Method for manufacturing SiC semiconductor device and SiC semiconductor device
By forming a growth layer on a SiC single crystal wafer and isolating a part of the SiC semiconductor device, the warpage problem is solved, high-quality and economical SiC semiconductor device manufacturing is achieved, and process stability is improved.
Patent Information
- Application Number
- CN202080065954.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-09-24
AI Technical Summary
In the manufacturing of SiC semiconductor devices, due to the warping problem of SiC single crystal wafers, the difficulty of device manufacturing increases, and problems such as material loss and machine stoppage affect the economy and quality of the process.
High-quality SiC is achieved by forming a growth layer on a SiC single crystal wafer, suppressing the occurrence of warpage, forming a part of the SiC semiconductor device in the growth layer, then separating the part, and using heat treatment and etching steps to eliminate strain and crystal defects. Wafer manufacturing.
It effectively suppresses wafer warpage, improves the quality and economy of SiC semiconductor devices, reduces material loss, and improves the stability of the manufacturing process.
Smart Images

Figure CN114423890B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a SiC semiconductor device and a SiC semiconductor device. Background Art
[0002] Silicon carbide (SiC) has superior material properties such as dielectric breakdown strength, thermal conductivity, and radiation resistance compared to silicon (Si), and is therefore being researched and developed as a material for electronic devices.
[0003] The quality of SiC semiconductor devices is affected by the warpage caused by the internal stress of SiC single crystal wafers. The warpage may make patterning on SiC single crystal wafers difficult, for example. In addition, the warpage may cause suction errors of SiC single crystal wafers, machine stoppages, and cracks of SiC single crystal wafers, which are major factors hindering device manufacturing.
[0004] Therefore, in the manufacture of SiC semiconductor devices, a SiC wafer having a larger substrate thickness than required is sometimes used, and there is room for improvement in terms of economic efficiency.
[0005] Patent document 1 discloses an invention regarding a manufacturing method for manufacturing SiC substrates having an epitaxial layer one by one, the method comprising growing an epitaxial layer on a seed crystal substrate and growing a SiC substrate, and also comprising the step of removing the SiC substrate having the obtained epitaxial layer from the seed crystal substrate.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-24932 Summary of the invention
[0009] Technical problem to be solved by the invention
[0010] However, according to the description of Patent Document 1, since the SiC substrate having the obtained epitaxial layer is sent to the subsequent element manufacturing process, it is difficult to say that the influence of the above-mentioned warpage on the manufacturing process of the SiC semiconductor device can be eliminated.
[0011] In view of the above situation, the technical problem to be solved by the present invention is to provide a high-quality SiC semiconductor device.
[0012] Means used to solve problems
[0013] In order to solve the above problems, the present invention includes: a growth step of forming a growth layer on a workpiece including a SiC single crystal; a device formation step of forming at least a portion of a SiC semiconductor device in the growth layer; and a separation step of separating at least a portion of the SiC semiconductor device from the workpiece. By adopting such a structure, the present invention can separate the SiC wafer including the portion after forming at least a portion of the SiC semiconductor device on a SiC wafer in which wafer warpage is suppressed, thereby achieving the manufacture of SiC semiconductor devices with excellent economic efficiency while suppressing the influence of wafer warpage on SiC processes.
[0014] In a preferred embodiment of the present invention, the growth step heat treats the treated body in an atmosphere containing Si and C. By adopting such a structure, it is possible to manufacture high-quality SiC wafers and SiC semiconductor devices while eliminating or suppressing strain, crystal defects, basal plane dislocations (BPD) and macroscopic step bunching (MSB).
[0015] In a preferred embodiment of the present invention, the growth step heat treats the object to be processed in a quasi-enclosed space where the SiC material is exposed. By adopting such a structure, the present invention can manufacture high-quality SiC wafers and SiC semiconductor devices while eliminating strain, crystal defects, BPD and MSB or suppressing their generation.
[0016] In a preferred embodiment of the present invention, the device forming step performs a patterning step of forming a circuit pattern on the processed object. By adopting such a structure, the present invention can appropriately perform patterning on a SiC wafer with suppressed wafer warpage, and can manufacture a high-quality SiC semiconductor device.
[0017] In a preferred embodiment of the present invention, the device forming step performs a doping step of introducing dopant atoms into the processed object. By adopting such a structure, the present invention can appropriately dope on a SiC wafer with suppressed wafer warpage, and can manufacture a high-quality SiC semiconductor device.
[0018] In a preferred embodiment of the present invention, the device forming step performs an insulating film forming step of introducing an insulating film into the processed object. By adopting such a structure, the present invention can appropriately form an insulating film on a SiC wafer with suppressed wafer warpage, and can manufacture a high-quality SiC semiconductor device.
[0019] In a preferred embodiment of the present invention, the device forming step performs an electrode forming step of forming an electrode on the processed object. By adopting such a structure, the present invention can appropriately form electrodes on a SiC wafer with suppressed wafer warpage, and can manufacture a high-quality SiC semiconductor device.
[0020] In a preferred embodiment of the present invention, the separation step includes: a separation layer forming step of forming a separation layer inside the processed object; and a peeling step of peeling a portion of the processed object starting from the separation layer. By adopting such a structure, the present invention can achieve separation of a SiC wafer including at least a portion of a SiC semiconductor device while suppressing material loss.
[0021] In a preferred embodiment of the present invention, the separation layer forming step forms the separation layer by irradiating the object with laser light so that the inner part becomes a focus. By adopting such a structure, the present invention can form a separation layer in the SiC single crystal as a starting point of peeling flatly.
[0022] In a preferred embodiment of the present invention, an etching step of etching the object by heat-treating the object in an atmosphere containing Si element and C element is performed.
[0023] By adopting such a structure, the present invention can manufacture a high-quality SiC wafer and a SiC semiconductor device while eliminating strain, crystal defects, BPD, and MSB or suppressing their generation.
[0024] In a preferred embodiment of the present invention, the etching step heat treats the object to be processed in a quasi-enclosed space where the SiC material is exposed. By adopting such a structure, the present invention can manufacture high-quality SiC wafers and SiC semiconductor devices while eliminating strain, crystal defects, BPD and MSB or suppressing their generation.
[0025] In a preferred embodiment of the present invention, the separation step, the etching step, and the growth step are sequentially included. By adopting such a structure, the present invention can repeatedly manufacture a higher quality SiC wafer including at least a portion of a SiC semiconductor device, thereby realizing the manufacture of a SiC semiconductor device with excellent economic efficiency.
[0026] In a preferred embodiment of the present invention, the separation step and the growth step are included in sequence. By adopting such a structure, the present invention can repeatedly manufacture high-quality SiC wafers including at least a portion of a SiC semiconductor device, thereby achieving economical manufacturing of SiC semiconductor devices.
[0027] In order to solve the above problems, the present invention includes a basal plane dislocation density of <100 / cm2 The growth layer is an n-type or p-type substrate. By adopting such a structure, the present invention can realize a high-quality SiC semiconductor device that suppresses the generation of stacking defects that are a major factor in deterioration of forward characteristics.
