Cosmetics containing powder
By layer-coating titanium oxide and iron oxide on the surface of mica, and combining it with spherical powder of a specific particle size, a dense layered composite powder is formed using a precipitation method, which solves the problem of titanium oxide and iron oxide-coated composite powder in the existing technology. The problem of poor surface uniformity of mica achieves the effect of high UV ray blocking and long-term even application of makeup.
Patent Information
- Application Number
- CN202180005180.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-29
AI Technical Summary
In existing cosmetics, titanium oxide and iron oxide-coated composite powders have poor uniformity on the mica surface, resulting in insufficient UV-blocking capabilities or uneven application, and are prone to dryness, making it difficult to apply makeup evenly for a long time.
By coating the mica surface with 30-50% titanium oxide in a layer, and covering it with 0.1-3.0% iron oxide, combined with spherical powder of a specific particle size and titanium oxide/zinc oxide, the oxidation is carried out using a precipitation method rather than an adsorption method. The dense layered coating of titanium, combined with a hydrophobizing treatment agent, forms a non-brightening composite powder that is oriented on the skin surface to achieve even application and high UV protection.
It achieves a high UV-blocking effect, hides spots naturally and evenly without feeling dry, and can apply makeup evenly and continuously for a long time.
Smart Images

Figure GDA0005029426580000141 
Figure GDA0005029426580000171 
Figure GDA0005029426580000181
Abstract
Description
Technical Field
[0001] The present invention relates to a powder-containing cosmetic, which contains: a composite powder without brilliance in which titanium oxide is layered on the surface of mica and then iron oxide is coated, a spherical powder with a specific size, and coated titanium oxide with a specific particle size; more specifically, the present invention relates to a powder-containing cosmetic, which does not feel burdensome when applied to the skin, especially evenly and naturally covers spots and uneven skin color, and does not feel dry even after a long time, and can be applied evenly continuously, while having a high shielding ability in the ultraviolet range. Background Art
[0002] In the past, in cosmetics containing powders, various concealing powders have been developed and researched for blending in order to naturally and evenly cover uneven skin color such as high spots, liver spots, age spots, acne marks, etc. that consumers are troubled by. In particular, titanium oxide is widely used as a concealing powder due to its high refractive power, excellent whiteness and coloring power, and is also widely used for the purpose of having an ultraviolet protection effect. On the other hand, iron oxide is widely used as a coloring pigment for color matching in order to suit various skin types.
[0003] For example, in order to achieve the purpose of having an anti-ultraviolet effect and excellent moldability, the following solid powder cosmetics have been developed: by using two or more plate-like powders with an aspect ratio of 10 or more without brilliance coated on the surface of mica, spots and uneven skin color are naturally hidden, while preventing ultraviolet rays from protecting the skin (for example, refer to patent document 1). Furthermore, by combining plate-like powders coated with fine-particle inorganic powders with high anti-ultraviolet effect with spherical powders coated with the same fine-particle inorganic powders, powder cosmetics with excellent anti-ultraviolet effect and usability have been developed (for example, refer to patent document 2). Moreover, solid powder cosmetics with the following cosmetic effects have been developed: in cosmetics using composite powders in which metal oxides with limited particle sizes are coated on plate-like powders, there is no squeaking feeling, powdery feeling, dullness, and a transparent feeling after coating (for example, refer to patent document 3).
[0004] On the other hand, in order to achieve natural makeup with covering properties, a powder obtained by coating the surface of titanium oxide with a specific particle size with iron oxide has been developed, and a cosmetic film has been developed that has covering power, is white and does not look unnatural, and has less dark color caused by long-term immersion (for example, refer to Patent Document 4).
[0005] Furthermore, as powders for covering up uneven skin surfaces such as pores and spots, spherical powders of various particle sizes and compositions have been developed, and spherical cellulose powders having a soft focus effect through diffuse reflection of visible light have been developed. Also, cosmetics having a smooth feel without a sticky feeling and excellent long-term stability have been developed (for example, see Patent Document 5).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 05558061
[0009] Patent Document 2: Japanese Patent Application Publication No. 2012-240999
[0010] Patent Document 3: Japanese Patent Application Publication No. 2017-081858
[0011] Patent Document 4: Japanese Patent Application Publication No. 2007-145778
[0012] Patent Document 5: Japanese Patent Application Publication No. 2013-231020 Summary of the invention
[0013] Problem that the invention aims to solve
[0014] However, in the prior art of the above-mentioned Patent Document 1, as a method for coating titanium oxide on plate-like mica, a method is to mix and fix titanium oxide and mica using a bead mill, etc., but titanium oxide is not evenly coated on the surface of mica, and there are cases where the ultraviolet shielding ability or the sense of touch without burden is poor. There is room for further improvement in the coating method or the composition of the composite powder. Furthermore, in Patent Documents 2 and 3, the fine particle inorganic powder coated on the plate-like powder is a specific granular shape, and the surface smoothness is poor compared with the layered coating, so the spreadability is not good, the oil absorption becomes high, and a dry feeling is felt, and it is difficult to arrange evenly on the skin surface. It is hoped that a plate-like powder that can maximize the ultraviolet shielding ability and does not have a brilliance layered coated metal oxide can be smoothly applied to the skin without feeling dry.
[0015] On the other hand, when it is desired to provide a higher UV shielding capability in a powder-containing cosmetic material using the prior art technology of the above-mentioned Patent Document 4, in the iron oxide-coated titanium oxide that naturally hides spots or uneven skin color, the monomer combination thereof is poor, and thus the function can be improved by combining it with a particulate metal oxide, but the application is burdensome and the makeup is unnatural, and therefore it is desired to develop a powder-containing cosmetic material that can provide both natural makeup and high UV shielding capability.
[0016] In addition, in the prior art of the above-mentioned patent document 5, while studying the repair of pores or bumps, absorbing sebum secreted for a long time and continuously and evenly applying makeup, there is no in-depth study on the following problem: these powders, by combining with other matched applied powders, are easy to selectively exist in the concave parts of the skin, effectively absorb the sebum in the pores, and reduce the dryness of the convex parts.
[0017] As described above, conventional techniques have not considered various surface shape controls that can promote appropriate placement of powder on the skin while exerting various effects.
[0018] Means of solving the problem
[0019] The present inventors have conducted intensive research to solve the above-mentioned problems, and as a result, have discovered the following powder-containing cosmetic material, thereby completing the invention: by combining a composite powder having a layered coating of titanium oxide on the surface of mica and then coated with iron oxide without luster, a spherical powder having a specific size and titanium oxide having a specific particle size and surface coating, it is possible to apply the powder evenly without a sense of burden, and at the same time, the makeup has a natural appearance, has a uniform concealing effect on spots and uneven skin color, does not feel dry over time, can be applied for a long time, and has an excellent ultraviolet shielding effect.
[0020] That is, the present invention is a powder-containing cosmetic, characterized in that it is based on the technical consideration that spherical powder with a specific particle size is oriented in the grooves, and on the other hand, iron oxide and titanium oxide-coated plate-like mica are oriented in the hillocks, and contains the following components (A) to (C), and further contains (D).
[0021] [1] A powder-containing cosmetic comprising the following ingredients (A) to (C);
[0022] (A) A composite powder, which is a plate-like composite powder without brilliance, wherein the surface of mica is coated with 30 to 50% by mass of titanium oxide and further coated with 0.1 to 3.0% by mass of iron oxide in a layered manner.
