Polyamide composition

By introducing a large number of branched polyamides with excess amine end groups and heat stabilizers into the polyamide, a high-proportion branched polyamide composition is formed, which solves the problem of the decline in mechanical properties of polyamide at high temperatures and achieves high temperature stability. Excellent mechanical properties and fatigue resistance.

CN114423822BActive Publication Date: 2024-10-29BASF SE
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202080066008.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-25
Publication Date
2024-10-29
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

The mechanical properties of existing polyamide compositions decrease at high temperatures, making it difficult to maintain good fatigue resistance and mechanical properties when exposed to temperatures up to 160°C or higher for a long time.

Method used

By introducing a large amount of branched polyamide with excess amine end groups and an appropriate amount of heat stabilizer into the polyamide, a composition containing a high proportion of branched polyamide is formed to improve its thermal aging stability and fatigue resistance.

Benefits of technology

The composition exhibits excellent mechanical property retention and fatigue resistance at temperatures up to 200°C, significantly improving the service life and durability of polyamide products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004522869580000161
    Figure GDA0004522869580000161
  • Figure GDA0004522869580000171
    Figure GDA0004522869580000171
  • Figure GDA0004522869580000181
    Figure GDA0004522869580000181
Patent Text Reader

Abstract

The present invention relates to a polyamide composition [composition (C)] comprising: -0% to 30% by weight of at least one polyamide [polyamide (A)]; -more than 30% to 99.99% by weight of at least one branched polyamide different from polyamide (A).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polyamide compositions having improved resistance to aging and cyclic stresses, such as fatigue resistance or resistance to pressure pulsations. Background Art

[0002] Polyamides are synthetic polymers widely used to prepare a variety of shaped articles, including molded and injected parts, and are often recommended for use in high-end electrical, electronic and automotive industries.

[0003] In these fields of application, the molded polyamide articles come into contact with heat sources during their normal service life, which often reach and / or reach temperatures far exceeding 100° C. for a prolonged period of time. The heat source can be a heat generating device or heating means or can be the surrounding environment in which the molded article is placed. Examples of heating devices or heat generating devices are engines or components thereof, as well as electrical and electronic devices such as circuit breakers, connectors, inverters, LEDs, etc. For the automotive sector, high temperature applications are usually found in so-called under-the-hood or under-the-hood applications, here referred to as high-temperature automotive applications. Therefore, the present invention relates in particular to polyamides suitable for the preparation of molded articles for the electrical, electronic and automotive industries.

[0004] Molded articles and molding compositions based on polyamides for the electrical, electronic and automotive industries generally have to meet a complex performance profile, which for the molded compositions includes good dimensional stability, a high heat distortion temperature (HDT) and good mechanical properties (such as high tensile strength, tensile modulus and fatigue resistance). Polyamide materials generally tend to show decreased mechanical properties due to thermal degradation of the polymer. This effect is known as heat aging. This effect may occur to an undesirable extent. In particular, using polyamides as thermoplastic polymers, the deterioration effects of exposure to high temperatures may be very significant.

[0005] In an attempt to improve heat aging characteristics, it is conventional practice to add heat stabilizers to polyamide compositions. The role of the heat stabilizer is to better maintain the properties of the composition when the molded article is exposed to elevated temperatures. When a heat stabilizer is used, the useful life of the molded material can be significantly extended, depending on the type of material, the conditions of use, and the type and amount of heat stabilizer. Examples of heat stabilizers commonly used in polyamides are organic stabilizers, such as phenolic antioxidants and aromatic amines, and copper (in the form of copper salts in combination with potassium iodide or potassium bromide, or in the form of elemental copper), and metal powders, particularly iron powder.

[0006] The existing technology, while it is possible to improve long-term heat aging resistance, is still insufficient for more demanding applications (involving exposure to higher temperatures); in many applications, the retention of mechanical properties after long-term exposure to temperatures up to 160°C, or even 180-200°C and higher, becomes an essential requirement. The number of special applications requiring compositions with improved heat aging performance is also increasing.

[0007] In this context, US 4,945,129 discloses a polyamide composition comprising (i) an amine-terminated polyamide, which is preferably of the polycaprolactam type and which may contain branching materials, such as Jeffamine products (i.e. propylene oxide triamine), or trifunctional and tetrafunctional ethyleneamines; (ii) another additional polyamide and (iii) an olefin reactive copolymer. The composition may further contain stabilizers and inhibitors of oxidation, heat and UV degradation, among which a combination of a Group I metal halide and a cuprous halide is mentioned. Such a composition shows improved impact strength, especially at low temperatures.

[0008] Furthermore, WO 2013 / 004531 discloses a polyamide composition comprising:

[0009] - prepolymer Y, obtained by polycondensation of a multifunctional monomer and an AA / BB monomer mixture and an AB monomer, having a molecular weight of 600-3500 g / mol, the prepolymer preferably having an unbalanced end group, in particular an excess of amine end groups;

[0010] - a first linear prepolyamide X1 consisting essentially of AA-BB repeating units; and

[0011] - a second linear prepolyamide X2 consisting mainly of AB repeating units. The composition may also contain conventional additives such as heat stabilizers and antioxidants. The above composition is mixed in the molten state to provide a high molecular weight branched polyamide by reactive extrusion, wherein the concentration difference between the amine end groups and the carboxylic acid end groups (AEG-CEG) is generally 0 to 35 meq / kg (i.e., providing a slight excess of amine end groups).

[0012] Similarly, WO 2013 / 004548 discloses a polyamide composition comprising:

[0013] - prepolymer Y, obtained by polycondensation of a polyfunctional monomer and an AA / BB monomer mixture, having a molecular weight of 600-3500 g / mol, said prepolymer having preferably unbalanced end groups, in particular an excess of amine end groups;

[0014] - a linear prepolyamide X consisting of AA-BB repeating units. The composition may also contain conventional additives such as heat stabilizers and antioxidants. The above composition is mixed in the molten state to provide a high molecular weight branched polyamide by reactive extrusion, wherein the concentration difference between the amine end groups and the carboxylic acid end groups (AEG-CEG) is generally 0 to 35 meq / kg (i.e., providing a slight excess of amine end groups).

[0015] US 9,856,375 discloses a polyamide composition [composition (C)] comprising:

[0016] - 20 to 95% by weight of at least one polyamide [polyamide (A)];

[0017] 1 to 30% by weight of at least one branched polyamide different from polyamide (A), said branched polyamide comprising repeating units derived from the polycondensation of a mixture [mixture (B)] comprising:

[0018] - at least one polyamine monomer comprising at least three amine functional groups selected from secondary amine groups of formula -NH- and primary amine groups of formula -NH2 [monomer (FN)], and

[0019] -ε-caprolactam (or its derivatives);

[0020] The branched polyamide has an amine end group (AEG) concentration and a carboxyl end group (CEG) concentration such that the difference AEG-CEG is at least 100 meq / kg [polyamide (B)]; and

[0021] - 0.01 to 3.5% by weight of at least one thermal stabilizer [stabilizer (S)].

[0022] Although such polyamide compositions exhibit excellent heat aging resistance, for certain applications there may still be a need to improve their mechanical durability and fatigue resistance.

[0023] The object of the present invention is therefore to provide a polyamide composition which has superior heat aging properties and improved fatigue resistance compared to known compositions, thereby providing the possibility of producing moldings which can be used at higher continuous use temperatures than moldings prepared with known compositions and which have excellent mechanical properties during high-temperature use.

[0024] The inventors have now found that by incorporating into polyamide-based compounds a well-defined amount of a specific branched polyamide comprising a significant excess of amine end groups over carboxylic acid end groups, it is possible to effectively produce an excellent synergistic heat aging stability effect, in particular excellent mechanical properties even after long-term exposure to temperatures up to 200° C., while providing excellent fatigue resistance, for example under pressure pulsations. Summary of the invention

[0025] Therefore, the present invention relates to a polyamide composition [composition (C)] comprising:

[0026] - 0 to 30% by weight of at least one polyamide [polyamide (A)];

[0027] - from more than 30% by weight to 99.99% by weight of at least one branched polyamide different from polyamide (A), said branched polyamide comprising repeating units derived from the polycondensation of a mixture [mixture (B)] comprising:

[0028] (i) at least one polyamine monomer comprising at least three amine functional groups selected from secondary amine groups of the formula -NH- and primary amine groups of the formula -NH2 [monomer (FN)], and

[0029] (ii) ε-caprolactam (or its derivatives);

[0030] The branched polyamide has an amine end group (AEG) concentration and a carboxyl end group (CEG) concentration such that the difference AEG-CEG is at least 80 meq / kg [polyamide (B)]; and

[0031] - 0.01% to 3.5% by weight of at least one thermal stabilizer [stabilizer (S)],

[0032] - optionally, 0 to 60% by weight of at least one filler [filler (F)];

[0033] - optionally, 0 to 30% by weight of at least one impact-modified rubber [rubber (I)];

[0034] - optionally, 0 to 10% by weight of other conventional additives,

[0035] The % by weight are relative to the total weight of the composition (C).

[0036] The inventors have unexpectedly discovered that the simultaneous introduction of a heat stabilizer in the amounts detailed above and a large amount of amine-terminated branched polyamide is effective and unexpected in providing excellent heat aging stability, improved heat aging performance at temperatures up to 200°C, ensures excellent mechanical property retention, and has significantly better performance than polyamide compounds containing only a heat stabilizer or a smaller amount of branched polyamide.

