exist individually or in any combination. For example, the various features discussed below with respect to any of the illustrated embodiments of the present disclosure may be incorporated into any of the above-mentioned aspects of the present disclosure individually or in any combination. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 is a cross section of an example ingot growth system;

[0011] Figure 2 is a schematic diagram of a control system for controlling and / or monitoring ingot growth;

[0012] Figure 3 is a schematic diagram of a system for receiving measurements from one or more sensors of an ingot growth system;

[0013] Figure 4 is a schematic diagram of an operation device for controlling an ingot growth system;

[0014] Figure 5 is a schematic diagram of a control system for controlling and / or monitoring ingot growth;

[0015] Figure 6 is a dynamic state diagram comprising four sections, wherein each section is associated with an ingot growth parameter; and

[0016] Figure 7 is a dynamic state diagram comprising seven sections, wherein each section is associated with an ingot growth parameter.

[0017] Corresponding reference characters indicate corresponding parts throughout the drawings. DETAILED DESCRIPTION

[0018] The present disclosure provides methods and systems for growing a single crystal silicon ingot. In an example method, a dynamic state diagram containing a visual representation of multiple growth parameters is provided. The dynamic state diagram may be described herein as being used in a continuous Czochralski process in which polycrystalline silicon is added to a crucible continuously or intermittently. The dynamic state diagram may also be used in a batch Czochralski system.

[0019] exist Figure 1 6 shows an example ingot growth system 5 for making an ingot 60 by a continuous Czochralski process. The ingot growth system 5 includes a crucible assembly 10 having a plurality of weirs 20, 30, 40 or fluid barriers that separate the melt into different melt zones. In the illustrated embodiment, the crucible assembly 10 includes a first weir 20 (broadly, a fluid barrier) that defines an inner melt zone 22 of a silicon melt. The inner melt zone 22 is a growth region from which a single crystal silicon ingot 60 is grown. A second weir 30 defines an intermediate melt zone 32 of the silicon melt. A third weir 40 defines an outer melt zone 42 of the silicon melt.

[0020] Feed tube 46 feeds polycrystalline silicon (which may be in granular, chunky, or a combination of granular and chunky) into outer melt zone 42 at a rate sufficient to maintain a substantially constant melt height level and volume during growth of ingot 60. First weir 20, second weir 30, and third weir 40 each have a generally annular shape and have at least one opening defined therein to allow molten silicon to flow radially inwardly toward a growth area of ​​inner melt zone 22.

[0021] Figure 1 The crucible configuration depicted in is exemplary and suitable for practicing the process of the present disclosure. Other configurations suitable for continuous Czochralski may be used without departing from the scope of the present disclosure. For example, the crucible assembly 10 may be devoid of the second weir 30 and / or may be devoid of the third weir 40.

[0022] In general, the melt from which the ingot 60 is drawn is formed by loading polycrystalline silicon into a crucible to form an initial silicon charge. In general, the initial charge is between about 100 kg and about 200 kg of polycrystalline silicon, which may be granular, chunky, or a combination of granular and chunky. The mass of the initial charge depends on the desired crystal diameter and the hot zone design. The initial charge does not reflect the length of the crystal because the polycrystalline silicon is fed continuously during crystal growth. For example, if the polycrystalline silicon is fed continuously and the chamber has sufficient height, the crystal length may extend to a length of 2000 mm, 3000 mm, or even 4000 mm.

[0023] Various sources of polycrystalline silicon may be used, including, for example, granular polycrystalline silicon produced by thermal decomposition of silane or halosilane in a fluidized bed reactor or polycrystalline silicon produced in a Siemens reactor. Once the polycrystalline silicon is added to the crucible to form a charge, the charge is heated to a temperature above about the melting temperature of silicon (e.g., about 1412° C.) to melt the charge, and thereby form a silicon melt comprising molten silicon. The silicon melt has an initial volume of molten silicon and has an initial melt height level, and these parameters are determined by the size of the initial charge. In some embodiments, the crucible comprising the silicon melt is heated to a temperature of at least about 1425° C., at least about 1450° C., or even at least about 1500° C.

[0024] A pulling mechanism 114 is provided within the system 5 for growing and pulling the ingot 60 from the melt within the internal melt zone 22. The pulling mechanism 114 includes a pulling cable 118, a seed holder or chuck 120 coupled to one end of the pulling cable 118, and a seed 122 for initiating crystal growth coupled to the seed holder or chuck 120. One end of the pulling cable 118 is connected to a pulley (not shown) or a drum (not shown) or any other suitable type of lifting mechanism (e.g., a shaft), and the other end is connected to the chuck 120 holding the seed 122. In operation, the seed 122 is lowered to contact the melt in the internal melt zone 22. The pulling mechanism 114 is operated to cause the seed 122 to rise along the pulling axis A. This causes the single crystal silicon ingot 60 to be pulled from the melt.

