A preparation method of modified cobalt vanadate material and supercapacitor
By nickel-doping and silicon dioxide coating cobalt vanadate materials, the structural instability and ion dissolution issues are addressed, leading to improved cycle performance and specific capacitance in supercapacitors.
Patent Information
- Application Number
- CN202111607932.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-12-24
AI Technical Summary
Cobalt vanadate materials used as electrode materials in supercapacitors suffer from poor cycle performance due to structural expansion/contraction and metal ion dissolution, leading to poor cycle stability and short service life.
A preparation method involving nickel doping and silicon dioxide coating of cobalt vanadate materials to regulate morphology, reduce particle size, increase electrochemical active sites, and inhibit structural changes, thereby enhancing cycle performance and specific capacitance.
The modified cobalt vanadate materials exhibit improved cycle performance and high specific capacitance, resulting in enhanced stability and efficiency of supercapacitors.
Smart Images

Figure CN114420466B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to a preparation method of a modified cobalt vanadate material and a supercapacitor. Background Art
[0002] Supercapacitors, also known as electrochemical capacitors, are energy storage devices between traditional capacitors and traditional batteries, with the characteristics of long life, good reversibility, fast charge and discharge speed, and high output power. It is a good supplementary power source and can be well applied in many power devices.
[0003] Supercapacitors are mainly composed of four parts: current collector, electrode, electrolyte and diaphragm. The electrode material is the key factor that determines the performance of supercapacitors. At present, supercapacitor electrode materials mainly include carbon materials, conductive polymers and transition metal oxides, which mainly rely on double layer and redox pseudocapacitive charge storage to store electrical energy. Transition metal oxides belong to an important class of pseudocapacitive supercapacitor materials. Among the many transition metal oxides, vanadium-based compound electrode materials have become the preferred choice for supercapacitors due to their unique layered structure and multivalent vanadium. Among vanadium-based compounds, cobalt vanadate is a class of inorganic compounds with stable and excellent chemical properties, good heat resistance and crystallization properties, and a new type of binary vanadium-based compound with good optical, electrochemical and catalytic properties. Compared with monobasic vanadium-based compounds, it can improve electronic and ionic conductivity and pseudocapacitive reaction based on the interface effect and synergistic effect of vanadium and cobalt bimetallic, so it has good application prospects in supercapacitors.
[0004] However, although cobalt vanadate materials have outstanding theoretical capacity advantages, when used as electrode materials, the H3O2 in the electrolyte solution is + OH - Plasma "embedding" and "deembedding" in cobalt vanadate crystal particles will cause the crystal structure to expand / contract. After multiple cycles, the microstructure of the cobalt vanadate electrode will be destroyed, resulting in poor cycle performance. At the same time, long-term contact between the electrode material and the electrolyte will cause some metal ions in the electrode material to dissolve into the electrolyte, resulting in loss of electrode active materials, further deteriorating the cycle stability. Therefore, when cobalt vanadate material is used as an electrode material for supercapacitors, it has poor cycle stability and short service life, which limits its application. Summary of the invention
[0005] The main purpose of the present invention is to provide a preparation method of a modified cobalt vanadate material and a supercapacitor, aiming to solve the problem of poor cycle performance when the existing cobalt vanadate material is used as an electrode material for a supercapacitor.
[0006] To achieve the above object, the present invention provides a method for preparing a modified cobalt vanadate material, the preparation method comprising the following steps:
[0007] S10, dissolving cobalt nitrate hexahydrate and nickel nitrate hexahydrate in deionized water to obtain a mixed solution, adding a complexing agent, a surfactant and an ammonium metavanadate solution to the mixed solution under stirring to obtain a reaction solution, transferring the reaction solution into a hydrothermal reactor, reacting at 180-200° C. for 12-20 h to obtain a solid-liquid mixture;
[0008] S20, separating the solid-liquid mixture into solid and liquid, washing the obtained solid, vacuum drying, and then calcining at 500-600° C. to obtain a nickel-doped cobalt vanadate material;
[0009] S30, crushing the nickel-doped cobalt vanadate material, and then adding it to a mixed solvent to obtain a solution A, adding tetraethyl orthosilicate and a nitric acid solution to the solution A, and stirring the mixture in a water bath at 60° C. to obtain a solution B;
[0010] S40, separating the precipitate in the solution B, washing, drying, and then calcining at 450-550° C. to obtain a modified cobalt vanadate material.
[0011] Optionally, in step S10:
[0012] The complexing agent comprises citric acid monohydrate; and / or,
[0013] The surfactant includes sodium lauryl sulfate.
[0014] Optionally, in the reaction solution, the concentration of ammonium metavanadate is 0.07-0.13 mol / L.
[0015] Optionally, in the reaction solution, the molar ratio of the cobalt nitrate hexahydrate, the nickel nitrate hexahydrate, the complexing agent, the surfactant and the ammonium metavanadate is (1-x): x: 2: 0.1: 2, wherein 0 <x≤0.1。
[0016] Optionally, in step S20:
[0017] The vacuum drying has a drying temperature of 70-90°C and a drying time of 10-14 h; and / or,
[0018] The heating rate during the calcination process is 5-10°C / min, and the calcination time is 3-5h.
[0019] Optionally, in step S30:
[0020] The mixed solvent comprises water and anhydrous ethanol; and / or,
[0021] In the nitric acid solution, the mass fraction of nitric acid is 65-68%.