[0037] In a preferred embodiment, the polyamide composition of the present invention comprises:

[0038] - 0 to 30% by weight of at least one polyamide [polyamide (A)];

[0039] - from more than 30% by weight to 99.99% by weight of at least one branched polyamide different from polyamide (A), said branched polyamide comprising repeating units derived from the polycondensation of a mixture [mixture (B)] comprising:

[0040] - at least one trifunctional or tetrafunctional polyamine monomer comprising three or four amine functional groups selected from secondary amine groups of formula -NH- and primary amine groups of formula -NH2 [monomer (FN)], and

[0041] -ε-caprolactam (or its derivatives);

[0042] in,

[0043] When the monomer (FN) is a trifunctional polyamine monomer, the amount of the monomer (FN) is such that the molar ratio of the monomer (FN) / ε-caprolactam (or its derivative) is at least 0.002 and at most 0.030, and

[0044] When the monomer (FN) is a tetrafunctional polyamine monomer, the amount of the monomer (FN) is such that the molar ratio of the monomer (FN) / ε-caprolactam (or its derivative) is at least 0.001 and at most 0.030;

[0045] The branched polyamide has an amine end group (AEG) concentration and a carboxyl end group (CEG) concentration such that the difference AEG-CEG is at least 100 meq / kg and at most 300 meq / kg [polyamide (B)]; and

[0046] - 0.01% to 3.5% by weight of at least one thermal stabilizer [stabilizer (S)],

[0047] - optionally, 0 to 60% by weight of at least one filler [filler (F)];

[0048] - optionally, 0 to 30% by weight of at least one impact-modified rubber [rubber (I)];

[0049] - optionally, 0 to 30% by weight of other conventional additives,

[0050] The above % by weight is relative to the total weight of the composition (C). DETAILED DESCRIPTION

[0051] In this specification, where an element or component is considered to be included in and / or selected from a list of listed elements or components, it should be understood that in the relevant embodiments explicitly considered herein, the element or component may also be any one of the elements or components listed individually, or may also be selected from any two or more of the explicitly listed elements or components.

[0052] The term "comprising" includes "consisting essentially of and "consisting of.

[0053] Unless otherwise specified, the symbol "%" or "weight %" means "weight percent".

[0054] In the present specification, the description of the value range of a variable defined by a lower limit or an upper limit or by a lower limit and an upper limit also includes embodiments in which the variable is selected within the numerical range: excluding the lower limit, excluding the upper limit, or excluding the lower limit and the upper limit, respectively.

[0055] In this specification, when an element or component is considered to be included in and / or selected from a list of listed elements or components, it should be understood that in the relevant embodiments explicitly considered herein, the element or component may also be any one of the elements or components listed individually, or may also be selected from any two or more of the explicitly listed elements or components.

[0056] For example, when describing in one embodiment that an element is selected from a group of elements, the following elements are also explicitly described:

[0057] - select two or more elements from a group,

[0058] - Selecting elements from a subgroup of elements consisting of a group of elements from which one or more elements have been removed.

[0059] As used herein, the singular "a" or "one" includes the plural unless specifically stated otherwise.

[0060] In addition, unless otherwise expressly stated, if the term "about" is used before a quantitative value, the present teachings also include the specific quantitative value itself. As used herein, unless otherwise expressly stated, the term "about" refers to a variation of ±10% from the nominal value.

[0061] Polyamide (A)

[0062] The expression "polyamide (A)" is intended to mean any polymer comprising recurring units derived from:

[0063] - a polycondensation reaction of at least one dicarboxylic acid component (or a derivative thereof) and at least one diamine component (or a derivative thereof), and / or

[0064] - polycondensation of at least one aminocarboxylic acid and / or at least one lactam.

[0065] In addition to the recurring units, the polyamide (A) may comprise recurring units derived from diols, polyols or other functional compounds comprising heteroatoms (eg O, P, S).

[0066] In certain preferred embodiments, the polyamide (A) of the present invention comprises at least 50 mol%, preferably at least 60 mol%, more preferably at least 70 mol%, still more preferably at least 80 mol% and most preferably at least 90 mol% of such repeating units. Excellent results are obtained when the polyamide (A) consists essentially of said repeating units, it being understood that small amounts (e.g. less than 0.5 mol%) of repeating units derived from other monomers (e.g. multifunctional monomers) may still be present without this changing the thermodynamic properties of the polyamide (A).

[0067] More precisely, the polyamide (A) can be obtained by condensation reaction of at least one mixture selected from the group consisting of:

[0068] a mixture (M1) comprising at least one diacid [acid (DA)] (or a derivative thereof) and at least one diamine [amine (NN)] (or a derivative thereof);

[0069] - a mixture (M2) comprising at least one lactam [lactam (L)];

[0070] - a mixture (M3) comprising at least one aminocarboxylic acid [amino acid (AN)]; and

[0071] - combinations thereof.

[0072] Acid (DA) derivatives include in particular salts, anhydrides, esters and acid halides, which are capable of forming amide groups; similarly, amine (NN) derivatives include in particular salts thereof, which are likewise capable of forming amide groups.

[0073] The acid (DA) may be an aromatic dicarboxylic acid comprising two reactive carboxylic acid groups [acid (AR)] or an aliphatic or cycloaliphatic dicarboxylic acid comprising two reactive carboxylic acid groups [acid (AL)]. For the purposes of the present invention, a dicarboxylic acid is considered "aromatic" when it comprises one or more than one aromatic group.

[0074] Non-limiting examples of acids (AR) are, inter alia, phthalic acid, including isophthalic acid (IA) and terephthalic acid (TA), 2,5-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-pyridinedicarboxylic acid, 2,2-bis(4-carboxyphenyl)propane, bis(4-carboxyphenyl)methane, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 2,2-bis(4-carboxyphenyl)ketone, bis(4-carboxyphenyl)sulfone, 2,2-bis(4-carboxyphenyl) 3-carboxyphenyl)propane, bis(3-carboxyphenyl)methane, 2,2-bis(3-carboxyphenyl)hexafluoropropane, 2,2-bis(3-carboxyphenyl)ketone, bis(3-carboxyphenoxy)benzene, naphthalene dicarboxylic acid, including 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 1,2-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid or 1,4-cyclohexane dicarboxylic acid.

[0075] Among the acids (AL), mention may be made especially of oxalic acid (HOOC-COOH), malonic acid (HOOC-CH2-COOH), succinic acid [HOOC(CH2)2-COOH], glutaric acid [HOOC-(CH2)3-COOH], 2,2-dimethylglutaric acid [HOOC-C(CH3)2-(CH2)2-COOH], adipic acid [HOOC-(CH2)4-COOH], 2,4,4-trimethyladipic acid [HOOC-CH(CH3)-CH2-C(CH3)2-CH2-COOH], pimelic acid [HOOC-(CH2)3-COOH], 5- COOH], suberic acid [HOOC-(CH2)6-COOH], azelaic acid [HOOC-(CH2)7-COOH], sebacic acid [HOOC-(CH2)8-COOH], undecanedioic acid [HOOC-(CH2)9-COOH], dodecanedioic acid [HOOC-(CH2) 10 -COOH], tetradecanedioic acid [HOOC-(CH2) 12 -COOH], octadecane dioic acid [HOOC-(CH2) 16 -COOH].

[0076] Preferably, the acid (DA) used for the preparation of the polyamide (A) is an acid (AL) as detailed above, possibly in combination with a small amount of an acid (AR) as detailed above.

[0077] The amine (NN) is generally selected from aliphatic and cycloaliphatic alkylenediamines, aromatic diamines and mixtures thereof.

[0078] The aliphatic alkylenediamine is generally an aliphatic alkylenediamine having 2 to 18 carbon atoms.

[0079] The alicyclic alkylenediamine is generally an alicyclic alkylenediamine having 5 to 18 carbon atoms.

[0080] The aliphatic alkylenediamine is advantageously selected from 1,2-diaminoethane, 1,2-diaminopropane, 1,3-diamine, 1,3-diaminobutane, 1,4-diaminobutane, 1,5-diaminopentane, 1,5-diamino-2-methylpentane, 1,4-diamino-1,1-dimethylbutane, 1,4-diamino-1-ethylbutane, 1,4-diamino-1,2-dimethylbutane, 1,4-diamino-1,3-dimethylbutane, 1,4-diamino- 1,4-dimethylbutane, 1,4-diamino-2,3-dimethylbutane, 1,2-diamino-1-butylethane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,6-diamino-2,5-dimethylhexane, 1,6-diamino-2,4-dimethylhexane, 1,6-diamino-3,3-dimethylhexane, 1,6-diamino-2,2-dimethylhexane, 1,9-diaminononane, 1,8-diamino-2-methyloctane , 1,6-diamino-2,2,4-trimethylhexane, 1,6-diamino-2,4,4-trimethylhexane, 1,7-diamino-2,3-dimethylheptane, 1,7-diamino-2,4-dimethylheptane, 1,7-diamino-2,5-dimethylheptane, 1,7-diamino-2,2-dimethylheptane, 1,10-diaminodecane, 1,8-diamino-1,3-dimethyloctane, 1,8-diamino-1,4-dimethyloctane, 1,8-diamino- 2,4-dimethyloctane, 1,8-diamino-3,4-dimethyloctane, 1,8-diamino-4,5-dimethyloctane, 1,8-diamino-2,2-dimethyloctane, 1,8-diamino-3,3-dimethyloctane, 1,8-diamino-4,4-dimethyloctane, 1,6-diamino-2,4-diethylhexane, 1,9-diamino-5-methylnonane, 1,11-diaminoundecane, 1,12-diaminododecane and 1,13-diaminotridecane.

[0081] The aliphatic alkylenediamine preferably comprises at least one diamine selected from the group consisting of 1,6-diaminohexane, 1,8-diamino-octane, 1,10-diaminodecane, 1,12-diaminododecane, and mixtures thereof. More preferably, the aliphatic alkylenediamine comprises at least one diamine selected from the group consisting of 1,6-diaminohexane, 1,10-diaminodecane, and mixtures thereof.

[0082] Examples of alicyclic diamines are isophoronediamine, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, 4,4′-diaminodicyclohexylmethane and (4,4′-bis(aminocyclohexyl)methane.

[0083] The aromatic diamine is preferably selected from meta-xylylenediamine and para-xylylenediamine.

[0084] Preferably, the amine (NN) used for the preparation of the polyamide (A) will be an aliphatic alkylenediamine as detailed above, possibly in combination with a small amount of an aromatic diamine as detailed above.