[0023] (B) Spherical powder with an average particle size of 1 to 40 μm
[0024] (C) Titanium oxide and / or zinc oxide having an average particle size of 0.1 to 1.2 μm coated with one or more oxides or hydroxides selected from iron, aluminum and silicon.
[0025] [2] The powder-containing cosmetic according to [1], wherein the titanium oxide of the component (A) does not form particles on the surface of mica, and the average thickness of the titanium oxide layer is 50 to 100 nm.
[0026] [3] The powder-containing cosmetic according to [1] or [2], wherein the component (A) is further coated with a hydrophobicizing agent.
[0027] [4] The powder-containing cosmetic according to any one of [1] to [3], wherein the component (A) is further coated with 0.1 to 4% by mass of zinc oxide.
[0028] [5] The powder-containing cosmetic according to any one of [1] to [4], wherein the component (C) is titanium oxide coated with one or more oxides or hydroxides selected from iron, aluminum and silicon.
[0029] [6] The powder-containing cosmetic according to any one of [1] to [5], wherein the component (B) is a spherical powder of one or more selected from cellulose, silicon dioxide, calcium carbonate, starch, calcium alginate, silicone, and polyurethane.
[0030] [7] The powder-containing cosmetic according to any one of [1] to [6], wherein the transmittance at wavelengths of 300 nm and 360 nm of a coating film obtained by applying and drying a solution containing 40% by mass of the component (A) is less than 25%, respectively.
[0031] [8] The powder-containing cosmetic according to any one of [1] to [7], further comprising 2 to 40% by weight of component (D): a powder surface-treated with cross-linked silicone.
[0032] In addition, the present technology may further adopt the following configurations.
[0033] [9] The powder-containing cosmetic according to any one of [1] to [8], further comprising ingredient (E): one or more selected from 1,2-alkanediol, ethylhexylglycerin, chlorphenesin, and dipropylene glycol.
[0034]
[10] The powder-containing cosmetic according to any one of [1] to [9], wherein the oil absorption of the component (B) is 60 to 350 ml / 100 g.
[0035]
[11] The powder-containing cosmetic according to any one of [1] to
[10] , wherein the oil absorption of the component (A) is less than 70 ml / 100 g.
[0036]
[12] A makeup method, characterized in that the makeup mask containing the solid powder cosmetic material described in any one of [1] to
[11] is configured such that component (A) is placed on the skin hillocks, and component (B) is placed on the skin grooves.
[0037] Effects of the Invention
[0038] The powder-containing cosmetic material of the present invention has a high ultraviolet shielding effect, and at the same time has a natural and uniform concealing effect on spots and uneven skin color, and does not feel dry and can be applied evenly for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 : Iron oxide / titanium oxide-coated sericite of the present invention prepared by the precipitation method (Production Example 5).
[0040] Figure 2 : Conventional titanium oxide / zinc oxide-coated sericite prepared by an adsorption method (Comparative Production Example 1).
[0041] Modes for Carrying Out the Invention
[0042] The preferred embodiments of the present invention are described in detail. However, the present invention is not limited to the following preferred embodiments and can be freely changed within the scope of the present invention. Moreover, in this specification, percentages are expressed by mass unless otherwise specified. In addition, in this specification, when a numerical range is expressed by ~, the range includes the numerical values at both ends. Moreover, the "average particle size" in the present invention is a value (median diameter D50) obtained by observing the surface state using a scanning electron microscope (manufactured by JEOL, JSM-7800prime) and measuring with an image analyzer (Luzer AP, manufactured by Nileco), which refers to the major diameter of the particles.
[0043] The component (A) used in the present invention is a plate-like composite powder without brilliance, in which 30 to 50% by mass of titanium oxide and further 0.1 to 3% by mass of iron oxide are layered on the surface of mica. The composite powder does not feel dry and can be applied evenly for a long time, and has a high ultraviolet shielding effect.
[0044] The mica of the mother powder of the plate-like composite powder of component (A) of the present invention has a plate shape, and examples thereof include: phlogopite, muscovite, especially natural mica such as sericite, synthetic phlogopite, or synthetic mica such as (fluoride / hydroxide / oxidation) / (Mg / K / silicon). Its aspect ratio is preferably 10 to 50, and more preferably 10 to 30. When the aspect ratio is small, the amount of titanium oxide coated decreases, so there is a poor ultraviolet shielding effect, and the orientation of the skin hillock decreases, resulting in a poor uniform cosmetic film. In addition, when the aspect ratio is large, the bulk specific gravity becomes high, so there is a limit on the amount of cosmetics containing the powder.
[0045] Among them, sericite with high whiteness which hardly has brilliance when composited in layers is preferred, or synthetic phlogopite which has little color change when immersed in oil and whose surface treatment during coating can control brilliance and adhesion of metal oxides is preferred, and sericite which can be purchased cheaply is particularly preferred.
[0046] The method for coating the titanium oxide of the component (A) of the present invention on mica is different from the following methods (hereinafter collectively referred to as adsorption methods): using mechanical force such as a bead mill, Henchel mixer, pulverizer, etc. to mechanochemically fix (adsorb) titanium oxide or iron oxide prepared in advance on the surface, or spraying and adsorbing a dispersed solvent; instead, the method is to precipitate and grow titanium oxide densely on the surface of mica (hereinafter referred to as precipitation method). For example, mica is suspended in a dilute strongly acidic solution of titanyl sulfate at ambient temperature, and the solution is rapidly heated to 90 to 100° C. and kept at this temperature for about 2 to 3 hours to precipitate a hydrous oxide layer on the substrate by hydrolyzing the titanium sulfate solution; or a substrate is suspended in hot water, a strongly acidic concentrated titanyl sulfate solution is rapidly added, and the hot water is continuously heated until the hydrolysis is completed, thereby causing hydrolysis and precipitation of titanium hydroxide on the mica. According to these precipitation methods, the entire surface of the plate-like mica can be coated with titanium oxide having ultraviolet shielding ability in a layered manner, so that compared with the conventional adsorption method, there is no aggregation of titanium oxide, and a composite powder with no burdensome feel can be obtained.
[0047] The amount of titanium oxide in the component (A) of the present invention is preferably 30 to 50%. When the amount is too small, the ultraviolet shielding effect is poor. When the amount exceeds 50%, an excessive amount is formed on the mica surface, and it is difficult to form a uniform layer and cannot be composited. In some cases, it precipitates as particles alone. In this case, the touch of application is poor, and the composite powders agglomerate with each other, and effective ultraviolet shielding ability cannot be obtained. In addition, it is difficult to distribute smoothly on the skin, and a uniform concealing effect cannot be expected, and a dry feeling may be felt. Layered coating means that the titanium oxide on the mica surface does not form a particle shape on the mica surface. The thickness of the titanium oxide layer is preferably 50 to 100 nm, and it is preferred to have a smooth layer with few unevenness, but the thickness is not particularly limited. If it is within the thickness range of this layer, it is difficult to produce covering power, the ultraviolet shielding effect is efficient, and it is easy to achieve uniform spreading in the skin bumps. There are few unevenness and the oil absorption is difficult to increase, so the dry feeling can be reduced in the skin bumps that are prone to dryness.