[0025] Once the charge is liquefied to form a silicon melt including molten silicon, the silicon seed 122 is lowered to contact the melt within the internal melt zone 22. The silicon seed 122 is then extracted from the melt, wherein silicon is attached to the silicon seed 122 to form a neck 52, thereby forming a melt-solid interface near or at the surface of the melt. Generally speaking, the initial pull speed for forming the neck 52 is high. In some embodiments, the silicon seed 122 and the neck 52 are extracted at a neck portion pull rate of at least about 1.0 mm / min, such as between about 1.5 mm / min and about 6 mm / min, such as between about 3 mm / min and about 5 mm / min. The neck 52 may have a length between about 300 mm and about 700 mm, such as between about 450 mm and about 550 mm. However, the length of the neck 52 may vary outside these ranges.

[0026] The pulling mechanism 114 can rotate the seed crystal 122 and the ingot 60 connected thereto. The crucible drive unit 44 can rotate the crucible assembly 10. In some embodiments, the silicon seed crystal 122 and the crucible assembly 10 are rotated in opposite directions, that is, counter-rotated. Counter-rotation realizes convection in the silicon melt. The rotation of the seed crystal 122 is mainly used to provide a symmetrical temperature profile, suppress the angular variation of impurities and also control the crystal melt interface shape. In some embodiments, the silicon seed crystal 122 is rotated at a rate between about 5rpm and about 30rpm, or between about 5rpm and about 20rpm, or between about 8rpm and about 20rpm, or between about 10rpm and about 20rpm. In some embodiments, the crucible assembly 10 is rotated at a rate between about 0.5rpm and about 10rpm, or between about 1rpm and about 10rpm, or between about 4rpm and about 10rpm, or between about 5rpm and about 10rpm. In some embodiments, the seed crystal 122 is rotated at a rate faster than the crucible assembly 10. In some embodiments, the seed crystal 122 is rotated at a rate that is at least 1 rpm higher than the rotation rate of the crucible assembly 10 , such as at least about 3 rpm higher or at least about 5 rpm higher.

[0027] After forming the neck 52, an outwardly flared seed-cone portion 54 is grown adjacent the neck 52. Generally, the pull rate is reduced from the neck portion pull rate to a rate suitable for growing the outwardly flared seed-cone portion 54. For example, the seed-cone pull rate during the growth of the outwardly flared seed-cone may be between about 0.5 mm / minute and about 2.0 mm / minute, such as about 1.0 mm / minute. In some embodiments, the outwardly flared seed-cone 54 has a length between about 100 mm and about 400 mm, such as between about 150 mm and about 250 mm. The length of the outwardly flared seed-cone 54 may vary outside of these ranges. In some embodiments, the outwardly flared seed-cone 54 is grown to a terminal diameter of about 150 mm, at least about 150 mm, about 200 mm, at least about 200 mm, about 300 mm, at least about 300 mm, about 450 mm, or even at least about 450 mm. The terminal diameter of the flared seed-cone 54 is generally equivalent to the diameter of the constant diameter of the main body 56 of the single crystal silicon ingot 60 .

[0028] After forming the neck 52 and the outwardly flared seed-cone 54 adjacent the neck 52, a constant diameter portion 56 or "body" is then grown. The diameter of the body 56 can vary and in some embodiments, the diameter can be about 150 mm, at least about 150 mm, about 200 mm, at least about 200 mm, about 300 mm, at least about 300 mm, about 450 mm, or even at least about 450 mm. The body 56 of the single crystal silicon ingot 60 is ultimately grown to be at least about 1000 mm long, such as at least 1400 mm long, such as at least 1500 mm long, or at least 2000 mm long, or at least 2200 mm (e.g., 2200 mm), or at least about 3000 mm long, or at least about 4000 mm long.

[0029] As the ingot 60 is pulled from the melt, silicon is added to the outer melt zone 42 through a tube 46 or other passage to replenish the melt in the ingot growth system 5. Solid polysilicon may be added from a polysilicon feed system 66 and may be added continuously or intermittently to the ingot growth system 5 to maintain the melt level. In general, polysilicon may be metered into the ingot growth system 5 by any method available to one skilled in the art.