[0085] Preferred mixtures (M1) are:

[0086] - a mixture of adipic acid and 1,6-diaminohexane;

[0087] - a mixture of adipic acid, terephthalic acid and 1,6-diaminohexane;

[0088] - a mixture of sebacic acid and 1,6-diaminohexane,

[0089] - a mixture of terephthalic acid and 1,10-diaminodecane,

[0090] - a mixture of adipic acid, terephthalic acid and 1,10-diaminodecane,

[0091] - A mixture of adipic acid and 1,10-diaminodecane.

[0092] The lactam (L) suitable for preparing the polyamide (A) may be any one of β-lactam and ε-caprolactam.

[0093] Preferred mixtures (M2) comprise ε-caprolactam.

[0094] The amino acid (AN) suitable for preparing the polyamide (A) can be selected from 6-aminocaproic acid, 9-aminononanoic acid, 10-aminodecanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.

[0095] Still within the scope of the invention, one or more than one polyfunctional acid / amine monomers containing more than two carboxylic acid and amine groups are added to any of the mixtures (M1), (M2), (M3) and combinations thereof, such as polycarboxylic acids having three or more carboxylic acid groups, polyamines having three or more amine groups, polyfunctional diacids comprising two carboxylic acid groups and one or more amine groups, polyfunctional diamines comprising two amine groups and one or more carboxylic acid groups. The introduction of such polyfunctional acid / amine monomers generally results in star-shaped or tree-shaped branched structures, such as those described in WO 97 / 24388 and WO 99 / 64496, among others.

[0096] It is further understood that one or more than one end-capping agent [reagent (M)] may be added to any of the mixtures (M1), (M2), (M3) and combinations thereof for the preparation of polyamide (A) without departing from the scope of the present invention. Reagent (M) is typically selected from acids containing only one reactive carboxylic acid group [acid (MA)] and amines containing only one reactive amine group [reagent (MN)].

[0097] The acid (MA) is preferably selected from acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, stearic acid, cyclohexanecarboxylic acid, benzoic acid, preferably from acetic acid and benzoic acid.

[0098] The amine (MN) is preferably selected from methylamine, ethylamine, butylamine, hexylamine, octylamine, benzylamine, dodecylamine, cyclohexylamine.

[0099] The polyamide (A) generally comprises at least 50 mol % of recurring units of any one of the formula (I) or formula (II) [recurring units (R PA )] (relative to the total number of moles of repeating units of polyamide (A):

[0100] Formula (I): -NH-R 1 -CO-

[0101] Formula (II): -NH-R 2 -NH-CO-R 3 -CO-,

[0102] in:

[0103] -R 1 , which are the same or different at each occurrence, are divalent hydrocarbon radicals having 3 to 17 carbon atoms;

[0104] -R 2 , which are the same or different at each occurrence, are divalent hydrocarbon radicals having 2 to 18 carbon atoms; and

[0105] -R 3 , which are the same or different from each other at each occurrence, are a bond or a divalent hydrocarbon group having 1 to 16 carbon atoms.

[0106] The polyamide (A) composition is preferably an aliphatic polyamide, that is, R 1 , R 2 and R 3 It is an aliphatic group.

[0107] In particular, exemplary repeating units (R PA )for:

[0108] (j) -NH-(CH2)5-CO-, i.e. a repeating unit obtainable, inter alia, by polycondensation of ε-caprolactam [repeating unit (R6)];

[0109] (jj) -NH-(CH2)8-CO-, i.e. a repeating unit obtainable, inter alia, by polycondensation of 9-aminononanoic acid [repeating unit (R9)];

[0110] (jjj)-NH-(CH2)9-CO-, i.e., a repeating unit obtainable in particular by polycondensation of 10-aminodecanoic acid [repeating unit (R 10 )];

[0111] (jv)-NH-(CH2) 10 -CO-, i.e., a repeating unit obtainable in particular by polycondensation of 11-aminoundecanoic acid [repeat unit (R 11 )];

[0112] (v)-NH-(CH2) 11 -CO-, i.e., a repeating unit obtainable in particular by polycondensation of laurolactam [repeat unit (R 12 )];

[0113] (vj) -NH-(CH2)6-NH-CO-(CH2)4-CO-, i.e., a repeating unit obtainable in particular by polycondensation of hexamethylenediamine and adipic acid [repeat unit (R 6,6 )];

[0114] (vjj)-NH-(CH2)6-NH-CO-(CH2) 10 -CO-, i.e., a repeating unit obtainable in particular by polycondensation of hexamethylenediamine and dodecanedioic acid [repeating unit (R 6,12 )];

[0115] (vjjj)-NH-(CH2)6-NH-CO-(CH2) 12 -CO-, i.e., a repeating unit obtainable in particular by polycondensation of hexamethylenediamine and tetradecanedioic acid [repeat unit (R 6,14 )];

[0116] (jx)-NH-(CH2) 10 -NH-CO-(CH2) 10 -CO-, i.e., a repeating unit obtainable in particular by polycondensation of decamethylenediamine and dodecanedioic acid [repeat unit (R 10,12 )];

[0117] (x)-NH-(CH2)6-NH-CO-(CH2)7-CO-, i.e., a repeating unit obtainable in particular by polycondensation of hexamethylenediamine and azelaic acid (also known as nonanedioic acid) [repeat unit (R 6,9 )];

[0118] (xj)-NH-(CH2) 12 -NH-CO-(CH2) 10 -CO-, i.e., a repeating unit obtainable in particular by polycondensation of dodecamethylenediamine and dodecanedioic acid [repeating unit (R 12,12 )];

[0119] (xjj)-NH-(CH2) 10 -NH-CO-(CH2)8-CO-, i.e., a repeating unit obtainable in particular by polycondensation of decanediamine and sebacic acid [repeating unit (R 10,10 )];

[0120] (xjjj)-NH-(CH2)4-NH-CO-(CH2)4-CO-, i.e., a repeating unit obtainable in particular by polycondensation of 1,4-butanediamine and adipic acid [repeat unit (R 4,6 )];

[0121] (xjv)-NH-(CH2)4-NH-CO-(CH2)8-CO-, i.e., a repeating unit obtainable in particular by polycondensation of 1,4-butanediamine and sebacic acid [repeat unit (R 4,10 )];

[0122] (xv) -HN-(CH2)6-NH-CO-(CH2)8-CO-, i.e., a repeating unit obtainable in particular by polycondensation of 1,6-hexamethylenediamine and sebacic acid [repeat unit (R 6,10 )];

[0123] (xvi)-HN-(CH2) 10 -NH-CO-(CH2)4-CO-, i.e., a repeating unit obtainable in particular by polycondensation of 1,10-decanediamine and adipic acid [repeat unit (R 10,6 )].

[0124] More than 50 mol %, preferably more than 60 mol %, even more preferably more than 70 mol % of the recurring units of the polyamide (A) are recurring units (R PA ).

[0125] The repeating unit (R PA) may be all the same, thereby making the polyamide (A) a homopolyamide, or may be different in kind, thereby making the polyamide (A) a copolyamide.

[0126] According to certain preferred embodiments, the polyamide (A) consists essentially of repeating units (R 6,6 ), that is, polyamide (A) is a homopolyamide PA66. It should be understood that end chains, defects and other irregularities may exist in the polyamide (A) chain without affecting its performance.

[0127] The end groups of the polyamide (A) may be of any type, including non-functional (capped) end groups, carboxylic acid end groups (CEG) and amine end groups (AEG).

[0128] However, it is generally understood that according to a preferred embodiment, the polyamide (A) comprises a concentration of carboxylic acid end groups exceeding the concentration of amine end groups.

[0129] For this purpose, the polyamide (A) can preferably be prepared by polycondensation in the presence of an excess of carboxylic acid groups in the monomer mixture, this excess generally being in the form of an excess of at least one carboxylic acid comprising two or more than two carboxylic acid groups, preferably more than two.

[0130] The composition (C) will generally comprise at most 30% by weight, preferably less than 25% by weight, more preferably less than 20% by weight, even more preferably less than 15% by weight, even more preferably less than 10% by weight and most preferably less than 5% by weight of polyamide (A) as described above in detail, relative to the total weight of the composition (C).

[0131] Polyamide (B)

[0132] As described above, composition (C) comprises from more than 30 wt.-% (preferably more than 40 wt.-%, more than 50 wt.-%, more than 60 wt.-%, more than 70 wt.-%, more than 80 wt.-% or more than 90 wt.-%) to 99.99 wt.-% of at least one branched polyamide different from polyamide (A), said branched polyamide comprising repeating units derived from the polycondensation of a mixture [mixture (B)] comprising:

[0133] - at least one monomer (FN) as defined above, and

[0134] -ε-caprolactam (or its derivatives);

[0135] The branched polyamide has an AEG and a CEG such that the difference AEG-CEG is at least 80 meq / kg [polyamide (B)].

[0136] In a preferred embodiment, the weight percentage of polyamide (B) is at least 70 weight %, preferably at least 75 weight %, more preferably at least 80 weight %, even more preferably at least 90 weight %, for example 100 weight %, relative to the total weight of polyamide (A) and polyamide (B) in composition (C).

[0137] Monomer (FN) is preferably a trifunctional polyamine monomer comprising three amine groups as detailed above, or a tetrafunctional polyamine monomer comprising four amine groups as detailed above.

[0138] As examples of monomers (FN), mention may be made of tris(aminoalkyl)amines, for example tris(2-aminoethyl)amine (TREN); polyoxyalkylene triamines, for example Jeffamine T(R) from Huntsman, including Jeffamine T403(R) (polyoxypropylene triamine); polyalkylene polyamines, such as polyethyleneimine, which may advantageously have variable molecular weights, 1,8-diamino-4-aminomethyl-octane (TAN) and dialkylene triamines, such as diethylene triamine (DETA), bis(hexamethylene) triamine (BHT) and cyclohexane-1,3,5-triamine and 2,2,6,6-tetrakis(2-aminoethyl)cyclohexanone.

