Composite polymer electrolyte membrane, electrolyte membrane with catalyst layer, membrane electrode complex and solid polymer fuel cell
By combining polymer electrolyte with porous substrate in the composite polymer electrolyte membrane, the problem of insufficient mechanical characteristics of electrolyte membrane in the dry and wet cycle in the prior art is solved, and high durability and excellent machinery in any state are achieved Features improve the performance of fuel cells.
Patent Information
- Application Number
- CN202080063046.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-20
- Filing Date
- 2020-09-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-09-11
AI Technical Summary
The existing composite polymer electrolyte membranes have insufficient mechanical properties during the dry and wet cycle, resulting in insufficient durability of fuel cells, especially in the water-containing state, which is prone to fracture.
Using the composite of polymer electrolyte and porous substrate, the composite polymer electrolyte membrane with good mechanical characteristics in both dry and aqueous states, including polymer electrolyte and porous substrate, ensures dry stretching per unit width. The elastic modulus and the water-containing tensile elastic modulus reach a specific threshold, and a fluorine-based porous substrate and aromatic hydrocarbon-based polymer are preferably used.
It significantly improves the wet and dry cycle durability of the fuel cell, ensures that the electrolyte membrane has excellent mechanical properties in any state, reduces resistance and improves proton conductivity and output performance.
Smart Images

Figure BDA0003538060340000121 
Figure BDA0003538060340000122 
Figure BDA0003538060340000181
Abstract
Description
Technical Field
[0001] The present invention relates to a composite polymer electrolyte membrane, a composite polymer electrolyte membrane with a catalyst layer formed by sandwiching the two sides of the composite polymer electrolyte membrane with a catalyst layer, a membrane electrode complex including the composite polymer electrolyte membrane, and a solid polymer fuel cell including the composite polymer electrolyte membrane. Background Art
[0002] Fuel cells are a type of power generation device that extracts electrical energy by electrochemically oxidizing fuels such as hydrogen and methanol. In recent years, they have attracted attention as a clean energy supply source. Among them, solid polymer fuel cells are expected to be widely used as power generation devices for smaller-scale distributed power generation facilities, automobiles, ships and other mobile bodies because their standard operating temperature is as low as 100°C and their energy density is high. In addition, they are also attracting attention as power sources for small mobile devices and portable devices, and are expected to replace secondary batteries such as nickel-metal hydride batteries and lithium-ion batteries and be installed in mobile phones, personal computers, etc.
[0003] Fuel cells are usually composed of unit cells formed by sandwiching a membrane electrode assembly (MEA) with a diaphragm. MEA is obtained by configuring catalyst layers on both sides of the electrolyte membrane and further configuring gas diffusion layers on both sides. In MEA, a pair of electrode layers are formed by the catalyst layer and the gas diffusion layer arranged on both sides with the electrolyte membrane sandwiched therebetween, one of which is the anode electrode and the other is the cathode electrode. Electricity is produced by electrochemical reaction by contacting the anode electrode with a fuel gas containing hydrogen and contacting the cathode electrode with air. The electrolyte membrane is mainly composed of a polymer electrolyte material. Polymer electrolyte materials are also used as binders for catalyst layers.
[0004] In the past, as a polymer electrolyte material, "Nafion" (registered trademark) (manufactured by Chemours (KK)) as a fluorine-based polymer electrolyte has been widely used. "Nafion" (registered trademark) shows high proton conductivity under low humidification conditions through a proton conduction channel caused by a cluster structure. On the other hand, since "Nafion" (registered trademark) is manufactured through multi-stage synthesis, it is very expensive. In addition, there is also a problem that the fuel permeation (crossover) is large due to the aforementioned cluster structure. In addition, under the operating conditions of the fuel cell, dry-wet cycles are repeated, and in particular, the electrolyte membrane is repeatedly swollen and shrunk. At this time, the electrolyte membrane is constrained by the diaphragm, etc., so wrinkles and relaxations occur. Due to local stress concentration, the membrane breaks, and there is a problem of losing the mechanical strength of the membrane and the durability of dry-wet cycles. In addition, the problem of low softening point and inability to use at high temperatures, as well as the problem of waste disposal after use and the difficulty of recycling materials are pointed out. In order to overcome such problems, the development of hydrocarbon-based electrolyte membranes that are cheap and have excellent membrane properties that can replace "Nafion" (registered trademark) has also been active in recent years.
[0005] In such a solid polymer fuel cell, in order to improve the long-term durability of the fuel cell, it is important to improve the mechanical properties and dry-wet cycle durability of the electrolyte membrane. So far, the dry-wet cycle durability of the electrolyte membrane is not sufficient, so as mentioned above, there is the following problem: the electrolyte membrane breaks due to wrinkles and relaxation during the dry-wet cycle, thereby losing the dry-wet cycle durability. Therefore, in order to improve the mechanical properties and dry-wet cycle durability of the electrolyte membrane, a composite electrolyte membrane formed by compounding a polymer electrolyte with a porous substrate such as nanofibers and microporous membranes is proposed.
[0006] Patent Document 1 describes a membrane that suppresses swelling by compounding a hydrocarbon polymer electrolyte with a nanofiber (hereinafter referred to as NF) nonwoven fabric of polybenzimidazole (hereinafter referred to as PBI). Patent Document 2 describes a membrane that suppresses swelling by compounding a fluorine-based electrolyte with a soluble PBI NF nonwoven fabric. Patent Document 3 describes a membrane that improves proton conductivity and mechanical properties by compounding a sulfonated polyimide with an acid-impregnated PBI NF nonwoven fabric. Patent Document 4 describes a membrane that improves mechanical properties by compounding a sulfonated polyarylene with stretched porous polytetrafluoroethylene (ePTFE).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2017 / 141878
[0010] Patent Document 2: Japanese Patent Application No. 2017-532716
[0011] Patent Document 3: Japanese Patent Application Publication No. 2015-28850
[0012] Patent Document 4: Japanese Patent Application Publication No. 2005-166557 Summary of the invention
[0013] Problems to be solved by the invention
[0014] However, in Patent Document 1, the thickness ratio of the NF nonwoven fabric of PBI is small relative to the thickness of the composite polymer electrolyte membrane, and the mechanical properties in the water-containing state are insufficient, and it cannot necessarily be said that the dry-wet cycle durability is excellent. In Patent Document 2, the NF nonwoven fabric of the solvent-soluble PBI is composited without drying after spinning, and there are the following problems: in the membrane-making process, the NF nonwoven fabric of PBI swells, deforms, and softens due to the solvent, so the mechanical properties in the water-containing state become insufficient, and the dry-wet cycle durability is insufficient. In addition, in Patent Document 3, there are the following problems: due to the increase in water absorption due to the infiltration of acid into the nanofiber nonwoven fabric, the mechanical properties in the water-containing state are insufficient, and the dry-wet cycle durability is insufficient. In Patent Document 4, since the membrane is formed by impregnating ePTFE, which is a hydrophobic and oleophobic compound, with an N-methylpyrrolidone (NMP) solution of polyarylene which does not contain fluorine atoms and has extremely low affinity with ePTFE, the membrane actually becomes a membrane having a large number of pores. Therefore, there are problems such as insufficient mechanical properties, especially in the water-containing state, and insufficient dry-wet cycle durability.
[0015] In view of the above background, the present invention aims to provide an electrolyte membrane which is a composite of a polymer electrolyte and a porous substrate, has good mechanical properties in both a dry state and a water-containing state, and can improve the dry-wet cycle durability of a fuel cell.
[0016] Means for solving problems
[0017] In order to solve the above problems, the composite polymer electrolyte membrane of the present invention has the following structure. That is:
[0018] A composite polymer electrolyte membrane comprises a polymer electrolyte and a porous substrate, wherein the composite polymer electrolyte membrane has a dry tensile elastic modulus per unit width of 100 N / cm or more and a hydrated tensile elastic modulus per unit width of 35 N / cm or more.
[0019] The electrolyte membrane with a catalyst layer of the present invention has the following structure. That is:
[0020] A composite polymer electrolyte membrane with a catalyst layer formed by sandwiching the above-mentioned composite polymer electrolyte membrane on both sides.
[0021] The membrane electrode assembly of the present invention has the following structure. That is:
[0022] A membrane electrode assembly comprising the above composite polymer electrolyte membrane.
[0023] The solid polymer fuel cell of the present invention has the following structure. That is:
[0024] A solid polymer fuel cell comprising the composite polymer electrolyte membrane.
[0025] The composite polymer electrolyte membrane of the present invention preferably has a water-containing tensile elastic modulus per unit cross-sectional area of 400 MPa or more.
[0026] In the composite polymer electrolyte membrane of the present invention, it is preferred that the ratio of the water-containing tensile elastic modulus to the dry tensile elastic modulus is 0.3 or more.
[0027] The composite polymer electrolyte membrane of the present invention preferably has a hydrated tensile elongation at break of 60% or more.
[0028] The composite polymer electrolyte membrane of the present invention preferably has a water-containing tensile strength of 5 N / cm or more.
[0029] In the hybrid polymer electrolyte membrane of the present invention, the porous substrate is preferably a fluorine-based porous substrate.
[0030] In the hybrid polymer electrolyte membrane of the present invention, the porous substrate preferably has an oxygen atom content of 10% by mass or less.
[0031] In the composite polymer electrolyte membrane of the present invention, it is preferred that the polymer electrolyte is a hydrocarbon polymer having an ionic group.
[0032] The composite polymer electrolyte membrane of the present invention preferably further contains a nonionic fluorine-based surfactant.
[0033] In the composite polymer electrolyte membrane of the present invention comprising the nonionic fluorine-based surfactant, the nonionic fluorine-based surfactant is preferably a compound having a fluorine-containing group formed of a fluorinated alkyl group, a fluorinated alkenyl group or a fluorinated aryl group and a nonionic mediophilic group.
[0034] In the hybrid polymer electrolyte membrane of the present invention, the porous substrate is preferably an aromatic hydrocarbon-based porous substrate.
[0035] In the hybrid polymer electrolyte membrane of the present invention, the porous substrate is preferably a polyazole-based porous substrate.
[0036] In the hybrid polymer electrolyte membrane of the present invention, the porous substrate is preferably formed of polybenzimidazole.
[0037] The composite polymer electrolyte membrane of the present invention preferably has a haze value of 20% or more and 45% or less when light is transmitted therethrough in the thickness direction.
[0038] The composite polymer electrolyte membrane of the present invention preferably has a diffuse transmittance of 20% or more and 40% or less when light is transmitted in the thickness direction.
[0039] Effects of the Invention
[0040] The electrolyte membrane of the present invention has good mechanical properties in both a dry state and a water-containing state, and can improve the wet-dry cycle durability of a fuel cell. DETAILED DESCRIPTION
[0041] Hereinafter, the present invention will be described in detail. Hereinafter, in this specification, "to" represents a range of numerical values including both ends thereof.
[0042] <Electrolyte membrane>
[0043] The electrolyte membrane of the present invention is an electrolyte membrane having a composite layer formed by a polymer electrolyte and a porous substrate, and is an electrolyte membrane having a dry tensile elastic modulus per unit width of more than 100N / cm and a water-containing tensile elastic modulus per unit width of more than 35N / cm. In a fuel cell, two diaphragms are usually compressed with screws, etc., so that each component is closely fitted, the resistance is reduced, and the power generation performance is improved, but when the dry tensile elastic modulus per unit width is less than 100N / cm, the electrolyte membrane is easily deformed and perforated due to the external force borne from the catalyst layer, the gas diffusion layer, etc., so that the dry-wet cycle durability becomes insufficient. In addition, when the water-containing tensile elastic modulus per unit width is less than 35N / cm, the softening of the electrolyte membrane in the water-containing state cannot be suppressed, and the dry-wet cycle durability as a fuel cell becomes insufficient. The porous substrate is preferably as described below with a hydrophobic compound as the main component, and is more preferably formed by a fluorine-based polymer compound with excellent water resistance and chemical resistance. In addition, a porous substrate formed by a hydrophobic aromatic hydrocarbon polymer compound having excellent elastic modulus and breaking strength can also be used appropriately. By using a porous substrate with a hydrophobic compound as the main component, it is easy to suppress the softening of the electrolyte membrane in a water-containing state and improve the water-containing tensile elastic modulus. By using such a polymer electrolyte membrane with excellent mechanical properties, the dry-wet cycle durability as a fuel cell can be improved. In the present invention, the dry tensile elastic modulus per unit width and the water-containing tensile elastic modulus per unit width are calculated using the methods described in (15) and (16) in the project of the embodiment, respectively.
[0044] The water-containing tensile elastic modulus per unit width of the electrolyte membrane is preferably 40 N / cm or more, more preferably 45 N / cm or more, and further preferably 48 N / cm or more. If the water-containing tensile elastic modulus per unit width is 40 N / cm or more, the softening of the electrolyte membrane in the water-containing state can be suppressed, and the dry-wet cycle durability as a fuel cell can be further improved.
[0045] The water-containing tensile elastic modulus per unit cross-sectional area of the electrolyte membrane is preferably 400MPa or more, more preferably 450MPa or more, and further preferably 500MPa or more. If the water-containing tensile elastic modulus per unit cross-sectional area is 400MPa or more, the softening of the electrolyte membrane in the water-containing state can be suppressed, and the dry-wet cycle durability as a fuel cell can be further improved. Not only that, the proton conductivity can be improved by thinning the electrolyte membrane while maintaining high mechanical properties, and the resistance as a fuel cell can be reduced to increase the output. The water-containing tensile elastic modulus per unit cross-sectional area is calculated using the method described in (16) in the project of the embodiment.
[0046] For the electrolyte membrane, the water-containing tensile elastic modulus / dry tensile elastic modulus, i.e., the value obtained by dividing the water-containing tensile elastic modulus per unit width by the dry tensile elastic modulus per unit width, is preferably 0.3 or more, and more preferably 0.35 or more. If the water-containing tensile elastic modulus / dry tensile elastic modulus is 0.3 or more, the difference in mechanical properties between the dry state and the water-containing state becomes smaller, so the generation of wrinkles and slack during dry-wet cycles is suppressed, and the dry-wet cycle durability as a fuel cell can be improved.
[0047] The aqueous tensile elongation at break of the electrolyte membrane is preferably 60% or more, more preferably 100% or more, and further preferably 140% or more. If the aqueous tensile elongation at break is 60% or more, even in the aqueous state where the electrolyte membrane is softened, even if it is subjected to stress concentration caused by wrinkles, relaxation, etc. caused by dry-wet cycles, the membrane is not easy to break, and the dry-wet cycle durability as a fuel cell can be improved. The aqueous tensile elongation at break is calculated using the method described in (16) in the project of the embodiment.
[0048] The aqueous tensile fracture strength of the electrolyte membrane is preferably 5 N / cm or more, more preferably 5.5 N / cm or more, and further preferably 6 N / cm or more. If the aqueous tensile fracture strength is 5 N / cm or more, even in the aqueous state where the electrolyte membrane is softened, even if it is subjected to stress concentration caused by wrinkles, relaxation, etc. caused by dry-wet cycles, the membrane is not easy to break, and the dry-wet cycle durability as a fuel cell can be improved. The aqueous tensile fracture elongation is calculated using the method described in (16) in the project of the embodiment.
[0049] The filling rate of the polymer electrolyte in the composite layer is preferably 50% or more, more preferably 60% or more. When the filling rate of the composite layer is 50% or more, the power generation performance can be improved by forming a continuous proton conduction path in the composite polymer electrolyte membrane as a whole. It should be noted that the filling rate of the composite layer in the present invention is a value indicating the proportion of the polymer electrolyte relative to the total volume of the composite layer, which can be calculated by the ion exchange capacity (IEC). Specifically, it is carried out by the method described in (4) in the project of the embodiment.