[0030] In some embodiments, dopants are also added to the melt during ingot growth. The dopants may be introduced from a dopant feed system 72. The dopants may be added as a gas or a solid and may be added to the outer melt zone 42.

[0031] The system 5 may include a heat shield 116 disposed about the ingot 60 to allow the growing ingot 60 to radiate its latent heat of solidification and heat flux from the melt. The heat shield 116 may be at least partially conical in shape and angled downward to create an annular opening in which the ingot 60 is disposed. A flow of an inert gas 64, such as argon, is typically provided along the length of the growing crystal. The ingot 60 is pulled through a growth chamber 78 that is sealed and isolated from the surrounding atmosphere.

[0032] A plurality of independently controlled annular bottom heaters 70 may be disposed in a radial pattern below the crucible assembly 10. The annular bottom heaters 70 apply heat in a relatively controlled distribution across the entire base surface area of ​​the crucible assembly 10. The annular base heaters 70 may be individually controlled planar resistive heating elements, as described in U.S. Pat. No. 7,635,414, which is incorporated herein by reference for all relevant and consistent purposes. The system 5 may include one or more side heaters 74 disposed radially outward of the crucible assembly 10 to control the temperature distribution throughout the melt.

[0033] Figure 1 The ingot growth system 5 shown in and described herein is exemplary and generally any system in which an ingot is produced by a continuous Czochralski process may be used unless otherwise stated.

[0034] The system 5 for manufacturing the silicon ingot 60 may include a control system 80 ( Figure 2 ). The system 80 may include a control unit 82 that controls the ingot growth system 5 based on user input and sensors that detect one or more parameters related to crystal growth. For example, a temperature sensor 84 (e.g., a phototube (or pyrometer)) measures the temperature of the melt at its surface. A diameter transducer 86 measures the diameter of the ingot 60. A level sensor measures the level of the melt in the ingot growth system 5. A weight sensor 96 may be used to measure the crucible weight or the ingot weight. The control unit 82 may also be communicatively connected to a user interface 88, where an operator may input one or more commands (e.g., set points) for controlling ingot growth. The system 5 may include other inputs and / or sensors 92, including system power, current, vacuum, length, travel, position, speed, distance, rotation, flow, pressure, volume, and / or weight.

[0035] The control unit 82 is used to adjust a plurality of process parameters, including, but not limited to, at least one of the crystal rotation rate, the crucible rotation rate, the ingot diameter, and the melt temperature. The control unit 82 may control the heater power supply 123 to control the heat output of the bottom heater 70 (which may also be independently controlled) and / or the side heater 74. The control unit 82 is communicatively connected to the pulling mechanism 114 to control the pulling rate and / or the rotation rate of the ingot 60 and to the crucible drive unit 44 to adjust the rotation rate of the crucible assembly 10. The control unit 82 may also control the polysilicon feed system 66 to adjust the rate at which polysilicon is added to the melt. The control unit 82 may also be connected to the dopant feed system 72 to adjust the addition of dopants to the melt. The control unit 82 may also control one or more pumps and valves to control the growth chamber pressure and / or filter cleaning. The control unit 82 may control the system 5 by using one or more algorithms (e.g., algorithms stored and / or executed by the control unit 82). Although one control unit 82 is shown, the system 80 may include two or more control units 82 for controlling one or more ingot growth parameters.

[0036] In various embodiments, the control unit 82 may include a processor that processes signals received from various sensors of the system 5 (including but not limited to the temperature sensor 84, the diameter transducer 86, and the level sensor 90), as well as one or more devices that control the system 5 (including but not limited to the crucible drive unit 44, the pulling mechanism 114, the heater power supply 123, the vacuum pump 131, the gas flow regulator 129, the polycrystalline feed system 66, the dopant feed system 72, and any combination thereof).

[0037] The control unit 82 may be a computer system. As described herein, a computer system refers to any known computing device and computer system. As described herein, all such computer systems include a processor and a memory. However, any processor in a computer system mentioned herein may also refer to one or more processors, wherein the processor may be in one computing device or multiple computing devices acting in parallel. In addition, any memory in a computer device mentioned herein may also refer to one or more memories, wherein the memory may be in one computing device or multiple computing devices acting in parallel.

[0038] The term processor as used herein refers to a central processing unit, a microprocessor, a microcontroller, a reduced instruction set circuit (RISC), an application specific integrated circuit (ASIC), a logic circuit, and any other circuit or processor capable of performing the functions described herein. The above is merely an example and is therefore not intended to limit the definition and / or meaning of the term "processor" in any way.