[0048] Furthermore, as a method for further coating the titanium oxide-coated mica of the component (A) of the present invention with iron oxide, it can be a dry method, a wet method, etc., without particular limitation. For example, after the slurry of the coated pigment is uniformly dispersed in an aqueous solution of a water-soluble iron salt (ferrous chloride, ferric chloride, ferrous sulfate, ferrous sulfate, ferrous nitrate, ferric nitrate, etc.), an aqueous solution of sodium acetate is slowly added under stirring to adjust the pH to 3 to 5, and the iron salt is hydrolyzed by heating to a temperature above 60°C, thereby selectively precipitating an amorphous hydrous oxide on the surface of the particles of the coated pigment, and an aqueous solution of alkali is added at the stage where the external color changes, and the pH of the system is adjusted to pH 8 to 9.5 while heating. Thereafter, the titanium oxide-coated mica coated with iron oxide can be obtained by filtering, washing with water, drying or sintering and pulverizing.
[0049] The amount of iron oxide in the component (A) of the present invention is not particularly limited. As a lower limit, it is preferably 0.1% or more, more preferably 1.0% or more, and further preferably 1.5%. As an upper limit, it is preferably 5% or less, more preferably 3%, and further preferably 2.5%. If it is within this range, the bluish whiteness of the composite powder itself is reduced, and a more natural color tone that is more suitable for the skin can be obtained. In addition, reducing the amount of iron oxide used for other purposes in cosmetics containing powders can reduce the cohesion of iron oxide and improve the ultraviolet shielding effect, especially in the UVA region. Moreover, when 0.1 to 4% by mass is coated with zinc oxide, the ultraviolet shielding effect is further improved, the anticorrosive power is also improved, and it is also easy to form metal soaps by reaction with the surface treatment agent, which can further impart excellent effects. If it is within this coating range, the cohesive force of zinc oxide will not hinder uniform application, so it is more preferred.
[0050] As a method for measuring the surface treatment of metals, for example, the surface treatment amount of each metal contained in a sample (powder) can be obtained by measuring the prepared sample by ICP (Inductively Coupled Plasma; ARCOS (Dospicto Corporation)) emission spectrometry using a general method.
[0051] Component (A) of the present invention does not have brilliance, but the presence or absence of brilliance can be measured and defined, for example, by the following measurement method. That is, a 40 mm wide double-sided tape manufactured by Nichiban is attached to the black part of the OPACITYCHARTS manufactured by LENETA, and the composite powder is evenly applied with a cosmetic puff. A digital variable angle gloss meter manufactured by Suga Testing Instruments is used to fix the coated sample at an incident angle of 45 degrees, and the gloss intensity (I20) at an angle of 20 degrees and the gloss intensity (I45) at an angle of 45 degrees are measured, and I45 / I20 is calculated. Their ratio is
[0052] I45 / I25=2.0 or above: Brightness
[0053] I45 / I25=2.0 Insufficient: No brilliance.
[0054] The UV transmittance of the composite powder of component (A) of the present invention is evaluated under the following conditions. First, in a nitrocellulose solution of 43.4% butyl acetate, 21.0% ethyl acetate, 14.6% IPA, and 21.0% nitrocellulose, the composite powder of component (A) is added to make the concentration 40%, and then dispersed under the conditions of a dispersion rotation number of 3000 rpm and 10 minutes. Then, the dispersion is used to prepare a coating film on a quartz plate using a scraper (12μm thickness) to make the thickness uniform, and the dried coating film is measured using a spectrophotometer (U-4100 made by HITACHI Co., Ltd.) The transmittance of the coating film in the wavelength range of 250 to 700nm. The transmittance at 360nm is used as an evaluation of the shielding ability in the UVA region of 320 to 400nm, and the transmittance at 300nm is used as an evaluation of the shielding ability in the UVB region of 280 to 320nm. It is preferred that the transmittance is less than 50%, and it is more preferred that the transmittance is less than 25%.
[0055] Furthermore, the average particle size of component (A) of the present invention is not particularly limited. As a lower limit, it is preferably 3 μm or more, and as an upper limit, it is preferably 30 μm or less, and more preferably 20 μm or less. In particular, it is more preferred that the particle size distribution is concentrated but a uniform cosmetic film is easily formed.
[0056] Moreover, the component (A) of the present invention preferably has a low oil absorption. The oil absorption of the present invention is defined as the oil absorption of triisooctanoin, a triglyceride similar to sebum, and the determination method thereof is based on the method of JIS K5105. To 100 g of spherical powder, triisooctanoin, a cortical component, is slowly added instead of linseed oil, and the end point is taken as the time when it becomes a slurry. There is no particular limitation, but it is preferably 100 ml / 100 g or less, and more preferably 70 ml / 100 g or less. The component (A) of the present invention is plate-shaped, so it is easy to adhere to the smooth convex part of the skin, but the matrix mica is thin and the metal oxide is compounded on the surface, so the oil absorption per unit weight is easy to become high, and it is a material with such a tendency. When the oil absorption is too high, the sebum on the skin surface is removed, and a dry feeling is easily felt, and the amount of compounding or surface treatment in the cosmetic becomes excessive, so there are cases where appropriate adjustment is required.
[0057] Therefore, the component (A) of the present invention can be applied smoothly and has a reduced dry feeling by the hydrophobic surface treatment, and can further improve the makeup durability. The hydrophobic treatment agent is not particularly limited, but will be described in detail later.
[0058] The amount of the powder-containing cosmetic material of the component (A) used in the present invention is preferably 1% or more, more preferably 3% or more, and even more preferably 5% or more as the lower limit. The upper limit is preferably 50% or less, more preferably 30% or less, and even more preferably 15% or less. Within this range, it is particularly good in terms of the UV shielding effect, natural makeup, and no dry feeling.
[0059] The spherical powder of component (B) used in the present invention has an average particle size of 1 to 40 μm. Spherical means that the ratio of the major diameter to the minor diameter is 1 to 1.5. In particular, even if there are slight irregularities on the surface, it does not matter if the inside is hollow. As a lower limit, the average particle size is 1 μm or more, preferably 3 μm or more, and as an upper limit, it is 40 μm or less, preferably 30 μm or less. When the average particle size is less than 1 μm, the cohesion in the furrow increases, and the effect of hiding irregularities such as pores or spots is poor. When it exceeds 40 μm, the application is not good, it will scatter and the makeup durability will deteriorate, so it is not preferred. The material is not particularly limited, and examples thereof include: nylon powder, polystyrene powder, polyethylene powder, polymethyl methacrylate resin powder, silicone resin powder, polyurethane powder, cellulose powder, cellulose acetate powder, silk powder, starch, polycalcium alginate, silicone, organic powders such as urethane, and inorganic powders such as silica and calcium carbonate. In view of the environmental problems of plastic particles in recent years, the blending of spherical cellulose, silicon dioxide, calcium carbonate, and starch is particularly preferred.
[0060] Furthermore, the metal oxide may be composited on the surface of component (B), preferably precipitating or adsorbing particles of 10 to 1200 nm on the surface, or may be contained within component (B). The metal oxide is not particularly limited, and preferably includes titanium oxide, zinc oxide, aluminum oxide, and cerium oxide. Component (C) may also be composited in component (B) in advance.
[0061] The amount of component (B) of the present invention is not particularly limited, but the lower limit is preferably 0.5% or more, more preferably 2% or more, and even more preferably 5% or more. The upper limit is preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less. Within this range, it can enter the concave parts of the skin, making the concave and convex parts less noticeable, and absorb sebum to maintain a uniform cosmetic film.