[0022] Optionally, in step S30:
[0023] The mixed solvent comprises water and anhydrous ethanol, wherein the volume ratio of water to anhydrous ethanol is 1:6; and / or,
[0024] The stirring reaction time is 4 to 6 h.
[0025] Optionally, in step S30, the mass ratio of the nickel-doped cobalt vanadate material, the mixed solvent, tetraethyl orthosilicate and the nitric acid solution is 1:8:0.00347-0.1735:0.2.
[0026] Optionally, in step S40:
[0027] The drying temperature of the drying is 110-130° C. and the drying time is 10-14 h; and / or,
[0028] The heating rate during the calcination process is 5-10°C / min, and the calcination time is 4-6h.
[0029] In addition, the present invention also provides a supercapacitor, which includes an electrode material, wherein the electrode material is a modified cobalt vanadate material, wherein the modified cobalt vanadate material is prepared by the preparation method of the modified cobalt vanadate material as described above.
[0030] In the technical solution provided by the present invention, the microscopic morphology of the cobalt vanadate material is regulated by doping with nickel elements, the particle size is reduced, the contact area between the electrolyte and the electrode material is increased, and the surface electrochemical active sites are increased, thereby increasing the specific capacitance of the electrode material. At the same time, the doping of nickel will cause the lattice of the cobalt vanadate material to shrink, and the distance between the anion and the cation is shortened, which can effectively inhibit the structural change of cobalt vanadate during the charge and discharge process, enhance the structural stability, and then improve the cycle performance of the cobalt vanadate material; by coating silicon dioxide on the surface of the cobalt vanadate material doped with nickel, the direct contact between the cobalt vanadate material doped with nickel and the electrolyte can be reduced to avoid the active metal elements in the cobalt vanadate material doped with nickel in the long-term charge and discharge cycle. Dissolution loss in the electrolyte, thereby further improving the cycle performance of the cobalt vanadate material doped with nickel. Therefore, the present invention uses coating modification and doping modification, and the two work together to make the obtained modified cobalt vanadate material have good cycle performance and high specific capacitance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 The modified cobalt vanadate material Co prepared in Example 1 of the present invention 0.9 Ni 0.1 XRD pattern of V2O6 / SiO2 and standard XRD pattern of cobalt vanadate material (JCPDS No. 51-0130);
[0033] Figure 2 The modified cobalt vanadate material Co prepared in Example 1 of the present invention 0.9 Ni 0.1 SEM image of V2O6 / SiO2;
[0034] Figure 3 This is a SEM image of the cobalt vanadate material CoV2O6 prepared in Comparative Example 1 of the present invention;
[0035] Figure 4 The nickel-doped cobalt vanadate material Co prepared in Comparative Example 2 of the present invention 0.9 Ni 0.1 SEM image of V2O6;
[0036] Figure 5 The modified cobalt vanadate material Co prepared in Example 1 of the present invention 0.9 Ni 0.1 The first constant current charge and discharge curve of V2O6 / SiO2.
[0037] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0039] In addition, the meaning of "and / or" appearing in the full text includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or a solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0040] The present invention provides a method for preparing a modified cobalt vanadate material, aiming to provide an electrode material with good cycle performance and high specific capacitance. In one embodiment, the preparation method comprises the following steps:
[0041] Step S10, dissolving cobalt nitrate hexahydrate and nickel nitrate hexahydrate in deionized water to obtain a mixed solution, adding a complexing agent, a surfactant and an ammonium metavanadate solution to the mixed solution under stirring to obtain a reaction solution, transferring the reaction solution into a hydrothermal reactor, reacting at 180-200° C. for 12-20 h to obtain a solid-liquid mixture.
[0042] Specifically, cobalt nitrate hexahydrate and nickel nitrate hexahydrate are dissolved in deionized water to obtain a mixed solution, and a complexing agent and a surfactant are added under stirring with a magnetic stirrer. After magnetic stirring for 0.5 hours, an ammonium metavanadate solution is added thereto, and stirring is continued for 3 to 5 hours to obtain a reaction solution, and the reaction solution is transferred into a hydrothermal reactor, and reacted at 180 to 200° C. for 12 to 20 hours to obtain a solid-liquid mixture, wherein the stirring rate of the magnetic stirrer is 200 to 400 rpm.
[0043] The complexing agent is first complexed with the cobalt salt and the nickel salt, and then reacts with the ammonium metavanadate solution at 180-200° C. to generate a solid, i.e., nickel-doped cobalt vanadate. The present invention does not limit the specific type of the complexing agent, which may be sodium citrate, sodium hydrogen citrate, trisodium citrate, citric acid monohydrate, etc. Preferably, the complexing agent is citric acid monohydrate. By selecting citric acid monohydrate, the generation reaction rate of the doped cobalt vanadate is regulated, thereby adjusting the morphology of the solid.
[0044] The addition of surfactant makes the solids less likely to agglomerate, which is conducive to forming solids with smaller particles and uniform particle size, so that the subsequently obtained nickel-doped cobalt vanadate material can reach nanometer level and have a large specific surface area. In this embodiment, the surfactant is sodium dodecyl sulfate.
