Controlled n-doping of III-V materials grown on (111)Si

By using a continuous flow of arsenic and staggered growth cycles on a (111) Si substrate, the growth of III-V materials is controlled, the problem of unintentional doping of GaAs materials is solved, and efficient n-type doping is achieved. Controlled and high-mobility growth of GaAs semiconductor materials.

CN114341408BActive Publication Date: 2024-10-29INTEGRATED SOLAR AS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202080049906.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-07
Publication Date
2024-10-29
Estimated Expiration
2040-07-07

AI Technical Summary

Technical Problem

In the molecular beam epitaxy growth process, GaAs materials are prone to unintentional doping, making it difficult to control their n-type doping properties. Especially when growing on (111) Si substrates, it is difficult to achieve efficient n-type semiconductor materials.

Method used

By using a continuous flow of arsenic flow concentration control on a (111) Si substrate, combined with a method of staggered growth and non-growth cycles, III-V materials are deposited, maintaining the growth temperature between 300°C and 580°C, using As4 and As2 The mixture acts as an arsenic current source, ensuring unintentional doping of the material and compensating doping via Si as the n-dopant.

Benefits of technology

Achieved efficient growth of n-type GaAs doped semiconductor on (111)Si, controlled the p-type doping concentration in the range of 2E14cm-3 to 3.6E16cm-3, and obtained a high mobility ≥1.6E3cm2/Vs The material ensures n-type doping and reduces the impact of unintentional doping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114341408B_ABST
    Figure CN114341408B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for providing n-doped III-V material grown on (111)Si, and in particular to a method comprising steps of growing III-V material interleaved with no-growth steps, wherein both the growing steps and the no-growth steps are subject to a constant, uninterrupted arsenic flow concentration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method of providing an n-doped group III-V material grown on (111) Si, and more particularly to a method comprising steps of growing the group III-V material interleaved with no-growth steps, wherein both the growing steps and the no-growth steps are subject to a constant, uninterrupted arsenic flux concentration.

[0002] background

[0003] Intrinsic semiconductor materials generally require dopants to form non-intrinsic semiconductors, such as n-type semiconductors, i.e., materials in which electrons are majority carriers and holes are minority carriers. P-type semiconductors include semiconductor materials in which holes are majority carriers and electrons are minority carriers. Doping of intrinsic semiconductor materials generally involves introducing impurity atoms into the intrinsic semiconductor. The impurity atoms are from an element different from the semiconductor material, and the impurity atoms are donors or acceptors of the intrinsic semiconductor. Donors contribute their extra valence atoms to the conduction band of the semiconductor. Acceptors accept electrons from the valence band of the semiconductor, thereby providing excess holes in the intrinsic semiconductor material, i.e., providing a p-type semiconductor. When manufacturing semiconductor devices, n-type and p-type semiconductors can be joined to form, for example, a pn junction.

[0004] However, it is known that when manufactured in a molecular beam epitaxy growth process, semiconductor materials may exhibit non-intentional doping, such as p-type or n-type. The reason may be the imperfect structural quality of the resulting semiconductor material (crystal defects, etc.). In such a case, if non-intentional p-doping or n-doping (sometimes referred to as self-doping, i.e., without the use of added dopants) has occurred in the semiconductor material, it may not be possible to use dopants to manufacture n-type or p-type semiconductors. For example, if non-intentional p-doping (or self-doping) has occurred in the epitaxial growth process, it is known that when making the material n-doped, it is possible to add n-dopants in a process called compensation doping. However, if compensation n-doping can be successful, this possibility usually depends at least on the level of p-doping present in the material.

[0005] GaAs is most commonly doped with silicon in order to make GaAs n-type, but may additionally be doped with germanium, sulfur, tellurium or tin, or beryllium, chromium or germanium, etc., in order to make it n-doped or p-doped, respectively. One type of dopant may actually act as both an n-dopant and a p-dopant, depending on the position it takes in the GaAs lattice. For GaAs, this is relevant to all members of the carbon family, which would be n-dopants if they occupied the As position, and p-dopants if they occupied the Ga position. Notation wise, a Ga atom occupying a Ga position in the GaAs lattice is denoted as Ga. Ga , and Ga occupying the As position is represented as Ga As , and so on.

[0006] The diatomic nature of GaAs makes it a highly challenging material to controllably dope. A non-single ratio between the two components, Ga and As, will, for example, provide a strong doping effect in the material, since Ga As will act as a p-dopant, and As Ga will act as an n-dopant. Thus, a slightly higher concentration of Ga during the formation of GaAs will result in a p-type material, while the opposite will result in an n-type material.