[0028] In a preferred embodiment of the present invention, the doping concentration of the growth layer is 1.0×10 17 / cm 3 By adopting such a structure, the present invention can realize a high-quality SiC semiconductor device in which the generation of stacking defects that are a major factor in deterioration of forward characteristics is suppressed.
[0029] Effects of the Invention
[0030] According to the present invention, a high-quality SiC semiconductor device can be provided.
[0031] Other technical problems, features and advantages to be solved will become apparent by reading the detailed description described below in conjunction with the drawings and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the manufacturing steps of a SiC semiconductor device.
[0033] Figure 2 is a schematic diagram of the growth steps.
[0034] Figure 3 Schematic diagram of a portion of the device formation steps.
[0035] Figure 4 Schematic diagram of a portion of the device formation steps.
[0036] Figure 5 is a schematic diagram of the electrode forming step after the separation step.
[0037] Figure 6 is a schematic diagram of the separation steps.
[0038] Figure 7 is a schematic diagram of the etching step.
[0039] Figure 8 It is a schematic diagram of the manufacturing steps of a SiC semiconductor device.
[0040] Fig. 9 is a schematic diagram of a SiC semiconductor device.
[0041] Fig.10 Schematic diagram of the raw material transportation involved in the growth step and the etching step.
[0042] Fig.11Schematic diagram of the raw material transportation involved in the growth step and the etching step.
[0043] Fig.12 It is a schematic diagram of the main container and the high melting point container.
[0044] Fig.13 This is a diagram for explaining the method of obtaining the BPD conversion rate.
[0045] Fig.14 is an explanatory diagram of a SiC wafer formed in a heat treatment step.
[0046] Fig.15 is an explanatory diagram of a SiC wafer formed in a heat treatment step.
[0047] Fig.16 is the Arrhenius diagram involved in the heat treatment steps. DETAILED DESCRIPTION
[0048] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. In addition, some of the reference numerals described below are not shown in the drawings.
[0049] The technical scope of the present invention is not limited to the embodiments shown in the drawings, and can be appropriately modified within the scope described in the claims.
[0050] like Figure 1 As shown, in one embodiment of the present invention, it includes: a growth step S1, forming a growth layer 10 on a processing body 1 including a SiC single crystal; a device formation step S2, forming at least a portion of a SiC semiconductor device 12 in the growth layer 10; and a separation step S3, separating at least a portion of the formed SiC semiconductor device 12 from the processing body 1.
[0051] In addition, the “SiC semiconductor device 12 ” in the description of this specification refers to a semiconductor device including at least a SiC material including a SiC device.
[0052] The object to be processed 1 includes an original substrate 11 composed of a SiC single crystal. The original substrate 11 may be a SiC ingot produced by a known crystal growth method such as a sublimation method, or a SiC wafer obtained by cutting the SiC ingot into a disk shape. In addition, the "polymorph of SiC single crystal" in the description in this specification refers to a known polymorph such as 3C, 4H, and 6H.
[0053] The cross-sectional size of the treated object 1 is several centimeters square, 2 inches (about 5.08 centimeters), 3 inches (about 7.62 centimeters), 4 inches (about 10.16 centimeters), 6 inches (about 15.24 centimeters), 8 inches (about 20.32 centimeters), or 12 inches (about 30.48 centimeters). There is no limit to the cross-sectional size.
[0054] The surface of the object 1 may have an off angle of several degrees (eg, 0.4 to 8.0°) from the (0001) plane or the (000-1) plane. In addition, "-" in the present specification refers to the horizontal sign in the notation of the Miller index.
[0055] The method for manufacturing the SiC semiconductor device 12 can be understood as follows.
[0056] 1) Growth Step S1 A growth layer 10 is formed on an original substrate 11 .
[0057] 2) Device Formation Step S2 Growth layer 10 is processed to form at least a portion of SiC semiconductor device 12 .
[0058] 3) Separation Step S3: At least a portion of the SiC semiconductor device 12 formed in the device formation step S2 is separated from the object 1 to be processed.
[0059] 《Growth Step S1》
[0060] like Figure 2 As shown, the growth step S1 performs the epitaxial growth step S11 and the bunching decomposition step S12 to form a growth layer 10 on the original substrate 11. In addition, in this specification, the mechanism involved in the growth step S1 will be described later. Figure 2 , a SiC semiconductor device 12 having a field effect transistor (FET) structure is illustrated.
[0061] The epitaxial growth step S11 performs crystal growth on the surface of the original substrate 11 having the step 101a and the step 101b with a reduced platform length W1 to form a growth layer 10 having the step 102a and the platform 102b with an increased platform length W2, or to form a growth layer 10 having a bunched (bundled) surface.
[0062] In addition, in the epitaxial growth step S11, a nanostructured carbon nanotube with a thickness of <100 / cm 2 A growth layer with a basal plane dislocation density (BPD density) of 100% or a crystal growth is performed in a manner that converts the BPD in the processed body 1 into other defects / dislocations including threading edge dislocations (TED) to form at least a portion of the growth layer 10.
[0063] The bunching decomposition step S12 decomposes the MSB of the surface of the object 1 on the surface of the growth layer 10 having the step 102a and the terrace 102b and causes the object 1 to undergo crystal growth to form a growth layer 10 having the step 103a and the terrace 103b with a reduced terrace length W3, or to form a flattened, bunch-free surface. At this time, the surface of the growth layer 10 may end at a step having the height of a full unit cell in the SiC single crystal.
[0064] The “flattened, bunching-free surface” in the description of this specification refers to a SiC surface after MSB is decomposed.
[0065] In addition, the term "MSB" in the description of this specification means that among the steps on the SiC surface, a step exceeding the height of the full unit cell of each polycrystalline form is formed by bunching.
[0066] That is, MSB is a step obtained by bundling more than 4 molecular layers (more than 5 molecular layers) in the case of 4H-SiC, and is a step obtained by bundling more than 6 molecular layers (more than 7 molecular layers) in the case of 6H-SiC.
[0067] The thickness of the growth layer 10 formed in one embodiment of the present invention is preferably 500 μm or less, more preferably 350 μm or less, more preferably 200 μm or less, more preferably 150 μm or less, further preferably 120 μm or less, further preferably 100 μm or less, further preferably 50 μm or less, further preferably 20 μm or less.
[0068] Furthermore, the thickness is preferably 20 μm or more, more preferably 50 μm or more, more preferably 100 μm or more, more preferably 150 μm or more, further preferably 200 μm or more, further preferably 350 μm or more.
[0069] The growth step S1 can also be performed in the formation of a 2 After a growth layer with a BPD density of 1000 nm is formed, SiC epitaxial growth is further performed based on a known film formation method such as physical vapor deposition (PVD) or chemical vapor deposition (CVD).
[0070] In addition, the nanostructured carbon nanotubes formed by the growth step S1 have a thickness of <100 / cm 2 A portion of the growth layer 10 having a BPD density of 1.0×10 17 / cm 3 above doping concentration.
[0071] The "object 1" in the description of this specification refers to the object 1 including the growth layer 10 in the case after the growth step S1. In addition, the "various treatments on the object 1" performed by the device formation step S2 or the separation step S3 described later can be understood as "various treatments on the growth layer 10 included in the object 1".