[0045] Among them, the ammonium metavanadate solution can be prepared in a conventional manner. In this embodiment, the preparation of the ammonium metavanadate solution includes the following steps: adding ammonium metavanadate to deionized water, heating in a water bath at 80°C for 0.5 to 2 hours under stirring with a magnetic stirrer to dissolve the ammonium metavanadate solution. The present invention does not limit the concentration of the ammonium metavanadate solution. In this embodiment, as long as the concentration of ammonium metavanadate in the reaction solution is 0.07 to 0.13 mol / L.
[0046] Furthermore, in order to make the doping ratio of nickel element appropriate, so as to improve the cycle performance and conductivity of cobalt vanadate material without changing the crystal structure of cobalt vanadate material itself, in this embodiment, in the reaction solution, the molar ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, complexing agent, surfactant and ammonium metavanadate is (1-x): x: 2: 0.1: 2, wherein 0 <x≤0.1。
[0047] Step S20, separating the solid-liquid mixture into solid and liquid, washing the obtained solid, vacuum drying, and then calcining at 500-600° C. to obtain a nickel-doped cobalt vanadate material.
[0048] The drying temperature of the vacuum drying is 70-90° C., and the drying time is 10-14 h; and / or the heating rate during the calcination process is 5-10° C. / min, and the calcination time is 3-5 h.
[0049] In a specific embodiment, step S20 includes: cooling the solid-liquid mixture to room temperature, centrifuging it, and washing the obtained solid with deionized water, repeating 3 times, vacuum drying at 80°C for 12 h, placing the dried product in a muffle furnace, heating it to 500~600°C at a heating rate of 5~10°C / min, and calcining it for 3~5h to obtain a nickel-doped cobalt vanadate material with a molecular formula of Co 1-x Ni x V2O6, of which 0 <x≤0.1。
[0050] Step S30, crushing the nickel-doped cobalt vanadate material, and then adding it to a mixed solvent to obtain solution A, adding tetraethyl orthosilicate and nitric acid solution to the solution A, stirring and reacting in a 60° C. water bath to obtain solution B.
[0051] The mixed solvent includes water and ethanol. Furthermore, in the mixed solvent, the volume ratio of water to ethanol is 1:6.
[0052] In this embodiment, the mass fraction of nitric acid in the nitric acid solution is 65-68%. In addition, it is found through multiple experiments that the reaction can be completed by stirring the reaction for 4-6 hours to obtain solution B.
[0053] Silicon dioxide is obtained by hydrolysis of tetraethyl orthosilicate, so that silicon dioxide is coated on the surface of the nickel-doped cobalt vanadate material. In this embodiment, the mass ratio of the nickel-doped cobalt vanadate material, the mixed solvent, tetraethyl orthosilicate and the nitric acid solution is 1:8:3.47y:0.2, wherein y is the mass fraction of silicon dioxide in the nickel-doped cobalt vanadate material, 0.001≤y≤0.05, and at this addition amount, the effect of silicon dioxide coating modification is good, so that the cycle performance of the prepared modified cobalt vanadate material is excellent. That is, the mass ratio of the nickel-doped cobalt vanadate material, the mixed solvent, tetraethyl orthosilicate and the nitric acid solution is 1:8:0.00347~0.1735:0.2.
[0054] In a specific embodiment, step S30 includes: grinding the nickel-doped cobalt vanadate material, and then adding it to a mixed solvent to obtain solution A, adding ethyl orthosilicate to the solution A under stirring with a magnetic stirrer, and then adding 65-68% nitric acid after the addition is complete, and continuing to stir in a 60°C water bath for 4-6 hours to obtain solution B.
[0055] Step S40, separating the precipitate in the solution B, washing, drying, and then calcining at 450-550° C. to obtain a modified cobalt vanadate material.
[0056] The drying temperature of the drying is 110-130° C., and the drying time is 10-14 h; and / or the heating rate during the calcination process is 5-10° C. / min, and the calcination time is 4-6 h.
[0057] In a specific embodiment, step S40 includes: centrifuging solution B to obtain a precipitate, then washing the precipitate with deionized water and centrifuging, repeating 3 times, drying in an oven at 120°C for 12 hours, placing the dried product in a muffle furnace, heating it to 450~550°C at a heating rate of 5~10°C / min, and calcining it for 4~6 hours to obtain a modified cobalt vanadate material co-modified by doping and coating, the molecular formula of which is Co 1-x Ni x V2O6 / SiO2.
[0058] In the technical solution provided by the present invention, the microscopic morphology of the cobalt vanadate material is regulated by doping with nickel elements, the particle size is reduced, the contact area between the electrolyte and the electrode material is increased, and the surface electrochemical active sites are increased, thereby increasing the specific capacitance of the electrode material. At the same time, the doping of nickel will cause the lattice of the cobalt vanadate material to shrink, and the distance between the anion and the cation is shortened, which can effectively inhibit the structural change of cobalt vanadate during the charge and discharge process, enhance the structural stability, and then improve the cycle performance of the cobalt vanadate material; by coating silicon dioxide on the surface of the cobalt vanadate material doped with nickel, the direct contact between the cobalt vanadate material doped with nickel and the electrolyte can be reduced to avoid the active metal elements in the cobalt vanadate material doped with nickel in the long-term charge and discharge cycle. Dissolution loss in the electrolyte, thereby further improving the cycle performance of the cobalt vanadate material doped with nickel. Therefore, the present invention uses coating modification and doping modification, and the two work together to make the obtained modified cobalt vanadate material have good cycle performance and high specific capacitance.