[0007] When controlling the doping of GaAs, the inevitable introduction of mono-vacancy and dopant-vacancy complexes further complicates matters. It has been reported that As vacancies (V As ) and gallium vacancies (V Ga ) both act as p-dopants (see http: / / onlinelibrary.wiley.com / doi / 10.1002 / pssa.2210960237 / abstract), and dopant-vacancy complexes such as Si Ga V Ga , by acting as an acceptor to compensate for n-doping, although Si usually acts as an n-dopant in GaAs. Ga V Ga The compensation for n-doping has been shown to be strongest for high Si-doping, in which case the Si atoms act as zwitterionic dopants by As In addition, a compensation effect is added.

[0008] During the film deposition of GaAs using, for example, molecular beam epitaxy (MBE), the balance of the Ga / As ratio is particularly challenging. During the MBE deposition of GaAs, As is deposited as a mixture between As, As2 and As4, all of which have different chemical adsorption properties. For example, As2 and As4 attach to GaAs differently, i.e., depending on the temperature and the concentration of Ga on the GaAs surface. It is reported that the maximum adhesion coefficients of As2 and As4 on GaAs are measured to be 0.75 and 0.5, respectively. When using MBE to deposit GaAs, keeping the vapor pressure (flow) of As higher than that of Ga is used to obtain a single ratio between the two elements. Therefore, the higher incorporation of Ga into the film than As will result in a p-doped film.

[0009] [1] T. Yamamoto, M. Inai, A. Shinoda, T. Takebe, in the article "Misorientation Dependence of Crystal Structures and Electrical Properties of Si-Doped AlAs Grown on (111) GaAs by Molecular Beam Epitaxy", Japanese Journal of Applied Physics, Vol. 32, p. 3346 (1993), disclosed how the misorientation of (111) GaAs affects the doping efficiency. When the misorientation is less than 3 degrees, the efficiency of the Si-doped AlAs layer on the misoriented (111) GaAs is reduced, which provides high resistance when grown on the (111) axis.

[0010] [2] T. Kawai, H. Yonezu, Y. Yamauchi, Y. Takano, and K. Pak, in “Initial growth mechanism of AlAs on Si(111) by molecular beam epitaxy”, Physics Letters 59, p. 2983 (1991), disclosed that As4 can be used to grow unfaceted AlAs and GaAs on Si. However, the effect of As4 on doping has never been studied.

[0011] [3] K. Winer, M. Kawashima, and Y. Horikoshi, "Si doping efficiency in GaAs grown at low temperatures", Applied Physics Letters 58, p. 2818 (1991), disclose the doping effect using different Ga / As4 flow ratios. The doping depends on the Ga / As4 flow ratio.

[0012] [4] A. Saletes, J. Massies, G. Neu, JP Contour: “AEffect of As4 / Ga flux ratio on electrical properties of NID GaAs layers grown by MBE””, Electronic Letters, Vol. 20, No. 21 (1984) discloses how the III / V flux ratio can be used to control the type and level of doping in GaAs films grown on a silicon (100) surface without adding any separate doping material. This effect is called non-intentional doping (NID) because the material exhibits a tendency to self-dope at variable levels by controlling the parameters of the growth in a molecular beam epitaxy system.

[0013] If the material becomes an unintentional p-doped material, compensating doping with, for example, Si may not always result in an n-doped material, ie compensating for the unintentional p-doping. In particular, compensating doping may not be possible if the p-doping concentration is too high.

[0014] The invention thus comprises a method of epitaxial growth in an MBE (Molecular Beam Epitaxy) machine which provides control over unintentional doping and which, for the purposes of the invention, will enable compensated n-doping of the material, resulting in n-type material.

[0015] When growing GaAs on silicon, it is known that unintentional doping may occur. Therefore, there is a need for an improved method of controlled doping of III-V materials on (111)Si. In particular, there is a need for improved growth of n-type semiconductors including at least GaAs on (111)Si in a molecular beam epitaxial growth process.

[0016] Purpose of the Invention

[0017] In particular, it may be seen as an object of the present invention to provide an n-type doped semiconductor comprising at least GaAs on Si(111) by continuously flowing an As flux concentration on the Si(111) growth interface in a molecular beam epitaxy (MBE) growth process.

[0018] A further object of the invention is to provide an alternative to the prior art.