[0062] The oil absorption of the spherical powder of component (B) is not particularly limited, but the oil absorption of triglycerides and triisooctanoin similar to sebum is preferably 60 ml / 100 g or more, more preferably 70 ml / 100 g or more as the lower limit, and preferably 350 ml / 100 g or less, and further preferably 200 ml / 100 g or less as the upper limit. In this range, the spherical powder oriented next to the pores in the furrows absorbs sebum moderately, and the makeup lasts for a long time. It does not absorb sebum more than necessary, so there is no feeling of dryness. Powders with porosity are preferred. However, the feeling of dryness can be adjusted by absorbing oil in advance, or it can be adjusted with a surface treatment agent, etc. For example, in the case of silicone resin powder, KSP-100 (oil absorption: 80 ml / 100 g) (manufactured by Shin-Etsu Chemical Co., Ltd.) can be cited, in the case of polyurethane powder, for example, plastic powder CS-400 (oil absorption: 90 ml / 100 g) (manufactured by Negami Industries) can be cited, in the case of silica, for example, God ball D11-796C (oil absorption 83-89 ml / 100 g) and God ball E-90C (110-140 ml / 100 g) (manufactured by Suzuki Oil & Fats Industries) can be cited, in the case of cross-linked polymethyl methacrylate, for example, MBP-8 (oil absorption 140 ml / 100 g) (manufactured by Sekisui Chemicals Co., Ltd.) can be cited, and in the case of spherical cellulose, for example, CELLULOBE ADS-10 (oil absorption: 150 ml / 100 g) (manufactured by Daito Chemicals Co., Ltd.) can be cited, etc.
[0063] The coated titanium oxide and / or zinc oxide of component (C) is titanium oxide and / or zinc oxide coated with one or two selected from silicon oxide or hydroxide, aluminum oxide or hydroxide, and iron oxide or strong oxide. The titanium oxide and / or zinc oxide particles, which are the mother core of the coated titanium oxide and / or zinc oxide of the present invention, are not particularly limited in shape and may be titanium oxide alone or titanium oxide containing zinc oxide, or zinc oxide alone (hereinafter referred to as the mother core).
[0064] The mother core titanium oxide before coating in the coated titanium oxide and / or zinc oxide of component (C) can be obtained by a known method for producing titanium oxide powder, or a commercially available product can be used as the mother core. In addition, the titanium oxide as the mother core has anatase type and rutile type crystal forms, but the photocatalytic activity is low and the refractive index is high, so the rutile type with high hiding power is suitable.
[0065] Alternatively, in order to stabilize the crystal shape, it is preferred that a small amount of zinc oxide is contained in the titanium oxide powder as the mother core. The zinc oxide content in the titanium oxide as the mother core is preferably 1 mass % or less, more preferably 0.1 to 0.8 mass %, and further preferably 0.2 to 0.7 mass %, when converted into oxide mass.
[0066] Alternatively, zinc oxide may be used alone as a mother core. This zinc oxide can be obtained by a known method for producing zinc oxide.
[0067] The shape of the titanium oxide and / or zinc oxide as the parent core of component (C) is not particularly limited, and examples thereof include: grass bundle shape, ribbon shape, sphere shape, needle shape, rod shape, plate shape, etc. Among them, the titanium oxide and / or zinc oxide used as the parent core of the present invention is preferably spherical or plate-shaped with a relatively smooth surface.
[0068] The coated titanium oxide and / or zinc oxide of component (C) is preferably coated with the surface treatment amount of each metal in the specific range described below. By staying within this range, the natural three-dimensional sense of the skin can be better obtained, and the bluish whiteness and yellow dullness of the skin can be further reduced, which can bring a natural and uniform concealing effect. The surface treatment amount of aluminum in the coated titanium oxide and / or zinc oxide of component (C) is preferably 1-6% in terms of oxide mass, more preferably 1-5%, and further preferably 2-5%. The surface treatment amount of silicon is preferably 0.5-6% in terms of oxide mass, more preferably 1-6%, and further preferably 3-6%. The surface treatment amount of iron is preferably 0.5-3% in terms of oxide mass, more preferably 0.5-2%, and further preferably 0.5-1.5%.
[0069] In addition, in the powder-containing cosmetic of the present invention, the content of component (C) is preferably 0.5% or more, more preferably 3% or more, and further preferably 5% or more as its lower limit. In addition, it is preferably 30% or less, more preferably 20% or less, and further preferably 15% or less as its upper limit.
[0070] Component (C) is preferably coated with silicon oxide or hydroxide on the surface of the parent core, so that the dispersibility is improved and has a uniform hiding power. Furthermore, it is more preferably coated with aluminum oxide or hydroxide or iron oxide or hydroxide. Moreover, it is further preferred to have three layers of these layers (hereinafter, each layer is referred to as "silicon coating layer", "aluminum coating layer" and "iron coating layer"). It is more preferred to coat the surface of the particle where the silicon coating layer and the aluminum coating layer are mixed together with iron oxide or hydroxide. By mixing these several coating layers on the surface, a natural makeup is formed, and the application property is good, and a uniform hiding power can be achieved. That is, by controlling the coating layer, the surface charge changes, and various surface treatment agents can be made into adsorption points, and the dispersibility in the cosmetic containing powder is good. As a result, component (C) can be evenly dispersed regardless of whether the skin is uneven, does not hinder the application of component (A) (B), and is appropriately attached and dispersed on the surface of component (A) or (B), which can bring a multiplication effect of uniform hiding power. In particular, when there is an iron coating layer, the skin affinity to the skin color is increased, the makeup effect is natural with good concealing power, and the makeup film is hardly broken, so the makeup lasting effect is improved, which is preferred.
[0071] The method for coating the silicon oxide or hydroxide of component (C) is not particularly limited, and it can be carried out by a known coating method. For example, it can be listed as: a method in which sodium silicate or the like is directly added to a water slurry containing raw material particles or added as an aqueous solution, and then an acid such as sulfuric acid is added to precipitate silicon dioxide or its hydrate; or a method in which the raw material particles are dispersed in a solvent (alcohol, water or a mixed solvent of alcohol and water, etc.), an alkoxysilane-based metal coupling agent such as tetraethoxysilane is added, and an acid or base is added, and silicon dioxide or its hydroxide is precipitated by heating, etc. Afterwards, the coated powder particles are obtained by washing, filtering, drying, etc.
[0072] The method for coating the aluminum oxide or hydroxide of component (C) is not particularly limited, and it can be carried out by a known coating method. For example, it can be mentioned that: in the water slurry containing the raw material particles, aluminum nitrate, aluminum sulfate, sodium aluminate, etc. or their aqueous solutions are directly added, and then an acid or base is added to precipitate the aluminum compound. In addition, the raw material particles are dispersed in a solvent (alcohol, water, or a mixed solvent of alcohol and water, etc.), an aluminum-based metal coupling agent is added, an acid or base is added, and aluminum or hydroxide is precipitated by heating, etc. Afterwards, the coated powder particles are obtained by washing, filtering, drying, etc.