[0039] As used herein, the term "database" may refer to a body of data, a relational database management system (RDBMS), or both. As used herein, a database may include any collection of data, including hierarchical databases, relational databases, flat file databases, object-relational databases, object-oriented databases, and any other structured collection of records or data stored in a computer system. The above examples are merely examples and are therefore not intended to limit the definition and / or meaning of the term database in any way. Examples of RDBMS include, but are not limited to, Database, MySQL, DB2, SQL Server, and PostgreSQL. However, any database that implements the systems and methods described herein may be used. (Oracle is a registered trademark of Oracle Corporation of Redwood Shore, California; IBM is a registered trademark of International Business Machines Corporation of Armonk, New York; Microsoft is a registered trademark of Microsoft Corporation of Redmond, Washington; and Sybase is a registered trademark of Sybase of Dublin, California.)

[0040] In one embodiment, a computer program is provided to enable the control unit 82 and is embodied on a computer readable medium. In an example embodiment, the computer system executes on a single computer system without being connected to a server computer. In a further embodiment, the computer system executes on a single computer system without being connected to a server computer. In another embodiment, the computer system is running in a host environment and The computer system may be operated in a server environment (UNIX is a registered trademark of X / Open Ltd. located in Reading, Berkshire, United Kingdom). Alternatively, the computer system operates in any suitable operating system environment. The computer program is flexible and designed to operate in a variety of different environments without compromising any primary functionality. In some embodiments, the computer system includes multiple components distributed among multiple computing devices. One or more components may be in the form of computer executable instructions embodied in a computer readable medium.

[0041] The computer systems and processes are not limited to the specific embodiments described herein. In addition, each component of the computer system and each process can be practiced independently and separately from other components and processes described herein. Each component and process can also be used in combination with other assembly packages and processes.

[0042] In one embodiment, the computer system may be configured as a server system. Figure 3 An example configuration of a server system 301 is illustrated for receiving measurements from one or more sensors (including but not limited to temperature sensor 84, diameter transducer 86, and level sensor 90, and any combination thereof) and controlling one or more devices of a system 5 (including but not limited to crucible drive unit 44, pull mechanism 114, heater power supply 123, feed system 66, vacuum pump 131, gas flow regulator 129, dopant feed system 72, and as described herein and in Figures 1 to 2 Any combination thereof described in the embodiments of the present invention). Figure 3 , the server system 301 may also include (but is not limited to) a database server. In this example embodiment, the server system 301 performs all steps for controlling one or more devices of the system 80 as described herein.

[0043] Server system 301 includes processor 305 for executing instructions. For example, the instructions may be stored in memory 310. Processor 305 may include one or more processing units (e.g., in a multi-core configuration) for executing instructions. The instructions may be executed on a variety of different operating systems (e.g., UNIX, LINUX, Microsoft It should also be appreciated that various instructions may be executed during initialization after initiating the computer-based method. Some operations may be required in order to perform one or more processes described herein, while other operations may be more general and / or specific to a particular programming language (e.g., C, C#, C++, Java, or any other suitable programming language).

[0044] The processor 305 is operably coupled to the communication interface 315, enabling the server system 301 to communicate with a remote device, such as a user system or another server system 301. For example, the communication interface 315 may receive a request (e.g., a request to provide an interactive user interface for receiving sensor input and controlling one or more devices of the system 80) from a client system via the Internet.

[0045] The processor 305 is also operably coupled to a storage device 134. The storage device 134 is any computer operating hardware suitable for storing and / or retrieving data. In some embodiments, the storage device 134 is integrated in the server system 301. For example, the server system 301 may include one or more hard disk drives as the storage device 134. In other embodiments, the storage device 134 is external to the server system 301 and can be accessed by multiple server systems 301. For example, the storage device 134 may include multiple storage units, such as hard disks or solid-state disks in a redundant array of inexpensive disks (RAID) configuration. The storage device 134 may include a storage area network (SAN) and / or a network attached storage (NAS) system.

[0046] In some embodiments, the processor 305 is operably coupled to the storage device 134 via a storage interface 320. The storage interface 320 is any component capable of providing access to the storage device 134 to the processor 305. The storage interface 320 may include, for example, an Advanced Attachment Technology (ATA) adapter, a Serial ATA (SATA) adapter, a Small Computer System Interface (SCSI) adapter, a RAID controller, a SAN adapter, a network adapter, and / or any component that provides access to the storage device 134 to the processor 305.