[0072] 《Device formation step S2》
[0073] like Figure 3 As shown, the device forming step S2 performs a patterning step S21 of forming a circuit pattern 211 on the object 1 on which the growth layer 10 is formed.
[0074] <Composition Step S21>
[0075] The patterning step S21 includes, for example, a resist coating step of coating a photoresist, an exposure step of exposing the photoresist via a photomask, and a development step of developing the exposed photoresist.
[0076] In the resist coating step, a known photoresist including a base resin that selectively reacts to the wavelength of a light source that can be used in an exposure step described later is coated on the object to be processed 1 .
[0077] For example, when the light source is g-ray (wavelength: 436 nm), the photoresist is a polymer material containing novolac resin and 1,2-naphthoquinonediazidesulfonate (NQD) compounds. In addition, when the light source is ArF laser (wavelength: 193 nm), the photoresist is a polymer material containing a base resin having an alicyclic group such as norbornene that can suppress light absorption near a wavelength of 200 nm.
[0078] In the resist coating step, a photoresist is coated on the object 1 to be processed using a known resist coating device such as spin coating or spray coating.
[0079] At this time, in the resist coating step, process conditions such as the rotation speed and the dripping amount involved in spin coating are set or optimized so as to obtain a desired film thickness involved in the photoresist.
[0080] In addition, in the resist coating step, before coating the photoresist, a silica agent such as hexamethyldisilazane (HMDS) from which hydroxyl groups have been removed may be coated on the surface of the object 1 to impart hydrophobicity to the surface of the object 1 .
[0081] Resist Coating Step After a photoresist is coated on the object 1 to be processed, the photoresist and the object 1 to be processed are subjected to heat treatment and pre-baking.
[0082] In addition, the resist coating step sets or optimizes process conditions such as heating temperature and heating time involved in pre-baking to obtain a desired film thickness or surface roughness involved in the photoresist or to appropriately transfer the circuit pattern 211.
[0083] The exposure step uses a known exposure device such as a close-fitting exposure device or a reduced projection exposure device including a known light source, an optical system, and a stage, and a photomask showing a circuit pattern 211 to expose a portion of the photoresist coated on the object to be processed 1. The projection method involved in the optical system can adopt a known projection method such as a lens method and a reflector method. In addition, the exposure device can also perform exposure in a maskless exposure mode without using a photomask as a tangible object.
[0084] In addition, the exposure step appropriately sets or optimizes process conditions such as exposure time so as to appropriately transfer the circuit pattern 211 .
[0085] The exposure step may use the following as light sources: g-line (436nm wavelength), i-line (365nm wavelength), KrF laser (248nm wavelength), ArF laser (193nm wavelength), F2 laser (157nm wavelength), Kr2 laser (146nm wavelength), Ar2 laser (126nm wavelength), soft X-ray (EUV: Extreme Ultraviolet, ~13.5nm wavelength), electron beam, X-ray, etc. In addition, the exposure step may also be performed in the liquid immersion lithography mode by inserting pure water between the projection optical system and the object 1 to be processed to increase the refractive index.
[0086] The exposure step may also include heat treatment and baking (PEB: Post Exposure Baking) of the photoresist after exposure.
[0087] Furthermore, in the exposure step, process conditions such as the heating temperature and the heating time involved in the baking are set or optimized so that the circuit pattern 211 can be appropriately transferred.
[0088] The development step removes (develops) a portion of the exposed photoresist using a developer. In this case, the developer material can be appropriately selected according to the photoresist material. The developer contains, for example, tetramethylammonium hydroxide (TMAH).
[0089] In addition, the developing step sets or optimizes process conditions such as the temperature of the developing solution or the developing time so as to properly transfer the circuit pattern 211 .
[0090] The development step performs a post-bake of the developed photoresist.
[0091] In addition, the developing step sets or optimizes the process conditions such as the heating temperature and the heating time involved in the baking so as to appropriately transfer the circuit pattern 211 .
[0092] The patterning step S21 may be performed, for example, before the resist coating step, by performing a hard mask forming step of forming a hard mask serving as a sacrificial layer on the object 1 using a known film forming method such as PVD or CVD.
[0093] The hard mask formation step can use silicon oxides such as SiO2 and TEOS-SiO2, silicon nitrides such as SiN and Si3N4, silicon nitride oxides such as SiON, boron nitrides such as BN, titanium nitrides such as TiN, and mixtures thereof as materials showing high hardness and low stress as hard masks. In addition, a structure in which B elements are appropriately added to the hard mask can also be used.
[0094] In the patterning step S21 , a hard mask and a photoresist may be formed in sequence, or a hard mask, an anti-reflection film such as a carbon film, and a photoresist may be formed in sequence, or a multilayer structure may be formed.
[0095] The patterning step S21 may also adopt a structure in which a photoresist is formed only on the object 1 to be processed, the photoresist is used as a hard mask having heat resistance, etching resistance and ion blocking ability, and the circuit pattern 211 is transferred.
[0096] The patterning step S21 may also be performed in a nanoimprint mode by using a mold made of, for example, SiO 2 material to transfer the circuit pattern 211 onto the object 1 to be processed.
[0097] The line width of the circuit pattern 211 formed in one embodiment of the present invention is preferably 10 μm or less, more preferably 5.0 μm or less, more preferably 2.0 μm or less, more preferably 1.0 μm or less, more preferably 0.5 μm or less, more preferably 0.2 μm or less, more preferably 0.1 μm or less, more preferably 50 nm or less, more preferably 20 nm or less, more preferably 10 nm or less. In addition, the line width is preferably 1.0 nm or more, more preferably 10 nm or more, more preferably 20 nm or more, more preferably 50 nm or more, more preferably 0.1 μm or more, more preferably 0.2 μm or more, more preferably 0.5 μm or more, more preferably 1.0 μm or more, more preferably 2.0 μm or more, and more preferably 5.0 μm or more.
[0098] The device forming step S2 performs a selective etching step after the patterning step S21 . The selective etching step uses the photoresist showing the circuit pattern 211 to etch the surface exposed below the photoresist.
[0099] The selective etching step etches the exposed surface on the object 1 to be processed to exhibit material selectivity. The term "exhibiting material selectivity" in the present specification means that, for example, the etching rates of the photoresist and the SiC single crystal are different from each other.
[0100] In the selective etching step, the exposed surface of the object 1 is etched by, for example, wet etching.
[0101] At this time, the selective etching step sets or optimizes the process conditions such as the etchant, etching time, and etching temperature to achieve the desired material selectivity, surface orientation dependence, etching rate, etc. The solution containing the etchant is, for example, a TMAH solution, a potassium hydroxide (KOH) solution, a potassium permanganate (KMnO4) solution, a hydrogen fluoride (HF) solution, etc.
[0102] In the selective etching step, the exposed surface of the object 1 is etched by known thermal etching such as reactive gas etching.