[0073] The method for coating the iron oxide or hydroxide of component (C) is not particularly limited, and can be carried out using a known method for coating treatment of iron oxide. For example, as an example, a caustic soda aqueous solution is heated to 30-35°C to disperse the powder particles, an aqueous solution containing iron sulfate is added and stirred, and the reaction is carried out at 90°C for about 2 hours. The obtained composite hydrate is washed with water, neutralized and dried. After crushing, the raw material particles and the iron oxide or hydroxide are sintered (for example, at about 750-900°C for about 1-3 hours). As the iron compound, there can be listed: iron oxide, ferrous oxide, ferrosoferric oxide, iron hydroxide, organic acid iron (for example, iron oxalate, iron citrate, etc.), inorganic acid iron (for example, ferric chloride, ferric sulfate, ferric sulfate, etc.), etc., and one or more of them can be selected. The iron compound exists in the particles as iron oxide or iron hydroxide.
[0074] In the coated titanium oxide and / or zinc oxide of component (C), the lower limit of the average particle size D50 according to the transmission electron microscope image analysis method is preferably 0.10 μm or more, more preferably 0.20 μm or more, and further preferably 0.25 μm or more. In addition, as the upper limit, it is preferably 1.20 μm or less, more preferably 1.00 μm or less, further preferably 0.8 μm or less, and further preferably 0.50 μm or less. By adopting such a particle size, it is easy to apply on the skin, the makeup is applied naturally, and uniform hiding power and makeup sustainability can be obtained.
[0075] In addition, the components (A), (B) and (C) of the present invention may be further surface treated within the scope of not impairing the effects of the present invention. By surface treatment, viscosity, dispersibility to oil, waterproofness and other accompanying cosmetic retention or usability can be imparted. The surface treatment can be performed using a known powder surface treatment method. As surface treatments for water repellency and / or oil repellency, for example, silicone compounds (e.g., dimethyl polysiloxane, methyl hydrogen polysiloxane, etc.), coupling agents (e.g., silanes such as alkyl alkoxy silane treatment, aluminums, titaniums, etc.), fluorine compounds (e.g., perfluoroalkyl alkoxy silane treatment), hydrocarbons, lecithin, hydrogenated lecithin, amino acids, peptides, amino acid derivatives (e.g., N-acyl amino acid treatments, lauroyl lysine treatment, sodium dilauroyl glutamate lysine treatment, sodium stearoyl glutamate treatment, sodium lauroyl aspartate treatment), polyethylene, waxes, fatty acids (e.g., stearic acid, palmitic acid, myristic acid), fatty acid salts, fatty acid esters, fatty acid amides, metal soaps, etc. can be used for treatment.
[0076] In the present invention, it is preferred to contain a powder treated with dimethiconol and aminopropyltriethoxysilane as a further component (D).
[0077] Component (D) may also contain a powder coated with a diorganopolysiloxane having reactive ends represented by the following general formula (1) and an amino group-containing silane compound represented by the following general formula (2):
[0078] R 1 R 2 2SiO-(R 2 2SiO) L -SiR 1 R 2 2(1)
[0079] (In the formula, each R 1 represents a hydroxyl group, each R 2 each independently represents a hydrocarbon group having 1 to 20 carbon atoms, and L represents an integer of 3 to 10,000)
[0080] R 3 R 4 m SiX (3-m) (2)
[0081] (Where R 3 represents a hydrocarbon group having 1 to 20 carbon atoms and having at least one amino group, R 4 represents an alkyl group having 1 to 4 carbon atoms, X each independently represents an alkoxy group having 1 to 4 carbon atoms, and m is 0 or 1).
[0082] The preferred form of component (D) is the following powder: the surface coating treatment agents (1) and (2) are subjected to a condensation reaction, and the surface is coated with a polymer having a micro three-dimensional crosslinked structure of silicone (hereinafter referred to as "silicone micro-crosslinked product"). The silicone micro-crosslinked product can be any compound that does not have rubber elasticity, and the mass ratio of (a) and (b) can be obtained in the range of about 100:0.1 to 100:35. When (b) is less than 0.1% by mass, it is in the form of viscous silicone oil or rubber, and when it is more than 35% by mass, it is in the form of elastic silicone elastomer, and there is a tendency for the waterproofness of the surface-coated powder to decrease.
[0083] In addition, as component (D), it is preferred to contain a polymer having a polydimethylsiloxane structure having a three-dimensional crosslinked structure in a portion obtained by crosslinking an organic polysiloxane. The polymer having a polydimethylsiloxane structure having a three-dimensional crosslinked structure is not particularly limited, but preferably has a divinyldimethylpolysiloxane crosslinked structure, or a structure crosslinked with an alkyl group having 3 to 20 carbon atoms. In addition, its shape is not particularly limited as long as it can be coated on the surface of the powder. For example, there can be listed: a divinyldimethylpolysiloxane crosslinked (polydimethylsiloxane / vinyldimethylpolysiloxane) crosslinked polymer, and a polydimethylsiloxane crosslinked polymer having an alkyl group in the crosslinked portion. In addition, there is no particular limitation even if it is a polymer containing a polyoxyalkylene group in the molecule or a polymer containing a polyoxyalkylene group and a long-chain alkyl group in the molecule.
[0084] The amount of component (D) in the powder-containing cosmetic is preferably 1 to 50%, and a more suitable range is 2 to 40%. Within this range, particularly good performance can be obtained in terms of effect discovery or makeup application. In addition, components (A), (B), and (C) can also be surface-treated with a surface treatment agent of component (D).
[0085] Furthermore, as component (E) preservative, dipropylene glycol, 1,2-alkanediol, ethylhexylglycerin, chlorphenesin ether may be added. In the powder-containing cosmetic of the present invention, when used together with component (E), components (A) to (C) do not hinder the spreadability and can provide an antiseptic effect.
[0086] The amount of component (E) in the powder-containing cosmetic is preferably 0.001 to 0.5%, and more preferably 0.01 to 0.3%. Within this range, the antiseptic property of the powder-containing cosmetic can be ensured, and a powder-containing cosmetic that does not hinder usability, can maintain the makeup durability, and can further ensure the safety to the skin can be provided. In particular, when a powder-containing cosmetic is provided without using parabens, the effect can be more exerted.
[0087] The powder-containing cosmetic of the present invention may contain any other ingredients in addition to the above-mentioned ingredients according to the purpose within the scope of not impairing the effect of the present invention. Examples thereof include: oily ingredients, pigments, pH adjusters, moisturizers, thickeners, surfactants, dispersants, stabilizers, colorants, preservatives, antioxidants, metal chelating agents, astringents, anti-inflammatory agents, ultraviolet absorbers, fragrances, other pigments, etc.
[0088] The powder-containing cosmetic of the present invention can be made into a dosage form containing a large amount of powder or a dosage form requiring ultraviolet shielding ability. Preferred examples include: powder, powder solid, oily, oily solid, emulsified, and emulsified solid.
[0089] The powder-containing cosmetic of the present invention can be used, for example, in cosmetics (e.g., whitening powder, primer, foundation, concealer, scented powder, color control, sunscreen cosmetics, eye shadow, eyeliner, mascara, blush, talcum powder, perfume powder, baby powder, etc.), body cosmetics, etc. Among them, whitening powder, primer, foundation, concealer, scented powder, color control, sunscreen cosmetics, talcum powder, etc. are preferred, and powder-containing cosmetics that can be used on the face are more preferred, because the present invention can obtain a natural three-dimensional effect. Example
[0090] The present technology will be described in more detail below with reference to Examples and Comparative Examples, etc. However, these do not limit the present invention in any way.