[0050] Electrolyte membrane can be formed with a polymer electrolyte layer that is not composited with reinforcing materials such as porous substrates on both sides or one side of the composite layer. By having such a layer, the bonding property of the electrolyte membrane and the electrode can be improved, and interface peeling can be suppressed. In the case of forming a polymer electrolyte layer that is not composited with reinforcing materials in contact with both sides or one side of the composite layer, the polymer electrolyte constituting the layer is preferably a polymer identical to the polymer electrolyte filled in the composite layer.
[0051] The electrolyte membrane of the present invention has a composite layer, which can reduce the dimensional change rate in the plane direction. By reducing the dimensional change rate in the plane direction, when used as an electrolyte membrane of a fuel cell, it is possible to reduce the stress caused by swelling and shrinkage at the edge of the electrolyte membrane during dry-wet cycles, and it is easy to improve durability. The dimensional change rate λ in the plane direction of the electrolyte membrane xy It is preferably 10% or less, more preferably 8% or less, and further preferably 5% or less.
[0052] In addition, regarding the dimensional change rate in the plane direction of the electrolyte membrane, it is preferred that the anisotropy in MD and TD be small. Specifically, it is preferred that the dimensional change rate λ in MD be MD Dimension change rate λ relative to TD TD The ratio of MD / λ TD Satisfy 0.5≤λ MD / λ TD ≤2.0. Here, MD is the abbreviation of Machine Direction, which refers to the direction in which the porous substrate, coater or coating substrate is moved in the electrolyte membrane manufacturing process described later. As to which of the porous substrate, coater or coating substrate is moved, it is appropriately determined according to the coating process and is not particularly limited. In the case of a process for moving multiple elements of a porous substrate, a coater or a coating substrate, most of the elements are usually moved in the same direction, but a process for moving them in different directions can also be applied. In this case, the order of movement is determined in (1) coating substrate, (2) coater, and (3) porous substrate, and the direction that is the same as the highest-ranking element among the moving elements is defined as MD. TD is the abbreviation of Traverse Direction, which is the direction orthogonal to MD in the surface direction of the electrolyte membrane.
[0053] Dimensional change rate of MD λ MD Dimension change rate λ relative to TD TD The ratio (λ MD / λ TD ) satisfies 0.5≤λ MD / λ TD When ≤2.0, the design of the unit cell of the fuel cell is not restricted. Even at the edge orthogonal to the direction of large dimensional change in the MD and TD directions, the concentration of stress caused by swelling and shrinkage is small. Therefore, this edge is not likely to become the starting point of electrolyte membrane rupture, which can improve dry-wet cycle durability.
[0054] Here, the dimensional change rate is an index showing the change between the dimension of the electrolyte membrane in a dry state and the dimension of the electrolyte membrane in a wet state, and is specifically measured by the method described in item (6) of the Examples.
[0055] The thickness of the composite layer in the electrolyte membrane is not particularly limited, but is preferably 0.5 μm or more, more preferably 1 μm or more. In addition, it is preferably 50 μm or less, more preferably 40 μm or less. When the composite layer is 0.5 μm or more and 50 μm or less, the proton conductivity is high, electrical short circuits and fuel permeation can be suppressed, and a composite polymer electrolyte membrane with excellent dry-wet cycle durability can be obtained.
[0056] For the electrolyte membrane, the haze when light is transmitted in the thickness direction is preferably 20% to 45%, more preferably 30% to 45%, and further preferably 35% to 45%. In the case where there is a substance with a refractive index different from that of the polymer electrolyte, such as a porous substrate, in the electrolyte membrane, haze is sometimes generated due to light scattering at the interface between the polymer electrolyte and the substance with a different refractive index. If the haze is 20% to 45%, the polymer electrolyte responsible for the conduction of protons and the porous substrate responsible for improving mechanical properties such as elastic modulus, elongation at break, and breaking strength are composited with good balance, thereby obtaining an electrolyte membrane with excellent proton conductivity and mechanical properties, which can simultaneously achieve excellent output and dry-wet cycle durability as a fuel cell. The haze is calculated using the method described in (17) in the project of the embodiment.
[0057] For the electrolyte membrane, the diffusion transmittance when light is transmitted in the thickness direction is preferably 20% to 40%, and more preferably 30% to 40%. If the diffusion transmittance is 20% to 40%, an electrolyte membrane having excellent proton conductivity and mechanical properties can be obtained, and excellent output and dry-wet cycle durability can be achieved as a fuel cell. The diffusion transmittance is calculated using the method described in (17) in the example.
[0058] 〔Polymer electrolyte〕
[0059] The polymer electrolyte used in the present invention refers to a polymer having proton conductivity due to having an ionic group, and may be any of a fluorine-based polymer electrolyte and a hydrocarbon-based polymer.
[0060] Here, the so-called fluorine-based polymer electrolyte refers to an electrolyte in which most or all of the hydrogen in the alkyl and / or alkylene groups in the polymer is replaced by fluorine atoms. As a representative example of a fluorine-based polymer electrolyte with an ionic group, commercial products such as "Nafion" (registered trademark) (Chemours (Strain) system), "Aquivion" (registered trademark) (Solvay Company system), "Flemion" (registered trademark) (AGC (Strain) system) and "Aciplex" (registered trademark) (Asahi Chemical (Strain) system) can be cited.
[0061] These fluorine-based polymer electrolytes are usually very expensive, and there is a tendency for gas permeation to be large. Therefore, from the aspects of mechanical strength, dry-wet cycle durability, chemical stability, etc., it is also preferred that the polymer electrolyte used in the present invention is a hydrocarbon polymer. That is, in the present invention, it is preferred that the polymer electrolyte is a hydrocarbon polymer with an ionic group. In particular, in the composite membrane of the present invention, from the aspect of having excellent mechanical properties in any state in a dry state and a water-containing state, the mode in which the polymer electrolyte is a hydrocarbon polymer is also particularly preferred.
[0062] As the hydrocarbon polymer, an aromatic hydrocarbon polymer having an aromatic ring in the main chain is preferred. Here, as the aromatic ring, not only hydrocarbon aromatic rings formed only by carbon atoms and hydrogen atoms such as a benzene ring and a naphthalene skeleton are included, but also heterocyclic rings such as a pyridine ring, an imidazole ring, and a thiol ring may be included. In addition, a part of the aliphatic unit may constitute the polymer together with the aromatic ring unit.
[0063] As specific examples of aromatic hydrocarbon polymers, there can be cited polymers having an aromatic ring and a structure selected from polysulfone, polyethersulfone, polyphenylene ether, polyarylene ether polymer, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene polymer, polyarylene ketone, polyetherketone, polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone on the main chain. It should be noted that the so-called polysulfone, polyethersulfone, polyetherketone, etc. here are collectively referred to as structures having sulfone bonds, ether bonds, and ketone bonds on their molecular chains, including polyetherketoneketone, polyetheretherketone, polyetheretherketoneketone, polyetherketoneetherketoneketone, polyetherketonesulfone, etc. The hydrocarbon skeleton can have a variety of structures in these structures. Among these, as aromatic hydrocarbon polymers, polymers having a polyetherketone skeleton, i.e., polyetherketone polymers, are particularly preferred.
[0064] As the polymer electrolyte, a polymer electrolyte that forms a co-continuous or layered phase separation structure is preferred. Such a phase separation structure can be formed, for example, in a molded body formed of a blend of two or more incompatible polymers such as a hydrophilic polymer having an ionic group and a hydrophobic polymer not having an ionic group, or in a molded body formed of a segment (S) containing an ionic group.E1 ) and segments without ionic groups (S E2 ) is presented in a block copolymer formed by two or more incompatible segments such as . In the co-continuous and layered phase separation structure, the hydrophilic domain and the hydrophobic domain both form a continuous phase, so a continuous proton conduction channel can be formed, thereby easily obtaining an electrolyte membrane with excellent proton conductivity. At the same time, a continuous hydrophobic skeleton can also be formed, thereby easily obtaining an electrolyte membrane with excellent mechanical properties not only in a dry state but also in a water-containing state. Here, the so-called domain refers to a block formed by the aggregation of similar substances and segments in a membrane.
[0065] As the polymer electrolyte, it is particularly preferred to have a segment (S) containing an ionic group. E1 ), and segments without ionic groups (S E2 ) each with one or more block copolymers. Here, the so-called segment is a partial structure in the copolymer polymer chain formed by repeating units showing specific properties, indicating a structure with a molecular weight of 2,000 or more. By using a block copolymer, a co-continuous or lamellar phase separation structure having finer domains than a polymer blend can be presented, and better power generation performance and dry-wet cycle durability can be achieved.
[0066] Hereinafter, the segment containing an ionic group (S E1 ) or polymers are described as "ionic blocks", and the segments without ionic groups (S E2 ) or polymer is described as a "nonionic block". However, the statement "does not contain ionic groups" in this specification does not exclude the mode in which the segment or polymer contains a small amount of ionic groups within a range that does not hinder the formation of a phase separation structure.
[0067] In such a block copolymer, the molar composition ratio (S) of the ionic block to the nonionic block is E1 / S E2 ) is preferably 0.20 or more, more preferably 0.33 or more, and further preferably 0.50 or more. E1 / S E2 ) is preferably 5.00 or less, more preferably 3.00 or less, and further preferably 2.50 or less. E1 / S E2 ) is 0.20 or more or 5.00 or less, a composite polymer electrolyte membrane having high proton conductivity under low humidification conditions and excellent hot water resistance and dry-wet cycle durability can be obtained. E1 / S E2), represents the ratio of the number of moles of repeating units present in the ionic block to the number of moles of repeating units present in the nonionic block. The so-called "number of moles of repeating units" is the value obtained by dividing the number average molecular weight of the ionic block and the nonionic block by the molecular weight of the corresponding structural unit.
[0068] The ionic groups possessed by the polymer electrolyte can be any ionic groups having proton exchange capacity. As such functional groups, preferably sulfonic acid groups, sulfonimide groups, sulfate groups, phosphonic acid groups, phosphoric acid groups, and carboxylic acid groups are used. Two or more ionic groups may be included in the polymer. Among them, from the perspective of high proton conductivity, the polymer more preferably has at least one selected from sulfonic acid groups, sulfonimide groups, and sulfate groups, and from the perspective of raw material cost, it is most preferably to have a sulfonic acid group.
[0069] Considering the balance between proton conductivity and water resistance, the ion exchange capacity (IEC) of the polymer electrolyte is 0.1 meq / g or more, preferably 5.0 meq / g or less. IEC is more preferably 1.4 meq / g or more, and further preferably 1.7 meq / g or more. In addition, IEC is more preferably 3.5 meq / g or less, and further preferably 3.0 meq / g or less. When IEC is 0.1 meq / g or more and 5.0 meq / g or less, excellent proton conductivity and water resistance can be achieved simultaneously.
[0070] Here, the so-called IEC is the molar amount of the ionic group introduced per unit dry weight of the polymer electrolyte, and the larger the value, the more the amount of ionic group introduced. In the present invention, IEC is defined as the value obtained by neutralization titration. The calculation of IEC based on neutralization titration is performed by the method described in (2) in the project of the embodiment.
[0071] In the present invention, as the polymer electrolyte, it is particularly preferred to use an aromatic hydrocarbon block copolymer, and more preferably a polyetherketone block copolymer. Among them, it is particularly preferred to use a polyetherketone block copolymer containing a segment of a structural unit containing an ionic group represented by the following general formula (S1) and a segment of a structural unit containing no ionic group represented by the following general formula (S2).
[0072] [Chemical formula 1]
[0073]
[0074] In the general formula (S1), Ar 1 ~Ar 4 represents any divalent arylene group, Ar 1 and / or Ar 2 Contains ionic groups, Ar 3 and Ar4 It may or may not contain an ionic group. 1 ~Ar 4 The arylene group may be arbitrarily substituted, and two or more arylene groups may be used independently of each other. * represents a bonding site to the general formula (S1) or other structural units.
[0075] [Chemical formula 2]
[0076]
[0077] In the general formula (S2), Ar 5 ~Ar 8 represents an arbitrary divalent arylene group, which may be arbitrarily substituted but does not contain an ionic group. 5 ~Ar 8 Two or more arylene groups may be used independently of each other. * represents a bonding site to the general formula (S2) or other structural units.
[0078] Here, regarding Ar 1 ~Ar 8 Preferred divalent arylene groups include hydrocarbon arylene groups such as phenylene, naphthylene, biphenylene, and fluorenediyl, and heteroarylene groups such as pyridinediyl, quinoxalinediyl, and thiophenediyl, but are not limited to these. Here, "phenylene" may be o-phenylene, m-phenylene, and p-phenylene, depending on the position of the bonding site with the benzene ring and other structural units, but in this specification, it is used as a general term for them without special limitations. The same is true for other divalent arylene groups such as "naphthylene" and "biphenylene". Ar 1 ~Ar 8 Preferably, it is a phenylene group and a phenylene group containing an ionic group, and most preferably, it is a p-phenylene group and a p-phenylene group containing an ionic group. 5 ~Ar 8 It may be substituted with a group other than an ionic group, but is more preferably unsubstituted from the viewpoint of proton conductivity, chemical stability, and wet-dry cycle durability.
[0079] In addition, in order to obtain sufficient dimensional stability, mechanical strength, dry-wet cycle durability, fuel barrier properties, and solvent resistance, the polymer electrolyte is preferably a crystalline aromatic hydrocarbon polymer. Here, "crystalline" means: having the property of being crystallizable (crystallizable when heated) or having been crystallized.
[0080] The presence or absence of crystallinity can be confirmed by differential scanning calorimetry (DSC) or wide-angle X-ray diffraction. In the present invention, it is preferred that the heat of crystallization measured by differential scanning calorimetry after film formation is 0.1 J / g or more, or the degree of crystallinity measured by wide-angle X-ray diffraction is 0.5% or more. That is, when no crystallization peak is observed in differential scanning calorimetry, it can be considered that the film has been crystallized and the polymer electrolyte is amorphous. In the case of crystallization, according to wide-angle X-ray diffraction, the degree of crystallinity is 0.5% or more.
[0081] For aromatic hydrocarbon polymers with crystallinity, the processability of the electrolyte membrane is sometimes poor. In this case, a protecting group can be introduced into the aromatic hydrocarbon polymer to temporarily suppress crystallinity. Specifically, the membrane is formed in a state where the protecting group is introduced, and then deprotection is performed, so that the aromatic hydrocarbon polymer with crystallinity can be used as a polymer electrolyte in the present invention.
[0082] 〔Porous substrate〕
[0083] The porous substrate used in the present invention can be classified into a hydrocarbon porous substrate with a hydrocarbon polymer compound as the main component and a fluorine porous substrate with a fluorine polymer compound as the main component. Examples of the hydrocarbon polymer compound include polyethylene (PE), polypropylene (PP), polystyrene (PS), polyacrylate, polymethacrylate, polyvinyl chloride (PVC), polyvinylidene chloride (PVdC), polyester, polycarbonate (PC), polysulfone (PSU), polyethersulfone (PES), polyphenylene ether (PPO), polyarylene ether polymer, polyphenylene sulfide (PPS), polyphenylene sulfide sulfone, polyparaphenylene (PPP), polyarylene polymer, polyarylene ketone, polyether ketone (PEK), polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole (PBO), polyphenylene Thiazole (PBT), polybenzimidazole (PBI), polyamide (PA), polyimide (PI), polyetherimide (PEI), polyimide sulfone (PIS), etc., as fluorine-based polymer compounds, polytetrafluoroethylene (PTFE), polyhexafluoropropylene, tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVdF), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxy fluororesin (PFA), ethylene-chlorotrifluoroethylene copolymer (ECTFE), etc., but are not limited to these. From the viewpoint of water resistance, chemical resistance, mechanical properties, preferably PE, PP, PPS, PEK, PBO, PBT, PBI, PTFE, polyhexafluoropropylene, FEP, PFA.