[0103] At this time, the selective etching step sets or optimizes the process conditions such as the partial pressure or heat treatment temperature of the etchant (reactive gas) or the reactive gas to achieve the desired material selectivity, plane orientation dependence, etching rate, etc. The etchant is, for example, a mixture of H2, HCl, Cl2, O2, CIF3, etc.
[0104] The selective etching step etches the exposed surface of the object 1 by known dry etching such as reactive ion etching (RIE). Reactive ion etching forms plasma in a known manner such as ICP or CCP, and appropriately combines known gases such as Ar gas, O2 gas, NF3 gas, PF3 gas, BF3 gas, CF4 gas, CHF3 gas, SF6 gas, and XeF2.
[0105] In addition, the selective etching step sets or optimizes process conditions such as bias power, gas type, gas partial pressure, and discharge time to achieve desired anisotropy, etching rate, etc.
[0106] In addition, the selective etching step may also perform anisotropic etching or deep trench etching to form a three-dimensional shape such as a U groove or a V groove on the object 1 to be processed.
[0107] <Doping Step S22>
[0108] like Figure 3 As shown, the device forming step S2 performs a doping step S22 of introducing dopant atoms into the processed body 1 so as to form an n-type and / or p-type region, or a pn junction region, in the processed body 1 .
[0109] The doping step S22 includes, for example, an ion implantation step of irradiating the object 1 with ionized dopant atoms, namely, dopant ions, and an activation step of heat-treating and activating the object 1 irradiated with the dopant ions.
[0110] The ion implantation step includes, for example, a beam extraction step of extracting an ion beam from an ion source containing a doping element; a mass analysis step of mass-separating a desired ion species from among the ion species contained in the ion beam; an acceleration step of imparting acceleration energy to the ion beam containing the mass-separated ion species; and a scanning step of scanning the ion beam imparted with the acceleration energy and irradiating the object to be processed 1. In addition, the ion implantation step utilizes a sacrificial layer having ion blocking capability, i.e., the circuit pattern 211, to irradiate the desired region with dopant ions.
[0111] The ion implantation step ionizes known doping elements such as N, P, Al, and B, and irradiates the ion implantation element onto the object 1. At this time, N and P are added to the SiC single crystal to form an n-type region, and Al and B are added to the SiC single crystal to form a p-type region.
[0112] In addition, an element that forms an n-type or p-type region in a SiC single crystal can be appropriately used as the dopant ion.
[0113] In addition, in the ion implantation step, a non-doping element such as C element, Si element, Cl element, Ar element, etc. may be ionized and irradiated onto the object to be processed 1 in the same manner.
[0114] The beam extraction step extracts an ion beam containing dopant ions from an ion source containing the dopant element disposed in a vacuum chamber to obtain a desired mean free path.
[0115] In addition, the beam extraction step extracts the ion beam by, for example, applying an extraction voltage to the ion source. In addition, the beam extraction step extracts the ion beam by, for example, ionizing the ion source under a plasma environment.
[0116] The ion source may be a solid material, a gaseous material, a liquid metal ion source (LMIS), or may be configured to combine a supporting gas and a solid material for forming a plasma environment that promotes ionization. In addition, the plasma environment is appropriately formed based on known methods utilizing a DC power supply or an AC power supply, etc.
[0117] The mass analysis step analyzes the mass and charge ratio (m / z) involved in the ion beam containing the dopant ions extracted by the beam extraction step to perform mass separation on the desired ion species. The mass analysis step, for example, applies a voltage to the ion beam and passes it through a magnetic field, adjusts the voltage and / or magnetic field strength, and selects the m / z corresponding to the ion species.
[0118] The mass analysis step may be appropriately adopted as long as it is a known mass analysis method such as a sector magnetic field, a quadrupole, a time of flight (TOF), an ion trap type, or the like.
[0119] The acceleration step imparts acceleration energy to the ion beam containing the dopant ions to achieve a desired ion implantation depth or a desired dopant distribution. In addition, the acceleration step can be performed after the mass analysis step or before and after the mass analysis step.
[0120] The scanning step scans an ion beam containing dopant ions on at least a portion of a surface of a target, that is, a treatment object 1, disposed in a vacuum chamber, to provide an implantation angle to the dopant ions. In addition, the scanning step may also evaluate a beam current of the ion beam irradiated onto the target using a Faraday cup or the like. In addition, the beam current and the beam irradiation time are used to evaluate a dose involved in the ion beam.
[0121] In addition, the ion implantation step sets or optimizes the above-mentioned process conditions such as acceleration energy, implantation angle, and dosage to form a desired dopant distribution.
[0122] The ion implantation step may also be performed by co-ion implantation of two or more ion species, which may be, for example, multiple types of dopant ions or C ions and dopant ions, and there is no limitation on the combination thereof.
[0123] The ion implantation step may irradiate the dopant ions onto the processed object 1 multiple times, or irradiate the dopant ions onto the processed object 1 while changing the acceleration energy in multiple levels, or irradiate the dopant ions onto the processed object 1 while heating the processed object 1, so as to form a desired dopant distribution.
[0124] In addition, the ion implantation step may irradiate dopant ions onto the object 1 to form a box-shaped distribution with a constant dopant concentration. In addition, the "desired dopant distribution" in the description of this specification may be appropriately changed according to the structure of the SiC semiconductor device to be manufactured.
[0125] The activation step heat-treats the object 1 irradiated with the dopant ions in an inert atmosphere such as an Ar atmosphere to restore crystal damage caused by the irradiation with the dopant ions and activate the dopant ions.
[0126] In addition, the activation step sets or optimizes the process conditions such as heating temperature, heating time, partial pressure, etc. to form a desired dopant distribution or to increase the activation rate of the dopant ions.
[0127] In the activation step, for example, a carbon layer or a passivation film such as SiO 2 is formed on the surface of the object 1 to prevent carbonization of the surface of the object 1 .
[0128] The doping step S22 introduces dopant atoms into the object 1 to form n + and / or - area to form p + and / or - region, to form an n-type or p-type drift region 220, to form an n-type or p-type well region 221, to form an n-type or p-type contact region 222, to form an n-type or p-type body region, to form an n-type or p-type base region, to form an n-type or p-type source region, to form an n-type or p-type collector region, to form an n-type or p-type field stop region, to form an n-type or p-type pillar region, to form an n-type or p-type buffer region, to form an n-type or p-type recombination promotion region, to form an n-type or p-type embedded region, to form a halo structure, to form a shallow junction structure, or to form a super junction structure.
[0129] Furthermore, the doping step S22 introduces dopant atoms into the object 1 to be processed to form n-type or p-type regions exhibiting a distribution seen in known Si-based electronic devices.
[0130] In addition, it should be understood that the “region” included in the n-type region, drift region, etc. in the description of this specification is the same as the “layer” included in the n-type layer, drift layer, etc.
[0131] The dopant concentration of the n-type or p-type region formed in the doping step S22 is preferably 1.0×10 21 / cm 3 Below, more preferably 1.0×10 20 / cm 3 Below, more preferably 1.0×10 19 / cm 3 Below, more preferably 1.0×10 18 / cm 3 Below, more preferably 1.0×10 17 / cm 3 Below, more preferably 1.0×10 16 / cm 3 In addition, the dopant concentration is preferably 1.0×10 15 / cm 3More preferably, 1.0×10 16 / cm 3 More preferably, 1.0×10 17 / cm 3 More preferably, 1.0×10 18 / cm 3 More preferably, 1.0×10 19 / cm 3 More preferably, 1.0×10 20 / cm 3 above.