[0139] Preferred multifunctional monomers are bis(hexamethylene)triamine (BHT), tris(2-aminoethyl)amine (TREN), 1,8-diamino-4-aminomethyl-octane (TAN), and combinations thereof.

[0140] The expression "derivatives thereof" when used in conjunction with the expression "ε-caprolactam" is intended to mean any derivative that readily reacts under polycondensation conditions to produce an amide bond. Examples of amide-forming derivatives include the corresponding amino acid linear compounds, monoalkyl esters, such as the monomethyl, ethyl or propyl esters thereof; the monoaryl esters thereof; the monoacid halides thereof; the monoacid amides thereof, the monocarboxylates thereof and the monoammonium salts thereof. Examples of such derivatives are aminoundecanoic acid (PA11), aminododecanoic acid (PA12) and lauryl lactam, and copolymers thereof.

[0141] However, it is generally understood that it is preferred to use ε-caprolactam itself for the preparation of polymer (B).

[0142] The amount of monomer (FN) is not particularly limited, as long as it can particularly help deliver appropriate AEG and CEG so that the AEG-CEG value is within the claimed range. A person skilled in the art will be able to determine the required amount based on routine experiments, especially taking into account the number of amine groups of the monomer (FN) and the final molecular properties sought for the polymer (B).

[0143] However, it is generally understood that the amount of monomer (FN) used is such that the molar ratio of monomer (FN) / ε-caprolactam (or its derivative) is at least 0.001 and / or at most 0.1, preferably at most 0.040.

[0144] When the monomer (FN) is a trifunctional polyamine monomer, the amount of the monomer (FN) used is such that the molar ratio of monomer (FN) / ε-caprolactam (or its derivative) is at least 0.002, preferably at least 0.003, more preferably at least 0.004 and / or at most 0.040, more preferably at most 0.030, even more preferably at most 0.020.

[0145] When monomer (FN) is a tetrafunctional polyamine monomer, the amount of monomer (FN) used is such that the molar ratio of monomer (FN) / ε-caprolactam (or its derivative) is at least 0.001, preferably at least 0.002, and / or at most 0.003 and / or at most 0.030, preferably at most 0.020, more preferably at most 0.015.

[0146] It is particularly preferred that the molar ratio of monomer (FN) / ε-caprolactam (or its derivative) is from 0.002 to 0.030 for trifunctional polyamine monomers and from 0.001 to 0.030 for tetrafunctional polyamine monomers.

[0147] The mixture (B) which forms the polymer (B) by polycondensation may additionally comprise at least one diacid [acid (DA)] as described above in detail for polymer (A) and / or at least one diamine [amine (NN)] as described above in detail for polymer (A). Preferably, the mixture (B) does not contain any amine (NN) as described above in detail.

[0148] Preferred embodiments are those wherein said mixture (B) comprises at least one acid (DA), preferably adipic acid, optionally in combination with at least one said amine (NN), it being understood however that the mixture (B) is preferably free of amine (NN).

[0149] Without being bound by any theory, the present inventors believe that the acid (DA) in the mixture (B) can be beneficial to adjusting the melt viscosity of the polymer (B), so that the mixture (B) will be easier to recover from the polymerization reactor in a molten state and easier to process in subsequent compounding.

[0150] The acid (DA) used in the mixture (B) may be the acid (AL) or the acid (AR) as detailed above. Preferably, the acid (DA) used in the mixture (B) will be the acid (AL) as detailed above, possibly in combination with a small amount of the acid (AR) as detailed above. The best results were obtained when the mixture (B) comprised adipic acid as the acid (DA).

[0151] When acid (DA) is present in the mixture (B) for preparing the polyamide (B), it may be used in such an amount that the molar ratio of acid (DA) / monomer (FN) does not exceed the limit 0.44+1 / x, wherein x is the number of said amine groups in the monomer (FN).

[0152] Therefore, when the monomer (FN) is a trifunctional polyamine monomer comprising three of said amine groups, the molar ratio of acid (DA) / monomer (FN) preferably does not exceed the limit 0.44+1 / 3, ie 0.7733.

[0153] The minimum amount of acid (DA) is not particularly critical and will preferably be chosen by a person skilled in the art according to the target molecular weight, ie to be able to obtain a polymer (B) with a number average molecular weight of at least 10 000 g / mol.

[0154] It is also understood that when acid (DA) is present, it is present in an amount such that the total number of carboxyl groups of the acid (DA) is less than the total number of amine groups of the monomer (FN), more precisely such that the difference AEG-CEG is at least 80 meq / kg.

[0155] The polymerization of the mixture (B) to give the polymer (B) can be carried out according to standard techniques known in the art for preparing PA6 and / or PA66; such techniques may involve, in particular, a continuous polymerization process or a discontinuous polymerization process.

[0156] In polymer (B), the difference AEG-CEG is advantageously at least 100 meq / kg. The difference AEG-CEG is preferably at most 300 meq / kg, more preferably at most 200 meq / kg. The preferred range of the difference AEG-CEG is 80 meq / kg to 300 meq / kg, more preferably 100 meq / kg to 300 meq / kg.

[0157] Polymer (B) is advantageously semicrystalline, ie it has a distinguishable melting point. The melting point of polymer (B) is advantageously between 150 and 250°C.

[0158] When at 250℃, 100s -1 The melt viscosity of polymer (B) is advantageously from 10 to 5000 Pa×s when measured at a shear rate of 1.5 to 2.0 Pa×s.

[0159] The number average molecular weight of polymer (B) is advantageously at least 10,000 g / mol, preferably at least 12,000 g / mol, more preferably at least 14,000 g / mol.

[0160] The dispersibility (IP) of polymer (B) is advantageously at most 5, preferably at most 4, more preferably at most 3.

[0161] Number average molecular weight (M n) and dispersion (IP) are determined by equations (I) and (II):

[0162] (I)

[0163] (II)

[0164] Wherein R represents the molar ratio of acid (DA) / monomer (FN); Co and CEG represent the concentration of monomer (FN) and carboxyl end groups in polymer (B), respectively, in meq / kg; f represents the functionality of monomer (FN).

[0165] Heat Stabilizer

[0166] The composition (C) further comprises one or more than one thermal stabilizer or antioxidant [stabilizer (S)] in the amounts described above.

[0167] One or more than one stabilizer (S) may be used in the composition (C) of the present invention.

[0168] Heat stabilizers (S) known in the art for heat stabilization of polyamides can be effectively used.

[0169] The stabilizer (S) used in the composition (C) is generally selected from copper-containing stabilizers, hindered amine compounds, hindered phenol compounds, polyols (PHA) and phosphorus compounds.

[0170] Copper stabilizer

[0171] The stabilizer (S) preferably comprises at least one copper-containing stabilizer. Although these copper-containing stabilizers can be used alone in the composition (C), they can also be used in combination with one or more of the alternative stabilizers (S) described above.

[0172] However, preferred embodiments are those in which a copper-containing stabilizer is used alone, ie the stabilizer (S) is a copper-containing stabilizer.

[0173] The copper-containing stabilizer useful in the practice of the present invention may be characterized as comprising a copper compound [compound (Cu)] and an alkali metal halide [halide (M)]. More specifically, the copper-containing stabilizer will consist essentially of a copper compound [compound (Cu)] and an alkali metal halide [halide (M)], wherein the copper compound [compound (Cu)] is selected from cuprous (I) oxide, cuprous (II) oxide, copper (I) salts such as cuprous acetate, cuprous stearate, organic cuprous complexes such as cuprous acetylacetonate, cuprous halides, and the like. According to certain preferred embodiments, the copper-containing stabilizer will consist essentially of a copper halide selected from cupric iodide and cupric bromide, and the alkali metal halide will preferably be selected from iodides and bromides of lithium, sodium, and potassium.

[0174] A particularly preferred combination is the combination of CuI and KI. Another very advantageous combination is a mixture of Cu2O and KBr.

[0175] The copper-containing stabilizer will preferably consist of a copper compound [compound (Cu)] (preferably copper having an oxidation state of +1) and an alkali metal halide [halide (M)], wherein the atomic weight ratio of Cu:halide, i.e. the weight ratio between the total copper content of compound (Cu) and the total halogen content of halide (M) and possible compound (Cu) (if the latter contains halogen), is from 1:99 to 30:70, preferably from 5:95 to 20:80. A particularly effective weight ratio of Cu:halide has been found to be about 0.15 (i.e. equivalent to about 13:87).

[0176] The combined weight of compound (Cu) and halide (M) in composition (C), i.e., the combined weight of copper-containing stabilizer, is from about 0.01 to about 3 weight percent, preferably from about 0.02 to about 2.5 weight percent, more preferably from about 0.1 to about 1.5 weight percent, based on the total weight of composition (C).

[0177] The amount of compound (Cu) in the copper-containing stabilizer is generally sufficient to provide copper at a level of about 25 to about 1000 ppm, preferably about 50 to about 500 ppm, more preferably about 75 to about 150 ppm in composition (C).

[0178] Hindered amine compounds

[0179] The expression "hindered amine compound" is used according to its customary meaning in the art and is generally intended to denote derivatives of 2,2,6,6-tetramethylpiperidine well known in the art (see for example: Plastics Additives Handbook, 5th edition, Hanser, 2001). The hindered amine compound of the composition according to the invention may be of low molecular weight or high molecular weight.

[0180] The low molecular weight hindered amine compound generally has a molecular weight of at most 900, preferably at most 800, more preferably at most 700, still more preferably at most 600 and most preferably at most 500 g / mol.

[0181] Examples of low molecular weight hindered amine compounds are listed in Table 1 below:

[0182] Table 1

[0183]

[0184]

[0185] Among these low molecular weight compounds, the hindered amine is preferably selected from those corresponding to formula (a1), (a2), (a11) and (a12). More preferably, the hindered amine is selected from those corresponding to formula (a1), (a2) and (a12). Still more preferably, the hindered amine is a hindered amine corresponding to formula (a2).