[0084] Fluorine-based porous substrates are usually based on fluorine-based polymer compounds with extremely high hydrophobicity. Therefore, by being composited with polymer electrolytes, water resistance is given to the electrolyte membrane, and the mechanical properties in the water-containing state are improved to suppress the effect of dimensional change. In addition, usually, the polymer compound containing fluorine atoms has low solubility in medicines and is stable relative to chemical reactions. Therefore, chemical resistance and chemical durability can also be given to the electrolyte membrane, so it is preferred. From the viewpoint of chemical resistance and chemical durability, PTFE, polyhexafluoropropylene, FEP, PFA are more preferred, and PTFE is particularly preferred from the perspective of having high mechanical strength through molecular orientation.
[0085] From the viewpoint of water resistance, the porous substrate is preferably a fluorine-based porous substrate containing 50% by mass or more of fluorine atoms, more preferably a fluorine-based porous substrate containing 60% by mass or more of fluorine atoms, and particularly preferably a fluorine-based porous substrate containing 70% by mass or more of fluorine atoms. The fluorine atom content in the porous substrate is a value measured by ion chromatography of a solution that absorbs the gas generated by burning the porous substrate, and specifically, it can be measured by the method described in (10) in the project of the embodiment described later.
[0086] The oxygen atom content of the porous substrate measured by X-ray photoelectron spectroscopy (XPS) is preferably 10% by mass or less, more preferably 8% or less, and further preferably 5% or less. When the oxygen atom content is within the above-mentioned preferred range, the water absorption of the porous substrate does not increase, and the dimensional change of the electrolyte membrane when absorbing water can be suppressed. Specifically, the oxygen atom content of the porous substrate can be measured by the method described in (14) in the item of the embodiment described later.
[0087] Aromatic hydrocarbon-based porous substrates with hydrocarbon-based polymer compounds having aromatic rings on the main chain as the main component are also generally hydrophobic compounds, and have excellent elastic modulus and breaking strength, and therefore can be used appropriately. Among them, from the viewpoints of elastic modulus, breaking strength, and chemical durability, PPS, PBO, PBT, PBI, and PEK are more preferred, from the viewpoints of chemical resistance and processability, PBO, PBT, and PBI as polyazole compounds are particularly preferred, and from the viewpoints of cost and circulation, PBI is most preferred.
[0088] In addition, when analyzing the porous substrate present in the electrolyte membrane after being composited with the polymer electrolyte, only the porous substrate can be extracted by immersing the electrolyte membrane in a solvent that dissolves only the polymer electrolyte.
[0089] As forms of porous substrates, there can be cited: a stretched microporous membrane in which a raw material membrane is stretched along the membrane surface direction to form fine pores; a wet coagulation microporous membrane obtained by preparing a raw material solution and forming a membrane, and then immersing the raw material in a poor solvent for the raw material while maintaining a solvent-containing state to cause it to coagulate; a nonwoven fabric formed of solution spun fibers obtained by spinning a raw material solution; a nonwoven fabric formed of melt spun fibers obtained by melting the raw material of the porous substrate and spinning it, etc.
[0090] Methods for solution spinning include: dry spinning, in which a raw material solution ejected from a nozzle in the form of fibers is dried using hot air; wet spinning, in which the raw material solution ejected in the form of fibers is immersed in a poor solvent for the raw material to coagulate it; and electrostatic spinning, in which a raw material solution is ejected into a space to which a high voltage is applied and the solution is stretched into fibers using static electricity.
[0091] Examples of the melt spinning method include melt blow spinning in which a molten raw material of a porous base material is blown out from a nozzle in the form of fibers.
[0092] The porous substrate preferably has a structure in which coarse fibrous nodes are arranged substantially in parallel in the in-plane direction. With this structure, an electrolyte membrane having excellent mechanical properties in a direction parallel to the nodes, particularly in a water-containing state, can be obtained.
[0093] The porous substrate preferably contains nodes having an aspect ratio of 10 or more calculated from the length / diameter, more preferably contains nodes having an aspect ratio of 20 or more, and further preferably contains nodes having an aspect ratio of 50 or more. If the porous substrate contains nodes having an aspect ratio of 10 or more, it has a structure with a strong continuous hydrophobic skeleton, and therefore, the softening of the entire membrane is suppressed not only in a dry state but also in a hydrated state where the polymer electrolyte is usually softened due to water absorption, thereby obtaining an electrolyte membrane with excellent mechanical properties, which can improve the dry-wet cycle durability as a fuel cell.
[0094] The average diameter of the nodes is preferably 0.01 μm or more, more preferably 0.1 μm, and further preferably 0.2 μm. In addition, it is preferably 10 μm or less, more preferably 5 μm or less, and further preferably 2 μm or less. When the average diameter of the nodes is 0.01 μm or more and 10 μm or less, softening of the electrolyte membrane in a water-containing state can be suppressed, and an electrolyte membrane with high proton conductivity can be obtained, so that a fuel cell with high output can be manufactured.
[0095] The porous substrate preferably has fibrillar fibrils that connect the aforementioned nodes to each other in the in-plane direction to form a ladder-like structure. The aforementioned fibrils more preferably include fibrils arranged approximately orthogonally to the aforementioned nodes. By having this structure, an electrolyte membrane having excellent mechanical properties not only in the in-plane direction parallel to the nodes but also in the direction orthogonal to the nodes, especially in a water-containing state, can be obtained.
[0096] The diameter ratio calculated from the average diameter of the aforementioned nodes / the average diameter of the aforementioned fibrils is preferably 2 or more, more preferably 3 or more, and further preferably 5 or more. In addition, the diameter ratio is preferably 20 or less, more preferably 10 or less. When a porous substrate having a diameter ratio of 2 or more and 20 or less is used, the obstruction of proton conduction caused by the nodes is suppressed, thereby an electrolyte membrane having high proton conductivity can be obtained, so that a fuel cell having high output can be manufactured, and swelling in a direction orthogonal to the nodes and / or in a direction parallel to the nodes can be suppressed, so that a composite polymer electrolyte membrane having low anisotropy and excellent mechanical properties can be manufactured.
[0097] Here, the structure of the porous substrate such as the orientation and average diameter of nodes and the orientation and average diameter of fibrils can be analyzed using a scanning electron microscope (SEM) by the method described in item (18) of the Examples.
[0098] There is no particular restriction on the thickness of the porous substrate used in the present invention, which should be determined according to the purpose of the electrolyte membrane. However, in practice, a porous substrate with a film thickness of 0.5 μm to 50 μm can be used, and preferably a porous substrate with a film thickness of 1 μm to 40 μm can be used.
[0099] The porosity of the porous substrate before being composited with the polymer electrolyte is not particularly limited, but is preferably 50 to 98%, more preferably 70 to 98%, from the viewpoint of achieving both proton conductivity and mechanical strength of the obtained electrolyte membrane. It should be noted that the porosity Y1 (volume %) of the porous substrate is defined as a value obtained using the following mathematical formula.
[0100] Y1=(1-Db / Da)×100
[0101] (Here, Da is the specific gravity of the raw material material constituting the porous substrate, and Db is the specific gravity of the entire porous substrate.)
[0102] [Nonionic fluorinated surfactant]
[0103] In the electrolyte membrane of the present invention, it is preferred to include a nonionic fluorine-based surfactant (hereinafter, sometimes referred to as "surfactant"). By using a nonionic fluorine-based surfactant, the affinity of the polymer electrolyte and the porous substrate is improved, thereby, not only is it easy to manufacture the electrolyte membrane, but also the interface bonding of the polymer electrolyte in the electrolyte membrane and the porous substrate becomes firm, suppressing the interface peeling of the two that occurs due to the volume change of the electrolyte membrane in the dry-wet cycle, thereby improving the dry-wet cycle durability of the fuel cell. In particular, when using a hydrocarbon-based polymer electrolyte and a fluorine-based porous substrate, the affinity of the two can be significantly improved, so it is more preferred.
[0104] The surfactant is preferably a compound having a fluorine-containing group formed by a fluoroalkyl, fluoroalkenyl or fluoroaryl group obtained by substituting a hydrogen atom in an alkyl, alkenyl or aryl group with a fluorine atom, and a nonionic mesophilic group (hydrophilic group or lipophilic group).
[0105] The fluorine-containing group is preferably a perfluoroalkyl group, a perfluoroalkenyl group or a perfluoroaryl group obtained by replacing all hydrogen atoms in the alkyl group, the alkenyl group or the aryl group with fluorine atoms.
[0106] As the fluorine-containing group, a fluoroalkenyl group or a fluoroaryl group is more preferred from the viewpoint of excellent surface active effect, and a fluoroalkenyl group is further preferred from the viewpoint of having a flexible structure and exhibiting a high surface active effect.
[0107] The number of carbon atoms of the fluorine-containing group is preferably 2 or more, more preferably 4 or more, and particularly preferably 6 or more. In addition, the number of carbon atoms is preferably 20 or less, more preferably 15 or less, and particularly preferably 10 or less. When the number of carbon atoms is within the above preferred range, volatility and water solubility remain moderately in the electrolyte membrane, and the dry-wet cycle durability is excellent. On the other hand, it is not easy to separate from the polymer electrolyte, and the dry-wet cycle durability is excellent.
[0108] Specific examples of the fluorinated alkyl group include, but are not limited to, a fluorinated ethyl group, a fluorinated propyl group, a fluorinated butyl group, a fluorinated pentyl group, a fluorinated hexyl group, a fluorinated heptyl group, a fluorinated octyl group, a fluorinated nonyl group, and a fluorinated decyl group.
[0109] Examples of the fluoroalkenyl group include fluorovinyl, fluoropropenyl, fluorobutenyl, fluoropentenyl, fluorohexenyl, fluoroheptenyl, fluorooctenyl, fluorononenyl and fluorodecenyl, but are not limited thereto.
[0110] Among these, from the perspective of volatility, low water solubility, and being easily retained in the electrolyte membrane, it is more preferably fluorohexyl, fluoroheptyl, fluorooctyl, fluorononyl, fluorodecyl, fluorohexenyl, fluoroheptenyl, fluorooctenyl, fluorononenyl, and fluorodecenyl. Here, as "fluoroethyl", according to the number of fluorine atoms contained in one functional group, it can be 5 functional groups of monofluoroethyl, difluoroethyl, trifluoroethyl, tetrafluoroethyl, and pentafluoroethyl, but in this specification, "fluoroethyl" is used as a general term for them. It is also the same for other functional groups such as "fluoropropyl" and "fluorobutyl". In addition, in the case of the aforementioned difluoroethyl, it is a functional group with 2 carbon atoms and 2 fluorine atoms, and there are 3 structural isomers such as 1,1-difluoroethyl, 1,2-difluoroethyl, and 2,2-difluoroethyl, but in this specification, "difluoroethyl" is used as a general term for them. The same is true for other functional groups such as "trifluoroethyl" and "tetrafluoroethyl". In addition, in "fluorobutyl", the term "butyl" is a general term for functional groups formed by a skeleton with 4 carbon atoms. There are 4 structures, namely butyl, 1-methylpropyl, 2-methylpropyl, and 1,1-dimethylethyl, but in this specification, "butyl" is used as a general term for them. The same is true for other functional groups such as "fluoropentyl" and "fluorohexyl".
[0111] The structure of the fluorine-containing group can be linear, branched, cyclic, etc., wherein, in the case of a branched structure, the interaction between the fluorine compounds becomes weak, and the surface tension is easily reduced, so it is preferred. In the present invention, a surfactant having a fluorine-containing group formed by a structure shown in the following formula (F1) is particularly preferred.
[0112] [Chemical formula 3]
[0113]
[0114] In formula (F1), * indicates a bonding position with other atomic groups.
[0115] As a nonionic fluorine-based surfactant, a compound having 10% or more fluorine atoms in one molecule can be preferably used. More preferably, a compound having 20% or more fluorine atoms, and further preferably a compound having 40% or more fluorine atoms. When the fluorine atom content in one molecule is within the above-mentioned preferred range, the affinity with the porous substrate is excellent, and a sufficient effect of improving power generation performance can be obtained. In addition, the solubility in water and acid is low, and it is difficult to dissolve in water and acid generated when the electrochemical unit cell of a fuel cell or the like is operated, so it will not dissolve from the electrolyte membrane, and the affinity of the polymer electrolyte and the catalyst layer can be prevented from decreasing.
[0116] The mediophilic group may be a hydrophilic group or a lipophilic group, but is preferably a hydrophilic group.
[0117] The hydrophilic group is not particularly limited as long as it is a nonionic group having a hydrophilic element selected from the group consisting of oxygen, nitrogen, phosphorus, sulfur and boron, but is preferably a group comprising a polyether group, a carboxylate group, a sulfonate group, a phosphite group or a phosphate group. From the perspective of excellent affinity with polymer electrolytes by forming hydrogen bonds with ionic groups and excellent chemical stability, a group comprising a polyether group is more preferred. Among them, the hydrophilic group is preferably a group having a polyalkyl ether structure represented by the following general formula (C1) or a polyacrylate structure represented by the following general formula (C2). In particular, from the perspective of excellent affinity with polymer electrolytes, a polyalkyl ether represented by the following general formula (C1) is more preferred.
[0118] [Chemical formula 4]
[0119]
[0120] In the general formula (C1), q and r are natural numbers satisfying r=2q, and s is an integer of 1 to 1,000, which represents the number of repetitions of the alkyl ether structure. In the general formula (C2), R is at least one group selected from an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 1 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms, and t is an integer of 1 to 1,000, which represents the number of repetitions of the acrylate structure. In (C1) or (C2), when s or t is 2 or more, the multiple alkyl ether structures or acrylate structures may be the same or different.
[0121] Examples of the lipophilic group include an alkyl group, an alkenyl group, an alkynyl group, and a phenyl group that do not contain a fluorine atom.
[0122] In the present invention, the nonionic fluorine-based surfactant is preferably a compound having a vapor pressure of less than 2 kPa at 150°C, more preferably a compound having a vapor pressure of less than 1 kPa at 150°C, and most preferably a compound having no boiling point, that is, a compound that begins to thermally decompose without boiling. In the present invention, it is particularly preferred that the surfactant is a compound having a 5% weight loss temperature of 150°C or more in thermogravimetric differential thermal analysis. If it is such a surfactant, it will not volatilize or decompose during film formation, so it can remain in the electrolyte membrane.
[0123] In the present invention, the nonionic fluorine-based surfactant is preferably a compound having a weight average molecular weight of 1,000 or more, more preferably a compound having a weight average molecular weight of 1,500 or more, and further preferably a compound having a weight average molecular weight of 2,000 or more. In addition, the nonionic fluorine-based surfactant is preferably a compound having a weight average molecular weight of 10,000 or less, more preferably a compound having a weight average molecular weight of 8,000 or less, and further preferably a compound having a weight average molecular weight of 5,000 or less. When the weight average molecular weight of the surfactant is within the above-mentioned preferred range, the volatility is moderate and it is difficult to dissolve in solvents such as water. Therefore, the affinity between the polymer electrolyte and the porous substrate and the catalyst layer described later is maintained, and it is not easy to peel off and break at the interface between the two, and the durability is excellent. On the other hand, in the electrolyte membrane, only the surfactant aggregates, and it is not easy to form a sea island-like phase separation structure, and it is not easy to break at the interface between the surfactant and the polymer electrolyte and the porous substrate, and the durability is excellent.