[0059] Furthermore, the present invention also provides a supercapacitor, the supercapacitor comprising an electrode material, the electrode material being a modified cobalt vanadate material, wherein the modified cobalt vanadate material is prepared by the preparation method of the modified cobalt vanadate material as described above. Since the modified cobalt vanadate material as the electrode material has good conductivity and structural stability, the supercapacitor provided by the present invention has excellent cycle stability and high specific capacitance.
[0060] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0061] Example 1
[0062] (1) Add 1.23 g of ammonium metavanadate into 50 mL of deionized water, and heat in a water bath at 80° C. for 0.5 h under stirring with a magnetic stirrer at a stirring rate of 300 rpm to dissolve the ammonium metavanadate solution.
[0063] (2) 1.38 g of cobalt nitrate hexahydrate and 0.15 g of nickel nitrate hexahydrate were dissolved in 80 mL of deionized water to obtain a mixed solution. Under stirring with a magnetic stirrer at a stirring rate of 300 rpm, 2.21 g of citric acid monohydrate and 0.15 g of sodium dodecyl sulfate were added to the mixed solution. After magnetic stirring for 0.5 hour, the above ammonium metavanadate solution was added thereto. Deionized water was added to make the total volume of the solution 150 mL. The stirring was continued for 3 hours to obtain a reaction solution (that is, the concentration of ammonium metavanadate in the reaction solution was 0.07 mol / L), and the molar ratio of the components added to the reaction solution was cobalt nitrate hexahydrate: nickel nitrate hexahydrate: citric acid monohydrate: sodium dodecyl sulfate: ammonium metavanadate = 0.9:0.1:2:0.1:2.
[0064] (3) The reaction solution was transferred into a 200 mL hydrothermal reactor and reacted at 180° C. for 15 hours. After the reaction was completed, a solid-liquid mixture was obtained, which was naturally cooled to room temperature and then centrifuged. The obtained solid was washed with deionized water. After repeating this process for 3 times, the solid was vacuum dried at 80° C. for 12 hours. The dried product was placed in a muffle furnace, heated to 550° C. at a heating rate of 5° C. / min, and then calcined for 3 hours. The product was cooled to room temperature with the furnace to obtain a nickel-doped cobalt vanadate material with a molecular formula of Co 0.9 Ni 0.1 V2O6.
[0065] (4) After grinding the nickel-doped cobalt vanadate material, pour it into 10.8 g of a mixed solvent (the mixed solvent is a mixture of water and anhydrous ethanol in a volume ratio of 1:6) to obtain solution A. Under stirring with a magnetic stirrer at a stirring rate of 300 rpm, 0.14 g of tetraethyl orthosilicate is added dropwise to solution A. After the addition is complete, 0.27 g of 65-68% nitric acid solution is added, and stirring is continued for 5 hours in a water bath at 60° C. to obtain solution B, wherein the mass ratio of the added components is the nickel-doped cobalt vanadate material: mixed solvent: tetraethyl orthosilicate: nitric acid = 1:8:0.1:0.2, and the mass of silicon dioxide obtained by hydrolysis of tetraethyl orthosilicate accounts for 3% of the mass of the nickel-doped cobalt vanadate material.
[0066] (5) Solution B was centrifuged to obtain a precipitate, which was then washed with deionized water and centrifuged. This process was repeated three times and then dried in an oven at 120°C for 12 h. The dried product was placed in a muffle furnace, heated to 500°C at a heating rate of 5°C / min, and then calcined for 4 hours. The product was cooled to room temperature with the furnace to obtain a modified cobalt vanadate material co-modified by doping and coating, with the molecular formula Co 0.9 Ni 0.1 V2O6 / SiO2.
[0067] Example 2
[0068] (1) Add 1.88 g of ammonium metavanadate into 50 mL of deionized water, and heat in a water bath at 80° C. for 2 hours under stirring with a magnetic stirrer at a stirring rate of 200 rpm to dissolve the ammonium metavanadate solution.
[0069] (2) 2.17 g of cobalt nitrate hexahydrate and 0.16 g of nickel nitrate hexahydrate were dissolved in 80 mL of deionized water to obtain a mixed solution. Under stirring with a magnetic stirrer at a stirring rate of 300 rpm, 3.36 g of citric acid monohydrate and 0.23 g of sodium dodecyl sulfate were added. After magnetic stirring for 0.5 hour, the above ammonium metavanadate solution was added thereto. Deionized water was added to make the total volume of the solution 150 mL. The stirring was continued for 4 hours to obtain a reaction solution (that is, the concentration of ammonium metavanadate in the reaction solution was 0.11 mol / L), and the molar ratio of the components added to the reaction solution was cobalt nitrate hexahydrate: nickel nitrate hexahydrate: citric acid monohydrate: sodium dodecyl sulfate: ammonium metavanadate = 0.93:0.07:2:0.1:2.
[0070] (3) The reaction solution was transferred into a 200 mL hydrothermal reactor and reacted at 200 °C for 20 hours. After the reaction was completed, a solid-liquid mixture was obtained, which was naturally cooled to room temperature and then centrifuged. The obtained solid was washed with deionized water. After repeating this process for 3 times, the solid was vacuum dried at 90 °C for 10 hours. The dried product was placed in a muffle furnace, heated to 600 °C at a heating rate of 8 °C / min, and then calcined for 4 hours. The product was cooled to room temperature with the furnace to obtain a nickel-doped cobalt vanadate material with a molecular formula of Co 0.93 Ni 0.07 V2O6.