[0019] Overview

[0020] Therefore, the objects described above and several other objects are intended to be achieved in a first aspect of the present invention by providing a method for controllable n-doping in a molecular beam epitaxy (MBE) growth process comprising growing a Group III-V material on a (111) Si substrate, wherein the nucleation layer comprises a Group III-Sb material, the method comprising the following steps:

[0021] -Growth of nucleation layer, thereafter

[0022] - directing a continuous flow of arsenic towards the growth interface of the (111) Si substrate,

[0023] - depositing a III-V material in steps comprising a period in which the deposition of the III-V material is carried out in a first step, followed by a second step in which the deposition of the III-V material is stopped,

[0024] - continuing to deposit the III-V material according to the first step and the second step while the arsenic flow continues to flow until the final material composition grows,

[0025] - Maintaining the temperature of the epitaxial growth process between 300°C and 580°C,

[0026] - where the deposited material is unintentionally doped with 2E14 cm -3 To 3.6E16cm -3 The resulting p-type doping concentration is in the range of 1.6E3cm at room temperature. 2 / Vs mobility, enabling compensatory doping with n-dopants.

[0027] Respective aspects of the invention may each be combined with any other aspects.These and other aspects of the invention will be apparent from and elucidated with reference to the embodiments described hereinafter.

[0028] Attached photos

[0029] The method of controlled n-doping of the present invention will now be described in more detail with reference to the accompanying drawings. The accompanying drawings illustrate examples of embodiments of the present invention and should not be interpreted as limiting other possible embodiments falling within the scope of the appended claim group. In addition, the corresponding examples of the embodiments can each be combined with any other examples of the embodiments.

[0030] Figure 1a An example of a perfect GaAs crystal is shown.

[0031] Figure 1b An example of a GaAs crystal lacking an arsenic atom is shown.

[0032] Figure 2 An example of the growth process of the present invention is schematically illustrated.

[0033] Figure 3a An example of mobility measurement in an example of an embodiment of the present invention is illustrated.

[0034] Figure 3b An example of carrier density measurement in an example of an embodiment of the present invention is illustrated.

[0035] Figure 4 Examples of process steps in an example of an embodiment of the present invention are illustrated.

[0036] Figure 5 Examples of parameter settings for the growth process and the results obtained are illustrated.

[0037] Figure 6a The diagram shows 2D growth on a miss-cut (111) Si substrate surface.

[0038] Figure 6a The diagram shows 3D growth on a (111) Si substrate surface with no missed cuts.

[0039] Figure 7 The results obtained in an example of an embodiment of the present invention are shown graphically.

[0040] Figure 8 Further results obtained in examples of embodiments of the present invention are illustrated.

[0041] Fig. 9 Further results obtained in examples of embodiments of the present invention are illustrated.

[0042] Fig.10 An example of growing an n-doped material in an MBE (Molecular Beam Epitaxy) machine according to an example of an embodiment of the present invention is illustrated.

[0043] Fig. 11a and Fig. 11b disclose different examples of layer structures of examples of embodiments of the present invention.

[0044] Detailed Description

[0045] Although the present invention has been described in conjunction with specific embodiments, the present invention should not be interpreted as being limited to the current examples in any way. The scope of the present invention is set forth by the appended claim group. In the context of the claims, the terms "comprising" or "comprises" do not exclude other possible elements or steps. In addition, references such as "a" or "an" should not be interpreted as excluding more than one. The use of reference numerals in the claims with respect to elements shown in the drawings should also not be interpreted as limiting the scope of the present invention. In addition, individual features mentioned in different claims may be advantageously combined, and mentioning these features in different claims does not exclude that a combination of features is impossible and advantageous.

[0046] Figure 1a The diagram shows a perfect GaAs crystal containing Ga atoms and As atoms, where the corresponding atoms are bonded together to form a crystal structure.

[0047] Figure 1b The diagram shows the case where an arsenic atom is missing from the crystal structure. Typically, this is an example of unintentional p-type doping in a III-V material structure. The missing arsenic atom forms dangling bonds with neighboring gallium atoms. These dangling bonds can act as electron donors, resulting in localized positive charges. The movement of these charges throughout the crystal is p-type conduction.

[0048] Figure 2 A schematic diagram of an example of applying flux concentration during epitaxial growth on a substrate is illustrated. As is known in the prior art, a beam comprising atoms of a corresponding material with a defined flux concentration can be directed toward a substrate at a given temperature. The atoms contained in the corresponding beam are then deposited onto the surface of the substrate and combined with atoms on the substrate surface. Turning the corresponding beam on and off, changing the flux concentration, temperature and pressure, and other parameters, can add several layers to the growing interface, which layers can include different material compositions. In this way, semiconductor materials with specific properties as known in the prior art can be designed.

[0049] Relative to about Figure 1b As discussed above, aspects of the present invention are the main concept of having a high flux concentration of arsenic atoms to fill the arsenic vacancies in the crystal and then using, for example, Si as an n-dopant in the process. Figure 2 Arsenic flux concentrations using a mixture containing As2, As4, and Si as the n-dopant material are illustrated.