[0124] As a surfactant, the molecular weight of the fluorine-containing group is preferably 200 or more, more preferably 400 or more, and further preferably 1,000 or more. In addition, the molecular weight of the fluorine-containing group is preferably 5,000 or less, more preferably 3,000 or less, and further preferably 2,000 or less. When the molecular weight of the fluorine-containing group is within the above-mentioned preferred range, the flexibility and freedom of the molecular chain in the fluorine-containing group are excellent, thereby maintaining affinity with the porous substrate and the catalyst layer, and it is not easy to peel off and break at the interface with the polymer electrolyte, and the durability is excellent. On the other hand, in the electrolyte membrane, only the surfactant aggregates, and it is not easy to form an island-like phase separation structure, and it is not easy to break at the interface between the surfactant and the polymer electrolyte and the porous substrate, and the durability is excellent.
[0125] In the case of a surfactant having a hydrophilic group as a mesophilic group, the molecular weight of the hydrophilic group is preferably 100 or more, more preferably 200 or more, and further preferably 500 or more. In addition, the molecular weight of the hydrophilic group is preferably 4,000 or less, more preferably 2,500 or less, and further preferably 1,500 or less. When the molecular weight of the hydrophilic group is within the above preferred range, the flexibility and freedom of the molecular chain in the hydrophilic group are excellent, thereby maintaining affinity with the polymer electrolyte, not easily breaking at the interface with the porous substrate, and having excellent durability. On the other hand, the water solubility is moderate, and thus it is difficult to dissolve in water and acid generated when operating an electrochemical unit cell such as a fuel cell, and dissolution from the electrolyte membrane is prevented. Therefore, the affinity between the polymer electrolyte and the porous substrate is maintained, and it is not easy to break at the interface between the polymer electrolyte and the porous substrate when the size changes, and the durability is excellent.
[0126] In addition, the surfactant is preferably a compound that is insoluble in any one of water, 10% sulfuric acid, and 10% sodium hydroxide aqueous solution, more preferably a compound that is insoluble in water, and most preferably a compound that is insoluble in any one of them. Here, the so-called insoluble means that the saturated solubility at 25°C is less than 0.1% by mass. When the surfactant is insoluble in the solvent and / or solution, it becomes difficult to dissolve in water and acid generated when the electrochemical unit cell such as a fuel cell is operated, and the dissolution from the electrolyte membrane can be suppressed, so that the affinity of the polymer electrolyte with the porous substrate and the catalyst layer can be maintained, so that the reduction in durability caused by peeling and rupture at the interface of the polymer electrolyte with the porous substrate and the catalyst layer when the size changes can be suppressed.
[0127] Examples of the nonionic fluorine-based surfactant used in the present invention include MEGAFACE (registered trademark) F-251, MEGAFACE F-253, MEGAFACE F-281, MEGAFACE F-430, MEGAFACE F-477, MEGAFACE F-551, MEGAFACE F-552, MEGAFACE F-553, MEGAFACE F-554, MEGAFACE F-555, MEGAFACE F-556, MEGAFACE F-557, MEGAFACE F-558, MEGAFACE F-559, MEGAFACE F-560, MEGAFACE F-561, MEGAFACE F-562, MEGAFACE F-563, MEGAFACE F-565, MEGAFACE F-568, MEGAFACE F-570, MEGAFACE F-571, MEGAFACE F-572, MEGAFACE F-573, MEGAFACE F-574, MEGAFACE F-575, MEGAFACE F-576, MEGAFACE F-577, MEGAFACE F-578, MEGAFACE F-579, MEGAFACE F-580, MEGAFACE F-581, MEGAFACE F-582, MEGAFACE F-583, MEGAFACE F-584, MEGAFACE F-585 MEGAFACE RS-76-E, MEGAFACE RS-76-NS, MEGAFACE DS-21, MEGAFACE F444, MEGAFACE TF-2066, "SURFLON" (registered trademark) made by AGC Co., Ltd. S-141, SURFLON S-145, SURFLON S-241, SURFLON S-242, SURFLON S-243, SURFLON S-386, SURFLON S-420, SURFLON S-611, SURFLON S-651, "Ftergent" (registered trademark) 251 made by NEOS Co., Ltd., Ftergent 208M, Ftergent 212M, Ftergent 215M, Ftergent 250, Ftergent 209F, Ftergent 222F, Ftergent 245F, Ftergent 208G, Ftergent 218GL、Ftergent 240G、Ftergent 212P、Ftergent 220P、Ftergent 228P、Ftergent FTX-218、Ftergent DFX-18、Ftergent710FL、Ftergent 710FM、Ftergent 710FS、Ftergent 730FL、Ftergent 730FM、Ftergent 610FM、Ftergent 683、Ftergent 601AD、Ftergent 601ADH2、Ftergent 602A、Ftergent 650AC、Ftergent 681、EF-PP31N04、EF-PP31N09、EF-PP31N15、EF-PP31N22 made by Mitsubishi Materials Electronic Chemicals Co., Ltd.、FC-4430、FC-4432 made by 3M、PF-151N、PF-636、PF-6320、PF-656、PF-6520、PF-652-NF、PF-3320 made by OMNOVA SOLUTIONS、Daikin TG-9131 manufactured by KOGYO Industries, Ltd., "ZEFFLE" (registered trademark) GH-701, "Fluorolink" (registered trademark) A10-P manufactured by Solvay Japan Co., Ltd., and the like.
[0128] The content of the nonionic fluorine-based surfactant in the electrolyte membrane is preferably 0.005 or more, more preferably 0.01 or more, in terms of the mass ratio relative to the total amount of the polymer electrolyte contained in the electrolyte membrane. In addition, it is preferably 0.20 or less, more preferably 0.10 or less. When the ratio is within the above-mentioned preferred range, the affinity of the polymer electrolyte with the porous substrate and the catalyst layer is maintained, and it is not easy to peel off and break at the interface of the polymer electrolyte with the porous substrate and the catalyst layer when the size changes, and the durability is excellent. On the other hand, the amount of surfactant is moderate, and the proton conductivity of the electrolyte membrane is excellent. It should be noted that the content of the surfactant here is the amount of the surfactant remaining in the completed electrolyte membrane, which refers to the amount excluding the surfactant that falls off during the manufacturing process.
[0129] As a method for analyzing the nonionic fluorinated surfactant contained in the electrolyte membrane, there can be cited a method of dissolving the surfactant together with the polymer electrolyte membrane in a predetermined solvent. The dried product after removing the solution and solvent of the polymer electrolyte membrane is subjected to infrared spectroscopy (IR) analysis. 1 H nuclear magnetic resonance (NMR) analysis, 19F-NMR analysis, MALDI-MS analysis, thermal decomposition GC / MS analysis, thereby, the chemical structure of various surfactants can be analyzed and the content of surfactant can be calculated. In addition, it is also appropriate to perform a conventional purification treatment such as solvent extraction and reprecipitation on the above-mentioned solution and dried solid and only extract the nonionic fluorine-based surfactant.
[0130] The solvent used in the analysis of the above-mentioned nonionic surfactant can be appropriately selected according to the types of polymer electrolyte and nonionic surfactant constituting the electrolyte membrane. For example, aprotic polar solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, cyclopentane, 1,3-dimethyl-2-imidazolidinone, hexamethylphosphoric triamide, carbonate solvents such as ethylene carbonate and propylene carbonate, alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, methanol, ethanol, propanol, butanol, and alcohol solvents such as propylene carbonate can be preferably used. Ketone, methyl ethyl ketone, methyl isobutyl ketone and other ketone solvents, γ-butyrolactone, ethyl acetate, butyl acetate, ethyl lactate and other ester solvents, hexane, cyclohexane and other hydrocarbon solvents, benzene, toluene, xylene and other aromatic hydrocarbon solvents, chloroform, dichloromethane, 1,2-dichloroethane, perchloroethylene, chlorobenzene, dichlorobenzene and other halogenated hydrocarbon solvents, ether, tetrahydrofuran, 1,4-dioxane and other ether solvents, nitrile solvents such as acetonitrile, nitromethane, nitroethane and other nitrated hydrocarbon solvents, water, etc. In addition, a mixed solvent obtained by mixing two or more of these solvents can also be used. Here, as "propanol", there is a structure in which one of the hydrogen atoms contained in the propane molecule is replaced by a hydroxyl group, and there are two structural isomers such as 1-propanol and 2-propanol, but in this specification, "propanol" is used as a general term for them. The same is true for other solvents such as "butanol" and "xylene".
[0131] When the electrolyte membrane is insoluble, different analysis methods can be used. The electrolyte membrane containing the nonionic fluorine-based surfactant can be subjected to IR analysis, solid NMR analysis, MALDI-MS analysis, and thermal decomposition GC / MS analysis to analyze the chemical structure and content of the surfactant. It is also appropriate to analyze the electrolyte membrane by immersing it in a solvent and dissolving and extracting only the nonionic fluorine-based surfactant.
[0132] As the nonionic fluorine-based surfactant used in the present invention, it is preferably a nonionic fluorine-based surfactant that does not contain metals as impurities. Here, the so-called metals include simple substances of metal elements, metal ions, nonionic metal compounds, metal oxides, etc., but are not limited to these. In the case of not containing metals, it is not easy for the hydrophilic group and lipophilic group of the nonionic fluorine-based surfactant to interact with the metals. Therefore, even in the polymer electrolyte membrane, it has a high degree of freedom and can maintain the function as a surfactant, so it can suppress the reduction of durability caused by peeling and rupture at the interface of the polymer electrolyte and the porous substrate and the catalyst layer when the size changes.
[0133] 〔Catalyst layer〕
[0134] The catalyst layer is a layer containing catalyst particles formed in contact with both surfaces of the electrolyte membrane, and is generally a layer containing catalyst particles and a polymer electrolyte formed of a fluorine-based polymer electrolyte. As the fluorine-based polymer electrolyte, the above-mentioned fluorine-based polymer electrolyte can be used.
[0135] In the electrolyte membrane with a catalyst layer of the present invention, it is preferred that the catalyst layer contains a perfluoro polymer having an ionic group from the perspective of power generation performance and chemical durability. By using a perfluoro polymer having an ionic group, the acidity of the ionic group contained in the catalyst layer becomes higher, the proton conductivity is further improved, and since there are a large number of chemically stable CF bonds, the chemical durability of the catalyst layer can be further improved.
[0136] As catalyst particles, carbon particles loaded with catalysts obtained by loading catalyst substances on carbon particles can be generally used. As catalyst substances, not only platinum can be cited, but also metals such as palladium, ruthenium, iridium, rhodium, osmium, and iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum of platinum group elements or their alloys, or oxides, composite oxides, etc. can be cited. For the type of carbon particles, as long as they are microparticle-shaped and have electrical conductivity, and will not corrode or deteriorate due to reaction with the catalyst, there is no particular limitation, and carbon black, graphite, black lead, activated carbon, carbon fiber, carbon nanotubes, and fullerene particles can be used.
[0137] The mass ratio of the content of the polymer electrolyte in the catalyst layer to the content of the catalyst particles is preferably in the range of 0.2 to 2.5, and particularly preferably in the range of 0.5 to 2.0. When the mass ratio of the content of the polymer electrolyte to the content of the catalyst particles is within the above-mentioned preferred range, the catalyst layer is not easily broken, and on the other hand, the gas diffusion is not impaired, and the power generation performance is excellent.
[0138] The thickness of the catalyst layer is preferably 0.03 μm to 2,000 μm. In order to easily obtain good power generation performance and durability, the thickness of the catalyst layer is more preferably 0.5 μm or more, and particularly preferably 1 to 30 μm.
[0139] <Method for producing electrolyte membrane>
[0140] In the present invention, as a first method, the electrolyte membrane can be manufactured by the following method: after impregnating the porous substrate with a polymer electrolyte solution, the polymer electrolyte solution is dried to remove the solvent contained in the polymer electrolyte solution. In this case, a method in which the nonionic fluorine-based surfactant is pre-mixed in the polymer electrolyte solution and then impregnated in the porous substrate is also suitable. The details of the polymer electrolyte, porous substrate and nonionic fluorine-based surfactant used in the manufacturing method of the first method and the second method described later are as described above, so they are omitted here.
[0141] As mentioned above, the content of the surfactant in the polymer electrolyte solution is preferably 0.005 or more, more preferably 0.01 or more, in terms of mass ratio relative to the total amount of the polymer electrolyte. In addition, it is preferably 0.20 or less, more preferably 0.10 or less. When this ratio is within the above-mentioned preferred range, the affinity between the polymer electrolyte and the catalyst layer is maintained, and the effect of improving the power generation performance can be fully obtained. On the other hand, the amount of the surfactant is appropriate, and the proton conductivity of the electrolyte membrane is excellent.
[0142] In the present invention, the electrolyte membrane can also be produced as a second aspect by impregnating a porous substrate to which a nonionic fluorine-based surfactant has been applied in advance with a polymer electrolyte solution and then drying the porous substrate to remove the solvent contained in the polymer electrolyte solution.
[0143] In this case, as a method of providing the surfactant to the porous substrate, the following method can be mentioned.
[0144] (1) A method of controlling the amount of surfactant solution applied by lifting a porous substrate immersed in a surfactant solution and removing excess solution.
[0145] (2) A method of coating a surfactant solution on a porous substrate by casting.
[0146] (3) A method in which a porous substrate is laminated onto a supporting substrate coated with a surfactant solution by casting and impregnated with the supporting substrate.
[0147] When the impregnation is performed by the method (3), the solvent can be dried while maintaining the original state. In addition, when the impregnation is performed by the method (1) or (2), from the perspective of reducing wrinkles and uneven thickness of the porous substrate and improving the quality, it is preferred to dry the solvent of the fluorinated nonionic surfactant solution in a state where the porous substrate is attached to a separately prepared supporting substrate.
[0148] When the surfactant is in liquid or oily form, the surfactant itself may be impregnated instead of the aforementioned surfactant solution. However, in order to adjust the viscosity in a manner that allows the surfactant to easily penetrate into the porous substrate, or to dilute in a manner that does not impart an excessive amount of surfactant, it is preferred to use a surfactant solution obtained by dissolving it in a specified solvent.
[0149] As a method for casting the surfactant solution, knife coating, direct roll coating, Meyer rod coating, gravure coating, reverse coating, air knife coating, spray coating, brush coating, dip coating, die coating, vacuum die coating, curtain coating, flow coating, spin coating, screen printing, inkjet coating and the like can be used.
[0150] In the second mode, the mass of the porous substrate is set to 100 mass%, and the surfactant is preferably given 1 mass% or more, and more preferably 5 mass% or more. In addition, similarly, it is preferably given 30 mass% or less, and more preferably 20 mass% or less. When the amount of surfactant given is within the above-mentioned preferred range, the affinity of the polymer electrolyte and the porous substrate is maintained, and it is easy to composite. On the other hand, the amount of surfactant becomes appropriate, and it is not easy to block the pores of the porous substrate, and the proton conductivity of the composite electrolyte membrane is excellent.
[0151] In the second embodiment, it is preferred that the contact angle of the solvent used in the polymer electrolyte solution on the surface of the porous substrate is 120° or less by imparting a surfactant, more preferably 80° or less, and further preferably 50° or less. When the contact angle is within the above preferred range, the polymer electrolyte solution is easily impregnated in the porous substrate containing the surfactant.