[0047] Memory 310 may include, but is not limited to, random access memory (RAM), such as dynamic RAM (DRAM) or static RAM (SRAM), read-only memory (ROM), erasable programmable read-only memory (EPROM), electrically erasable programmable read-only memory (EEPROM), and non-volatile RAM (NVRAM). The above memory types are merely exemplary and thus do not limit the types of memory that can be used for storage of computer programs.

[0048] In another embodiment, the computer system may be a computing device (e.g., computing device 402 ( Figure 4 4. The computing device 402 includes a processor 404 for executing instructions. In some embodiments, the executable instructions are stored in a memory 406. The processor 404 may include one or more processing units (e.g., in a multi-core configuration). The memory 406 is any device that allows information (e.g., executable instructions and / or other data) to be stored and retrieved. The memory 406 may include one or more computer-readable media.

[0049] In another embodiment, the memory contained in the computing device of the control unit 143 may include multiple modules. Each module may include instructions configured to be executed using at least one processor. The instructions contained in the multiple modules may implement at least a portion of the method for simultaneously adjusting multiple process parameters as described herein when executed by one or more processors of the computing device. Non-limiting examples of modules stored in the memory of the computing device include: a first module for receiving measurements from one or more sensors and a second module for controlling one or more devices of the system 80.

[0050] The computing device 402 also includes a media output component 408 for presenting information to the user 400. The media output component 408 is any component capable of conveying information to the user 400. In some embodiments, the media output component 408 includes an output adapter, such as a video adapter and / or an audio adapter. The output adapter is operably coupled to the processor 404 and is further configured to be operably coupled to an output device, such as a display device (e.g., a liquid crystal display (LCD), an organic light emitting diode (OLED) display, a cathode ray tube (CRT), or an "electronic ink" display) or an audio output device (e.g., a speaker or headphones).

[0051] In some embodiments, the client computing device 402 includes an input device 410 for receiving input from the user 400. The input device 410 may include, for example, a keyboard, a pointing device, a mouse, a stylus, a touch-sensitive panel (e.g., a touch pad or touch screen), a camera, a gyroscope, an accelerometer, a position detector, and / or an audio input device. A single component (e.g., a touch screen) may serve as both an output device of the media output component 408 and an input device 410.

[0052] The computing device 402 may also include a communication interface 412 configured to be communicatively coupled to a remote device, such as the server system 301 or a website server. The communication interface 412 may include, for example, a wired or wireless network adapter or a wireless data transceiver for use with a mobile phone network, such as the Global System for Mobile Communications (GSM), 3G, 4G, 5G, or Bluetooth, or other mobile data networks, such as the Worldwide Interoperability for Microwave Access (WIMAX).

[0053] For example, computer readable instructions for providing a user interface to a user 400 via a media output component 408 and optionally receiving and processing input from an input device 410 are stored in the memory 406. The user interface may include a web browser and an application, among other possibilities. The web browser enables the user 400 to display and interact with media and other information, typically embedded on a web page or website from a website server. The application allows the user 400 to interact with a server application. The user interface facilitates the display of information related to the process of manufacturing a single crystal silicon ingot with a low oxygen content via one or both of a web browser and an application.

[0054] In some embodiments and Figure 5 , control unit 82 includes processor 404 and memory 406. Memory 406 stores instructions that, when executed by processor 404, cause processor 404 to determine a plurality of growth parameters associated with the growth of single crystal silicon ingot 60. Processor 404 may also display a dynamic state diagram 504 ( Figure 6 ) are provided to users, as discussed below.

[0055] In some embodiments, the control system 80 ( Figure 2 ) is configured to provide a plurality of growth parameters related to the growth of the single crystal silicon ingot 60 to the user. Figure 5 As shown in FIG. 1 , the control system 80 may be configured to receive information from the sensor system 94 (which may include Figure 2 The input device 410 can also communicate to the control unit 82. The control unit 82 can, for example, Figure 5 The media output 408 shown in FIG. 1 is communicatively connected to the user interface 88. The user interface 88 includes a plurality of growth parameters related to the growth of the single crystal silicon ingot. The user interface 88 may include visual media (e.g., a screen that displays information and / or is capable of accepting information from a user). The user interface may include a program, an application, and / or a web browser or the like.