[0186] The high molecular weight hindered amine compounds are typically polymeric and typically have a molecular weight of at least 1000, preferably at least 1100, more preferably at least 1200, still more preferably at least 1300 and most preferably at least 1400 g / mol.

[0187] Examples of high molecular weight hindered amine compounds are listed in Table 2 below:

[0188] Table 2

[0189]

[0190]

[0191] "n" in formulae (b1) to (b6) of Table 2 represents the number of repeating units in the polymer, and is generally an integer equal to or greater than 4.

[0192] Among these high molecular weight compounds, the hindered amine is preferably selected from those corresponding to formula (b2) and (b5). More preferably, the high molecular weight hindered amine is a hindered amine corresponding to formula (b2).

[0193] If used, hindered amine compounds are generally present in an amount advantageously of at least 0.01 wt%, more preferably at least 0.05 wt%, still more preferably at least 0.1 wt%, based on the total weight of the composition.

[0194] Similarly, when a hindered amine compound is present, it is also generally advantageously present in an amount of up to 3.5 weight percent, preferably up to 3 weight percent, more preferably up to 2.5 weight percent, still more preferably up to 2.0 weight percent, even more preferably up to 0.8 weight percent and most preferably up to 0.6 weight percent, based on the total weight of the composition.

[0195] Hindered phenol compounds

[0196] The expression "hindered phenol compound" is used according to its customary meaning in the art and is generally intended to mean derivatives of ortho-substituted phenol, especially (but not limited to) di-tert-butylphenol derivatives well known in the art.

[0197] Examples of hindered phenol compounds are listed in Table 3 below:

[0198] Table 3

[0199]

[0200]

[0201]

[0202] A particularly effective hindered phenol compound in composition (C) has been found to be N,N'-hexane-1,6-diylbis(3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)) of formula (d4) as described above.

[0203] If used, hindered phenol compounds are generally present in an amount advantageously of at least 0.01 weight percent, more preferably at least 0.05 weight percent, still more preferably at least 0.1 weight percent, based on the total weight of the composition.

[0204] Similarly, when a hindered phenol compound is present, it is also generally advantageously present in an amount of up to 3.5 weight percent, preferably up to 3 weight percent, more preferably up to 2.5 weight percent, still more preferably up to 2.0 weight percent, even more preferably up to 0.8 weight percent and most preferably up to 0.6 weight percent, based on the total weight of the composition.

[0205] Polyols

[0206] The stabilizer (S) may be at least one polyol (PHA).

[0207] The expressions "polyol" and "PHA" are used in the context of the present invention to denote organic compounds containing three or more hydroxyl groups in the molecule. The PHA may be aliphatic, cycloaliphatic, araliphatic or aromatic and may contain one or more than one heteroatom (including N, S, O, halogen and / or P) and may contain additional functional groups (in addition to hydroxyl groups), such as ether, amine, carboxylic acid, amide or ester groups.

[0208] According to a preferred embodiment, when PHA is used as stabilizer (S), it conforms to the formula R-(OH) n (I)

[0209] in:

[0210] - n is an integer from 3 to 8, preferably an integer from 4 to 8; and

[0211] -R is C1-C 36 Hydrocarbon.

[0212] Typically, the hydroxyl groups of PHAs are bonded to aliphatic carbon atoms; in other words, PHAs are typically not phenolic compounds.

[0213] Furthermore, it is generally preferred that the hydroxyl group is not sterically hindered. For this purpose, the carbon atom in the alpha position to the aliphatic carbon bearing the hydroxyl group generally contains no sterically hindering substituents, and more specifically, it contains no branched aliphatic groups.

[0214] PHA compounds which are particularly suitable as stabilizers (S) within the scope of the present invention are in particular:

[0215] -triols, in particular selected from glycerol, trimethylolpropane, trimethylolbutane, 2,3-bis(2'-hydroxyethyl)-cyclohexan-1-ol, hexane-1,2,6-triol, 1,1,1-tri(hydroxymethyl)ethane, 3-(2'-hydroxyethoxy)propane-1,2-diol, 3-(2'-hydroxypropoxy)-propane-1,2-diol, 2-(2'-hydroxyethoxy)-hexane-1,2-diol, 6-(2'-hydroxypropoxy)-hexane-1,2-diol, 1,1,1-tri- [(2'-hydroxyethoxy)-methylethane, 1,1,1-tris-[(2'-hydroxypropoxy)-methyl-propane, 1,1,1-tris-(4'-hydroxyphenyl)ethane, 1,1,1-tris-(hydroxyphenyl)-propane, 1,1,5-tris-(hydroxyphenyl)-3-methylpentane, trimethylolpropane ethoxylate, trimethylolpropane propoxylate, tris(hydroxymethyl)aminomethane, N-(2-hydroxy-1,1-bis(hydroxymethyl)ethyl)glycine (also known as tricosin) and its salts;

[0216] - tetraols, in particular chosen from diglycerol, di(trimethylolpropane), pentaerythritol, 1,1,4-tris-(dihydroxyphenyl)-butane;

[0217] - polyols containing 5 hydroxyl groups, in particular triglycerides;

[0218] - polyols containing 6 hydroxyl groups, in particular dipentaerythritol;

[0219] - polyols containing 8 hydroxyl groups, in particular tripentaerythritol;

[0220] - carbohydrate polyols, in particular selected from cyclodextrins, D-mannose, glucose, galactose, sucrose, fructose, arabinose, D-mannitol, D-sorbitol, D- or L-arabitol, xylitol, iditol, talitol, altritol, sorbitol (gulitol), erythritol, threitol, D-gulono-1,4-lactone.

[0221] PHAs which have been found to provide particularly good results within the scope of the present invention are diglycerol, triglycerol, pentaerythritol, dipentaerythritol (DPE), tripentaerythritol (TPE) and di(trimethylolpropane), of which dipentaerythritol (DPE) and tripentaerythritol (TPE) are preferred, and dipentaerythritol (DPE) is particularly preferred.

[0222] It is also understood that the PHA may be reacted with polyamide (A) and / or polyamide (B).

[0223] Thus, it is generally understood that when the stabilizer is or comprises a PHA, embodiments in which at least a portion of the PHA is bonded to the polyamide (A) and / or the polyamide (B) are still within the scope of the present invention.

[0224] According to these latter embodiments, the fraction of PHA that can thus be bound to the polyamide molecule is at least 50 mol %, preferably at least 70 mol % and even more preferably at least 80 mol %, relative to the total number of moles of PHA used.

[0225] When PHA is used as stabilizer (S), it is present in an amount of at least 0.1 wt.-%, preferably at least 0.5 wt.-%, even more preferably at least 0.75 wt.-% and at most 3.5 wt.-%, preferably at most 3 wt.-%, even more preferably at most 2.5 wt.-%, relative to the weight of polyamide (A).

[0226] When at least part of the PHA is chemically bonded to polyamide (A) and / or polyamide (B), it is understood that composition (C) will contain, if any, less than 2% by weight, preferably less than 1.5% by weight, more preferably less than 1% by weight of non-chemically bonded PHA, relative to the total weight of composition (C).

[0227] Phosphorus compounds

[0228] The stabilizer (S) may be at least one phosphorus compound selected from the group consisting of hypophosphites, phosphites, phosphonites of alkali metals or alkaline earth metals and mixtures thereof.

[0229] Sodium hypophosphite and calcium hypophosphite are preferred alkali metal or alkaline earth metal hypophosphites.

[0230] Phosphites can be represented by the formula P(OR)3, while phosphonites can be represented by the formula P(OR)2R, wherein each R can be the same or different and is generally independently selected from C 1-20 Alkyl, C 3-22 Alkenyl, C 6-40 Cycloalkyl, C 7-40 Cycloalkylene, aryl, alkaryl or arylalkyl moiety.

[0231] Examples of phosphites are listed in Table 4 below:

[0232] Table 4

[0233]

[0234]

[0235]

[0236] Examples of phosphonites are listed in Table 5 below:

[0237] Table 5

[0238]

[0239] When a phosphorus compound is used in composition (C), it is preferably present in an amount of at least 0.01 wt%, more preferably at least 0.05 wt%, based on the total weight of the composition.

[0240] The phosphorus compound is also preferably present in an amount of at most 1 wt%, more preferably at most 0.5 wt%, still more preferably at most 0.25 wt%, based on the total weight of the composition.

[0241] Filler(F)

[0242] The composition optionally comprises 0 to 60% by weight, preferably 10 to 50% by weight, of one or more than one filler (F).

[0243] The filler (F) may be any reinforcing agent, but is preferably selected from calcium carbonate, glass fiber, glass flakes, glass beads, carbon fiber, talc, mica, wollastonite, calcined clay, kaolin, diatomaceous earth, magnesium sulfate, magnesium silicate, barium sulfate, titanium dioxide, sodium aluminum carbonate, barium ferrite, potassium titanate.

[0244] Therefore, from the morphological point of view, the filler (F) can be selected from fibrous fillers and particulate fillers.

[0245] Preferably, the filler is selected from fibrous fillers. Among the fibrous fillers, glass fibers are preferred; they include chopped strand A-glass fibers, E-glass fibers, C-glass fibers, D-glass fibers, S-glass fibers and R-glass fibers. Glass fibers with circular and non-circular cross sections can be used. The expression "glass fibers with non-circular cross sections" is used in this article according to its usual meaning, that is, it is intended to refer to glass fibers with cross sections, which have a main axis perpendicular to the longitudinal direction of the glass fibers and corresponding to the longest straight-line distance in the cross section, and a minor axis corresponding to the straight-line distance in the cross section perpendicular to the main axis direction. The non-circular cross section of the fiber can have a variety of shapes, including cocoon-shaped, rectangular, elliptical, polygonal, rectangular, but this enumeration is not exhaustive. The ratio of the length of the major axis to the minor axis is preferably between about 1.5:1 and about 6:1, more preferably between about 2:1 and about 5:1, and more preferably between about 3:1 and about 4:1.