[0050] However, it is also necessary to consider other factors that characterize the resulting semiconductor material. For example, as is known to those skilled in the art, excess arsenic may lead to defects in the crystal, affecting the electrical properties of the semiconductor material.

[0051] Specific considerations are achieving sufficient charge mobility in the crystal and achieving sufficient charge density in the semiconductor material. Conductivity is proportional to the product of mobility and carrier concentration. For example, the same conductivity may come from a smaller number of electrons and a higher mobility for each, or from a larger number of electrons and a lower mobility for each. In semiconductors, for example, transistors and other devices can behave very differently depending on whether there are many electrons with lower mobility or fewer electrons with higher mobility.

[0052] Therefore, mobility is an important parameter for semiconductor materials. Generally, when other characteristics or parameters of the device are roughly the same, higher mobility leads to better device performance.

[0053] Figure 3a and Figure 3b An example of measuring electrical mobility in an example of an unintentionally doped sample of a III-V semiconductor material is illustrated. Figure 3a Hall mobility is disclosed, which discloses the dependence of the electric field on the mobility of charges in a material as a function of magnetic flux density. Figure 3b The charge carrier concentration is plotted as a function of magnetic flux density. The conductivity of a material is proportional to the product of mobility and carrier concentration, as discussed above. These curves show that at room temperature, the intrinsic or p-type carrier concentration is about 3.5-3.6E16 cm -3 , and the mobility is about 1.6-1.7E3cm 2 / Vs.

[0054] Therefore, the main principle behind the present invention is to avoid missing arsenic atoms in e.g. III-V semiconductor materials by increasing the arsenic atomic flux concentration when growing the III-V semiconductor material and using e.g. Si as n-dopant when providing an n-type III-V semiconductor.

[0055] The arsenic source used in the example of the method according to the invention can be a solid As source with a cracker. The arsenic stream concentration is a mixture of As4 and As2.

[0056] When developing and testing some examples of material samples according to the present invention, the inventors used an "Arsenic Valved Cracker Mark V 500cc" provided by Veeco for arsenic flow generation. Using the factory recommended settings, and when using specific dopants (Si dopants) and substrate temperatures, the cracker provides an As2 / As4 flow ratio that results in n-type doped material during the growth process, even at very high total arsenic flow concentrations (up to and possibly above 3E-5T). By setting the temperature of the cracker, for example in the interval of 600°C to 900°C, the ratio between As4 and As2 is controllable. When the temperature of the cracker approaches 600°C, the concentration of As4 is greater than the concentration of As2, while when the temperature of the cracker approaches 900°C, the concentration of As4 is less than the concentration of As2.

[0057] The arsenic flux ratio is controllable as shown above and depends on the arsenic source settings. Under the most adverse conditions, the resulting material appears to always be a highly p-type semiconductor (>1E18cm -3 ), so n-type compensatory doping becomes almost impossible to achieve, because unintentional p-type doping will dominate the material. The inventors have studied the -3 Measurements made on an n-doped material intentionally doped n-type (calibrated on (100) GaAs) revealed that the material remains p-type under adverse conditions.

[0058] In an example of an embodiment of the present invention, the growth process on (111) Si includes using a mixture of different arsenic flux compositions, including but not limited to As2 and As4 molecules. During growth, other materials are added, which constitutes a complete III-V material structure with n-doping. These materials include (but are not limited to) gallium, aluminum, indium, arsenic, and n-doping (silicon), and antimony is optionally added. In the III-V structure, silicon constitutes the dopant, but can be exchanged with other n-dopants. Growth stops can be performed at certain intervals at the arsenic flux concentration to increase the arsenic content of the semiconductor.

[0059] Figure 4 An example of a growth process over time is illustrated. The illustrated process begins with depositing a certain amount of a selected material as disclosed, for example, in FIG1 onto a substrate. In this example, a constant arsenic flow composition is applied throughout the growth process, and while the arsenic flow concentration is still flowing, deposition of the selected III-V material or material combination continues in steps with non-growth periods. The thickness of the material increases in the corresponding steps including growth.

[0060] In an example of an embodiment of the present invention, periods with growth cessation and periods with growth may be periodically interchanged.

[0061] In another example of an embodiment of the present invention, the periods of growth arrest occur at randomized irregular intervals.

[0062] In another example of an embodiment of the present invention, increasing the As flux concentration can reduce the length of the corresponding growth arrest.

[0063] The period with growth cessation can be between 20 seconds long and 500 seconds long.