[0132] In addition, the dopant concentration may differ between different regions such as the n-type contact region and the drift region, for example.
[0133] The doping step S22 may also be performed each time SiC epitaxial growth is performed, after the patterning step S21, to introduce dopant atoms into the object 1. The SiC epitaxial growth may be performed by the growth step S1 or by a known film forming method such as PVD or CVD.
[0134] like Figure 3 As shown, the device forming step S2 may also repeat the patterning step S21 and the doping step S22.
[0135] In addition, the device forming step S2 may also repeat the SiC epitaxial growth, the patterning step S21 and the doping step S22 based on a plurality of circuit patterns 211 .
[0136] In addition, the device forming step S2 may also include performing the SiC epitaxial growth and doping step S22 without performing the patterning step S21 .
[0137] In addition, the device forming step S2 etches the photoresist and / or the hard mask showing the circuit pattern 211 each time the doping step S22 is performed.
[0138] <Insulating Film Formation Step S23>
[0139] like Figure 4 As shown, the device forming step S2 performs an insulating film forming step S23 of introducing the insulating film 230 into the object 1 to be processed.
[0140] The insulating film 230 functions as a gate insulating film, an interlayer insulating film for element isolation, or a cap layer for adjusting a flat band voltage in the gate electrode 240 in a SiC semiconductor device having a FET structure or the like, for example.
[0141] The EOT (Equivalent Oxide Thickness) of the insulating film 230 formed in the insulating film forming step S23 is preferably 100 nm or less, more preferably 50 nm or less, more preferably 20 nm or less, further preferably 10 nm or less, further preferably 5.0 nm or less, further preferably 2.0 nm or less. In addition, the EOT is preferably 1.0 nm or more, more preferably 2.0 nm or more, more preferably 5.0 nm or more, more preferably 10 nm or more, further preferably 20 nm or more, further preferably 50 nm or more.
[0142] In the insulating film forming step S23, for example, a known oxidation furnace and an oxidant such as dry oxygen (O2) or water vapor (H2O) are used to thermally oxidize the object 1 to form a thermally oxidized SiO2 film.
[0143] At this time, the insulating film forming step S23 sets or optimizes the process conditions such as oxidation temperature, oxidation time, and partial pressure of oxide gas to reduce the interface state density at the SiC / SiO2 interface, to reduce the roughness of the SiC / SiO2 interface, to inhibit carbon residues in the thermally oxidized SiO2 film, or to promote the generation of CO gas in the thermal oxidation reaction.
[0144] The insulating film forming step S23 may also be performed by performing a dry process using heat treatment or a plasma environment after forming the insulating film 230 to reduce the interface state density at the insulating film interface.
[0145] The insulating film forming step S23 may also be subjected to nitridation treatment, for example, after forming the thermally oxidized SiO2 film, to reduce the interface state density at the SiC / SiO2 interface. The nitridation treatment may be either a heat treatment in a nitrogen monoxide (NO) atmosphere or a treatment in a plasma environment obtained by exciting nitrogen oxides such as NO.
[0146] The insulating film forming step S23 may also be based on a known film forming method such as CVD or ALD (Atomic Layer Deposition) to form the insulating film 230. In this case, the insulating film 230 may also be composed of a metal oxide film such as an Al2O3 film or an AlON film in addition to a Si oxide film such as a thermally oxidized SiO2 film.
[0147] <Electrode Formation Step S24>
[0148] like Figure 4 and Figure 5 As shown, the device forming step S2 performs an electrode forming step S24 of forming electrodes on the object 1 to be processed.
[0149] The electrode forming step S24 forms electrodes on the processed body 1 to form a gate electrode 240, to form a source electrode 241, to form a drain electrode 242, to form a base electrode, to form an emitter electrode, to form a collector electrode, to form an anode electrode, to form a cathode electrode, to form an ohmic electrode, or to form a Schottky electrode.
[0150] The electrode forming step S24 forms a film of polysilicon (poly-Si) on the object 1 through a film forming process based on a known method such as a CVD method. The polysilicon is processed into a gate electrode 240 adjacent to the insulating film 230 through a patterning step S21, a doping step S22, and a selective etching step. In addition, the electrode forming step S24 may use a metal material other than polysilicon as the gate electrode 240 instead of or in addition to polysilicon.
[0151] The electrode formation step S24 forms a metal film such as Ni on the processed body 1 by, for example, a PVD method. The metal film is formed into an ohmic electrode, namely a source electrode 241 or a drain electrode 242, adjacent to the n-type or p-type contact area 222 through, for example, a composition step S21, a doping step S22 and a selective etching step.
[0152] The electrode forming step S24 may also be performed by performing a silicidation reaction by heat treating the object 1 after forming the metal film. Alternatively, the electrode forming step S24 may be performed by stacking a barrier metal such as TiN or TaN on the source electrode 241 or the drain electrode 242 .
[0153] In addition, the electrode forming step S24 sets or optimizes process conditions such as the heat treatment temperature or the heat treatment time in the silicidation reaction to form a Schottky electrode, or forms an ohmic electrode through the dopant segregation effect.
[0154] like Figure 5 As shown, the electrode forming step S24 may be performed after the separation step S3 by forming a metal film such as Ni on the object 1 by PVD, and forming an ohmic electrode adjacent to the n-type or p-type region, namely the drain electrode 242, as a back surface electrode.
[0155] In the device forming step S2, the insulating film 23 or the electrode formed in the insulating film forming step S23 or the electrode forming step S24 may also be used as the above-mentioned hard mask.
[0156] In addition, the "CVD method" described in this specification refers to known CVD methods such as thermal CVD, PECVD (Plasma-Enhanced CVD), MOCVD (Metal Organic CVD), etc., and can be used as a film formation method when introducing any of the various materials that constitute the SiC semiconductor device 12.
[0157] In addition, the "PVD method" described in this specification refers to known PVD methods such as vacuum evaporation, DC sputtering, RF sputtering, magnetron sputtering, reactive sputtering, and molecular beam epitaxy (MBE), and can be appropriately used as a film formation method when introducing any of the various materials that constitute the SiC semiconductor device 12.
[0158] The device forming step S2 may also include, for example, a doping step S22 , an insulating film forming step S23 , or an electrode forming step S24 after the selective etching step, so as to manufacture a SiC semiconductor device 12 having a trench gate structure.
[0159] The device forming step S2 may also be performed by performing at least a part of the insulating film forming step S23 after the electrode forming step S24.
[0160] In one embodiment of the present invention, at least a part of the steps included in the device forming step S2 may be performed in different orders according to the structure of the SiC semiconductor device to achieve a desired structure of the SiC semiconductor device 12 .
[0161] In one embodiment of the present invention, the device forming step S2 may also form a wiring region.
[0162] <Separation Step S3>
[0163] In the separation step S3 , a part of the object to be processed 1 is separated.