[0152] In addition, in the second embodiment, as a surfactant, a compound that is insoluble in the solvent of the polymer electrolyte solution to be impregnated is preferably used. When such a surfactant is used, it is possible to prevent the surfactant from diffusing from the surface of the porous substrate and the surface of the composite electrolyte membrane in contact with the catalyst layer into the polymer electrolyte during the impregnation of the polymer electrolyte solution, fully exerting the function as a surfactant, and preventing the reduction of proton conductivity caused by the presence of the surfactant in the polymer electrolyte.
[0153] In the first and second embodiments, the concentration of the polymer electrolyte solution is preferably 3 to 40% by mass, more preferably 5 to 25% by mass. If the concentration is within this range, the number of times of coating to fully fill the pores of the porous substrate with the polymer electrolyte can be reduced to about 1 to 2 times, and a composite layer with excellent surface smoothness can be easily obtained.
[0154] The viscosity of the polymer electrolyte solution is preferably 100 to 50,000 mPa·s, more preferably 300 to 10,000 mPa·s. When the viscosity is within the above preferred range, the pores of the porous substrate are easily filled with the polymer electrolyte, the thickness of the electrolyte membrane is easily uniform, and the surface smoothness of the electrolyte membrane is excellent.
[0155] The solvent used in the polymer electrolyte solution can be appropriately selected according to the type of polymer. As the solvent, for example, N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, cyclopentane, 1,3-dimethyl-2-imidazolidinone, hexamethylphosphoric triamide and other aprotic polar solvents, ethylene carbonate, propylene carbonate and other carbonate-based solvents, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether and other alkylene glycol monoalkyl ethers, methanol, ethanol, propanol, butanol and other alcohol solvents can be preferably used. , ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, ester solvents such as γ-butyrolactone, ethyl acetate, butyl acetate, ethyl lactate, hydrocarbon solvents such as hexane, cyclohexane, aromatic hydrocarbon solvents such as benzene, toluene, xylene, halogenated hydrocarbon solvents such as chloroform, dichloromethane, 1,2-dichloroethane, perchloroethylene, chlorobenzene, dichlorobenzene, ether solvents such as ether, tetrahydrofuran, 1,4-dioxane, nitrile solvents such as acetonitrile, nitrated hydrocarbon solvents such as nitromethane and nitroethane, water, etc. In addition, a mixed solvent obtained by mixing two or more of these solvents may be used.
[0156] Examples of a method for impregnating a porous substrate with a polymer electrolyte solution include the following methods.
[0157] (1) A method of controlling the film thickness by lifting a porous substrate immersed in a polymer electrolyte solution and removing excess solution.
[0158] (2) A method of coating a polymer electrolyte solution on a porous substrate by casting.
[0159] (3) A method in which a porous substrate is laminated onto a supporting substrate coated with a polymer electrolyte solution by casting and impregnated with the porous substrate.
[0160] Regarding the drying of the solvent, when the impregnation is performed by the method (3), it can be performed while maintaining the original state. In addition, when the impregnation is performed by the method (1) or (2), from the perspective of being able to reduce the wrinkles and uneven thickness of the electrolyte membrane and thus improve the membrane quality, it is preferred to dry the solvent of the polymer electrolyte solution in a state where a porous substrate is attached to a separately prepared supporting substrate.
[0161] As a method for casting the polymer electrolyte solution, knife coating, direct roll coating, Meyer rod coating, gravure coating, reverse coating, air knife coating, spray coating, brush coating, dip coating, die coating, vacuum die coating, curtain coating, flow coating, spin coating, screen printing, inkjet coating, etc. can be applied. Here, the device for casting the polymer electrolyte solution is referred to as a coater.
[0162] After the polymer electrolyte solution is applied to the substrate, an electrolyte membrane can be formed via a drying process. In the drying process, the film of the polymer electrolyte solution impregnated in the porous substrate is heated to evaporate the solvent. As long as the solvent can evaporate, there is no particular limitation on the heating method. For example, a heating device such as an oven or a heater, a device that uses infrared rays, warm wind, etc. to control the temperature near the electrolyte membrane, etc. can be used. In addition, heat can also be conducted to the film across the substrate. The temperature range of heating is preferably close to the boiling point of the solvent and below the glass transition temperature of the electrolyte membrane. In addition, the solvent can be removed without heating only by decompression and the introduction of airflow.
[0163] The drying time and drying temperature in the drying step can be appropriately determined experimentally, but it is preferred to dry at least to the extent that the film becomes a self-supporting film even if it is peeled off from the substrate. The drying method can be selected from known methods such as heating of the substrate, hot air, and infrared heaters. In consideration of the decomposition of the polymer electrolyte and the surfactant, the drying temperature is preferably 200° C. or less, more preferably 150° C. or less.
[0164] The polymer electrolyte in the solution can use a substance in which an ionic group forms a salt with a cation of an alkali metal or an alkaline earth metal. In this case, it is also preferred to form a film on a substrate and have a process of exchanging cations of an alkali metal or an alkaline earth metal with protons after a drying process. This process is more preferably a process of contacting the formed film with an acidic aqueous solution. In addition, the contact is further preferably a process of immersing the formed film in an acidic aqueous solution. In this process, the protons in the acidic aqueous solution are replaced with cations that are ionically bonded to the ionic groups, and the remaining water-soluble impurities, residual monomers, solvents, residual salts, etc. are removed at the same time. The acidic aqueous solution is not particularly limited, but sulfuric acid, hydrochloric acid, nitric acid, acetic acid, trifluoromethanesulfonic acid, methanesulfonic acid, phosphoric acid, citric acid, etc. are preferably used. The temperature, concentration, etc. of the acidic aqueous solution should also be appropriately determined, but from the perspective of productivity, it is preferred to use an aqueous sulfuric acid solution of 3% by mass or more and 30% by mass or less at a temperature of 0°C or more and 80°C or less.
[0165] [Method for producing electrolyte membrane with catalyst layer]
[0166] The catalyst coated membrane (CCM) of the present invention is formed by forming catalyst layers on both sides of the electrolyte membrane of the present invention. The method of forming the catalyst layer is not particularly limited, but from the perspective of simplicity of process and ability to suppress process costs, the following methods are preferred: a method of applying catalyst layer ink and drying it; a method of transferring the catalyst layer using a catalyst layer decal formed in advance on a decal substrate and then drying it.
[0167] In the case of the method of applying the catalyst layer ink, the coating method is not particularly limited as long as it can be applied into a target shape, and the method described in the above-mentioned polymer electrolyte solution coating step can be used.
[0168] The solvent contained in the catalyst layer ink is not particularly limited as long as it can disperse the polymer electrolyte and the carbon particles carrying the catalyst, but is preferably a solvent that can be easily evaporated and removed by heating. For example, a solvent having a boiling point of 140° C. or less is preferred. As the solvent of the catalyst layer ink, specifically, water, alcohols such as methanol, ethanol, propanol, butanol, and pentanol, ketones such as acetone, methyl ethyl ketone, pentanone, hexanone, heptanone, cyclohexanone, methylcyclohexanone, acetonylacetone, and diisobutyl ketone, ethers such as tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, anisole, methoxytoluene, and dibutyl ether, esters such as methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, methyl lactate, ethyl lactate, and butyl lactate, and one or a mixture of two or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, diethylene glycol, diacetone alcohol, and 1-methoxy-2-propanol can be used.
[0169] In the case of a method of transfer using catalyst layer printing, first, a catalyst layer ink is applied to a substrate, and a drying process is performed as needed to produce a catalyst layer printing. Then, the electrolyte membrane is sandwiched with a catalyst layer printing on the cathode electrode side and a catalyst layer printing on the anode electrode side, and hot pressing is performed in a manner that the surfaces of the two printings provided with the catalyst layer are in contact with the electrolyte membrane, thereby obtaining an electrolyte membrane with a catalyst layer. The temperature and pressure of the hot pressing can be appropriately selected according to the thickness, moisture content, catalyst layer, and printing substrate of the electrolyte membrane, but from the perspective of industrial productivity and suppression of thermal decomposition of the electrolyte membrane material, it is preferably carried out in the range of 0°C to 250°C, and more preferably under conditions higher than the glass transition temperature of the polymer electrolyte contained in the catalyst layer and below 200°C. From the perspective of protecting the electrolyte membrane and the electrode, the pressure in the hot pressing is preferably as weak as possible, and in the case of flat plate pressing, the pressure is preferably below 10MPa.
[0170] As the printing substrate used when applying the catalyst layer ink, in addition to the same resin film and substrate as the substrate used in the electrolyte membrane film formation, fluororesins such as PTFE, polyhexafluoropropylene, ETFE, ethylene-hexafluoropropylene copolymer, FEP, PFA, and PVdF can also be used. From the aspects of heat resistance, solvent resistance, chemical stability, and demolding properties, it is preferred to use a fluororesin film.
[0171] The catalyst layer can be dried by the same method as that described above in the drying of the polymer electrolyte solution.
[0172] The membrane electrode assembly of the present invention and the polymer electrolyte fuel cell of the present invention are formed using the electrolyte membrane of the present invention.
[0173] Example
[0174] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited thereto. It should be noted that various measurement conditions are as follows.
[0175] (1) Molecular weight of polymer
[0176] GPC is used to measure the number average molecular weight and weight average molecular weight of the polymer solution. As an integrated device of a UV detector and a differential refractometer, HLC-8022GPC manufactured by Tosoh Corporation is used. In addition, as a GPC column, two TSK gel SuperHM-H manufactured by Tosoh Corporation (inner diameter is 6.0 mm, length is 15 cm) are used. Using N-methyl-2-pyrrolidone solvent (N-methyl-2-pyrrolidone solvent containing 10 mmol / L of lithium bromide), the flow rate is measured at 0.2 mL / min, and the number average molecular weight and weight average molecular weight are obtained by converting to standard polystyrene.
[0177] (2) Ion exchange capacity (IEC)
[0178] The measurement was performed by neutralization titration method and the measurement was performed 3 times and the average value was taken.
[0179] After the electrolyte membrane was thoroughly washed with pure water by proton replacement and wiped clean of water on the membrane surface, it was vacuum dried at 100° C. for 12 hours or more, and the dry weight was determined.
[0180] 50 mL of a 5 mass % sodium sulfate aqueous solution was added to the electrolyte membrane, and the membrane was left to stand for 12 hours to perform ion exchange.
[0181] The generated sulfuric acid was titrated using a 0.01 mol / L sodium hydroxide aqueous solution, and a commercially available phenolphthalein solution for titration at 0.1 w / v% was added as an indicator, and the point at which the solution turned light purple was defined as the end point.
[0182] The ion exchange capacity (IEC) was calculated using the following formula.
[0183] IEC (meq / g) = [Concentration of sodium hydroxide aqueous solution (mmol / mL) × amount added (mL)] / dry weight of sample (g)
[0184] (3) Cross-sectional SEM measurement of electrolyte membrane
[0185] Cross-sectional SEM measurement was performed under the following conditions: Based on the obtained image, the central white area was regarded as the composite layer, and the two adjacent black areas were regarded as the other outer layers, and their thicknesses were measured.
[0186] Equipment: Field emission scanning electron microscope (FE-SEM) S-4800 (manufactured by Hitachi High-Technologies Corporation)
[0187] Accelerating voltage: 2.0 kV
[0188] Pretreatment: The cross-section sample prepared by the BIB method was coated with Pt and then measured.
[0189] BIB method: a device for preparing cross-section samples using an argon ion beam.
[0190] A shielding plate is placed right above the sample, and a broad ion beam of argon is irradiated from above to perform etching, thereby producing an observation surface and an analysis surface (cross section).
[0191] (4) Filling rate of polymer electrolyte in composite layer (filling rate of composite layer)
[0192] According to the above item (3), the cross section of the electrolyte membrane is observed using SEM, and the thickness T1 of the composite layer formed by the polymer electrolyte and the porous substrate, and the thicknesses T2 and T3 of other layers when there are other layers outside the composite layer are calculated respectively. The specific gravity of the polymer electrolyte forming the composite layer is set to D1, the specific gravity of the polymer electrolytes of the other layers forming the outside of the composite layer are set to D2 and D3 respectively, and the specific gravity of the electrolyte membrane is set to D. The IEC of the polymers forming each layer is set to I1, I2, and I3, and the IEC of the electrolyte membrane is set to I, and the filling rate Y2 (volume %) of the polymer electrolyte in the composite layer is calculated using the following formula.
[0193] Y2=[(T1+T2+T3)×D×I-(T2×D2×I2+T3×D3×I3)] / (T1×D1×I1)×100
[0194] (5) Observation of phase separation structure based on transmission electron microscopy (TEM) tomography
[0195] The sample of the electrolyte membrane was immersed in a 2 mass % lead acetate aqueous solution as a staining agent and left to stand at 25°C for 48 hours for staining. The stained sample was taken out, embedded with epoxy resin, and fixed by irradiating visible light for 30 seconds. Using an ultra-thin slicer, a 100 nm thin slice was cut at room temperature and observed under the following conditions.
[0196] Equipment: Field emission electron microscope (HRTEM) JEM2100F manufactured by JEOL Ltd.
[0197] Image acquisition: Digital Micrograph
[0198] System: Notation
[0199] Accelerating voltage: 200 kV
[0200] Shooting magnification: 30,000 times
[0201] Tilt angle: +61°~-62°
[0202] Reconstruction resolution: 0.71nm / pixel
[0203] The three-dimensional reconstruction process used a marking method. As positioning marks for the three-dimensional reconstruction, colloidal Au particles applied to the collodion film were used. Based on the marks, a total of 124 TEM images were obtained from a series of continuous tilt images in which the sample was tilted 1° at a time and TEM images were taken in the range of +61° to -62°, and CT reconstruction was performed to observe the three-dimensional phase separation structure.
[0204] (6) Dimensional change rate based on hot water test (λ xy ) determination
[0205] The electrolyte membrane was cut into a square of about 5 cm × about 5 cm, and after standing for 24 hours in a temperature and humidity controlled atmosphere of 23°C ± 5°C and 50 ± 5% RH, the length of MD and the length of TD (MD1 and TD1) were measured with a vernier caliper. After the electrolyte membrane was immersed in hot water at 80°C for 8 hours, the length of MD and the length of TD (MD2 and TD2) were measured again with a vernier caliper, and the dimensional change rate of MD and TD in the plane direction (λ) was calculated using the following formula. MD and λ TD ) and the dimensional change rate in the plane direction (λ xy )(% ).
[0206] λ MD =(MD2-MD1) / MD1×100
[0207] λ TD =(TD2-TD1) / TD1×100
[0208] λ xy =(λ MD +λ TD ) / 2.
[0209] (7) Proton conductivity
[0210] After the electrolyte membrane was immersed in pure water at 25°C for 24 hours, it was kept at 80°C in a constant temperature and humidity chamber with a relative humidity of 25% RH for 30 minutes, and the proton conductivity was measured using a constant potential AC impedance method. As a measuring device, an electrochemical measurement system (Solartron 1287 Electrochemical Interface and Solartron 1255B Frequency Response Analyzer) manufactured by Solartron was used, and constant potential impedance measurement was performed using a two-terminal method to determine the proton conductivity. The AC amplitude was set to 50mV. The sample used a membrane with a width of 10mm and a length of 50mm. The measuring fixture was made of phenolic resin, and the measuring part was released. As an electrode, a platinum plate (thickness of 100μm, 2 sheets) was used. The electrodes were arranged on the surface and back sides of the sample membrane in a manner that the distance between the electrodes was 10mm, parallel to each other and orthogonal to the length direction of the sample membrane.