[0246] In a preferred embodiment, glass fibers, and more particularly round cross-section glass fibers, are used as filler (F).

[0247] The composition (C) will comprise preferably at least 15% by weight, more preferably at least 20% by weight, of filler (F) as detailed above, relative to the total weight of the composition (C).

[0248] However, composition (C) generally comprises at most 60%, preferably at most 55% and even more preferably at most 50% by weight of filler (F) as detailed above, relative to the total weight of composition (C).

[0249] Particularly good results are obtained when the composition (C) comprises from about 10 to about 40% by weight of a filler (F) as detailed above, relative to the total weight of the composition (C).

[0250] Rubber (I)

[0251] The composition (C) optionally comprises 0 to 30% by weight, preferably 0 to 20% by weight, of at least one impact-modified rubber [rubber (I)].

[0252] The rubber (I) suitable for the composition (C) generally comprises at least one functional group capable of reacting with the polyamide (A), more particularly with the amine or carboxylic acid end groups of the polyamide (A) [functionalized rubber (IF)].

[0253] The functional groups of the functionalized rubber (IF) are generally selected from carboxylic acid groups and their derivatives (including especially salts and esters); epoxy groups; anhydride groups, oxazoline groups, maleimide groups or mixtures thereof.

[0254] The functionalized rubber (IF) can be an oligomeric or polymeric compound in which the functional groups can be introduced by copolymerizing the functional monomers during the polymerization of the impact modifier backbone or by grafting a preformed polymer backbone.

[0255] The functionalized rubber (IF) generally comprises repeating units derived from at least one of the following monomers: ethylene; higher α-olefins, including propylene, butene, octene; dienes, including butadiene and isoprene; acrylates, styrene, acrylonitrile; (meth)acrylic acid and its derivatives, including esters; vinyl monomers, including vinyl acetate and other vinyl esters. Other monomers may also be included in the structure of the functionalized rubber (IF).

[0256] The polymer backbone of the functionalized rubber (IF) is usually selected from elastomeric backbones comprising polyethylene and its copolymers, such as ethylene-butene; ethylene-octene; polypropylene and its copolymers; polybutene; polyisoprene; ethylene-propylene-rubber (EPR); ethylene-propylene-diene monomer rubber (EPDM); ethylene-acrylate rubber; butadiene-acrylonitrile rubber, ethylene-acrylic acid (EAA), ethylene-vinyl acetate (EVA); acrylonitrile-butadiene-styrene rubber (ABS), block copolymer styrene ethylene butadiene styrene (SEBS); block copolymer styrene butadiene styrene (SBS); methacrylate-butadiene-styrene (MBS) type core-shell elastomers, or a mixture of one or more of the above.

[0257] It should be understood that in the case where no functional groups are included in the polymer backbone, the functionalized rubber (IF) will further introduce residues from functional monomers by copolymerization or grafting, including any carboxylic acid group and its derivatives (especially including salts and esters); epoxy group; anhydride group, oxazoline group, maleimide group or mixtures thereof. It is further envisioned that the functional monomers can be used to further modify the backbone that may already contain functional groups.

[0258] Specific examples of functionalized rubbers (IF) are, in particular, terpolymers of ethylene, acrylate and glycidyl methacrylate, copolymers of ethylene and butyl acrylate; copolymers of ethylene, butyl acrylate and glycidyl methacrylate; ethylene-maleic anhydride copolymers; EPR grafted with maleic anhydride; styrene-maleimide copolymers grafted with maleic anhydride; SEBS copolymers grafted with maleic anhydride; styrene-acrylonitrile copolymers grafted with maleic anhydride; ABS copolymers grafted with maleic anhydride.

[0259] Functionalized rubbers (IF) which have been found to be particularly effective within the scope of the present invention are amorphous copolymers of ethylene grafted with maleic anhydride.

[0260] When said rubber (I) is present, its amount is generally at least 1 wt.%, preferably 2 wt.%, more preferably at least 3 wt.%, more preferably at least 4 wt.%, relative to the total weight of the composition (C). However, its amount is generally at most 30 wt.%, preferably at most 15 wt.%, more preferably at most 10 wt.%, even more preferably at most 8 wt.%, relative to the total weight of the composition (C).

[0261] Other Ingredients

[0262] Composition (C) may also contain other conventional additives commonly used in the art, including lubricants, plasticizers, colorants, pigments, antistatic agents, flame retardants, nucleating agents, catalysts, etc. When these ingredients are present, they are present in an amount of up to 30% by weight, preferably up to 20% by weight, more preferably up to 10% by weight, even more preferably up to 8% by weight, relative to the total weight of composition (C). Typical amounts depend on the specific conventional additives selected for introduction into composition (C) and will be selected by a person skilled in the art according to conventional practice.

[0263] Preparation of composition (C)

[0264] The present invention also relates to a process for preparing a composition (C) as described above in detail, said process comprising melt blending polyamide (A), polyamide (B), stabilizer (S) and any other optional ingredients.

[0265] Any melt blending method can be used to mix the polymeric composition and non-polymeric composition of the present invention.For example, the polymeric composition and non-polymeric composition can be fed into a melt mixer, such as a single screw extruder or a twin screw extruder, agitator, a single screw or a twin screw kneader or a Banbury (Banbury) mixer, and the addition step can be to add all the components at once or to add them stepwise in batches.When the polymeric composition and non-polymeric composition are added stepwise in batches, a part of the polymeric composition and / or the non-polymeric composition is first added, and then melt-mixed with the remaining polymeric composition and non-polymeric composition added subsequently, until a fully mixed composition is obtained.If the enhanced filler presents a long physical shape (for example, long glass fiber), the enhanced composition can be prepared using stretch extrusion molding.

[0266] Use of the composition (C)

[0267] The composition (C) as described above can be used to increase the long-term thermal stability at high temperatures and improve the fatigue resistance of molded or extruded articles made therefrom. The long-term thermal stability of the article can be evaluated by exposing a 4 mm thick test sample in an oven at different test temperatures for different test time periods (air oven aging). The oven test temperature of the composition disclosed herein includes 200°C and a test time of up to 2000 hours. After the test sample is aged in the air oven, the tensile modulus, tensile strength at break and elongation at break are tested according to the ISO 527-2 / 1A test method; and compared with a molded unexposed control having the same composition and shape. Comparison with the molded control provides the retention rate of tensile strength and / or the retention rate of elongation at break, so that the long-term thermal stability performance of various compositions can be evaluated.

[0268] The mechanical durability of articles made from composition (C) can be evaluated by the hot air pressure pulsation test described in the examples below.

[0269] In various embodiments, composition (C) has a retention of 200°C / 1000 hours tensile strength of at least 60%, preferably at least 70%, based on comparison to a molded unexposed control.

[0270] In another aspect, the present invention relates to the use of the composition (C) disclosed above for high temperature applications.

[0271] In yet another aspect, the present invention relates to a method for preparing an article by shaping the composition (C) of the present invention. Examples of articles are films, yarns, fibers, laminates, automotive parts or engine parts or electrical / electronic parts. "Shaping" refers to any shaping technique, such as extrusion, injection molding, thermoplasticization, compression molding or blow molding. Preferably, the article is shaped by injection molding or blow molding.

[0272] The molded or extruded thermoplastic articles disclosed herein can be applied to numerous vehicle parts that meet one or more of the following requirements: high impact requirements; significant weight reduction (e.g., relative to traditional metals); high temperature resistance; oil environment resistance; chemical resistance, such as coolants; and noise reduction, enabling more compact and integrated designs. Specific molded or extruded thermoplastic articles are selected from charge air coolers (CACs); cylinder head covers (CHCs); oil pans; engine cooling systems, including thermostats and heater housings and coolant pumps; exhaust systems, including mufflers and catalytic converter housings; intake manifolds (AIMs); and timing chain belt front covers. As an illustrative example of the desired mechanical resistance to long-term high temperature exposure, charge air coolers can be mentioned. Charge air coolers are part of the vehicle radiator and can improve engine combustion efficiency. Charge air coolers reduce charge air temperature and increase the density of compressed air in turbochargers, allowing more air to enter the cylinders to improve engine efficiency. Since the temperature of the incoming air may exceed 200°C when entering the charge air cooler, it is required that the component be made of a composition that maintains good mechanical properties for a long time at high temperatures.

[0273] If the disclosure of any patents, patent applications, and publications incorporated herein by reference conflicts with the description of the present application so as to render a term unclear, the present description shall control.

[0274] The present invention is further described by the following examples. It should be understood that the following examples are for illustrative purposes only and are not intended to limit the present invention.

[0275] analyze

[0276] The viscosity number (VN) (unit: mL / g) was measured in a formic acid solution according to ISO 307 standard.

[0277] The carboxylic acid end group (CEG) concentration and the amine end group (AEG) concentration (unit: meq / kg) were determined by potentiometric titration.

[0278] Melting temperature (T m ) and enthalpy (ΔH m ), crystallization temperature (T c ) was determined by differential scanning calorimetry (DSC) using a Mettler DSC3 at 10°C / min.

[0279] Example 1

[0280] The polymer (B) of the invention was synthesized by polymerizing ε-caprolactam in the presence of bis(hexamethylene)triamine, water (30 wt %) in a stainless steel kettle equipped with a mechanical stirrer in the following molar ratio: n(bis(hexamethylene)triamine) / n(ε-caprolactam)=0.0042, R=0. The mixture was gradually heated to a maximum of 245°C at 17.5 bar while water was distilled. The pressure was then gradually reduced to atmospheric pressure. The pressure was then gradually set to 500 mbar over 45 minutes and the temperature was maintained at 245°C. The vacuum was then broken and the polymer was extruded, cooled in a water bath and granulated. The oligomers were removed by washing several times in hot water so that the residual content of caprolactam was less than 0.3 wt %. Finally, the granules were dried before analysis.

[0281] The branched polyamide has the following characteristics:

[0282] VN = 108 mL / g, AEG = 154 meq / kg, CEG = 38 meq / kg; therefore, the AEG-CEG value is 116 meq / kg. Corresponding Mn = 12700 g / mol, IP = 1.7. Melting temperature T m =221℃.