[0064] Figure 5 Table 1 is depicted, disclosing some examples of different parameter settings that may be used in examples of the embodiments disclosed above.

[0065] exist Figure 5 Table 1 of FIG. 1 provides the results of III-V growth, as well as examples of process parameters and growth stop intervals. 0.95 In 0.05 As provides a mobility of 90 cm 2 / Vs3.5E18cm -3 n-doped, and another example Ga 0.83 In 0.17 As provides a mobility of 87 cm 2 / Vs2.80E+18cm -3 n-doping.

[0066] When studying the structural quality of the material being processed as discussed above, the structural quality may be improved. When referring to the prior art on (111)GaAs, the prior art indicates that the optimal growth temperature should be about 670°C. This may not be possible on (111)Si when the nucleation layer requires high levels of Sb, which is not possible to grow above 580°C. The inventors have determined that Sb is a preferred part of the nucleation layer when growing III-V materials on (111)Si substrates.

[0067] Furthermore, annealing at too high a temperature is also undesirable when obtaining high structural quality, because Sb diffusion will remove Sb from the nucleation layer and create voids or defects in the III-V material.

[0068] As discussed above, doping may result in defects in III-V structures which may act as acceptors or donors, and unintentional doping is the result. Therefore, it is advantageous to control the defects and / or doping levels of III-V materials when using these structures for different applications.

[0069] The use of n-type doping is important for many applications using III-V materials grown on (111) Si. For example, these applications include solar cells, photodetectors, semiconductor lasers, and high electron mobility transistors (HEMTs).

[0070] The process of n-doping of III-V materials grown on (111)Si has been discussed in the prior art. For example, [2] T. Kawai has shown on (111)Si that As4 can be used to successfully grow AlAs and GaAs without facets on silicon, but the effect of As4 on doping has never been studied. The doping of GaAs on GaAs (100) substrates has been studied by K. Winer et al. [3] using different As4 and Ga flows and shown to depend on the Ga / As4 flow ratio. Yamamoto et al. [1] studied Si-doped AlAs layers on misoriented (111)GaAs and found that the doping efficiency decreased when the misorientation was less than 3 degrees and had high resistance when grown on the (111) axis.

[0071] The growth process of the present invention on (111) Si includes examples using a mixture of different arsenic flux compositions, including but not limited to monoatomic arsenic, As2 and As4 molecules. During growth, other materials are added, which constitute a complete III-V material structure with n-doping. These materials include (but are not limited to) gallium, aluminum, indium, arsenic and n-dopants (silicon), and antimony is optionally added. In the III-V structure, silicon constitutes the n-dopant, but can be exchanged for other n-dopants.

[0072] According to an example of an embodiment of the present invention, regular growth stops or irregular growth stops (which may be randomized) are introduced at certain intervals under an arsenic flow, thereby increasing the arsenic content of the semiconductor material.

[0073] The results obtained with the method of the present invention provide unintentionally doped III-V materials on (111) Si substrates with an intrinsic p-doping concentration of 2E14 cm -3 To 3.6E16cm -3 This is a good starting point when providing controlled n-type doping of these materials, where due to the lower level of unintentional p-doping, n-dopant compensatory doping is possible and leads to a net n-type doping of the material. A further interesting aspect is that n-type doping of examples of material compositions grown according to the invention can provide a lower mobility, but this does not lead to too high an ohmic resistance of the material.

[0074] Furthermore, annealing at too high a temperature may not provide high structural quality, since Sb diffusion will remove Sb from the nucleation layer and create voids or defects in the III-V material. When Sb is applied, the growth temperature should not exceed 580°C.

[0075] Another aspect of growing III-V materials is that the surface of the semiconductor should be flat when the resulting semiconductor is to be used in solar cells (and for other applications). By adding indium to the III-V materials used in the growth process according to the present invention, it is possible to avoid, for example, crystal facets. The preferred at% amount of indium is from 1.1 at% to 21.4 at%. More specifically, In is selected from the group comprising the following amounts: 1.1 at%, 1.2 at%, 1.4 at%, 2.2 at%, 2.4 at%, 2.6 at%, 2.9 at%, 3.3 at%, 3.9 at%, 4.2 at%, 4.6 at%, 5.6 at%, 7.1 at%, 8.3 at%, 10.0 at%, 14.3 at%, 16.7 at%, or 21.4 at%. This has been shown to reduce defects in the resulting material.

[0076] It is known that unintentional p-doping of samples after post-growth annealing is caused by defects in the III-V structure acting as acceptors or donors, and unintentional p-doping is the result. Therefore, it is advantageous to control the defects and / or doping levels of III-V materials when using these structures for different applications.