[0211] (8) Fabrication of membrane electrode assembly (MEA) using electrolyte membrane
[0212] On a commercially available polytetrafluoroethylene film, the amount of platinum was 0.3 mg / cm 2 Catalyst prints are prepared by coating carbon particles TEC10E50E (platinum loading rate of 50% by mass) loaded with a platinum catalyst manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. and "Nafion" (registered trademark) ("NAFION" (registered trademark) manufactured by Chemours Co., Ltd.) in a mass ratio of 2:1 with a catalyst ink.
[0213] Two products obtained by cutting the above catalyst print into 5 cm squares were prepared, and the products were placed opposite and overlapped in a manner of sandwiching the electrolyte membrane, and heated and pressed at 150°C and 5 MPa for 3 minutes to obtain an electrolyte membrane with a catalyst layer. A commercially available gas diffusion electrode 24BCH manufactured by SGL was cut into 5 cm squares, and the obtained electrolyte membrane with a catalyst layer was sandwiched, so that one surface was a cathode and the other surface was an anode, and MEA was produced.
[0214] (9) Wet-dry cycle durability
[0215] The MEA prepared in (8) was installed in a JARI standard unit cell Ex-1 (electrode area 25 cm 2 ), with the cell temperature at 80°C, a cycle of supplying 160% RH nitrogen to both electrodes for 2 minutes, followed by supplying 0% RH nitrogen (dew point below -20°C) to both electrodes for 2 minutes was repeated. The hydrogen permeation amount was measured every 1,000 cycles, and the time point when the hydrogen permeation current exceeded 10 times the initial current was taken as the dry-wet cycle durability.
[0216] For the measurement of hydrogen permeation, hydrogen as fuel gas was supplied to one electrode and nitrogen was supplied to the other electrode. The test was conducted under humidification conditions: hydrogen gas 90% RH, nitrogen gas: 90% RH. The open circuit voltage was maintained until it became less than 0.2V, and the voltage was swept from 0.2 to 0.7V at 1mV / sec. The current value at 0.7V was taken as the hydrogen permeation current.
[0217] (10) Measurement of fluorine atom content in porous substrate
[0218] A porous base material sample was weighed under the following conditions and burned in a combustion tube of an analysis device. After the generated gas was absorbed into a solution, a portion of the absorption solution was analyzed by ion chromatography.
[0219] <Combustion and absorption conditions>
[0220] System: AQF-2100H, GA-210 (Mitsubishi Chemical Corporation)
[0221] Electric furnace temperature: inlet 900℃, outlet 1000℃
[0222] Gas: Ar / O 2 200mL / min, O 2 400mL / min
[0223] Absorption liquid: H 2 O 2 0.1%, internal standard Br 8μg / mL
[0224] Absorption liquid volume: 20mL
[0225] <Ion chromatography and anion analysis conditions>
[0226] System: ICS1600 (made by DIONEX)
[0227] Mobile phase: 2.7mmol / L Na 2 CO 3 / 0.3mmol / L NaHCO 3
[0228] Flow rate: 1.50mL / min
[0229] Detector: Conductivity detector
[0230] Injection volume: 20 μL
[0231] (11) Chemical structure analysis of surfactants
[0232] Perform infrared spectroscopy (IR) analysis, 1 H nuclear magnetic resonance (NMR) analysis, 19 The chemical structures of various surfactants were analyzed by F-NMR analysis, MALDI-MS analysis, and thermal decomposition GC / MS analysis, and the contents of fluorine atoms and hydrophilic elements (the total of oxygen, nitrogen, phosphorus, sulfur, and boron) were calculated.
[0233] (12) Determination of weight average molecular weight of surfactant
[0234] The weight average molecular weight of the surfactant was measured by gel permeation chromatography (GPC) analysis under the following conditions.
[0235] Device: Gel Permeation Chromatography GPC (Equipment No. GPC-27)
[0236] Detector: UV-visible absorption spectrophotometer (SPD-20AV manufactured by Shimadzu Corporation)
[0237] Column: TSKgel Super HZM-N 2 pieces
[0238] SuperHZ4000, 2500, 1000 each
[0239] Solvent: Tetrahydrofuran (THF)
[0240] Flow rate: 0.45mL / min
[0241] Column temperature: 40°C
[0242] Injection volume: 0.02mL
[0243] Standard sample: Monodisperse polyethylene glycol (PEG) manufactured by Tosoh Corporation and Agilent
[0244] Data processing: GPC data processing system manufactured by Toray Research Center, Inc.
[0245] (13) Amount of surfactant contained in the electrolyte membrane
[0246] The electrolyte membrane is weighed under the following conditions, burned in a combustion tube of an analysis device, and the generated gas is absorbed into a solution, and then a portion of the absorption liquid is analyzed by ion chromatography. The contribution of the surfactant is calculated by removing the contribution of the polymer electrolyte without surfactant measured in advance and the contribution of the porous substrate measured in advance by (10) from the analysis value, and the amount of surfactant contained in the composite electrolyte membrane is calculated from the amount of fluorine atoms contained in the surfactant, and the ratio of the surfactant contained in the composite membrane to the polymer electrolyte (surfactant / polymer electrolyte) is obtained.
[0247] <Combustion and absorption conditions>
[0248] System: AQF-2100H, GA-210 (Mitsubishi Chemical Corporation)
[0249] Electric furnace temperature: inlet 900℃, outlet 1000℃
[0250] Gas: Ar / O 2 200mL / min, O 2 400mL / min
[0251] Absorption liquid: H 2 O 2 0.1%, internal standard Br 8μg / mL
[0252] Absorption liquid volume: 20mL
[0253] <Ion chromatography and anion analysis conditions>
[0254] System: ICS1600 (made by DIONEX)
[0255] Mobile phase: 2.7mmol / L Na 2 CO 3 / 0.3mmol / L NaHCO 3
[0256] Flow rate: 1.50mL / min
[0257] Detector: Conductivity detector
[0258] Injection volume: 20 μL
[0259] (14) Measurement of oxygen content in porous substrates using XPS
[0260] The porous substrate cut into 5 mm square size in advance was rinsed with ultrapure water, dried at room temperature at 67 Pa for 10 hours, cooled in liquid nitrogen for 30 minutes, and processed twice for 5 minutes using a freezing mill to prepare the sample. The composition of the prepared sample was measured to calculate the oxygen atom content. The measuring device and conditions were as follows.
[0261] Measurement device: Quantera SXM
[0262] Excitation X-ray: Monochromatic Al Kα 1 , Kα 2 Radiation (1,486.6eV)
[0263] X-ray diameter: 200μm
[0264] Photoelectron escape angle: 45°
[0265] (15) Mechanical properties of electrolyte membrane in dry state
[0266] The electrolyte membrane as a test sample is placed in the device and a tensile test is carried out under the following conditions. The values of tensile strength and tensile elongation are the values at the moment when the maximum point stress is shown in the test. The elastic modulus is a value obtained by using any two points where the strain becomes 0.35% and the calculated value becomes the maximum. When calculating the tensile modulus of elasticity per unit width (N / cm), the value obtained by dividing the force (N) output in the tensile test by the membrane width (cm) is used as the strength (N / cm), and the difference in the strength between the above-mentioned two arbitrary points (N / cm) is further divided by the strain of 0.0035 (dimensionless quantity) to obtain the value obtained as the tensile modulus of elasticity per unit width (N / cm). When calculating the tensile modulus of elasticity per unit cross-sectional area (MPa), the force (N) output in the tensile test is divided by the cross-sectional area (mm 2 ), that is, the value obtained by multiplying the film width (mm) and the film thickness (mm) is taken as the stress (MPa), and the value obtained by further dividing the stress difference (MPa) between any two points mentioned above by the strain 0.0035 (dimensionless quantity) is taken as the tensile elastic modulus (MPa) per unit cross-sectional area. The maximum point stress and elastic modulus are calculated from the average value of 5 tests.
[0267] Measuring device: Autograph AG-IS (manufactured by Shimadzu Corporation)
[0268] Load range: 100N
[0269] Stretching speed: 100mm / min
[0270] Test piece: width 10mm x length 50mm
[0271] Distance between samples: 30mm
[0272] Test temperature and humidity: 23±1℃, 60±10%RH
[0273] Number of trials: n = 5
[0274] (16) Mechanical properties of electrolyte membranes in a water-containing state
[0275] The electrolyte membrane used as the test sample was cut into test pieces in advance and immersed in ultrapure water at 23°C for 24 hours. Then, a tensile test was performed using the same conditions and methods as (15) to calculate the tensile strength, tensile elongation and elastic modulus.
[0276] (17) Determination of haze and diffuse transmittance
[0277] The electrolyte membrane as a test sample was cut into a size of 5 cm × 5 cm, and the haze was measured under the following conditions. In the haze measurement, the total irradiation light quantity T was calculated in advance without a sample. 1 , device scattering rate T 3 Then, the total light transmittance T is measured with the sample set. 2 and the sample scattering rate T 4 , calculate the diffusion transmittance T d And haze.
[0278] Measuring device: Haze meter HGM-20P (manufactured by Suga Test Instruments Co., Ltd.)
[0279] (18) SEM observation of porous substrate
[0280] The porous substrate used as the test sample was cut into a size of 2 mm × 2 mm, and after platinum ion sputtering, SEM observation was performed to observe the morphology of the surface direction of the porous substrate. The orientation of the nodes and fibrils contained in the porous substrate was determined based on the structure when the SEM observation was performed within an arbitrary range of 15 μm × 15 μm. The diameters of the nodes and fibrils at 100 points were measured within an arbitrary range of 15 μm × 15 μm, and the average value was calculated, thereby calculating the average diameter of the nodes and fibrils. Ion sputtering and SEM observation were implemented using the following apparatus and conditions.
[0281] <Ion sputtering>
[0282] Sputtering device: Ion sputtering device E-1045 (manufactured by Hitachi High-Technologies Corporation)
[0283] Metal type: Pt
[0284] Ion emission current: 15mA
[0285] Splash time: 60 seconds
[0286] <SEM observation>
[0287] Measurement device: Scanning electron microscope S-5500 (manufactured by Hitachi High-Technologies Corporation)
[0288] Accelerating voltage: 5kV
[0289] Observation magnification: 2,000 to 20,000 times
[0290] [Synthesis example 1]
[0291] (Synthesis of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane (K-DHBP) represented by the following chemical formula (G1))
[0292] Into a 500 mL flask equipped with a stirrer, a thermometer and a distillation tube, 49.5 g of 4,4'-dihydroxybenzophenone, 134 g of ethylene glycol, 96.9 g of trimethyl orthoformate and 0.50 g of p-toluenesulfonic acid monohydrate were added and dissolved. Thereafter, the mixture was stirred at 78-82°C for 2 hours. Furthermore, the internal temperature was slowly raised to 120°C, and the distillation of methyl formate, methanol and trimethyl orthoformate was completely stopped. After the reaction solution was cooled to room temperature, the reaction solution was diluted with ethyl acetate, the organic layer was washed with 100 mL of 5% potassium carbonate aqueous solution, and the solvent was distilled off after separation. 80 mL of dichloromethane was added to the residue to precipitate crystals, which were filtered and dried to obtain 52.0 g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane represented by the following chemical formula (G1). The crystals were subjected to GC analysis, and the result was 99.9% of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane and 0.1% of 4,4′-dihydroxybenzophenone.
[0293] [Chemical formula 5]
[0294]
[0295] [Synthesis example 2]
[0296] (Synthesis of 3,3'-disulfonated-4,4'-difluorobenzophenone disodium salt represented by the following chemical formula (G2))
[0297] At 100°C, 109.1 g of 4,4'-difluorobenzophenone (Sigma-Aldrich Japan (same) reagent) was dissolved in fuming sulfuric acid (50% SO 3 ) (Fujifilm Wako Pure Chemical Industries, Ltd. reagent) 150 mL was reacted for 10 hours. Then, a small amount was added gradually into a large amount of water, neutralized with NaOH, and 200 g of common salt (NaCl) was added to precipitate the synthetic product. The obtained precipitate was separated by filtration and recrystallized with ethanol aqueous solution to obtain 3,3'-disulfonated-4,4'-difluorobenzophenone disodium salt represented by the following chemical formula (G2). The purity was 99.3%.
[0298] [Chemical formula 6]
[0299]
[0300] [Synthesis example 3]
[0301] (Synthesis of oligomer a1 not containing an ionic group represented by the following general formula (G3))
[0302] Into a 1,000 mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 16.59 g (120 mmol) of potassium carbonate (Sigma-Aldrich Japan (same) reagent), 25.8 g (100 mmol) of K-DHBP obtained in the above-mentioned Synthesis Example 1, and 20.3 g (93 mmol) of 4,4'-difluorobenzophenone (Sigma-Aldrich Japan (same) reagent) were placed. After nitrogen substitution, 300 mL of N-methylpyrrolidone (NMP) and 100 mL of toluene were added, and after dehydration at 160°C, the temperature was raised to remove toluene, and polymerization was carried out at 180°C for 1 hour. Reprecipitation and purification were carried out in a large amount of methanol to obtain an oligomer (terminal: hydroxyl group) without an ionic group. The number average molecular weight was 10,000.
[0303] Into a 500 mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 1.1 g (8 mmol) of potassium carbonate (Sigma-Aldrich Japan (same) reagent) and 20.0 g (2 mmol) of the aforementioned oligomer (terminal: hydroxyl group) without an ionic group were placed, and nitrogen substitution was performed. Then, 100 mL of NMP and 30 mL of toluene were added, and after dehydration at 100° C., the temperature was raised to remove the toluene, and 4.0 g (12 mmol) of decafluorobiphenyl (Sigma-Aldrich Japan (same) reagent) was added, and the reaction was carried out at 105° C. for 1 hour. Reprecipitation was performed in a large amount of isopropanol, and purification was performed to obtain an oligomer a1 (terminal: fluorine group) without an ionic group represented by the following general formula (G3). The number average molecular weight was 11,000.
[0304] [Chemical formula 7]
[0305]
[0306] [Synthesis Example 4]
[0307] (Synthesis of the ionic group-containing oligomer a2 represented by the following general formula (G4))
[0308] Into a 1,000 mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap were placed 27.6 g (200 mmol) of potassium carbonate (Sigma-Aldrich Japan (the same) reagent), 12.9 g (50 mmol) of K-DHBP obtained in Synthesis Example 1, 9.3 g (50 mmol) of 4,4'-biphenol (Sigma-Aldrich Japan (the same) reagent), 39.3 g (93 mmol) of 3,3'-disulfonated-4,4'-difluorobenzophenone disodium salt obtained in Synthesis Example 2, and 17.9 g (82 mmol) of 18-crown-6 (Fujifilm Wako Pure Chemical Industries, Ltd. reagent), and after nitrogen substitution, 300 mL of NMP and 100 mL of toluene were added, and after dehydration at 170°C, the temperature was raised to remove toluene, and polymerization was carried out at 180°C for 1 hour. The product was purified by reprecipitation in a large amount of isopropanol to obtain an ionic group-containing oligomer a2 (terminal: hydroxyl group) represented by the following general formula (G4). The number average molecular weight was 16,000.
[0309] [Chemical formula 8]
[0310]
[0311] (In general formula (G4), M represents H, Na or K.)