[0164] The separation step S3 may be performed by a multi-wire saw cutting method in which a plurality of wires are reciprocated to perform cutting, an electrical discharge machining method in which plasma discharge is intermittently generated to perform cutting, or a method in which a layer serving as a base point for cutting is formed by irradiating with laser light.
[0165] like Figure 6 As shown, the separation step S3 includes: a separation layer forming step S31 of forming a separation layer 300 inside the object 1 to be processed, and a peeling step S32 of peeling off a part of the object 1 to be processed starting from the separation layer 300 .
[0166] <Separation Layer Formation Step S31>
[0167] In the separation layer forming step S31, laser light of a wavelength that is transmissive in the object 1 is irradiated onto the object 1 and converged to form a separation layer 300 so that the interior of the object 1 becomes the focus at a depth equivalent to the thickness of the SiC semiconductor device 12 to be separated from the upper surface.
[0168] At this time, in the separation layer forming step S31 , it is preferable to irradiate the surface of the object 1 on which the SiC semiconductor device 12 is not formed with laser light.
[0169] The separation layer forming step S31 forms the separation layer 300 using a holding device capable of holding the object 1 by conventional means such as an adsorption chuck, a light source 311 capable of irradiating pulsed laser light, and a conventional focusing device 312 such as a lens capable of focusing the laser light.
[0170] In addition, the separation layer forming step S31 uses, for example, infrared laser as the laser.
[0171] In addition, the wavelength of the laser light may be either a wavelength similar to ultraviolet light or a wavelength similar to visible light, without limitation.
[0172] In addition, the separation layer forming step S31 sets or optimizes process conditions such as laser wavelength, laser output, laser scanning speed, beam spot diameter, pulse width, and pitch width so that the semiconductor device 12 can be properly separated from the object 1 to be processed.
[0173] <Peeling Step S32>
[0174] The stripping step S32 strips a portion of the object 1, namely, the SiC semiconductor device 12, starting from the separation layer 300. At this time, the stripping step S32 applies mechanical vibration to the object 1 by reciprocating a metal wire along the separation layer 300 or generating ultrasonic vibration, and strips the SiC semiconductor device 12 from the object 1 starting from the separation layer 300.
[0175] The stripping step S32 utilizes a holding device capable of holding the object 1 to be processed based on conventional methods such as an adsorption chuck, a vibration device formed of piezoelectric ceramics and capable of generating conventional mechanical vibrations including ultrasonic vibrations, and at least a portion of a liquid supply device capable of supplying liquids such as pure water, to strip the SiC semiconductor device 12 from the object 1 to be processed starting from the separation layer 300.
[0176] In the separation step S3 , a polymer layer serving as a stress generating layer may be formed on the object to be processed 1 before the separation layer forming step S31 or before the peeling step S32 .
[0177] In this case, the peeling step S32 may be performed by cooling the object 1 including the polymer layer to induce crack propagation in the separation layer 300 and peeling the SiC semiconductor device 12 from the object 1 starting from the separation layer 300 .
[0178] In this case, the peeling step S32 sets or optimizes the process conditions such as the composition, film thickness, cooling temperature, cooling rate, cooling time, etc. of the polymer layer so that the SiC semiconductor device 12 can be appropriately separated from the object 1 .
[0179] In addition, at this time, in the separation step S3 , it is preferable to form the polymer layer on the surface of the object 1 on which the SiC semiconductor device 12 is not formed, so as to suppress the generation of stress in the SiC semiconductor device 12 .
[0180] The separation step S3 can adopt known techniques.
[0181] In addition, the separation step S3 can adopt at least a part of the apparatus or method described in patent documents such as Japanese Patent Application Publication No. 2013-49161, Japanese Patent Application Publication No. 2018-207034, Japanese National Publication No. 2017-500725, and Japanese National Publication No. 2017-526161.
[0182] In addition, the separation step S3 can adopt at least a part of the devices or methods described in patent documents such as Japanese Patent Publication No. 2017-526161, Japanese Patent Publication No. 2017-500725, Japanese Patent Publication No. 2018-152582, Japanese Patent Publication No. 2019-500220, and Japanese Patent Publication No. 2019-511122.
[0183] 《Etching step S4》
[0184] like Figure 7 As shown, the etching step S4 etches the object 1 to be processed to form a flattened, non-bunching surface having a reduced terrace length W3. In addition, the mechanism involved in the etching step S4 will be described later.
[0185] The etching step S4, for example, heat treats the object 1 separated by the separation step S3, and etches the surface layer including the separation layer 300 remaining at the object 1. It can be understood that the separation layer 300 includes a crystal dislocation 301 or a damaged area 302. At this time, the surface of the growth layer 10 can end at a step showing the height of the full unit cell in the SiC single crystal. In addition, the separation layer 300 can also be understood as a strain layer or a damaged layer.
[0186] In addition, the etching step S4 includes a strain layer removal step S41, in which the object 1 is placed in a quasi-enclosed space with a Si / C atomic ratio of less than 1, heated, and etched. In addition, the etching step S4 includes a bunching decomposition step S42, in which the object 1 is placed in a quasi-enclosed space with a Si / C atomic ratio of more than 1, heated, and etched.
[0187] In the strained layer removal step S41 , the separation layer 300 is etched, and the object 1 is etched to expose the focused (bunched) surface.
[0188] The bunching decomposition step S42 etches the object 1 and decomposes the MSB on the surface of the object 1 to form a flattened surface without bunching. At this time, the surface ends at a step having a height of a full unit cell in the SiC single crystal.
[0189] like Figure 8 As shown, in one embodiment of the present invention, a plurality of steps including at least a growth step S1, a device formation step S2 and a separation step S3 may be repeatedly performed in a ring-forming manner.
[0190] Furthermore, in one embodiment of the present invention, the growing step S1 , the device forming step S2 , the separating step S3 , and the etching step S4 may be repeatedly performed in a manner of forming a ring.
[0191] Furthermore, in one embodiment of the present invention, at least a portion of each step of the device forming step S2 may also be performed after the separating step S3 .
[0192] One embodiment of the present invention can manufacture a SiC semiconductor device 12 having a known device structure including, for example, a Schottky barrier diode (SBD), a bipolar junction transistor (BJT), a FET, an insulated gate bipolar transistor (IGBT), and combinations thereof.
[0193] like Fig. 9 As shown, one embodiment of the present invention can manufacture a SiC semiconductor device 12 including an n-type or p-type substrate 111 adjacent to an electrode surface such as a drain electrode, an anode electrode, and a collector electrode.
[0194] like Fig. 9 As shown in (a) in the figure, one embodiment of the present invention can manufacture a SiC semiconductor device 12 with a FET structure, wherein the FET structure includes an n-type or p-type substrate 111, an n-type or p-type drift region 220, an n-type or p-type well region 221, an n-type or p-type contact region 222, an insulating film 230, a gate electrode 240, a source electrode 241 and a drain electrode 242.
[0195] In addition, if Fig. 9 As shown in (b) , one embodiment of the present invention can manufacture a SiC semiconductor device 12 having an SBD structure, wherein the SBD structure includes an n-type or p-type substrate 111 , a low concentration region 226 , an anode electrode 244 , and a cathode electrode 245 .