[0071] (4) After grinding the nickel-doped cobalt vanadate material, pour it into 16.4 g of a mixed solvent (the mixed solvent is a mixture of water and anhydrous ethanol in a volume ratio of 1:6) to obtain a solution A. Under stirring with a magnetic stirrer at a stirring rate of 400 rpm, 0.36 g of tetraethyl orthosilicate is added dropwise to the solution A. After the addition is complete, 0.41 g of a 65-68% nitric acid solution is added, and stirring is continued for 4 hours in a water bath at 60° C. to obtain a solution B, wherein the mass ratio of the added components is the nickel-doped cobalt vanadate material: mixed solvent: tetraethyl orthosilicate: nitric acid = 1:8:0.17:0.2, and the mass of the silicon dioxide obtained by hydrolysis of tetraethyl orthosilicate accounts for 5% of the mass of the nickel-doped cobalt vanadate material.
[0072] (5) Solution B was centrifuged to obtain a precipitate, which was then washed with deionized water and centrifuged. This was repeated three times and then dried in an oven at 110°C for 14 h. The dried product was placed in a muffle furnace, heated to 450°C at a heating rate of 10°C / min, and then calcined for 6 hours. The product was cooled to room temperature with the furnace to obtain a modified cobalt vanadate material co-modified by doping and coating, with the molecular formula Co 0.93 Ni 0.07 V2O6 / SiO2.
[0073] Example 3
[0074] (1) Add 2.28 g of ammonium metavanadate into 50 mL of deionized water, and heat in a water bath at 80° C. for 1.5 hours under stirring with a magnetic stirrer at a stirring rate of 400 rpm to dissolve the ammonium metavanadate solution.
[0075] (2) 2.81 g of cobalt nitrate hexahydrate and 0.03 g of nickel nitrate hexahydrate were dissolved in 80 mL of deionized water, and a mixed solution was obtained under stirring with a magnetic stirrer at a stirring rate of 400 rpm. Then, 4.1 g of citric acid monohydrate and 0.28 g of sodium dodecyl sulfate were added. After magnetic stirring for 0.5 hour, the above ammonium metavanadate solution was added thereto, and deionized water was added to make the total volume of the solution 150 mL. The stirring was continued for 5 hours to obtain a reaction solution (that is, the concentration of ammonium metavanadate in the reaction solution was 0.13 mol / L), and the molar ratio of the components added to the reaction solution was cobalt nitrate hexahydrate: nickel nitrate hexahydrate: citric acid monohydrate: sodium dodecyl sulfate: ammonium metavanadate = 0.99:0.01:2:0.1:2.
[0076] (3) The reaction solution was transferred into a 200 mL hydrothermal reactor and reacted at 190° C. for 12 hours. After the reaction was completed, a solid-liquid mixture was obtained, which was naturally cooled to room temperature and then centrifuged. The obtained solid was washed with deionized water. After repeating this process for 3 times, the solid was vacuum dried at 70° C. for 14 hours. The dried product was placed in a muffle furnace, heated to 500° C. at a heating rate of 10° C. / min, and then calcined for 5 hours. The product was cooled to room temperature with the furnace to obtain a nickel-doped cobalt vanadate material with a molecular formula of Co 0.99 Ni 0.01 V2O6.
[0077] (4) After grinding the nickel-doped cobalt vanadate material, pour it into 20g of a mixed solvent (the mixed solvent is a mixture of water and anhydrous ethanol in a volume ratio of 1:6) to obtain solution A. Under the stirring of a magnetic stirrer at a stirring rate of 300 rpm, 0.009g of tetraethyl orthosilicate is added dropwise to solution A. After the addition is complete, 0.5g of 65-68% nitric acid solution is added, and stirring is continued for 6 hours in a water bath at 60°C to obtain solution B. The mass ratio of the added components is the nickel-doped cobalt vanadate material: mixed solvent: tetraethyl orthosilicate: nitric acid = 1:8:0.0035:0.2, and the mass of silicon dioxide obtained by hydrolysis of tetraethyl orthosilicate accounts for 0.1% of the mass of the nickel-doped cobalt vanadate material.
[0078] (5) Solution B was centrifuged to obtain a precipitate, which was then washed with deionized water and centrifuged for three times. The precipitate was dried in an oven at 130°C for 10 h. The dried product was placed in a muffle furnace, heated to 550°C at a heating rate of 8°C / min, and calcined for 5 hours. The product was cooled to room temperature with the furnace to obtain a modified cobalt vanadate material co-modified by doping and coating, with the molecular formula Co0.99 Ni 0.01 V2O6 / SiO2.
[0079] Example 4
[0080] (1) Add 1.58 g of ammonium metavanadate into 50 mL of deionized water, and heat in a water bath at 80° C. for 1 hour under stirring with a magnetic stirrer at a stirring rate of 300 rpm to dissolve the ammonium metavanadate solution.