[0312] [Synthesis example 5]
[0313] (Synthesis of neopentyl 3-(2,5-dichlorobenzoyl)benzenesulfonate represented by the following chemical formula (G5))
[0314] 245 g (2.1 mol) of chlorosulfonic acid was added to a 3L three-necked flask equipped with a stirrer and a condenser, followed by 105 g (420 mmol) of 2,5-dichlorobenzophenone, and the mixture was reacted in an oil bath at 100°C for 8 hours. After a predetermined time, the reaction solution was slowly poured into 1,000 g of crushed ice and extracted with ethyl acetate. The organic layer was washed with saline, dried with magnesium sulfate, and then ethyl acetate was distilled off to obtain 3-(2,5-dichlorobenzoyl)benzenesulfonyl chloride in the form of pale yellow crude crystals. The crude crystals were used directly in the next step without purification.
[0315] 41.1 g (462 mmol) of 2,2-dimethyl-1-propanol (neopentyl alcohol) was added to 300 mL of pyridine and cooled to about 10°C. The crude crystals obtained above were slowly added thereto over about 30 minutes. After adding the entire amount, the mixture was stirred for a further 30 minutes to react. After the reaction, the reaction solution was injected into 1,000 mL of hydrochloric acid water to recover the precipitated solid. The obtained solid was dissolved in ethyl acetate, washed with an aqueous sodium bicarbonate solution and brine, dried with magnesium sulfate, and ethyl acetate was distilled off to obtain crude crystals. It was recrystallized in methanol to obtain white crystals of 3-(2,5-dichlorobenzoyl)benzenesulfonic acid neopentyl ester represented by the following chemical formula (G5).
[0316] [Chemical formula 9]
[0317]
[0318] [Synthesis example 6]
[0319] (Synthesis of an oligomer not containing an ionic group represented by the following general formula (G6))
[0320] In a 1L three-necked flask equipped with a stirrer, a thermometer, a condenser, a Dean-Stark tube, and a three-way valve for introducing nitrogen, 49.4g (0.29mol) of 2,6-dichlorobenzonitrile, 88.4g (0.26mol) of 2,2-bis(4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, and 47.3g (0.34mol) of potassium carbonate were weighed. After nitrogen substitution, 346mL of sulfolane and 173mL of toluene were added and stirred. The flask was placed in an oil bath and heated to reflux at 150°C. When the water generated by the reaction was azeotropic with toluene and the reaction was carried out while removing water from the system using a Dean-Stark tube, almost no water was observed to be generated after about 3 hours. Most of the toluene was removed while the reaction temperature was slowly increased, and the reaction was continued at 200°C for 3 hours. Next, 12.3 g (0.072 mol) of 2,6-dichlorobenzonitrile was added and the mixture was reacted for further 5 hours.
[0321] After the obtained reaction solution was placed to cool, 100 mL of toluene was added to dilute it. The precipitate of the inorganic compound generated as a by-product was filtered out, and the filtrate was put into 2 L of methanol. The precipitated product was filtered and separated, recovered and dried, and dissolved in 250 mL of tetrahydrofuran. It was reprecipitated in 2 L of methanol to obtain 107 g of the target oligomer represented by the following general formula (G6). The number average molecular weight was 11,000.
[0322] [Chemical formula 10]
[0323]
[0324] [Synthesis Example 7]
[0325] (Synthesis of polyethersulfone (PES)-based block copolymer precursor b4′ formed of a segment represented by the following chemical formula (G8) and a segment represented by the following general formula (G9))
[0326] 1.62 g of anhydrous nickel chloride and 15 mL of dimethyl sulfoxide were mixed and adjusted to 70° C. 2.15 g of 2,2′-bipyridine was added thereto, and the mixture was stirred at the same temperature for 10 minutes to prepare a nickel-containing solution.
[0327] Among them, 1.49 g of 2,5-dichlorobenzenesulfonic acid (2,2-dimethylpropyl) ester and 0.50 g of SUMIKAEXCEL PES5200P (manufactured by Sumitomo Chemical Co., Ltd., Mn=40,000, Mw=94,000) represented by the following general formula (G7) were dissolved in 5 mL of dimethyl sulfoxide to obtain a solution. 1.23 g of zinc powder was added and adjusted to 70°C. The above-mentioned solution containing nickel was injected thereinto, and a polymerization reaction was carried out at 70°C for 4 hours. The reaction mixture was added to 60 mL of methanol, and then 60 mL of 6 mol / L hydrochloric acid was added and stirred for 1 hour. The precipitated solid was separated by filtration and dried to obtain 1.62 g of an off-white block copolymer precursor b4' containing a segment represented by the following chemical formula (G8) and the following general formula (G9) at a yield of 99%. The weight average molecular weight is 230,000.
[0328] [Chemical formula 11]
[0329]
[0330] [Synthesis example 8]
[0331] (Synthesis of Polybenzimidazole (PBI))
[0332] In a nitrogen atmosphere, polyphosphoric acid (PAA) was used as a polymerization solvent, 3,3'-diaminobenzidine (DAB) 22.7g (106mol), 4,4'-oxybisbenzoic acid (OBBA) 27.3g (106mol) were weighed, PAA was added in a manner of 3 mass%, the temperature was slowly raised while stirring, and the mixture was stirred at 140°C for 12 hours for polycondensation. After the reaction, the mixture was cooled to room temperature, injected into ion exchange water, solidified, and then neutralized with an aqueous sodium hydroxide solution. After filtering, washing with ion exchange water, and drying under reduced pressure at 80°C overnight, the target polybenzimidazole was obtained. The weight average molecular weight was 430,000.
[0333] [Polymer electrolyte solution A] A polymer electrolyte solution comprising a block copolymer b1 obtained by copolymerizing an oligomer represented by the general formula (G4) as a segment containing an ionic group and an oligomer represented by the general formula (G3) as a segment not containing an ionic group.
[0334] Into a 500mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 0.56g (4mmol) of potassium carbonate (Sigma-Aldrich Japan (same) reagent) and 16g (1mmol) of the oligomer a2 (terminal: hydroxyl group) containing an ionic group obtained in Synthesis Example 4 were charged, and after nitrogen substitution, 100mL of N-methylpyrrolidone (NMP) and 30mL of cyclohexane were added. After dehydration at 100°C, the temperature was raised to remove the cyclohexane, and 11g (1mmol) of the oligomer a1 (terminal: fluoro group) containing no ionic group obtained in Synthesis Example 3 was charged, and the reaction was carried out at 105°C for 24 hours. The block copolymer b1 was obtained by reprecipitation purification in a large amount of isopropanol. The weight average molecular weight was 340,000. The ion exchange capacity (IEC) of the block copolymer b1 was 2.1.
[0335] For the 5 mass% N-methylpyrrolidone (NMP) solution obtained by dissolving the obtained block copolymer b1, an angle rotor RA-800 was set on a variable frequency small high-speed cooling centrifuge (model 6930) manufactured by Kubota Manufacturing Co., Ltd., and the polymerization stock solution was directly centrifuged at 25°C, 30 minutes, and a centrifugal force of 20,000G. Since the precipitated solid matter (cake) and the supernatant (coating liquid) can be well separated, the supernatant is recovered. Next, vacuum distillation is performed at 80°C while stirring, and pressure filtration is performed using a 1μm polypropylene filter to obtain a polymer electrolyte solution A (polymer electrolyte concentration is 13 mass%). The viscosity of polymer electrolyte solution A is 1,300mPa·s.
[0336] [Polymer electrolyte solution B] A polymer electrolyte solution formed of a block copolymer b2 obtained by copolymerizing an oligomer represented by the general formula (G4) as a segment containing an ionic group and an oligomer represented by the general formula (G3) as a segment not containing an ionic group.
[0337] Block copolymer b2 was synthesized in the same manner as block copolymer b1 except that the oligomer a2 having an ionic group obtained in Synthesis Example 4 was 20 g (1.25 mmol). The weight average molecular weight of the block copolymer b2 was 370,000, and the ion exchange capacity (IEC) was 2.4. In addition, the viscosity of the polymer electrolyte solution B obtained by operating in the same manner as the polymer electrolyte solution A except that the block copolymer b2 was used instead of the block copolymer b1 was 1,600 mPa·s.
[0338] [Polymer electrolyte solution C] A polymer electrolyte solution formed of a block copolymer b3 obtained by copolymerizing an oligomer represented by the general formula (G4) as a segment containing an ionic group and an oligomer represented by the general formula (G3) as a segment not containing an ionic group.
[0339] Block copolymer b3 was synthesized in the same manner as polymer electrolyte solution A except that the oligomer a2 having an ionic group obtained in Synthesis Example 4 was 25.6 g (1.6 mmol). The weight average molecular weight of the block copolymer b3 was 390,000, and the ion exchange capacity (IEC) was 2.7. In addition, the viscosity of polymer electrolyte solution C obtained by operating in the same manner as polymer electrolyte solution A except that block copolymer b3 was used instead of block copolymer b1 was 1,800 mPa·s.
[0340] [Polymer electrolyte solution D] Polymer electrolyte solution D formed from random copolymer
[0341] Into a 5 L reaction vessel equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 129 g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane synthesized in Synthesis Example 1, 93 g of 4,4'-biphenol (Sigma-Aldrich Japan (same) reagent), and 422 g (1.0 mol) of 3,3'-disulfonated-4,4'-difluorobenzophenone disodium salt synthesized in Synthesis Example 2 were added, and the mixture was stirred for 2 h. After nitrogen substitution, 3,000 g of N-methyl-2-pyrrolidone (NMP), 450 g of toluene, and 232 g of 18-crown ether-6 (Fujifilm Wako Pure Chemical Industries, Ltd. reagent) were added, and after confirming that all monomers were dissolved, 304 g of potassium carbonate (Sigma-Aldrich Japan (same) reagent) was added, and dehydration was performed at 160° C. while reflux, and then the temperature was raised to remove toluene, and desalting polycondensation was performed at 200° C. for 1 hour. The weight average molecular weight of the obtained random copolymer was 320,000, and the ion exchange capacity (IEC) was 2.1.
[0342] Next, NMP was added to dilute the polymerization stock solution in such a way that the viscosity of the polymerization stock solution became 500 mPa·s, and an angle rotor RA-800 was set on a variable frequency small high-speed cooling centrifuge (model 6930) manufactured by Kubota Corporation, and direct centrifugal separation of the polymerization stock solution was performed under the conditions of 25°C, 30 minutes, and a centrifugal force of 20,000G. Since the precipitated solid matter (sediment) and the supernatant (coating liquid) can be well separated, the supernatant is recovered. Next, vacuum distillation was performed at 80°C while stirring to remove NMP until the polymer concentration became 14% by mass, and further pressure filtration was performed with a 5μm polyethylene filter to obtain a polymer electrolyte solution D. The viscosity of the polymer electrolyte solution D is 1,000 mPa·s.
[0343] [Polymer electrolyte solution E] A polymer electrolyte solution composed of a polyarylene-based block copolymer represented by the following general formula (G10):
[0344] 540 mL of dried N,N-dimethylacetamide (DMAc) was added under a nitrogen atmosphere to a mixture of 135.0 g (0.336 mol) of neopentyl 3-(2,5-dichlorobenzoyl)benzenesulfonate, 40.7 g (5.6 mmol) of an oligomer containing no ionic group represented by the general formula (G6) synthesized in Synthesis Example 6, 6.71 g (16.8 mmol) of 2,5-dichloro-4'-(1-imidazolyl)benzophenone, 6.71 g (10.3 mmol) of bis(triphenylphosphine)nickel dichloride, 35.9 g (0.137 mol) of triphenylphosphine, 1.54 g (10.3 mmol) of sodium iodide, and 53.7 g (0.821 mol) of zinc.
[0345] The reaction system was heated (finally heated to 79° C.) under stirring and the reaction was carried out for 3 hours. During the reaction, the viscosity of the system was observed to increase. The polymerization reaction solution was diluted with 730 mL of DMAc, stirred for 30 minutes, and filtered using diatomaceous earth as a filter aid.
[0346] The filtrate was concentrated by an evaporator, 43.8 g (0.505 mol) of lithium bromide was added to the filtrate, and the reaction was carried out for 7 hours under a nitrogen atmosphere at an internal temperature of 110°C. After the reaction, it was cooled to room temperature and injected into 4 L of acetone to solidify. After the solidified product was collected by filtration and air-dried, it was crushed with a mixer and washed with 1,500 mL of 1N hydrochloric acid while stirring. After filtration, the product was washed with ion exchange water until the pH of the washing liquid became 5 or more, and then dried at 80°C overnight to obtain 23.0 g of the target polyarylene block copolymer. The weight average molecular weight of the deprotected polyarylene block copolymer was 190,000, and the ion exchange capacity (IEC) was 2.0. The obtained polyarylene block copolymer was dissolved in an organic solvent of N-methyl-2-pyrrolidone / methanol = 30 / 70 (mass %) in a manner of 0.1 g / g to obtain a polymer electrolyte solution E. The viscosity of the polymer electrolyte solution E was 1,200 mPa·s.
[0347] [Chemical formula 12]
[0348]
[0349] [Polymer electrolyte solution F] Polymer electrolyte solution F composed of polyethersulfone block copolymer
[0350] 0.23 g of the block copolymer precursor b4' obtained in Synthesis Example 7 was measured, added to a mixed solution of 0.16 g of lithium bromide monohydrate and 8 mL of NMP, and reacted at 120°C for 24 hours. The reaction mixture was injected into 80 mL of 6 mol / L hydrochloric acid and stirred for 1 hour. The precipitated solid was separated by filtration. The separated solid was dried to obtain an off-white block copolymer b4 formed by a segment represented by the aforementioned general formula (G9) and a segment represented by the following chemical formula (G11). The weight average molecular weight of the obtained polyethersulfone block copolymer was 190,000, and the ion exchange capacity (IEC) was 2.0. The obtained polyethersulfone block copolymer was dissolved in an organic solvent of N-methyl-2-pyrrolidone / methanol = 30 / 70 (mass %) in a manner of 0.1 g / g to obtain a polymer electrolyte solution F. The viscosity of the polymer electrolyte solution F was 1,300 mPa·s.
[0351] [Chemical formula 13]
[0352]
[0353] [Polytetrafluoroethylene (ePTFE) porous substrate P1]
[0354] "Poreflon" (registered trademark) WP-010-80 (manufactured by Sumitomo Electric Fine Polymer Inc.) was stretched 10 times in the transverse direction and then heat treated at 365°C. Then, it was stretched 2 times in the longitudinal direction to produce an ePTFE porous substrate P1 having a film thickness of 9 μm and a porosity of 80%. The results of SEM observation showed that it had a structure having nodes with an average diameter of 0.9 μm roughly parallel to the longitudinal direction and fibrils with an average diameter of 0.2 μm roughly parallel to the transverse direction.
[0355] [Polytetrafluoroethylene (ePTFE) porous substrate P2]
[0356] Poreflon (registered trademark) HP-045-30 (manufactured by Sumitomo Electric Fine Polymer Inc.) was stretched three times in both the longitudinal and transverse directions to produce an ePTFE porous substrate P2 having a thickness of 8 μm and a porosity of 89%. SEM observation showed that the fibrils with an average diameter of 0.3 μm formed a random spider web-like structure.
[0357] [Hydrophilicized ePTFE porous substrate P2']
[0358] In a glove box with a dew point of -80°C, the ePTFE porous substrate B was immersed in a solution consisting of 30 g of a 1% solution of a metal sodium-naphthalene complex / tetrahydrofuran (THF) and 70 g of THF. After 3 seconds, the substrate was taken out and immediately rinsed thoroughly with THF to produce a hydrophilized ePTFE porous substrate P2' with a film thickness of 8 μm and a porosity of 88%.