[0283] Example 2

[0284] The polymer (B) of the present invention was synthesized by polymerizing ε-caprolactam in the presence of bis(hexamethylene)triamine, H3PO4 (370 ppm monomer mixture) as catalyst, water (30 wt%) in a stainless steel kettle equipped with a mechanical stirrer in the following molar ratio: n(bis(hexamethylene)triamine) / n(ε-caprolactam)=0.0042, R=0. The mixture was gradually heated to 250°C at 17.5 bar while water was distilled. The pressure was then gradually reduced to atmospheric pressure, the temperature was raised to 260°C, and then kept stirring for 1 hour. The polymer was then extruded, cooled in a water bath and granulated. The oligomers were removed by washing several times in hot water so that the residual content of caprolactam was less than 0.3 wt%. Finally, the granules were dried before analysis.

[0285] The branched polyamide has the following characteristics:

[0286] VN = 117 mL / g, AEG = 138 meq / kg, and CEG = 20 meq / kg; therefore the AEG-CEG value is 119 meq / kg. Corresponding Mn = 16500 g / mol, IP = 1.6. Melting temperature T m =220℃.

[0287] Example 3

[0288] Similar to Example 2, the polymer (B) of the present invention was synthesized by polymerizing ε-caprolactam in the presence of bis(hexamethylene)triamine, adipic acid, H3PO4 (370 ppm of monomer mixture) as a catalyst, and water (30 wt%) having the following molar ratios: n(bis(hexamethylene)triamine) / n(ε-caprolactam)=0.008, R=n(adipic acid) / n(bis(hexamethylene)triamine)=0.5.

[0289] The branched polyamide has the following characteristics:

[0290] VN = 146 mL / g, AEG = 163 meq / kg, and CEG = 20 meq / kg; therefore the AEG-CEG value is 144 meq / kg. Corresponding Mn = 20700 g / mol, IP = 3.0. Melting temperature T m =216℃.

[0291] Example 4

[0292] Similar to Example 2, the polymer (B) of the present invention was synthesized by polymerizing ε-caprolactam in the presence of bis(hexamethylene)triamine, adipic acid, H3PO4 (370 ppm of monomer mixture) as a catalyst, and water (30 wt%) having the following molar ratios: n(bis(hexamethylene)triamine) / n(ε-caprolactam)=0.014, R=n(adipic acid) / n(bis(hexamethylene)triamine)=0.5.

[0293] The branched polyamide has the following characteristics:

[0294] VN = 100 mL / g, AEG = 273 meq / kg, CEG = 15 meq / kg; therefore, the AEG-CEG value is 257 meq / kg. Corresponding Mn = 13600 g / mol, IP = 2.8. Melting temperature T m =215℃.

[0295] Example 5

[0296] The polymer (B) of the present invention was synthesized by polymerizing ε-caprolactam in the presence of bis(hexamethylene)triamine, adipic acid, H3PO4 (370 ppm monomer mixture) as a catalyst, water (30 wt%) in the following molar ratios: n(bis(hexamethylene)triamine) / n(ε-caprolactam)=0.020, R=n(adipic acid) / n(bis(hexamethylene)triamine)=0.7. Here, the finishing step was maintained at atmospheric pressure, 260° C. with stirring for half an hour.

[0297] The branched polyamide has the following characteristics:

[0298] VN = 105 mL / g, AEG = 298 meq / kg, CEG = 18 meq / kg; therefore, the AEG-CEG value is 280 meq / kg. Corresponding Mn = 16500 g / mol, IP = 4.7. Melting temperature T m =213℃.

[0299] Example 6

[0300] Analogously to Example 2, the polymer (B) of the invention was synthesized by polymerizing ε-caprolactam in the presence of bis(hexamethylene)triamine, adipic acid, H3PO4 (370 ppm monomer mixture) as a catalyst, water (30 wt%) in the following molar ratios: n(bis(hexamethylene)triamine) / n(ε-caprolactam)=0.020, R=n(adipic acid) / n(bis(hexamethylene)triamine)=0.7. Here, the finishing step was carried out at 260° C. under a vacuum of 60 mbar and maintained under stirring for half an hour.

[0301] The branched polyamide has the following characteristics:

[0302] VN = 168 mL / g, AEG = 288 meq / kg, CEG = 3 meq / kg; therefore, the AEG-CEG value is 285 meq / kg. Corresponding Mn = 17800 g / mol, IP = 4.5. Melting temperature T m =215℃.

[0303] Comparative Example 1

[0304] Analogously to Example 1, branched PA6 was synthesized by polymerizing ε-caprolactam in the presence of bis(hexamethylene)triamine, adipic acid, H3PO4 (370 ppm monomer mixture) as a catalyst, water (30 wt%) in the following molar ratios: n(bis(hexamethylene)triamine) / n(ε-caprolactam)=0.040, R=n(adipic acid) / n(bis(hexamethylene)triamine)=0.75. Here, the finishing step was carried out at atmospheric pressure and 245° C. for 1 hour.

[0305] The branched polyamide has the following characteristics:

[0306] VN = 119 mL / g, AEG = 491 meq / kg and CEG = 10 meq / kg; therefore the AEG-CEG value is 481 meq / kg. Corresponding Mn = 11200 g / mol, IP = 5.4. Melting temperature T m =210℃.

[0307] Other raw materials used for compounding.

[0308] Polyamide compounds are prepared using the following ingredients:

[0309] PA6 S27 is a linear PA6 from Solvay synthesized by polymerizing ε-caprolactam in the presence of acetic acid as end-capping agent and then removing oligomers by washing in water, having: VN=142 mL / g, AEG=37 meq / kg, CEG=54 meq / kg; thus the AEG-CEG value is -17 meq / kg.

[0310] Acid-branched PA6 SX16 from Solvay is a branched PA6 synthesized by polymerizing ε-caprolactam in the presence of 2,2,6,6-tetra(carboxyethyl)cyclohexanone as a branching agent and then removing oligomers by water washing, having: VN=104 mL / g, AEG=16 meq / kg, CEG=180 meq / kg; therefore, the AEG-CEG value is -164 meq / kg.

[0311] The glass fibers were from Owens Corning and had a diameter of 10 μm (OCV 990).

[0312] The stabilizer bag contained 1.76% Cu2O, 24.56% KBr, 23.68% carbon black, 23.68% aniline black and 26.32% lubricant LT107.

[0313] General process steps for composite extrusion.

[0314] Before compounding, the polyamide pellets were dried to reduce the water content to less than 1500 ppm. The compositions were obtained by melt blending the selected ingredients in a Werner & Pleifeder ZSK 40 twin-screw extruder using the following parameters: 35 kg / hour, 230 rpm, 5 heating zones: 235°C, 240°C, 245°C, 250°C, 255°C. All ingredients were fed at the start of the extruder. The extruder strands were cooled in a water bath, then pelletized and the pellets obtained were stored in sealed aluminum lined bags to prevent moisture absorption. Table 6 gives the composition of the composites.

[0315] Table 6

[0316]

[0317]

[0318] Methodological procedures for evaluating heat aging resistance.

[0319] The composition was injection molded using a DEMAG H270.50 injection molding machine with a barrel temperature of about 250°C and a mold temperature set at 85°C to prepare 4 mm thick ISO527 specimens. The initial mechanical properties before aging (tensile modulus (E), tensile strength at break (TS) and elongation at break) were characterized by tensile measurements at 23°C and 170°C according to ISO 527 / 1A. The average value of 5 specimens was taken.

[0320] The samples were then heat aged in a circulating air oven (Heraeus TK62210) set at 200°C. After aging for 1000 and 2000 hours, the samples were removed from the oven, allowed to cool to room temperature and placed in sealed aluminum lined bags in preparation for testing. Mechanical properties were then measured at 23°C and 170°C according to ISO 527 / 1A. Table 7 shows that CE4 and E7 exhibit higher heat aging resistance compared to CE2 and CE3.

[0321] Table 7

[0322]

[0323]

[0324] Hot air pressure pulsation test description

[0325] The box-shaped parts were molded using a Ferromatik K-Tec 200 injection molding machine with a barrel temperature of approximately 255°C and a mold temperature set at 85°C. The parts were then placed in an oven set at 130°C and subjected to hot air cyclic pulses inside the box-shaped parts, with an air temperature of 220°C and a pressure varying sinusoidally between 0.1 and 2.3 bar at 1Hz. The hot air pressure pulses were repeated until the part broke, and the number of cycles to failure was taken as an indicator of the mechanical durability of the material. Repeatability tests were performed on 3 parts of each product.

[0326] The data in Tables 7 and 8 show that only E7 has both heat aging resistance and pressure pulsation resistance.

[0327] Table 8

[0328] Number of cycles to failure CE3 CE4 E7 The first sample 1 452 620 289 500 2 005 190 The second sample 1 758 510 375 070 2 048 860 The third sample 1 869 940 874 500 2 040 000 Mean number of cycles to failure 1 693 000 513 000 2 031 000

Claims

1. A polyamide composition (C), comprising: - 0 to 30% by weight of at least one polyamide (A); - from more than 60% to 99.99% by weight of at least one branched polyamide different from polyamide (A), said branched polyamide comprising repeating units derived from the polycondensation of a mixture (B) comprising: - at least one trifunctional or tetrafunctional polyamine monomer, i.e. monomer (FN), comprising three or four secondary amine groups selected from the group consisting of -NH- and -NH 2 The amine functional group of the primary amine group, and -ε-caprolactam or its derivatives; in, When the monomer (FN) is a trifunctional polyamine monomer, the amount of the monomer (FN) is such that the molar ratio of the monomer (FN) / ε-caprolactam or its derivative is at least 0.002 and at most 0.030, and When the monomer (FN) is a tetrafunctional polyamine monomer, the amount of the monomer (FN) is such that the molar ratio of the monomer (FN) / ε-caprolactam or its derivative is at least 0.001 and at most 0.030; The branched polyamide, polyamide (B), has an amine end group (AEG) concentration and a carboxyl end group (CEG) concentration such that the difference AEG-CEG is greater than 100 meq / kg and at most 300 meq / kg; and - 0.01 to 3.5% by weight of at least one thermal stabilizer, i.e. stabilizer (S), - optionally, 0 to 60% by weight of at least one filler (F); - optionally, 0 to 30% by weight of at least one impact-modified rubber (I); - optionally, 0 to 30% by weight of other conventional additives, The above weight % is relative to the total weight of the composition (C), and the sum of the weight percentages of the components of the composition (C) is 100%.