[0196] The thickness of the n-type or p-type substrate 111 is not limited within the thickness range of the growth layer 10. The n-type or p-type substrate 111 helps realize an ohmic electrode, for example.
[0197] One embodiment of the present invention can manufacture a SiC semiconductor device 12 having a planar gate structure. In this case, the SiC semiconductor device 12 can have a known device structure such as a FET structure or an IGBT structure.
[0198] One embodiment of the present invention can manufacture a SiC semiconductor device 12 having a trench gate structure to reduce the JFET resistance when the device is operating. In this case, the SiC semiconductor device 12 can have a known device structure such as a FET structure or an IGBT structure.
[0199] One embodiment of the present invention can manufacture a known SiC semiconductor device 12 having a superjunction structure including an n-type or p-type pillar region to reduce the drift resistance of the device during operation. In this case, the SiC semiconductor device 12 can have a known device structure such as a FET structure or an IGBT structure.
[0200] According to an embodiment of the present invention, a SiC semiconductor device 12 including an n-type or p-type embedded region can be manufactured to alleviate the electric field concentration effect during device operation.
[0201] In addition, the n-type or p-type embedded region in the SiC semiconductor device 12 can be set below the gate electrode 240 along the film thickness direction, or below the source electrode 241 along the film thickness direction, or as a guard ring arranged side by side with the n-type or p-type well region along a direction orthogonal to the film thickness direction.
[0202] One embodiment of the present invention can produce a substrate having a basal plane dislocation density (BPD density) of <100 / cm 2 Growth layer, including BPD density <10 / cm 2 Growth layer, or including BPD density <1.0 / cm 2 The SiC semiconductor device 12 is formed of a growth layer. As described above, the growth layer is at least a portion of the growth layer 10.
[0203] The growth layer refers to at least a part of the SiC structure constituting the SiC semiconductor device 12 including the above-mentioned n-type or p-type region.
[0204] In addition, the growth layer refers to, for example, an n-type or p-type substrate 111 .
[0205] In addition, the growth layer has a thickness of 1.0×10 17 / cm 3 Above, 2.0×10 17 / cm 3 Above, 5.0×10 17 / cm 3 Above, 1.0×10 18 / cm3 Above, 2.0×10 18 / cm 3 Above, or 5.0×10 18 / cm 3 Above the dopant concentration n + or p + area.
[0206] The cell pitch of the SiC semiconductor device 12 manufactured in one embodiment of the present invention is preferably 10 μm or less, more preferably 5.0 μm or less, more preferably 2.0 μm or less, more preferably 1.0 μm or less, more preferably 0.5 μm or less, more preferably 0.2 μm or less, more preferably 0.1 μm or less, more preferably 50 nm or less, more preferably 20 nm or less, and more preferably 10 nm. In addition, the cell pitch is preferably 1.0 nm or more, more preferably 10 nm or more, more preferably 20 nm or more, more preferably 50 nm or more, more preferably 0.1 μm or more, more preferably 0.2 μm or more, more preferably 0.5 μm or more, more preferably 1.0 μm or more, more preferably 2.0 μm or more, and more preferably 5.0 μm or more.
[0207] <Mechanism of Growth Step S1 and Etching Step S4>
[0208] This specification hereinafter describes a raw material conveying mechanism involved in a heat treatment step as the growth step S1 or the etching step S4.
[0209] In one embodiment of the present invention, the heat treatment step heat-treats the object 1 and the SiC raw material 4 so that a temperature difference is formed between the object 1 and the SiC raw material 4 .
[0210] The heat treatment step as the growth step S1 causes the object 1 to undergo crystal growth by placing the object 1 at a low temperature side, and forms a growth layer 10 on the surface of the object 1 .
[0211] In the heat treatment step as the etching step S4 , the object 1 is placed at a high temperature to etch the object 1 , thereby removing, for example, the separation layer 300 .
[0212] like Fig.10 As shown, by placing the object 1 to be processed on the low temperature side, the formation of the growth layer 10 on the rear surface 1 a and the etching of the SiC raw material 4 (the main surface 4 a ) are performed simultaneously.
[0213] The growth step S1 and the etching step S4 respectively heat treat the object 1 and the SiC raw material 4 in an atmosphere containing Si element and C element in a quasi-closed space.
[0214] In addition, the “quasi-enclosed space” in the description of this specification refers to a space in which at least a part of the vapor generated in the space can be enclosed, although the inside of the space can be evacuated.
[0215] like Fig.11 As shown, in the object 1 and the SiC raw material 4, the raw material transportation based on the following reactions 1) to 5) is continuously performed, and the growth layer 10 is formed.
[0216] 1)SiC(s)→Si(v)+C(s)
[0217] 2)2C(s)+Si(v)→SiC2(v)
[0218] 3) C(s)+2Si(v)→Si2C(v)
[0219] 4)Si(v)+SiC2(v)→2SiC(s)
[0220] 5)Si2C(v)→Si(v)+SiC(s)
[0221] Explanation of 1): Since the surface of the SiC raw material 4 is thermally decomposed, Si atoms (Si(v)) are released from the surface of the SiC raw material 4 .
[0222] Explanation of 2) and 3): Due to the detachment of Si atoms (Si(v)), C atoms (C(s)) remaining on the surface of the SiC raw material 4 react with Si vapor (Si(v)) in the raw material conveying space to become Si2C or SiC2, etc. and sublime in the raw material conveying space.
[0223] Explanation of 4) and 5): The sublimated Si2C or SiC2 etc. reaches / diffuses to the platform of the back surface 1a of the processed body 1 due to the temperature gradient, and reaches the step, thereby continuing the polytype of the back surface 1a, and forming a growth layer 10 while presenting a step flow growth state.
[0224] The growth step S1 includes a Si atom sublimation step of thermally sublimating Si atoms from the SiC raw material 4 and a C atom sublimation step of sublimating C atoms remaining on the main surface 4 a of the SiC raw material 4 by bonding with Si atoms in the raw material transport space.
[0225] Growth Step S1 forms a growth layer 10 based on the above-described step flow growth at the back surface 1a in the object 1. The respective steps included in the growth step S1 are sequentially performed.
[0226] In addition, the growth step S1 is understood to be a step based on PVT (physical vapor transport) because the transported Si 2 C or SiC 2 or the like becomes supersaturated and condenses to form the growth layer 10 .
[0227] Furthermore, by adopting such a structure, the growth step S1 can suppress the formation of MSBs on the surface of the object 1 to be processed, and obtain a planarized SiC surface showing a reduced terrace length.
[0228] The etching step S4 includes: a Si atom sublimation step of thermally sublimating Si atoms from the surface of the object 1; and a C atom sublimation step of bonding C atoms remaining at the surface of the object 1 with Si atoms in the raw material conveying space to sublime them, and the etching step S4 etches the surface of the object 1. By adopting such a structure, the etching step S4 can decompose the MSB on the surface of the object 1 and obtain a flattened SiC surface showing a reduced terrace length.