[0359] [Porous substrate P3 formed of PBI fibers]
[0360] The PBI obtained in Synthesis Example 8 was dissolved in dimethyl sulfoxide (DMSO) in an amount of 8% by weight, and the electrospinning unit manufactured by KATO TECH CO., LTD. was used to spin the nanofiber nonwoven fabric at a voltage of 20 kV, a syringe pump discharge rate of 0.12 mL / hour, and a distance of 100 mm between the syringe and the target. The obtained nanofiber nonwoven fabric was dried under reduced pressure at 80°C for 1 hour, and then laminated on a "Kapton" (registered trademark) substrate having a thickness of 125 μm, and heated at 400 degrees for 10 minutes in a nitrogen atmosphere, thereby obtaining a porous substrate P3 formed of PBI fibers having an average fiber diameter of 160 nm and a thickness of 7 μm. The porosity was 86%.
[0361] [Polytetrafluoroethylene (ePTFE) porous substrate P4]
[0362] "Tetratex" (registered trademark) TX1356 (manufactured by Donaldson) was used as the porous substrate P4. The film thickness was 8 μm and the porosity was 85%.
[0363] <Manufacturing of electrolyte membrane>
[0364] [Example 1]
[0365] 0.26 g of the polyoxyethylene ether surfactant "Ftergent" (registered trademark) 208G (manufactured by NEOS (Co., Ltd.)) (fluorine atom content of 54% by mass, hydrophilic element content of 11% by mass, weight average molecular weight of 1,800) was dissolved in 100 g of polymer electrolyte solution A to prepare an electrolyte-surfactant mixed solution with a mass ratio of polymer electrolyte to surfactant (hereinafter referred to as "surfactant / electrolyte") of 0.02. Using a doctor blade coater, the electrolyte-surfactant mixed solution was cast on a glass substrate and bonded to the ePTFE porous substrate P1. After keeping at room temperature for 1 hour, the electrolyte-surfactant mixed solution A was fully impregnated in the ePTFE porous substrate P1, and then dried at 100°C for 4 hours. The electrolyte-surfactant mixed solution A was cast again on the upper surface of the dried film, kept at room temperature for 1 hour, and dried at 100°C for 4 hours to obtain a film-like polymer. The membrane was immersed in a 10 mass % sulfuric acid aqueous solution at 80° C. for 24 hours to carry out proton substitution and deprotection reaction, and then immersed in a large excess of pure water for 24 hours to carry out thorough washing, thereby obtaining an electrolyte membrane (membrane thickness: 9 μm).
[0366] [Example 2]
[0367] An electrolyte membrane (membrane thickness: 9 μm) was obtained in the same manner as in Example 1 except that an electrolyte-surfactant mixed solution having a surfactant / electrolyte ratio of 0.10 was used.
[0368] [Example 3]
[0369] An electrolyte membrane (membrane thickness: 9 μm) was obtained in the same manner as in Example 1 except that an electrolyte-surfactant mixed solution having a surfactant / electrolyte ratio of 0.01 was used.
[0370] [Example 4]
[0371] An electrolyte membrane (membrane thickness: 9 μm) was obtained in the same manner as in Example 1 except that the polymer electrolyte solution B was used instead of the polymer electrolyte solution A.
[0372] [Example 5]
[0373] An electrolyte membrane (membrane thickness: 9 μm) was obtained in the same manner as in Example 1 except that the polymer electrolyte solution C was used instead of the polymer electrolyte solution A.
[0374] [Example 6]
[0375] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Example 1 except that the polymer electrolyte solution D was used instead of the polymer electrolyte solution A.
[0376] [Example 7]
[0377] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Example 1 except that the polymer electrolyte solution E was used instead of the polymer electrolyte solution A.
[0378] [Example 8]
[0379] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Example 1 except that the polymer electrolyte solution F was used instead of the polymer electrolyte solution A.
[0380] [Example 9]
[0381] The electrolyte membrane (membrane thickness: 10 μm) was obtained by the same operation as in Example 1 except that the polyoxyethylene ether surfactant "Ftergent" (registered trademark) FTX-218 (manufactured by NEOS (Co., Ltd.)) (fluorine atom content: 46% by mass, hydrophilic element content: 14% by mass, weight average molecular weight: 1,900) was used instead of "Ftergent" (registered trademark) 208G.
[0382] [Example 10]
[0383] A low metal content grade polyoxyethylene ether surfactant "Ftergent" (registered trademark) DFX-18 (manufactured by NEOS (Co., Ltd.)) (fluorine atom content of 46% by mass, hydrophilic element content of 14% by mass, weight average molecular weight of 1,900) was used instead of "Ftergent" (registered trademark) 208G. Except for this, the same operation as in Example 1 was carried out to obtain an electrolyte membrane (membrane thickness of 10 μm).
[0384] [Example 11]
[0385] An electrolyte membrane (membrane thickness: 10 μm) was obtained by the same operation as in Example 1, except that an oligomer-based surfactant "Ftergent" (registered trademark) 710FS (manufactured by NEOS Corporation) containing a fluorine-containing hydrophilic group / lipophilic group (fluorine atom content of 16% by mass, hydrophilic element content of 30% by mass, weight average molecular weight of 3,500) was used instead of "Ftergent" (registered trademark) 208G.
[0386] [Example 12]
[0387] An electrolyte membrane (membrane thickness: 8 μm) was obtained in the same manner as in Example 1 except that the ePTFE porous substrate P2 was used instead of the ePTFE porous substrate P1.
[0388] [Example 13]
[0389] An electrolyte membrane (membrane thickness: 9 μm) was obtained in the same manner as in Example 1, except that the oligomer surfactant "MEGAFACE" (registered trademark) F-555 (manufactured by DIC Corporation) containing a fluorine-containing hydrophilic group / lipophilic group was used instead of "Ftergent" (registered trademark) 208G.
[0390] [Example 14]
[0391] Use a doctor blade coater to cast polymer electrolyte solution A on a glass substrate and adhere to the PBI porous substrate P3. Keep it at room temperature for 1 hour, and after fully impregnating the PBI porous substrate P3 with polymer electrolyte solution A, dry it at 100°C for 4 hours. On the upper surface of the dried film, cast polymer electrolyte solution A again, keep it at room temperature for 1 hour, and dry it at 100°C for 4 hours to obtain a film-like polymer. Immerse it in a 10% by mass sulfuric acid aqueous solution at 80°C for 24 hours to perform proton substitution and deprotection reactions, and then immerse it in a large excess of pure water for 24 hours to fully wash it to obtain an electrolyte membrane (film thickness of 8μm).
[0392] [Example 15]
[0393] An electrolyte membrane (membrane thickness: 9 μm) was obtained in the same manner as in Example 1 except that the ePTFE porous substrate P4 was used instead of the ePTFE porous substrate P1.
[0394] [Comparative Example 1]
[0395] 100 g of polymer electrolyte solution A was cast on a glass substrate using a knife coater and then dried at 100° C. for 4 hours to obtain a film-like polymer. The substrate was immersed in a 10% by mass sulfuric acid aqueous solution at 80° C. for 24 hours to perform proton substitution and deprotection reactions, and then immersed in a large excess of pure water for 24 hours to perform thorough washing to obtain an electrolyte membrane (film thickness of 10 μm).
[0396] [Comparative Example 2]
[0397] An attempt was made to produce an electrolyte membrane in the same manner as in Example 1 except that “Ftergent” (registered trademark) 208G was not used. However, the polymer electrolyte solution A did not permeate into the porous substrate, and an electrolyte membrane could not be obtained.
[0398] [Comparative Example 3]
[0399] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Comparative Example 1 except that the polymer electrolyte solution B was used instead of the polymer electrolyte solution A.
[0400] [Comparative Example 4]
[0401] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Comparative Example 1 except that the polymer electrolyte solution C was used instead of the polymer electrolyte solution A.
[0402] [Comparative Example 5]
[0403] An electrolyte membrane (membrane thickness: 8 μm) was obtained in the same manner as in Example 5 except that the ePTFE porous substrate P2 was used instead of the ePTFE porous substrate P1.
[0404] [Comparative Example 6]
[0405] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Comparative Example 1 except that the polymer electrolyte solution D was used instead of the polymer electrolyte solution A.
[0406] [Comparative Example 7]
[0407] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Comparative Example 1 except that the polymer electrolyte solution E was used instead of the polymer electrolyte solution A.
[0408] [Comparative Example 8]
[0409] A composite electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Comparative Example 1 except that the polymer electrolyte solution F was used instead of the polymer electrolyte solution A.
[0410] [Comparative Example 9]
[0411] An electrolyte membrane (membrane thickness: 10 μm) was obtained in the same manner as in Comparative Example 2 except that the hydrophilized ePTFE porous substrate P2 ′ was used instead of the ePTFE porous substrate P1 .
[0412] [Comparative Example 10]
[0413] The surfactant "Triton" (registered trademark) X-100 (non-fluorine-based surfactant) (fluorine atom content of 0, hydrophilic element content of 27% by mass, weight average molecular weight of 700) was used instead of "Ftergent" (registered trademark) 208G. Except for this, the preparation of the electrolyte membrane was attempted in the same manner as in Example 1. However, the polymer electrolyte solution A did not penetrate into the porous substrate, and the electrolyte membrane could not be obtained.
[0414] [Comparative Example 11]
[0415] The surfactant perfluorooctane sulfonic acid (PFOS) (anionic fluorine-based surfactant) (fluorine atom content of 65% by mass, hydrophilic element content of 16% by mass, weight average molecular weight of 500) was used instead of "Ftergent" (registered trademark) 208G. Except for this, the electrolyte membrane (membrane thickness of 10 μm) was obtained in the same manner as in Example 1.
[0416] The electrolyte membranes produced in Examples 1 to 12, Comparative Examples 1, Comparative Examples 3 to 9, and Comparative Example 11 were evaluated for ion exchange capacity (IEC), filling rate of polymer electrolyte in the composite layer, and dimensional change rate λ. xy , proton conductivity, mechanical properties in a dry state, mechanical properties in a hydrated state, haze, diffusion permeability, and dry-wet cycle durability. In addition, for the polymer membrane containing ionic groups constituting the electrolyte membrane, the presence or absence of a phase separation structure was evaluated, and for the porous substrate, the fluorine atom content, oxygen atom content, and porosity were evaluated. Their evaluation results are shown in Tables 1 and 2. In addition, with regard to dry-wet cycle durability, the evaluation was terminated at 20,000 cycles when the hydrogen permeation current did not exceed 10 times the initial current even if more than 20,000 cycles were performed.
[0417] [Table 1]
[0418]
[0419] Note 1) Polymer electrolyte A: block copolymer b1, polymer electrolyte B: block copolymer b2, polymer electrolyte C: block copolymer b3, polymer electrolyte D: random copolymer, polymer electrolyte E: polyarylene-based block copolymer, polymer electrolyte F: polyethersulfone-based block copolymer b4
[0420] Note 2) Porous substrate P1: polytetrafluoroethylene (ePTFE) with a film thickness of 9 μm and a porosity of 80%, porous substrate P2: polytetrafluoroethylene (ePTFE) with a film thickness of 8 μm and a porosity of 89%, porous substrate P2': hydrophilized ePTFE with a film thickness of 8 μm and a porosity of 88%, porous substrate P3: polybenzimidazole (PBI) with a film thickness of 7 μm and a porosity of 86%, porous substrate P4: polytetrafluoroethylene (ePTFE) with a film thickness of 8 μm and a porosity of 85%.
[0421] [Table 2]
[0422]
[0423] Industrial Applicability
[0424] The electrolyte membrane of the present invention can be applied to various uses. For example, it can be applied to medical uses such as artificial skin, filtration uses, ion exchange resin uses such as chlorine-resistant reverse osmosis membranes, various structural material uses, electrochemical uses, humidification membranes, antifogging films, antistatic films, deoxidation membranes, solar cell membranes, and gas barrier membranes. Among them, it can be more preferably used for various electrochemical uses. As electrochemical uses, for example, solid polymer fuel cells, redox flow batteries, water electrolysis devices, chlor-alkali electrolysis devices, electrochemical hydrogen pumps, and water electrolysis hydrogen generation devices can be cited.
[0425] In solid polymer fuel cells, electrochemical hydrogen pumps, and water electrolysis hydrogen generation devices, the electrolyte membrane is used in a state where a catalyst layer, an electrode substrate, and a diaphragm are sequentially stacked on both sides. In particular, the product obtained by sequentially stacking a catalyst layer and a gas diffusion substrate on both sides of the electrolyte membrane (i.e., a product consisting of a layer of gas diffusion substrate / catalyst layer / electrolyte membrane / catalyst layer / gas diffusion substrate) is called a membrane electrode complex (MEA). The electrolyte membrane of the present invention can be suitably used as an electrolyte membrane constituting the aforementioned CCM and MEA.
Claims
1. A composite polymer electrolyte membrane comprising a polymer electrolyte and a porous substrate, wherein the composite polymer electrolyte membrane has a dry tensile elastic modulus per unit width of 100 N / cm or more, a hydrated tensile elastic modulus per unit width of 35 N / cm or more, and a hydrated tensile elongation at break of 60% or more, The polymer electrolyte is a fluorine-based polymer electrolyte having an ionic group or a hydrocarbon-based polymer having an ionic group. 2 . The composite polymer electrolyte membrane according to claim 1 , wherein the water-containing tensile elastic modulus per unit cross-sectional area is 400 MPa or more.
3. The composite polymer electrolyte membrane according to claim 1 or 2, wherein: The water-containing tensile elastic modulus / dry tensile elastic modulus is 0.3 or more.
4. The composite polymer electrolyte membrane according to claim 1 or 2, which has a water-containing tensile strength of 5 N / cm or more.
5. The composite polymer electrolyte membrane according to claim 1 or 2, wherein: The porous substrate is a fluorine-based porous substrate.
6. The composite polymer electrolyte membrane according to claim 1 or 2, wherein: The porous substrate has an oxygen atom content of 10 mass % or less.
7. The composite polymer electrolyte membrane according to claim 1 or 2, wherein: The polymer electrolyte is a hydrocarbon-based polymer having an ionic group. 8 . The composite polymer electrolyte membrane according to claim 1 , further comprising a nonionic fluorine-based surfactant.
9. The composite polymer electrolyte membrane according to claim 8, wherein: The nonionic fluorine-based surfactant is a compound having a nonionic mediophilic group and a fluorine-containing group consisting of a fluorinated alkyl group, a fluorinated alkenyl group or a fluorinated aryl group.
10. The composite polymer electrolyte membrane according to claim 1 or 2, wherein: The porous substrate is an aromatic hydrocarbon-based porous substrate.
11. The composite polymer electrolyte membrane according to claim 10, wherein: The porous substrate is a polyazole-based porous substrate.
12. The composite polymer electrolyte membrane according to claim 10, wherein: The porous substrate is formed of polybenzimidazole.
13. The composite polymer electrolyte membrane according to claim 1 or 2, wherein: The haze value when light is transmitted in the thickness direction is 20% or more and 45% or less.
14. The composite polymer electrolyte membrane according to claim 1 or 2, wherein: The diffuse transmittance when light is transmitted in the thickness direction is 20% or more and 40% or less.
15. A composite polymer electrolyte membrane with a catalyst layer, wherein the composite polymer electrolyte membrane according to any one of claims 1 to 14 is formed by sandwiching the catalyst layer on both sides. 16 . A membrane electrode assembly comprising the composite polymer electrolyte membrane according to claim 1 .
17. A solid polymer fuel cell comprising the composite polymer electrolyte membrane according to any one of claims 1 to 14.