[0077] Another consideration regarding MBE growth is growing on-cut (111) Si crystals versus off-cut crystals. In examples of embodiments of the present invention, on-cut crystals are preferred to prevent steps from appearing on the silicon surface, as described in detail in the accompanying drawings. Figure 6a Such steps in the surface will be one monolayer or several monolayers in height. In the latter case, these steps can lead to defects in the growing crystal. For up-cut crystals, the lack of steps leads to 3D-like growth on the surface, see Figure 6b . For example, when a nucleation layer of AlAsSb is started to grow on top of a (111)Si surface, this will appear as islands on the surface. These islands will eventually grow in size until they meet and will therefore cover the entire surface. Once such coverage has been achieved, growth switches to growth using gallium containing materials. Gallium helps reduce 3D-like growth to achieve a flat growth surface and thereby reduce defects. Also refer to the planarization layers 2 and 3 disclosed in Table 2 of Figure 11a.

[0078] Another aspect of the invention is to avoid unintentional n-doping of the nucleation layer.Thus, the nucleation layer is grown separately, while the III-V material deposited will be n-doped in higher layers above the nucleation layer.

[0079] In addition, it is within the scope of the invention to use a technique known as "digital alloy growth". This means using thinner AlInAs layers and thinner GaLnAs layers, which results in layers with a higher Al content. The effect of this approach is that the GaInAs layer can be doped without doping the AlInAs layer. See Ron Kaspi et al., "Digital alloy growth in mixed As / Sb hetero-structures", Journal of Crystal Growth, Vol. 251, No. 1-4, April 2003, pp. 515-520.

[0080] The use of n-type doping is important for many applications when using III-V materials grown directly on (111) Si. These applications include solar cells, photodetectors, semiconductor lasers and high electron mobility transistors (HEMTs). Referring to Table 2 in Figures 11a and 11b, a solar cell structure including an example of a layer according to the present invention is disclosed.

[0081] Figure 7 An example of the results of n-type doping obtained in an example of an embodiment of the present invention is shown. An example of the results of n-type doping obtained in an example of an embodiment of the present invention is shown. 0.83 In 0.17 n-type doping concentration in As. The material was grown at a temperature of 430°C using 50 nm intervals and a growth stop of 294 seconds between respective intervals. The arsenic flow was always present (applied), while the gallium and indium flows were present (applied) only during the growth intervals. See also Figure 5 Table 1 discloses the mobility and n-doping concentration obtained under different As flux concentrations etc.

[0082] Figure 8 The obtained n-type Ga 0.83 In 0.17 Example of electron mobility in As. The material was grown at a temperature of 430°C with 50nm thickness intervals and a growth stop of 294 seconds between the respective intervals. The arsenic flow was always present, while the gallium and indium flows were present only during the growth intervals. When relatively low flow rates are present, the mobility is low (e.g., in the case of Figure 7 At relatively moderate flow rates, the mobility is 80 cm 2 / Vs-90cm 2 / Vs, and at relatively high flow rates, the mobility decreases again. Figure 7 In contrast, there is no decrease in carrier concentration at high flow rates. Therefore, the decrease in mobility is due to defects associated with excess arsenic, which does not affect carrier concentration.

[0083] There is a relationship between the duration of growth arrest and the As flux concentration. If the As flux concentration is higher, the duration of growth arrest can be shorter. In this way, the As flux concentration can be manipulated relative to the duration of growth arrest.

[0084] In principle, there is no harm if the duration of the growth stop is too long. However, if the duration of epitaxial growth is long, impurities in the MBE chamber have a tendency to be trapped by the material sample. It is a well-known problem that impurities in the MBE machine itself can cause defects in the resulting material structure and thus lead to unintentional doping. Therefore, shorter growth stops at higher As flux concentrations are preferred. For example, see Figure 7 .

[0085] Fig. 9 The obtained n-type Ga 0.83 In 0.17 Example of electron mobility in As. The material was grown with an As flow of 2.0E-5 Torr, using 50nm intervals and corresponding growth stops of 294 seconds in between. The As flow was always present, while the Ga and In flows were only present during the growth intervals. For the example of the sample grown at 375°C, proper measurements were not possible due to the high resistivity of this sample. This indicates low mobility values ​​and / or low carrier concentrations, which is shown in the figure above as a peak at 0 cm 2 At 430°C, the mobility reaches a higher value (87 cm 2 / Vs), and does not provide a significant decrease at 500°C. Figure 5 Table 1, for Ga 0.83 In 0.17 As, the carrier concentration is lower at 500°C. The same Table 1 shows that the reduction in carrier concentration can be offset and even increased. The reduction in the indium content provides these effects when grown at these temperatures.