[0081] (2) 1.89 g of cobalt nitrate hexahydrate and 0.079 g of nickel nitrate hexahydrate were dissolved in 80 mL of deionized water to obtain a mixture. Under stirring with a magnetic stirrer at a stirring rate of 200 rpm, 2.84 g of citric acid monohydrate and 0.19 g of sodium dodecyl sulfate were added. After magnetic stirring for 0.5 hour, the above ammonium metavanadate solution was added thereto. Deionized water was added to make the total volume of the solution 150 mL. The stirring was continued for 4 hours to obtain a reaction solution (that is, the concentration of ammonium metavanadate in the reaction solution was 0.09 mol / L), and the molar ratio of the components added to the reaction solution was cobalt nitrate hexahydrate: nickel nitrate hexahydrate: citric acid monohydrate: sodium dodecyl sulfate: ammonium metavanadate = 0.96:0.04:2:0.1:2.
[0082] (3) The reaction solution was transferred into a 200 mL hydrothermal reactor and reacted at 180° C. for 18 hours. After the reaction was completed, a solid-liquid mixture was obtained, which was naturally cooled to room temperature and then centrifuged. The obtained solid was washed with deionized water. After repeating this process for 3 times, the solid was vacuum dried at 80° C. for 12 hours. The dried product was placed in a muffle furnace, heated to 550° C. at a heating rate of 5° C. / min, and then calcined for 4 hours. The product was cooled to room temperature with the furnace to obtain a nickel-doped cobalt vanadate material with a molecular formula of Co 0.96 Ni 0.04 V2O6.
[0083] (4) After grinding the nickel-doped cobalt vanadate material, pour it into 13.92 g of a mixed solvent (the mixed solvent is a mixture of water and anhydrous ethanol in a volume ratio of 1:6) to obtain a solution A. Under the stirring of a magnetic stirrer at a stirring rate of 200 rpm, 0.12 g of tetraethyl orthosilicate is added dropwise to the solution A. After the addition is complete, 0.35 g of a 65-68% nitric acid solution is added, and stirring is continued for 5 hours in a water bath at 60° C., wherein the mass ratio of the added components is the nickel-doped cobalt vanadate material: mixed solvent: tetraethyl orthosilicate: nitric acid = 1:8:0.07:0.2, and the mass of the silicon dioxide obtained by the hydrolysis of tetraethyl orthosilicate accounts for 2% of the mass of the nickel-doped cobalt vanadate material.
[0084] (5) Solution B was centrifuged to obtain a precipitate, which was then washed with deionized water and centrifuged. This process was repeated three times and then dried in an oven at 120°C for 12 hours. The dried product was placed in a muffle furnace, heated to 500°C at a heating rate of 5°C / min, and then calcined for 5 hours. The product was cooled to room temperature with the furnace to obtain a modified cobalt vanadate material co-modified by doping and coating, with the molecular formula Co 0.96 Ni 0.04 V2O6 / SiO2.
[0085] Comparative Example 1
[0086] (1) Add 1.23 g of ammonium metavanadate into 50 mL of deionized water, and heat in a water bath at 80° C. for 0.5 h under stirring with a magnetic stirrer at a stirring rate of 300 rpm to dissolve the ammonium metavanadate solution.
[0087] (2) 1.53 g of cobalt nitrate hexahydrate was dissolved in 80 mL of deionized water to obtain a mixed solution. Under stirring with a magnetic stirrer at a stirring rate of 300 rpm, 2.21 g of citric acid monohydrate and 0.15 g of sodium dodecyl sulfate were added. After magnetic stirring for 0.5 hour, the above ammonium metavanadate solution was added thereto. Deionized water was added to make the total volume of the solution 150 mL. The stirring was continued for 3 hours to obtain a reaction solution (that is, the concentration of ammonium metavanadate in the reaction solution was 0.07 mol / L), and the molar ratio of the components added to the reaction solution was cobalt nitrate hexahydrate: citric acid monohydrate: sodium dodecyl sulfate: ammonium metavanadate = 1:2:0.1:2.
[0088] (3) The reaction solution was transferred into a 200 mL hydrothermal reactor and reacted at 180 ° C for 15 hours. After the reaction, a solid-liquid mixture was obtained, which was naturally cooled to room temperature and then centrifuged. The solid was washed with deionized water. After repeating this process for 3 times, the mixture was vacuum dried at 80 ° C for 12 hours. The dried product was placed in a muffle furnace, heated to 550 ° C at a heating rate of 5 ° C / min, and then calcined for 3 hours. The mixture was cooled to room temperature along with the furnace to obtain a cobalt vanadate material with a molecular formula of CoV2O6.
[0089] Comparative Example 2
[0090] (1) Add 1.23 g of ammonium metavanadate into 50 mL of deionized water, and heat in a water bath at 80° C. for 0.5 h under stirring with a magnetic stirrer at a stirring rate of 300 rpm to dissolve the ammonium metavanadate solution.
[0091] (2) 1.38 g of cobalt nitrate hexahydrate and 0.15 g of nickel nitrate hexahydrate were dissolved in 80 mL of deionized water to obtain a mixed solution. Under stirring with a magnetic stirrer at a stirring rate of 300 rpm, 2.21 g of citric acid monohydrate and 0.15 g of sodium dodecyl sulfate were added to the mixed solution. After magnetic stirring for 0.5 hour, the above ammonium metavanadate solution was added thereto. Deionized water was added to make the total volume of the solution 150 mL. The stirring was continued for 3 hours to obtain a reaction solution (that is, the concentration of ammonium metavanadate in the reaction solution was 0.07 mol / L), and the molar ratio of the components added to the reaction solution was cobalt nitrate hexahydrate: nickel nitrate hexahydrate: citric acid monohydrate: sodium dodecyl sulfate: ammonium metavanadate = 0.9:0.1:2:0.1:2.