2. The composition (C) according to claim 1, wherein the polyamide (A) is obtained by condensation reaction of at least one mixture selected from the group consisting of: a mixture (M1) comprising at least one diacid, i.e. an acid (DA) or a derivative thereof and at least one diamine, i.e. an amine (NN) or a derivative thereof; - a mixture (M2) comprising at least one lactam (L); - a mixture (M3) comprising at least one aminocarboxylic acid, ie an amino acid (AN); and - combinations thereof.

3. The composition according to claim 2, wherein the polyamide (A) is obtained by condensation reaction of at least one mixture (M1) selected from: - a mixture of adipic acid and 1,6-diaminohexane; - a mixture of adipic acid, terephthalic acid and 1,6-diaminohexane; - a mixture of sebacic acid and 1,6-diaminohexane, - a mixture of terephthalic acid and 1,10-diaminodecane, - a mixture of adipic acid, terephthalic acid and 1,10-diaminodecane, - A mixture of adipic acid and 1,10-diaminodecane.

4. Composition (C) according to any one of the preceding claims, wherein the monomer (FN) is selected from tris(aminoalkyl)amines; polyoxyalkylenetriamines; polyalkylenepolyamines.

5. The composition (C) according to claim 4, wherein the tris(aminoalkyl)amine is tris(2-aminoethyl)amine (TREN).

6. The composition (C) according to claim 4, wherein the polyoxyalkylene triamine is Jeffamine from Huntsman 7. The composition (C) according to claim 6, wherein the Jeffamine For Jeffamine 8. Composition (C) according to claim 4, wherein the polyalkylene polyamine is a polyethylene imine, which may advantageously have a variable molecular weight.

9. The composition (C) according to any one of claims 1 to 3, wherein the monomer (FN) is selected from 1,8-diamino-4-aminomethyl-octane (TAN), dialkylene triamines, and cyclohexane-1,3,5-triamine.

10. Composition (C) according to claim 9, wherein the dialkylene triamine is selected from diethylene triamine (DETA) and bis (hexamethylene) triamine (BHT).

11. The composition (C) according to any one of claims 1 to 3, wherein the monomer (FN) is selected from bis(hexamethylene)triamine (BHT), tris(2-aminoethyl)amine (TREN), 1,8-diamino-4-aminomethyloctane (TAN) and combinations thereof.

12. Composition (C) according to any one of claims 1 to 3, wherein the mixture (B) does not contain any diamine, ie amine (NN).

13. Composition (C) according to claim 12, wherein the amount of acid (DA) present in mixture (B) is such that the molar ratio of acid (DA) / monomer (FN) does not exceed the limit 0.44+1 / x, where x is the number of said amine groups in monomer (FN).

14. The composition (C) according to any one of claims 1 to 3, wherein the stabilizer (S) is selected from the group consisting of copper-containing stabilizers, hindered amine compounds, hindered phenol compounds, polyols (PHA) and phosphorus compounds.

15. The composition (C) according to claim 14, wherein the stabilizer (S) comprises at least one copper-containing stabilizer.

16. The composition (C) according to claim 15, wherein the copper-containing stabilizer comprises a copper compound and an alkali metal halide (M).

17. The composition (C) according to claim 15, wherein the copper-containing stabilizer comprises a copper compound and an alkali metal halide (M), and the atomic weight ratio of the copper compound:alkali metal halide is 1:99 to 30:

70.

18. The composition (C) according to claim 17, wherein the atomic weight ratio of the copper compound:alkali metal halide is 5:95 to 20:

80.

19. A method for preparing an article by shaping the composition (C) according to any one of claims 1 to 18 by any shaping technique.

20. The method of claim 19, wherein the molding technique is selected from the group consisting of extrusion, injection molding, thermoplasticization, compression molding, and blow molding.

21. The method of claim 19, wherein the article is any one of a film, a yarn, a fiber, a laminate, an automobile part, an engine part, and an electrical / electronic part.

22. A method for preparing a polyamide composition (C), the polyamide composition (C) comprising: - 0 to 30% by weight of at least one polyamide (A); - from more than 60% to 99.99% by weight of at least one branched polyamide different from polyamide (A), said branched polyamide comprising repeating units derived from the polycondensation of a mixture (B) comprising: - at least one trifunctional or tetrafunctional polyamine monomer, i.e. monomer (FN), comprising three or four secondary amine groups selected from the group consisting of -NH- and -NH 2 The amine functional group of the primary amine group, and -ε-caprolactam or its derivatives; in, When the monomer (FN) is a trifunctional polyamine monomer, the amount of the monomer (FN) is such that the molar ratio of the monomer (FN) / ε-caprolactam or its derivative is at least 0.002 and at most 0.030, and When the monomer (FN) is a tetrafunctional polyamine monomer, the amount of the monomer (FN) is such that the molar ratio of the monomer (FN) / ε-caprolactam or its derivative is at least 0.001 and at most 0.030; The branched polyamide, polyamide (B), has an amine end group (AEG) concentration and a carboxyl end group (CEG) concentration such that the difference AEG-CEG is greater than 100 meq / kg and at most 300 meq / kg; and - 0.01 to 3.5% by weight of at least one thermal stabilizer, i.e. stabilizer (S), - optionally, 0 to 60% by weight of at least one filler (F); - optionally, 0 to 30% by weight of at least one impact-modified rubber (I); - optionally, 0 to 30% by weight of other conventional additives, The above weight % is relative to the total weight of the composition (C), and the sum of the weight percentages of the components of the composition (C) is 100%, The method comprises melt blending polyamide (A), polyamide (B), a heat stabilizer and any other optional ingredients.

23. The method according to claim 22, wherein the polyamide (A) is obtained by condensation reaction of at least one mixture selected from the group consisting of: a mixture (M1) comprising at least one diacid, i.e. an acid (DA) or a derivative thereof and at least one diamine, i.e. an amine (NN) or a derivative thereof; - a mixture (M2) comprising at least one lactam (L); - mixtures (M3) comprising at least one aminocarboxylic acid, ie amino acid (AN); and - combinations thereof.

24. The method according to claim 23, wherein the polyamide (A) is obtained by condensation reaction of at least one mixture (M1) selected from: - a mixture of adipic acid and 1,6-diaminohexane; - a mixture of adipic acid, terephthalic acid and 1,6-diaminohexane; - a mixture of sebacic acid and 1,6-diaminohexane, - a mixture of terephthalic acid and 1,10-diaminodecane, - a mixture of adipic acid, terephthalic acid and 1,10-diaminodecane, - A mixture of adipic acid and 1,10-diaminodecane.

25. The method according to any one of claims 22 to 24, wherein the monomer (FN) is selected from tris(aminoalkyl)amines; polyoxyalkylenetriamines; polyalkylenepolyamines.

26. The method of claim 25, wherein the tris(aminoalkyl)amine is tris(2-aminoethyl)amine (TREN).

27. The method of claim 25, wherein the polyoxyalkylene triamine is Jeffamine from Huntsman 28. The method according to claim 27, wherein the Jeffamine For Jeffamine 29. The method of claim 25, wherein the polyalkylene polyamine is a polyethylene imine, which may advantageously have a variable molecular weight.

30. The method according to any one of claims 22 to 24, wherein the monomer (FN) is selected from 1,8-diamino-4-aminomethyl-octane (TAN), dialkylene triamines, and cyclohexane-1,3,5-triamine.

31. The method of claim 30, wherein the dialkylene triamine is selected from diethylene triamine (DETA) and bis (hexamethylene) triamine (BHT).

32. The method according to any one of claims 22 to 24, wherein the monomer (FN) is selected from bis(hexamethylene)triamine (BHT), tris(2-aminoethyl)amine (TREN), 1,8-diamino-4-aminomethyloctane (TAN) and combinations thereof.

33. The process according to any one of claims 22 to 24, wherein the mixture (B) additionally comprises at least one diacid, acid (DA) and / or at least one diamine, amine (NN).

34. The process according to any one of claims 22 to 24, wherein the mixture (B) does not contain any diamine, ie amine (NN).

35. The process according to claim 33, wherein the amount of acid (DA) present in mixture (B) is such that the molar ratio of acid (DA) / monomer (FN) does not exceed the limit 0.44+1 / x, wherein x is the number of said amine groups in monomer (FN).

36. The method according to any one of claims 22 to 24, wherein the stabilizer (S) is selected from copper-containing stabilizers, hindered amine compounds, hindered phenol compounds, polyols (PHA) and phosphorus compounds.

37. The method according to claim 36, wherein the stabilizer (S) comprises at least one copper-containing stabilizer.

38. The method of claim 37, wherein the copper-containing stabilizer comprises a copper compound and an alkali metal halide (M).

39. The method according to claim 37, wherein the copper-containing stabilizer comprises a copper compound and an alkali metal halide (M), and the atomic weight ratio of the copper compound:alkali metal halide is 1:99 to 30:

70.

40. The method of claim 39, wherein the atomic weight ratio of the copper compound:alkali metal halide is 5:95 to 20:80.

Citation Information

Patent Citations

  • Polyamide compositions with high impact strength at low temperatures

    US4945129A

  • Polyamide composition

    US9856375B2

  • Polyamide, method for its manufacture and compounds containing it

    WO1997024388A1

  • Polyamides with high fluidity, method for making same, compositions comprising said polyamide

    WO1999064496A1