[0086] Fig.10 An example of a setup when a material sample is manufactured according to the present invention is illustrated.

[0087] The corresponding material source may be a solid source or a combination of a solid source and a gas source.Such a machine may utilize CVD (Chemical Vapor Deposition) deposition or MOCVD (Metal Organic Chemical Vapor Deposition) as known in the art.

[0088] Figure 11a discloses examples of material compositions of corresponding layers for five different material samples of a solar cell design. Figure 11b gives a short description of the corresponding layers.

[0089] The samples have been tested using the electron beam induced current (EBIC) technique, which is a semiconductor analysis technique performed in a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM). It is used to identify buried junctions or defects in semiconductors, or to examine minority carrier properties, as is known in the art.

[0090] For example, in a solar cell, photons of light fall across the cell, transferring energy and creating electron-hole pairs, and causing current to flow. In an EBIC, high-energy electrons play the role of photons, causing EBIC current to flow.

[0091] Referring to Table 2 in Figure 11a, the sample has been studied with a 10 keV beam. Kanaya and Okayama have developed the following formula for the penetration depth of the beam.

[0092] The formula is:

[0093]

[0094] Where R KO is the electron range in μm, A is the atomic weight (g / mole), Z is the atomic number, and ρ is the density (g / cm 3 ), and E0 is the beam energy (keV).

[0095] Using this formula in the example of the layers in Figure 11a, it is calculated that the electrons penetrate from 0.8 μm to 0.9 μm. This means that the current mainly comes from the III-V layers.

[0096] According to an example of an embodiment of the present invention, a method for providing controllable n-doping in a molecular beam epitaxy (MBE) growth process, the molecular beam epitaxy growth process comprising growing a Group III-V material on a (111) Si substrate, wherein the nucleation layer comprises a Group III-Sb material, the method comprising the following steps:

[0097] -Growth of nucleation layer, thereafter

[0098] - directing a continuous flow of arsenic towards the growth interface of the (111) Si substrate,

[0099] - depositing a group III-V material in a step comprising the following cycle: in a first step the deposition of the group III-V material is carried out, followed by a second step in which the deposition of the group III-V material is stopped,

[0100] - continuing to deposit the III-V material according to the first step and the second step while the arsenic flow continues to flow until the final material composition grows,

[0101] - Maintaining the temperature of the epitaxial growth process in the range of 300°C to 580°C,

[0102] - where the deposited material is unintentionally doped with -3 To 3.6E16cm -3 The resulting p-type doping concentration is in the range of 1.6E3cm 2 / Vs mobility, enabling compensatory doping with n-dopants.

[0103] Furthermore, a compensating n-dopant may be deposited simultaneously with the Group III-V material in a first step, resulting in an n-doped material.

[0104] In addition, the n-doping concentration can be from 16E17cm -3 To 3.5E18cm -3 within the range.

[0105] Furthermore, the n-dopant may be from the group consisting of silicon, sulfur, tellurium, tin, germanium, selenium.

[0106] Furthermore, the arsenic stream source is provided by a solid As source having a temperature controlled cracker in the range from 600°C to 900°C.

[0107] Furthermore, the arsenic stream concentration from the source is a mixture of As4 and As2.

[0108] Furthermore, at a cracker temperature close to 600°C, the concentration of As4 is greater than that of As2, while at a cracker temperature close to 900°C, the concentration of As4 is less than that of As2.

[0109] Furthermore, the arsenic flux concentration in the non-nucleation layer measured using beam equivalent pressure (BEP) is at least between 1.33322E-5 mbar (1.00E-05T) and 3.99967E-5 mbar (3E-5T), or higher than 3.99967E-5 mbar (3E-5T).

[0110] Furthermore, indium may be one of the Group III-V materials, which is deposited in an amount ranging from 1.1 atomic % to 21.4 atomic %.

[0111] In addition, indium can be one of the Group III-V materials, which is deposited in an amount according to one of the following amounts: 1.1 atomic %, 1.2 atomic %, 1.4 atomic %, 2.2 atomic %, 2.4 atomic %, 2.6 atomic %, 2.9 atomic %, 3.3 atomic %, 3.9 atomic %, 4.2 atomic %, 4.6 atomic %, 5.6 atomic %, 7.1 atomic %, 8.3 atomic %, 10.0 atomic %, 14.3 atomic %, 16.7 atomic % or 21.4 atomic %.

[0112] Furthermore, the continued deposition of the III-V material according to the first step and the second step of the method according to the present invention may be performed periodically.

[0113] Furthermore, periods of growth arrest can occur at randomized, irregular intervals.