[0092] (3) The reaction solution was transferred into a 200 mL hydrothermal reactor and reacted at 180° C. for 15 hours. After the reaction was completed, a solid-liquid mixture was obtained, which was naturally cooled to room temperature and then centrifuged. The obtained solid was washed with deionized water. After repeating this process for 3 times, the solid was vacuum dried at 80° C. for 12 hours. The dried product was placed in a muffle furnace, heated to 550° C. at a heating rate of 5° C. / min, and then calcined for 3 hours. The product was cooled to room temperature with the furnace to obtain a nickel-doped cobalt vanadate material with a molecular formula of Co 0.9 Ni 0.1 V2O6.
[0093] Comparative Example 3
[0094] (1) Add 1.23 g of ammonium metavanadate into 50 mL of deionized water, and heat in a water bath at 80° C. for 0.5 h under stirring with a magnetic stirrer at a stirring rate of 300 rpm to dissolve the ammonium metavanadate solution.
[0095] (2) 1.53 g of cobalt nitrate hexahydrate was dissolved in 80 mL of deionized water to obtain a mixed solution. Under stirring with a magnetic stirrer at a stirring rate of 300 rpm, 2.21 g of citric acid monohydrate and 0.15 g of sodium dodecyl sulfate were added. After magnetic stirring for 0.5 hour, the above ammonium metavanadate solution was added thereto. Deionized water was added to make the total volume of the solution 150 mL. The stirring was continued for 3 hours to obtain a reaction solution (that is, the concentration of ammonium metavanadate in the reaction solution was 0.07 mol / L), and the molar ratio of the components added to the reaction solution was cobalt nitrate hexahydrate: citric acid monohydrate: sodium dodecyl sulfate: ammonium metavanadate = 1:2:0.1:2.
[0096] (3) The reaction solution was transferred into a 200 mL hydrothermal reactor and reacted at 180 ° C for 15 hours. After the reaction, a solid-liquid mixture was obtained, which was naturally cooled to room temperature and then centrifuged. The solid was washed with deionized water. After repeating this process for 3 times, the mixture was vacuum dried at 80 ° C for 12 hours. The dried product was placed in a muffle furnace, heated to 550 ° C at a heating rate of 5 ° C / min, and then calcined for 3 hours. The mixture was cooled to room temperature along with the furnace to obtain a cobalt vanadate material with a molecular formula of CoV2O6.
[0097] (4) After grinding the above cobalt vanadate material, pour it into 10.8 g of a mixed solvent (the mixed solvent is a mixture of water and anhydrous ethanol in a volume ratio of 1:6) to obtain solution A. Under stirring with a magnetic stirrer at a stirring rate of 300 rpm, 0.14 g of tetraethyl orthosilicate is added dropwise to solution A. After the addition is complete, 0.27 g of 65-68% nitric acid is added, and stirring is continued for 5 hours in a water bath at 60°C to obtain solution B, wherein the mass ratio of the added components is cobalt vanadate material: mixed solvent: tetraethyl orthosilicate: nitric acid = 1:8:0.1:0.2, and the mass of silicon dioxide obtained by hydrolysis of tetraethyl orthosilicate accounts for 3% of the mass of the cobalt vanadate material.
[0098] (5) Solution B was centrifuged to obtain a precipitate, which was then washed with deionized water and centrifuged. This process was repeated three times and then dried in an oven at 120°C for 12 h. The dried product was placed in a muffle furnace, heated to 500°C at a heating rate of 5°C / min, and calcined for 4 hours. The product was cooled to room temperature in the furnace to obtain a cobalt vanadate material coated with silica, with the molecular formula being CoV2O6 / SiO2.
[0099] The modified cobalt vanadate materials prepared in the above examples 1-4 and the composite materials prepared in comparative examples 1-3 were tested for their electrochemical properties as follows:
[0100] The modified cobalt vanadate material powder (or the composite material obtained in the comparative example), the conductive agent acetylene black, and the binder polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and ground into slurry with N-methylpyrrolidone as solvent. After grinding for 1 hour, the slurry was evenly coated on the nickel foam and vacuum dried at 80°C for 12 hours. The traditional three-electrode system was adopted, with the active material coated on the nickel foam as the working electrode, the platinum sheet as the counter electrode, and Hg / HgO as the reference electrode, immersed in 2mol / L KOH electrolyte, and its constant current charge and discharge performance was tested, the voltage range was 0-0.5V, the current density was 1A / g, and the cycle performance test results were shown in Table 1 below:
[0101] Table 1 Electrochemical performance test
[0102]
[0103] It can be seen from Table 1 that the modified cobalt vanadate material prepared in the embodiment of the present invention has high specific capacitance and good capacity retention rate, that is, good cycle performance.