[0091] Table 1 shows the evaluation methods and evaluation results of the materials as component (A).
[0092]
Table 1
[0093] (quality%)
[0094]
[0095] Production Examples 1 to 9: produced by precipitation method A. The aspect ratio of the matrix was 20 to 30 for Production Examples 1 to 3 and 5 to 8, 10 to 20 for Production Example 4, and 68 for Production Example 9. The oil absorption was 65 ml / 100 g for Production Example 4 and 65 ml / 100 g for Production Example 5.
[0096] Comparative Manufacturing Example 1: Manufacturing using adsorption method B (mixing with a high-speed Henschel mixer at 3000 rpm and crushing with a crusher). MT-500B (manufactured by Teika Co., Ltd.), MZ-300 (manufactured by Teika Co., Ltd.), Sanshin Sericea FSE (manufactured by Sanshin Mining Co., Ltd.), and 3% isostearic acid were mixed.
[0097] Comparative Manufacturing Example 2: The same adsorption method B as in Comparative Manufacturing Example 1 was used to manufacture. MT-150EX (manufactured by TEICA Co., Ltd.) with an average particle size of 15 nm titanium oxide component 40%, TRY-100HP 1%, TRR-100HP 0.5%, (manufactured by Chitan Industries Co., Ltd.), and sericite LQ-15 (manufactured by Ochem Trading Co., Ltd.) were mixed. The oil absorption was 80 ml / 100 g.
[0098] Comparative Manufacturing Example 3: Cover Leaf PC-2035M (manufactured by Catalyst Chemical Industries, Ltd.)
[0099] Manufacturing Comparative Example 4: STA-20C (manufactured by Semantec Co., Ltd.), mother body (Sanshin Kinumo) Mother FSE (manufactured by Japan Sericite Corporation)
[0100] Comparative Manufacturing Example 5: Blondii Metallic Gold N-2000S (manufactured by CQV)
[0101] The surface state of the iron oxide / titanium oxide coated platy mica (Production Example 5) prepared by the precipitation method of component (A) of the present invention was observed using a scanning electron microscope (JSM-7800prime, manufactured by JEOL Ltd.) at an accelerating voltage of 5 kV and a magnification range of 5000 to 100000 times. The photograph is shown in FIG. Figure 1 As Figure 1 The detailed description is that the titanium oxide layer precipitated on the surface of the matrix mica is partially peeled off, and the thickness of the titanium oxide layer is magnified and confirmed at 20 locations, which is 50 to 100 nm. In addition, the composite powder of component (A) is subjected to element mapping (mapping) using energy dispersive X-ray analysis (X-MAX manufactured by Oxforfoto) at an acceleration voltage of 10 kV. It can be seen that the Ti element is uniformly present throughout, and further, the powder present in dots on its surface is the Fe element, so it can be determined that the powder present in dots is iron oxide.
[0102] On the other hand, zinc oxide and titanium oxide coated mica (Comparative Manufacturing Example 1) prepared by a mechanochemical method is shown in Figure 2 As Figure 2 The detailed description shows that zinc oxide and titanium oxide have a concavoconvex shape and are fixed to the surface of the matrix mica in the form of particles. In addition, the result of element mapping using energy dispersive X-ray analysis (EDX) shows that titanium oxide and zinc oxide are unevenly fixed to the surface because the Ti element and the Zn element exist in spots.
[0103] [Evaluation method: UVB transmittance (300nm), UVA transmittance (360nm)]
[0104] The ultraviolet shielding ability of the composite powder of component (A) of the present invention was evaluated under the following conditions. First, the composite powder of component (A) was added to a nitrocellulose solution of 43.4% butyl acetate, 21.0% ethyl acetate, 14.6% IPA, and 21.0% nitrocellulose to make a concentration of 40%, and then dispersed at a dispersion rotation number of 3000 rpm for 10 minutes. Then, the dispersion was used to prepare a coating on a quartz plate using a scraper (12 μm thickness) to make the thickness uniform, and the dried coating film was measured using a spectrophotometer (U-4100 manufactured by HITACHI) to measure the transmittance of the coating in the wavelength range of 250 to 700 nm. The transmittance at 360 nm was used as an evaluation of the shielding ability in the UVA region of 320 to 400 nm, and the transmittance at 300 nm was used as an evaluation of the shielding ability in the UVB region of 280 to 320 nm, and the shielding ability in a wide range of UVB to UVA was evaluated. The evaluation results of each composite powder and its transmittance and shielding ability are shown in Table 1. Evaluation levels were evaluated at the following levels.
[0105]
Evaluation criteria
[0106] ◎: Transmittance less than 25%. (◎*: Transmittance less than 20%)
[0107] ○: Transmittance is 25% or more and less than 50%
[0108] △: Transmittance is 50% or more and less than 75%
[0109] ×: Transmittance 75% or more to less than 100%
[0110] From Table 1, it can be seen that the composite powder of component (A) prepared by the precipitation method (manufacturing method A) of manufacturing examples 1 to 9 can block a wide range of UVB to UVA. Figure 1 As shown, it is speculated that the titanium oxide layer is uniformly and densely coated on the mica surface, and then the iron oxide is coated. On the other hand, the zinc oxide·titanium oxide coated plate-like mica and the titanium oxide coated mica prepared by the adsorption method (manufacturing method B) of manufacturing comparative examples 1 and 2 have poor UVB-UVA shielding capabilities because titanium oxide and zinc oxide are not uniformly fixed on the mica surface. In addition, in manufacturing comparative examples 3 and 4 prepared by the precipitation method (manufacturing method A), titanium oxide exists in the form of particles, and is an iron oxide·titanium oxide coated plate-like mica with the brilliance of manufacturing comparative example 5, but has poor UVB-UVA shielding capabilities.
[0111] [Evaluation method: Evenly applied, no covering power]
[0112] Furthermore, regarding the uniform application of each powder and the lack of covering power, 20 cosmetic evaluation specialists evaluated it on a 5-point scale based on the following criteria, and gave a score for each composite powder spreading on a certain area of skin. The average score of all the panelists was then determined based on the following criteria.
[0113]
Evaluation criteria
[0114] (Evaluation results): (rating)
[0115] Very good: 5 points
[0116] Good: 4 points
[0117] Normal: 3 points
[0118] Slightly bad: 2 points
[0119] Bad: 1 point
[0120]
Judgment criteria
[0121] (Average score): (Judgment)
[0122] 4.0 or above: ◎
[0123] 3.0 or more to less than 4.0: ○
[0124] 1.5 or more to less than 3.0: △
[0125] Less than 1.5: ×
[0126] According to Table 1, the composite powders of Manufacturing Examples 1 to 9 are excellent in terms of uniform application and lack of hiding power. In Manufacturing Comparative Examples 1 and 2, titanium oxide and zinc oxide are fixed to the mica surface in a particle form, so the surface is uneven, and there is a squeaking and powdery touch. It is not possible to obtain uniform application, and the particles are partially agglomerated, and the hiding power is easy to show. Although Manufacturing Comparative Examples 3, 4, and 5 can also be evenly applied, the ultraviolet shielding ability is low. Manufacturing Comparative Example 5 has a bright property, so the hiding power is particularly easy to show.
[0127] According to the following manufacturing method, foundations with the compositions shown in Tables 2 and 3 were prepared. All the foundations obtained were evaluated for "no burden on the skin when applied", "evenly concealing spots and uneven color", "natural application", "no prolonged drying feeling", "makeup lasting effect", and "ultraviolet shielding effect" using the following evaluation method.