[0056] In some embodiments, the control system 80 for modifying, changing or controlling the ingot growth system 5 includes a control unit 82 that is different from the control unit used to generate the dynamic state diagram described below. In other embodiments, the control system 80 for modifying, changing or controlling the ingot growth system 5 is part of the same system (i.e., uses the same control unit 82) that generates a user interface 88 including the dynamic state diagram. The user interface 88 may include a development environment, such as Microsoft Visual Studio, Oracle Java, Siemens Wincc, Wonderware Intouch, or the like. The development environment is used to generate features of the interface. A program (e.g., a runtime application) runs on a machine (e.g., a computer or server) to provide the user interface 88.

[0057] In some embodiments, the user interface 88 includes or otherwise displays a dynamic state chart that can be viewed by a user. For example, the dynamic state chart can provide a visual (e.g., graphical) representation of multiple growth parameters that change in response to changes in growth parameters. Figure 6 An example dynamic state chart 504 is shown in FIG. The example dynamic state chart 504 is a circular state chart divided into segments 518, 528, 538, 548. Each segment is associated with a different growth parameter. Figure 6 , but the state diagram 504 may include more or fewer segments associated with ingot growth parameters (e.g., 2 or more segments, 3 or more, 4 or more, 5 or more, 6 or more, 8 or more, or 10 or more segments). Suitable ingot growth parameters that may be associated with the segments of the dynamic state diagram 504 include, for example and without limitation, ingot target length, ingot diameter, seed lift speed, distance between heat shield and melt surface (i.e., heat shield position), polycrystalline feed rate to crucible (as in a continuous Czochralski system), dopant feed rate to crucible, ingot puller pressure, ingot growth rate (e.g., radial growth rate in the crown), or the like.

[0058] In some embodiments, the circular state diagram may have one or more dynamic features. For example, one or more segments 518, 528, 538, 548 may change size in response to a change in the value of a corresponding ingot growth parameter. Each segment 518, 528, 538, 548 may have a rotational velocity from the center C of the circular state diagram. 504 Extending to the respective outer edges E of segments 518, 528, 538, 548 518 、E 528 、E 538 、E 548 The radius R 518 , R 528 , R538 , R 548 Radius R 518 , R 528 , R 538 , R 548 changes in response to a change in the value of a growth parameter.

[0059] One or more of the segments 518, 528, 538, 548 of the circular state chart 504 may include a minimum growth parameter visual 520 and / or a maximum growth parameter visual 525. In the illustrated embodiment, the minimum growth parameter visual 520 is a first arc and the maximum growth parameter visual 525 is a second arc disposed radially outward from the first arc. The first and second arcs 520, 525 define an annular segment 530. The annular segment 530 may represent an acceptable range for the respective growth parameter.

[0060] In the illustrated embodiment, the dynamic state chart 504 also includes a target growth parameter visual 540. The target growth parameter visual 540 can be associated with each segment and represents the target value of the corresponding growth parameter. The target growth parameter visual 540 can be as follows: Figure 6 The third arc shown in .

[0061] The ingot growth parameters may be normalized within the radius of the circular state diagram 504. For example, the minimum, maximum, and target growth parameter arcs for each segment 518, 528, 538, 548 may be at the same respective radial locations (i.e., relative to the circular state diagram center C 504 The segments 518, 528, 538, 548 are at the same distance apart) such that the minimum arc 520 forms a circle, the target growth parameter arc 540 forms a circle, and the maximum arc 525 forms a circle. In other embodiments, the arcs of the segments 518, 528, 538, 548 are at different radial locations.

[0062] In some embodiments, each segment 518, 528, 538, 548 changes color and / or darkness in response to a change in the value of the corresponding ingot growth parameter. For example, a segment below or at a target value (shown by target arc 540) may be a first color (represented by a first stippled pattern in the first, second, and third segments 518, 528, 538), and a segment above the target value may be a second color (represented by a second stippled pattern in the fourth segment 548). In some embodiments, the color or intensity of the color may change within a segment. For example, the color within a segment may change from a center C to a center C. 504 Towards the outer edge E 518 、E 528 、E 538 、E 548 Becomes progressively darker (eg, with the segment darkest at the maximum target growth parameter visual 525).

[0063] The circular state chart 504 may include one or more petals 522, 524, 526, 532 to monitor one or more ingot growth parameters. The petals 522, 524, 526, 532 may change their distance from the center C of the circular chart based on changes in the ingot growth parameters. 504 Alternatively, the petals 522, 524, 526, 532 may change color or size in response to changes in ingot growth parameters.

[0064] State diagram 504 is an example state diagram and other state diagrams that provide information to a user related to two or more ingot growth parameters may be used unless otherwise stated.