[0104] Comparative Examples 1-3 are the same as the preparation process of Example 1, except that Comparative Example 1 does not perform nickel doping and coating modification on the cobalt vanadate material, Comparative Example 2 only performs nickel doping on the cobalt vanadate material, and Comparative Example 3 only performs coating modification. Compared with Comparative Examples 1 and 3, the modified cobalt vanadate material prepared in Example 1 has better specific capacitance and capacity retention rate when used as an electrode material. Although the composite material prepared in Comparative Example 2 has a high first discharge specific capacitance, its capacity retention rate (i.e., cycle performance) is much worse than that of the modified cobalt vanadate material prepared in Example 1. It can be seen that coating modification and doping modification play an important role in improving the cycle performance of electrode materials. Even if one of them is missing, the cycle performance of the product will be significantly weakened, indicating that coating modification and nickel doping play a synergistic role in improving the cycle performance of electrode materials; in addition, nickel doping modification can improve the specific capacitance of electrode materials.
[0105] Figure 1 The modified cobalt vanadate material Co prepared in Example 1 of the present invention 0.9 Ni 0.1 The XRD pattern of V2O6 / SiO2 and the standard XRD pattern of cobalt vanadate material (JCPDS No. 51-0130) are Figure 1 It can be seen that the modified cobalt vanadate material has a triclinic structure, indicating that the doping of a small amount of nickel and the surface coating of silicon dioxide do not change the crystal structure of the cobalt vanadate material.
[0106] Figure 2 The modified cobalt vanadate material Co prepared in Example 1 of the present invention 0.9 Ni 0.1 SEM image of V2O6 / SiO2, Figure 3 This is a SEM image of the cobalt vanadate material CoV2O6 prepared in Comparative Example 1 of the present invention. Figure 4 The nickel-doped cobalt vanadate material Co prepared in Comparative Example 2 of the present invention 0.9 Ni 0.1 SEM image of V2O6. From the comparison of these three images, it can be seen that compared with the cobalt vanadate material, the particle size of the cobalt vanadate material after doping and doping / coating is significantly reduced, indicating that the microstructure of the cobalt vanadate material is regulated by doping with nickel elements and the particle size is reduced.
[0107] Figure 5 The modified cobalt vanadate material Co prepared in Example 1 of the present invention 0.9 Ni 0.1 The first constant current charge and discharge curve of V2O6 / SiO2 is Figure 5It can be seen that the charge and discharge voltage range is 0-0.5V, and the first discharge specific capacitance is 398.5F / g at a current density of 1A / g.
[0108] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for preparing a modified cobalt vanadate material, characterized in that: The following steps are involved: S10, dissolving cobalt nitrate hexahydrate and nickel nitrate hexahydrate in deionized water to obtain a mixed solution, adding a complexing agent, a surfactant and an ammonium metavanadate solution to the mixed solution under stirring to obtain a reaction solution, transferring the reaction solution into a hydrothermal reactor, reacting at 180-200° C. for 12-20 h to obtain a solid-liquid mixture; S20, separating the solid-liquid mixture into solid and liquid, washing the obtained solid, vacuum drying, and then calcining at 500-600° C. to obtain a nickel-doped cobalt vanadate material; S30, crushing the nickel-doped cobalt vanadate material, and then adding it to a mixed solvent to obtain a solution A, adding tetraethyl orthosilicate and a nitric acid solution to the solution A, and stirring the mixture in a water bath at 60° C. to obtain a solution B; S40, separating the precipitate in the solution B, washing, drying, and then calcining at 450-550° C. to obtain a modified cobalt vanadate material; In the reaction solution, the molar ratio of the cobalt nitrate hexahydrate, the nickel nitrate hexahydrate, the complexing agent, the surfactant and the ammonium metavanadate is (1-x): x: 2: 0.1: 2, wherein 0 <x≤0.1; In step S30, the mass ratio of the nickel-doped cobalt vanadate material, the mixed solvent, tetraethyl orthosilicate and the nitric acid solution is 1:8:0.00347-0.1735:0.
2.
2. The method for preparing the modified cobalt vanadate material according to claim 1, characterized in that: In step S10: The complexing agent comprises citric acid monohydrate; and / or, The surfactant includes sodium lauryl sulfate.
3. The method for preparing the modified cobalt vanadate material according to claim 1, characterized in that: In the reaction solution, the concentration of ammonium metavanadate is 0.07-0.13 mol / L.
4. The method for preparing the modified cobalt vanadate material according to claim 1, characterized in that: In step S20: The vacuum drying has a drying temperature of 70-90°C and a drying time of 10-14 h; and / or, The heating rate during the calcination process is 5-10°C / min, and the calcination time is 3-5h.
5. The method for preparing the modified cobalt vanadate material according to claim 1, characterized in that: In step S30: The mixed solvent comprises water and anhydrous ethanol; and / or, In the nitric acid solution, the mass fraction of nitric acid is 65-68%.
6. The method for preparing the modified cobalt vanadate material according to claim 1, characterized in that: In step S30: The mixed solvent comprises water and anhydrous ethanol, wherein the volume ratio of water to anhydrous ethanol is 1:6; and / or, The stirring reaction time is 4 to 6 h.
7. The method for preparing the modified cobalt vanadate material according to claim 1, characterized in that: In step S40: The drying temperature of the drying is 110-130° C. and the drying time is 10-14 h; and / or, The heating rate during the calcination process is 5-10°C / min, and the calcination time is 4-6h.
8. A supercapacitor, characterized in that: The supercapacitor comprises an electrode material, wherein the electrode material is a modified cobalt vanadate material, wherein the modified cobalt vanadate material is prepared by the preparation method of the modified cobalt vanadate material according to any one of claims 1 to 7.