[0128]
Table 2
[0129] (quality%)
[0130]
[0131]
[0132]
[0133] *1: MPY-100M (manufactured by TEICA)
[0134] *2: SMT-500SAM (manufactured by TEICA)
[0135] *3: Talc JA-13R (manufactured by Asada Flour Mill Co., Ltd.) 2.8% treatment
[0136] *4: KSP-100 (manufactured by Shin-Etsu Chemical Co., Ltd.) (Oil absorption: 80 ml / 100 g)
[0137] *5: CELLULOBE ADS D-10 (manufactured by Daito Chemical Industry Co., Ltd.) (Oil absorption: 150 ml / 100 g)
[0138] *6: CELLULOBE ADS-30 (manufactured by Daito Chemical Industry Co., Ltd.)
[0139] *7: Cosmetic silica CQ4 (manufactured by Fuji Silicone Co., Ltd.) (Oil absorption: 300 ml / 100 g)
[0140]
Table 3
[0141] (quality%)
[0142]
[0143]
[0144]
[0145] [Manufacturing method]
[0146] (1) Use a Henschel mixer to evenly disperse ingredients 1 to 25.
[0147] (2): Mix components 26 to 32 uniformly.
[0148] (3): Add (2) to (1), disperse evenly, and then pulverize to obtain a solid powder foundation.
[0149] [Evaluations: "No feeling of burden on the skin when applying", "Evenly hides spots and uneven skin tone", "Applies naturally", "No feeling of dryness for a long time", "Makeup lasts long"]
[0150] 20 cosmetic evaluation panelists were asked to use the foundations of Examples 1 to 16 and Comparative Examples 1 to 9 and evaluate the foundations on a 5-point scale according to the following criteria: "No burden on the skin when applied", "Evenly hides spots and uneven skin tone", "Natural makeup", and "Makeup lasting effect". Each foundation was scored, and the average score of all panelists was determined according to the following criteria. In addition, the "makeup lasting effect" was evaluated by comparing the state 6 hours after the foundation application (daily life) with the state immediately after the application.
[0151]
Evaluation criteria
[0152] (Evaluation results): (rating)
[0153] Very good: 5 points
[0154] Good: 4 points
[0155] Normal: 3 points
[0156] Slightly bad: 2 points
[0157] Bad: 1 point
[0158]
Judgment criteria
[0159] (Average score): (Judgment)
[0160] 4.0 or above: ◎
[0161] 3.0 or above to 4.0: ○
[0162] 2.0 or more to less than 3.0: △
[0163] Less than 2.0: ×
[0164]
Evaluation: "UV blocking effect"
[0165] The foundations of Examples 1 to 16 and Comparative Examples 1 to 9 were heated to 2 mg / cm 2 After coating on a PMMA plate, the mixture was left to stand for 20 minutes to prepare a sample, and SPF measurement was performed using an SPF analyzer (UV-2000S manufactured by Labsphere).
[0166] (a) 4-level evaluation criteria
[0167] (Evaluation): (Judgment)
[0168] SPF value = 20 or more: ◎
[0169] SPF value = 15 or more but less than 20: ○
[0170] SPF value = 8 or more but less than 15: △
[0171] SPF value = less than 8: ×
[0172] From the results in Table 2, it can be seen that the foundations of Examples 1 to 16 of the present invention are excellent powder cosmetics in all items of "no burden on the skin when applied", "evenly hides spots and uneven skin tone", "natural makeup application", "no long-term dry feeling", "makeup lasting effect", and "ultraviolet shielding effect".
[0173] On the other hand, as can be seen from the results in Table 3, the results show that in Comparative Example 1 without component (A) and Comparative Examples 2 and 3 in which component (A) is added instead of component (A), the "effect of uniformly hiding spots and uneven skin color", "makeup lasting effect", and "ultraviolet shielding effect" are low. Furthermore, Comparative Example 4 containing fine metal oxide and component (D) instead of component (A) is poor in "no burden on the skin when applied", "natural makeup", "no long-term dry feeling", and "makeup lasting effect". It is presumed that this is because component (A) cannot be evenly applied to the skin bumps, the concealing effect of component (A) is lost, and its makeup effect is reduced. Comparative Example 5 which does not contain component (C) but contains metal oxide instead is unsatisfactory in "no burden on the skin when applied", "evenly hiding spots and uneven skin color", and "makeup lasting effect". Comparative Examples 6 and 7 which do not contain component (B) are poor in "evenly hiding spots and uneven skin color", "natural makeup", and "makeup lasting effect". This is presumably because component (B) present in the furrows has poor sebum absorption capacity, so the makeup film cannot last through long-term sebum secretion. In addition, Comparative Example 9, which contains particles larger than component (C), has a worse "no burden on the skin when applied". Comparative Example 8, which does not contain component (C) but increases the amount of component (A), has a high "ultraviolet shielding effect", but is poor in "no burden on the skin when applied" and "makeup lasting effect".
[0174] Example 17: Solid powder foundation
[0175]
[0176]
[0177] *8: Micro-mica MK-200K (manufactured by Katakura Composite Co., Ltd.)
[0178] *9: MZX-300M (manufactured by TEICA)
[0179] *10: CS-400 (manufactured by Negami Industry Co., Ltd.) (oil absorption 90 ml / 100 g)
[0180] *11: KSP-300 (manufactured by Shin-Etsu Chemical Co., Ltd.)
[0181] *12: KF-6018 (manufactured by Shin-Etsu Chemical Co., Ltd.)
[0182] *13: Sensiva SC50 (manufactured by Schulke & Mayr)
[0183] (Manufacturing method)
[0184] 1: Components 1 to 13 are uniformly dispersed using a Henschel mixer (manufactured by Mitsui Miike Co., Ltd.).
[0185] 2: Mix and dissolve ingredients 14 to 20 evenly.
[0186] 3: Add (2) to (1) while stirring with a Henschel mixer and disperse evenly.
[0187] 4: Crush (3) using a crusher.
[0188] 5: Mix (4) with an appropriate amount of purified water to obtain a slurry-like mixture.
[0189] 6: Fill (5) in a gold dish, compress and shape, and then dry to remove the solvent to obtain a solid powder foundation.
[0190] (evaluate)
[0191] The solid powder foundation of Example 17 is excellent in "no burden on the skin when applied", "evenly hides spots and uneven skin tone", "natural makeup", "no prolonged dry feeling", "makeup lasting effect", and "ultraviolet shielding effect".
[0192] Example 18: Solid powder blush
[0193]
[0194] *14: Aminomoto LL (manufactured by Ajinomoto Co., Ltd.)
[0195] *15: KSG-16 (manufactured by Shin-Etsu Chemical Co., Ltd.)
[0196] (Manufacturing method)
[0197] 1: Components 1 to 14 are uniformly dispersed using a Henschel mixer (manufactured by Mitsui Miike Co., Ltd.).
[0198] 2: Mix and dissolve ingredients 15 to 19 evenly.
[0199] 3: Add (2) to (1) while stirring with a Henschel mixer and disperse evenly.
[0200] 4: Crush (3) using a crusher.
[0201] 5: Mix (4) with an appropriate amount of isododecane to obtain a slurry-like mixture.