[0065] Can be in ingot growth system 5( Figure 1 ) directly measure one or more growth parameters monitored in state diagram 504. For example, the parameters may be measured by sensor system 94 ( Figure 5 ) sensor measurements. Example sensors include temperature sensor 84, diameter transducer 86, and level sensor 90 and weight sensor 96. Instead of direct measurement, one or more growth parameters may be generated by an algorithm (such as an algorithm stored in control unit 82).

[0066] The methods of embodiments of the present disclosure have several advantages over conventional methods and systems for growing single crystal silicon ingots in a continuous Czochralski process. By providing a dynamic state diagram, several ingot growth parameters can be quickly accessed by an operator, which allows changes to the ingot growth system to be made more quickly relative to a system in which parameters are accessed in multiple locations (e.g., multiple pages). In embodiments in which the dynamic state diagram is a dynamic circular diagram divided into segments, each segment can be associated with an ingot growth parameter, which allows the operator to obtain a quick overview of the performance of the system. Ingot growth parameters can be normalized in the dynamic state diagram, which allows the parameters to have a common growth vision (e.g., a minimum growth vision, a maximum growth vision, and / or a target growth vision, each of which can be represented by an arc in the dynamic state diagram). The dynamic state diagram provides the operator with quick access to system parameters without providing too much information to the operator.

[0067] Examples

[0068] The process of the present disclosure is further illustrated by the following examples. These examples should not be considered in a limiting sense.

[0069] Example 1: Dynamic state diagram with four ingot growth parameters

[0070] exist Figure 6, a dynamic state chart developed for controlling ingot growth in a continuous Czochralski ingot growth system is shown in FIG. The dynamic state chart is a dynamic circular chart having four segments 518, 528, 538, 548 (shown as separated by dashed lines). The first segment 518 and the third segment 538 monitor a "value D" representing other ingot growth parameters (e.g., weight, temperature, diameter, level, system pressure, or the like). The second segment 528 monitors seed lift (i.e., the rate at which the seed 122 is raised in the ingot puller). The fourth segment 548 monitors the growth rate of the ingot. As shown in FIG. Figure 6 , "Value D" is at or near the target growth value indicated by the middle arc 540. The seed lift is below the target value and the growth rate is above the target value. The dynamic state chart allows multiple growth parameters to be monitored and controlled in a single view.

[0071] Example 2: Dynamic state diagram containing seven ingot growth parameters

[0072] exist Figure 7 6 shows a dynamic state diagram 604 showing seven ingot growth parameters. The dynamic state diagram is a dynamic circular state diagram that includes a first segment 618 monitoring the position of the heat shield, a second segment 628 monitoring the seed lift speed, a third segment 638 monitoring the diameter of the ingot, a fourth segment 648 monitoring the target length of the ingot, a fifth segment 658 monitoring the ingot growth system pressure, a sixth segment 668 monitoring the dopant feed rate to the melt, and a seventh segment 678 monitoring the rate at which silicon is added to the melt. The monitored parameters may be directly measured or may be the output of one or more algorithms. The growth parameters have been normalized so that the target growth visual (i.e., arc) for each segment is at a distance C from the center of the circular diagram. 604 at the same distance.

[0073] As used herein, the terms "about," "substantially," "substantially," and "approximately" when used in conjunction with ranges of size, concentration, temperature, or other physical or chemical properties or characteristics are meant to encompass variations that may exist in the upper and / or lower limits of the range of the property or characteristic, including, for example, those resulting from rounding off, variations in the method of measurement, or other statistical variations.

[0074] When introducing elements of the present disclosure or embodiment(s) of the present disclosure, the articles "a," "an," "the," and "said" are intended to mean that there are one or more elements. The terms "comprising," "including," "containing," and "having" are intended to be inclusive and mean that there may be additional elements in addition to the listed elements. The use of terms indicating a particular orientation (e.g., "top," "bottom," "side," etc.) is for convenience of description and does not require any particular orientation of the items being described.

[0075] As various changes could be made in the above constructions and methods without departing from the scope of the disclosure, it is intended that all matter contained in the above description and shown in the accompanying drawing(s) shall be interpreted in an illustrative and non-limiting sense.