[0114] In addition, a higher As flux concentration from the As source can achieve a shorter growth stop.

[0115] Furthermore, the period with growth cessation can be between 20 seconds long and 500 seconds long.

[0116] Furthermore, the nucleation layer contains As in an amount of <20 atomic %.

[0117] In addition, the (111) Si substrate may have a leak cut angle that provides a step pattern on the surface of the (111) Si substrate, wherein the height of the corresponding step does not exceed one molecular monolayer.

[0118] Furthermore, the (111) Si substrate may be an up-cut crystal.

[0119] Furthermore, the epitaxial growth process can be of the digital alloy growth type.

Claims

1. A method for providing controllable n-doping in a molecular beam epitaxy (MBE) growth process, the molecular beam epitaxy growth process comprising growing a Group III-V material on a (111) Si substrate, wherein the nucleation layer comprises a Group III-Sb material, the method comprising the following steps: grow the nucleation layer, thereafter directing a continuously flowing stream of arsenic toward a growth interface of the (111) Si substrate, depositing a group III-V material in a step comprising the following cycle: wherein the deposition of said group III-V material is carried out in a first step, followed by a second step in which said deposition of said group III-V material is stopped, continuing to deposit the III-V material according to the first step and the second step while the arsenic flux continues to flow until a final material composition grows, The temperature of the epitaxial growth process is maintained in the range of 300°C to 580°C, The deposited material was unintentionally doped with 2E14 cm -3 To 3.6E16cm -3 The resulting p-type doping concentration is in the range of 1.6E3cm 2 / Vs, compensatory doping with an n-dopant can be achieved, wherein the compensatory n-dopant is deposited simultaneously with the III-V group material in the first step to produce an n-doped material.

2. The method according to claim 1, wherein the n-doping concentration is from 16 to 17 cm -3 To 3.5E18cm -3 within the range.

3. The method of claim 1, wherein the n-dopant is from the group consisting of silicon, sulfur, tellurium, tin, germanium, selenium.

4. The process of claim 1, wherein the arsenic stream source is provided by a solid As source having a temperature controlled cracker in the range from 600°C to 900°C.

5. The method of claim 4, wherein the arsenic stream concentration from the source is a mixture of As4 and As2.

6. The method of claim 5, wherein at a cracker temperature approaching 600°C, the concentration of As4 is greater than the concentration of As2, and at a cracker temperature approaching 900°C, the concentration of As4 is less than the concentration of As2.

7. The method of claim 1, wherein the arsenic flux concentration in the non-nucleation layer measured using beam equivalent pressure (BEP) is at least between 1.33322E-5 mbar and 3.99967E-5 mbar, or higher than 3.99967E-5 mbar. 8 . The method of claim 1 , wherein indium is one of the Group III-V materials, and the indium is deposited in an amount from 1.1 atomic % to 21.4 atomic %.

9. The method of claim 1 , wherein indium is one of the Group III-V materials and the indium is deposited in an amount according to one of the following amounts: 1.1 atomic %, 1.2 atomic %, 1.4 atomic %, 2.2 atomic %, 2.4 atomic %, 2.6 atomic %, 2.9 atomic %, 3.3 atomic %, 3.9 atomic %, 4.2 atomic %, 4.6 atomic %, 5.6 atomic %, 7.1 atomic %, 8.3 atomic %, 10.0 atomic %, 14.3 atomic %, 16.7 atomic % or 21.4 atomic %. 10 . The method of claim 1 , wherein continuing to deposit the Group III-V material according to the first step and the second step is performed periodically.

11. The method of claim 1, wherein the period of growth arrest occurs at irregular intervals.

12. The method of claim 1, wherein increasing the As flux concentration from the As source reduces the growth stop duration.

13. A method according to any of claims 11-12, wherein the period of growth cessation is between 20 seconds long and 500 seconds long.

14. The method of claim 1, wherein the nucleation layer comprises As in an amount <20 atomic %.

15. The method of claim 1, wherein the (111) Si substrate has a leak cut angle that provides steps on the surface of the (111) Si substrate, wherein the height of the corresponding step does not exceed one molecular monolayer.

16. The method of claim 1, wherein the (111) Si substrate is an up-cut crystal.

17. The method of claim 1, wherein the epitaxial growth process can be a digital alloy growth type.

Citation Information

Patent Citations

  • Method of controlling doping concentration of N-type GaAs film by optimizing category of As molecule

    CN105428225A

  • A method for growing iii-v materials on a non iii-v material substrate comprising steps improving dislocation fault density of a finished material structure suitable for use in semiconductor manufacturing and semiconductor applications

    EP2748838A1