[0202] 6: Fill (5) into a gold basin, compress and shape it, and then dry it to remove the solvent to obtain a solid powder blush.
[0203] (evaluate)
[0204] The solid powder blush of Example 18 is excellent in “no burden on the skin when applied”, “evenly hides spots and uneven skin tone”, “natural makeup application”, “no prolonged dry feeling”, “makeup lasting effect”, and “ultraviolet shielding effect”.
[0205] Example 19: Solid powder eye shadow
[0206]
[0207] *16. Corn starch (manufactured by Japan Corn Starch Co., Ltd.)
[0208] (Production method) (1): Components 1 to 9 are uniformly dispersed using a Henschel mixer (manufactured by Mitsui Miike Co., Ltd.).
[0209] (2): Mix components 10 to 15 evenly.
[0210] (3): Add (2) to (1), disperse evenly, and then grind to obtain a solid powder eye shadow.
[0211] (evaluate)
[0212] The solid powder eye shadow of Example 19 is excellent in “no burden on the skin when applied”, “evenly hides spots and uneven skin tone”, “natural makeup application”, “no prolonged dry feeling”, “makeup lasting effect”, and “ultraviolet shielding effect”.
[0213] Example 20: Face color in solid powder form
[0214]
[0215] *17. PC chalk (made by Shiraishi Industries)
[0216] (Manufacturing method)
[0217] (1): Components 1 to 8 are uniformly dispersed using a Henschel mixer.
[0218] (2): Mix ingredients 9 to 12 evenly.
[0219] (3): Add (2) to (1), disperse evenly, and then grind to obtain a solid powder.
[0220] (evaluate)
[0221] The solid powdery facial color described in Example 20 has excellent "no burden on the skin when applied", "evenly hides spots and uneven skin tone", "natural makeup", "no prolonged dryness", "makeup lasting effect", and "ultraviolet shielding effect".
[0222] Example 21: Solid powdered white powder
[0223]
[0224]
[0225] (Manufacturing method)
[0226] (1) Mix 1 to 12 evenly using a Henschel mixer.
[0227] (2): Mix 13 to 16 evenly and dissolve them.
[0228] (3): Add (2) to (1) and mix evenly.
[0229] (4): (3) is crushed and filled into a container to obtain loose white powder.
[0230] (evaluate)
[0231] The white powder described in Example 21 is excellent in "no burden on the skin when applied", "evenly hides spots and uneven skin tone", "natural makeup application", "no prolonged dry feeling", "makeup lasting effect", and "ultraviolet shielding effect".
[0232] Example 22: Foundation in the capillary domain
[0233]
[0234]
[0235] *18: Goodball-90C (manufactured by Suzuki Oil & Fats Industries) (average particle size 30 μm)
[0236] *19: XZ-3000F (manufactured by Sakai Chemical Industry Co., Ltd.)
[0237] (Manufacturing method)
[0238] A. Mix ingredients 1 to 11 evenly using a super mixer.
[0239] B. Mix and dissolve components 12 to 23 uniformly at 80°C.
[0240] C. Mix components 24 to 28 evenly.
[0241] D. Add B and C to A at 25°C and mix evenly using a universal mixer.
[0242] E. After D is filled into a container using a filling machine equipped with a screw feeder, it is press-molded with a three-dimensional logo relief to obtain a foundation.
[0243] The capillary field foundation of Example 22 is excellent in "no burden on the skin when applied", "evenly hides spots and uneven skin tone", "natural makeup", "no prolonged dry feeling", "makeup lasting effect", and "ultraviolet shielding effect".
[0244] Example 23: Concealer (oily solid)
[0245]
[0246]
[0247] *20: Yunifeirma HVY (manufactured by Chiba Flour Milling Co., Ltd.)
[0248] (Manufacturing method)
[0249] A. Dissolve components (1) to (13) uniformly at 80 to 90°C.
[0250] B. Add ingredients (14) to (25) into A and mix and disperse evenly.
[0251] C. Dissolve B in a resin dish at 90°C and fill it.
[0252] D. Cool C at room temperature and solidify to obtain concealer.
[0253] The concealer (oily solid) of Example 23 is excellent in "no burden on the skin when applied", "evenly hides spots and uneven skin tone", "natural application", "no prolonged dry feeling", "makeup lasting effect", and "ultraviolet shielding effect".
[0254] Example 24: W / O solid foundation
[0255]
[0256]
[0257] *21.KF-9021 (manufactured by Shin-Etsu Chemical Co., Ltd.)
[0258] (Manufacturing method)
[0259] A. After heating and dissolving components 1 to 7 at 110°C, add and mix components 10 to 14.
[0260] B. Then, components 8 to 9 and 20 are mixed and the temperature is adjusted at 80°C.
[0261] C. Component 18 is swollen with a portion of component 15, and components 16 to 19 are mixed and the mixture is adjusted to 70°C.
[0262] D. Add emulsified C to B, fill it into a container, let it cool, and you will get the foundation.
[0263] The foundation of Example 24 is excellent in "no burden on the skin when applied", "evenly hides spots and uneven skin tone", "natural makeup application", "no prolonged dry feeling", "makeup lasting effect", and "ultraviolet shielding effect".
Claims
1. A powder-containing cosmetic comprising the following ingredients (A) to (C); (A) A composite powder, which is a plate-like composite powder without brilliance, wherein 30 to 50% by mass of titanium oxide is layered on the surface of mica, and further 0.1 to 3% by mass of iron oxide is layered on the surface of mica; the mica of the mother powder of the composite powder has an aspect ratio of 10 to 50; (B) Spherical powder with an average particle size of 1 to 40 μm; (C) titanium oxide and / or zinc oxide having an average particle size of 0.1 to 1.2 μm coated with one or more selected from iron oxide or hydroxide, aluminum oxide or hydroxide, and silicon oxide or hydroxide; The titanium oxide of the component (A) does not form particles on the surface of mica, and the average thickness of the titanium oxide layer is 50 to 100 nm.
2. The powder-containing cosmetic according to claim 1, wherein The component (A) is further coated with a hydrophobizing agent.
3. The powder-containing cosmetic according to claim 1 or 2, wherein: Component (C) is titanium oxide and / or zinc oxide coated with at least two or more of silicon oxide or hydroxide and iron oxide or hydroxide or coated with at least two or more of silicon oxide or hydroxide and aluminum oxide or hydroxide and having these layers.
4. The powder-containing cosmetic according to claim 1 or 2, wherein: The component (A) is further coated with 0.1 to 4 mass % of zinc oxide.
5. The powder-containing cosmetic according to claim 1 or 2, wherein: The component (B) is one or more spherical powders selected from cellulose, silicon dioxide, calcium carbonate, starch, calcium alginate, silicone, and polyurethane.
6. The powder-containing cosmetic according to claim 1 or 2, wherein: In a coating film obtained by applying and drying a solution containing 40% by mass of the component (A) dispersed therein, the transmittances at wavelengths of 300 nm and 360 nm were less than 50%.
7. The powder-containing cosmetic according to claim 1 or 2, wherein: The present invention further contains 2 to 40% by mass of component (D): a powder surface-treated with cross-linked silicone.
Citation Information
Patent Citations
Complexion-colored sintered pigment and cosmetic containing the same
JP2007145778A
Powder cosmetic
JP2012240999A
Cosmetic
JP2013231020A
Solid powder cosmetic
JP2017081858A
JP1968025644B1