Claims

1. A method for growing a single crystal silicon ingot in a Czochralski process, the method comprising: preparing a silicon melt in a crucible; extracting a single crystal silicon ingot from the melt; providing a plurality of growth parameters associated with the growth of the single crystal silicon ingot; providing a dynamic state graph including a visual representation of the plurality of growth parameters, the dynamic state graph being a circular state graph divided into a plurality of segments, each segment being associated with a growth parameter; and The circular state chart including graphical representations of the plurality of growth parameters is displayed on a screen, the circular state chart including minimum and maximum growth parameter visuals associated with each growth parameter, the minimum and maximum growth parameter visuals being graphical representations. 2 . The method of claim 1 , further comprising adding polycrystalline silicon to the melt to replenish silicon in the crucible as the silicon ingot is withdrawn from the melt.

3. The method of claim 1 wherein the circular state diagram has a center and each segment has an outer edge and a radius extending from the center of the circular state diagram to the outer edge, the radius changing in response to a change in the value of the growth parameter.

4. The method of claim 1, wherein the minimum growth parameter visual is a first arc and the maximum growth parameter visual is a second arc disposed radially outward from the first arc, the first arc and the second arc defining an annular segment representing an acceptable range for the growth parameter. 5 . The method of claim 4 , wherein the dynamic state diagram includes a target growth parameter visual, the target growth parameter visual being a third arc disposed between the first arc and the second arc.

6. The method according to claim 4, wherein: The first arc of each segment is at the same distance from the center of the circular state diagram, so that the first arcs are combined to form a first circle; and The second arc of each segment is at the same distance from the center of the circular state diagram, so that the second arcs are combined to form a second circle concentric with the first circle.

7. The method of claim 1, wherein the plurality of growth parameters are selected from the group consisting of ingot target length, ingot diameter, seed lift speed, heat shield position, polysilicon feed rate, dopant feed rate, ingot puller pressure, and ingot growth rate.

8. The method of claim 1, further comprising changing a color of the visual representation based on a change in one or more growth parameter values.

9. The method of claim 1, wherein the plurality of growth parameters are provided by: measuring the growth parameter in an ingot growth system, the crucible being disposed in a growth chamber of the ingot growth system; or The growth parameters are generated from an algorithm.

10. An ingot growing system for manufacturing a single crystal silicon ingot, the system comprising Growth chambers; a crucible disposed within the growth chamber and configured to hold a melt comprising molten silicon; an ingot pulling mechanism for extracting an ingot from the melt; A control unit comprising a processor and a memory, the memory storing instructions which, when executed by the processor, cause the processor to: determining a plurality of growth parameters associated with the growth of the single crystal silicon ingot; and providing a dynamic state chart including a visual representation of the plurality of growth parameters to a user, the dynamic state chart being a circular state chart divided into a plurality of segments, each segment being associated with a growth parameter; and A user interface to which the control unit is communicatively connected, the user interface comprising a screen on which the user interface displays the circular status chart, the circular status chart including minimum and maximum growth parameter visuals associated with each growth parameter, the minimum and maximum growth parameter visuals being graphical representations.

11. The ingot growing system of claim 10, further comprising a polysilicon feed system for adding polysilicon to the melt to replenish silicon in the crucible as a silicon ingot is withdrawn from the melt.

12. The ingot growth system of claim 10, wherein the circular state diagram has a center and each segment has an outer edge and a radius extending from the center of the circular state diagram to the outer edge, the radius changing in response to a change in the value of the growth parameter.

13. The ingot growth system of claim 10, wherein the minimum growth parameter visual is a first arc and the maximum growth parameter visual is a second arc disposed radially outward from the first arc, the first arc and the second arc defining an annular segment representing an acceptable range for the growth parameter.

14. The ingot growth system of claim 13, wherein the dynamic state graph includes a target growth parameter visual, the target growth parameter visual being a third arc disposed between the first arc and the second arc.

15. The ingot growing system of claim 13, wherein: The first arc of each segment is at the same distance from the center of the circular state diagram, so that the first arcs are combined to form a first circle; and The second arc of each segment is at the same distance from the center of the circular state diagram, so that the second arcs are combined to form a second circle concentric with the first circle.

16. The ingot growth system of claim 10, wherein the plurality of growth parameters are selected from the group consisting of ingot target length, ingot diameter, seed lift speed, heat shield position, polysilicon feed rate, dopant feed rate, ingot puller pressure, and ingot growth rate.

17. The ingot growth system of claim 10, wherein the memory stores instructions that, when executed by the processor, cause the processor to change a color of the visual representation based on a change in a growth parameter value.

18. The ingot growth system of claim 10, wherein the system comprises a sensor system that measures one or more ingot growth parameters, the sensor system being communicatively connected to the control unit.

19. The ingot growth system of claim 10, wherein the system is configured to generate one or more ingot growth parameters according to an algorithm.