[0229] The mechanisms involved in each of the growth step S1 and the etching step S4 can be understood as the transportation of the raw material containing Si element and C element.
[0230] The driving force for raw material transport can be understood as the vapor pressure difference between the processed body 1 and the SiC raw material 4 caused by the formed temperature gradient. Therefore, it can be understood that not only the temperature difference at the surface of the processed body 1 and the SiC raw material 4, but also the chemical potential difference caused by the crystal structure between the processed body 1 and the SiC raw material 4 can become the driving force for raw material transport.
[0231] In each of the growth step S1 and the etching step S4, the SiC raw material 4 may be a SiC ingot produced by a sublimation method or the like, a SiC wafer obtained by cutting the SiC ingot into a disk shape, or a SiC polycrystal. In addition, the SiC raw material 4 may be a processed product such as a sintered body containing SiC polycrystal.
[0232] Furthermore, in each of the growth step S1 and the etching step S4 , the SiC material forming the quasi-closed space or the SiC material exposed in the quasi-closed space may be the SiC raw material 4 .
[0233] During the raw material transportation in the growth step S1 , the doping concentration of the growth layer 10 can be adjusted by supplying a doping gas into the quasi-enclosed space using a doping gas supply device.
[0234] It can be understood that, in the case where no doping gas is supplied, the growth layer 10 inherits the doping concentration in the quasi-enclosed space.
[0235] The raw material supply in each of the growth step S1 and the etching step S4 is preferably performed in an environment having a gas-phase species containing Si element and a gas-phase species containing C element.
[0236] Furthermore, the raw material transportation in each of the growth step S1 and the etching step S4 is performed under a SiC—Si or SiC—C equilibrium vapor pressure environment.
[0237] The "SiC-Si vapor pressure environment" in the description of this specification refers to the vapor pressure environment when SiC (solid) and Si (liquid phase) are in phase equilibrium through the gas phase. The SiC-Si equilibrium vapor pressure environment is formed by heat treating a quasi-enclosed space in which the Si / C atomic ratio exceeds 1.
[0238] The "SiC-C equilibrium vapor pressure environment" in the description of this specification refers to the vapor pressure environment when SiC (solid phase) and C (solid phase) are in phase equilibrium through the gas phase. The SiC-C equilibrium vapor pressure environment is formed by heat treating a quasi-enclosed space with a Si / C atomic ratio of 1 or less.
[0239] The heat treatment temperature in each of the growth step S1 and the etching step S4 is preferably above 1400°C, more preferably above 1500°C, more preferably above 1600°C, more preferably above 1700°C, more preferably above 1800°C, further preferably above 1900°C, further preferably above 2000°C, further preferably above 2100°C, further preferably above 2200°C.
[0240] In addition, the heat treatment temperature is preferably below 2300°C, more preferably below 2200°C, more preferably below 2100°C, more preferably below 2000°C, more preferably below 1900°C, further preferably below 1800°C, further preferably below 1700°C, further preferably below 1600°C, further preferably below 1500°C.
[0241] In addition, the growth rate or etching rate involved in each of the growth step S1 and the etching step S4 is determined by the heat treatment temperature.
[0242] The temperature gradient between the object 1 and the SiC raw material 4 in each of the growth step S1 and the etching step S4 is preferably 0.1°C / mm or more, more preferably 0.2°C / mm or more, more preferably 0.5°C / mm or more, further preferably 1.0°C / mm or more, further preferably 2.0°C / mm or more. In addition, the temperature gradient is preferably 5.0°C / mm or less, more preferably 2.0°C / mm or less, more preferably 2.0°C / mm or less, more preferably 1.0°C / mm or less, further preferably 0.5°C / mm or less, further preferably 0.2°C / mm or less.
[0243] In addition, the temperature gradient may be the same or may have a distribution.
[0244] <Apparatuses involved in growth step S1 and etching step S4 respectively>
[0245] The following description of the present specification details the apparatuses used in growth step S1 and etching step S4. In addition, for structural elements that are substantially the same as those shown in the above manufacturing method, the same reference numerals are assigned and their descriptions are simplified.
[0246] As Fig.12 As shown, the manufacturing apparatus related to the manufacturing method of the SiC semiconductor device includes a main body container 141, a high melting point container 142, and a heating furnace 143.
[0247] The main body container 141 is made of a material containing SiC polycrystals, for example. Therefore, at least a part of the main body container 141 can become a supply source (SiC raw material 4) during raw material transportation.
[0248] Desirably, the environment inside the heated main body container 141 is, for example, a vapor pressure environment of a mixed system of gas-phase species containing Si elements and gas-phase species containing C elements. As the gas-phase species containing Si elements, Si, Si2, Si3, Si2C, SiC2, SiC, etc. can be exemplified.
[0249] In addition, as the gas-phase species containing C elements, Si2C, SiC2, SiC, C, etc. can be exemplified.
[0250] The dopant and doping concentration of the main body container 141 can be selected according to the dopant and doping concentration of the growth layer 10 to be formed.
[0251] In addition, as long as the structure generates the vapor pressure of gas-phase species containing Si elements and gas-phase species containing C elements in the internal space during the heat treatment of the main body container 141, such a structure can be adopted. For example, a structure in which SiC polycrystals are exposed at a part of the inner surface, or a structure in which SiC polycrystals are separately provided inside the main body container 141 can be shown.
[0252] The main body container 141 includes a setting tool 141a capable of setting the object to be processed 1. In addition, the main body container 141 is a fitting container including an upper container 141c and a lower container 141b that can be fitted to each other. A minute gap is formed at the fitting portion of the upper container 141c and the lower container 141b, and it is configured to be able to evacuate (vacuum) the inside of the main body container 141 from this gap.
[0253] <Si vapor supply source>
[0254] The main body container 141 has a Si vapor supply source. The Si vapor supply source is used to adjust the Si / C atomic ratio in the quasi-enclosed space in the main body container 141 to be greater than 1. As the Si vapor supply source, solid Si (Si particles such as Si flakes or Si powder) or Si compounds can be exemplified.
[0255] For example, as in one embodiment of the present invention, when the main body container 141 is entirely composed of SiC polycrystal, by providing a Si vapor supply source, the Si / C atomic ratio in the main body container 141 exceeds 1. Specifically, when a processed object 1 and a SiC raw material 4 satisfying a stoichiometric ratio of 1:1 and a Si vapor supply source are provided in the main body container 141 of SiC polycrystal satisfying a stoichiometric ratio of 1:1, the Si / C atomic ratio in the main body container 141 exceeds 1.
[0256] The SiC-Si equilibrium vapor pressure environment according to one embodiment of the present invention is formed by heating a quasi-enclosed space in which the Si / C atomic ratio exceeds 1. In addition, the SiC-C equilibrium vapor pressure environment according to one embodiment of the present invention is formed by heating a quasi-enclosed space in which the Si / C atomic ratio is less than 1. The main body container 141 according to one embodiment of the present invention may also be configured to appropriately accommodate predetermined components respectively to form a SiC-Si equilibrium vapor pressure environment or a SiC-C equilibrium vapor pressure environment.
[0257] The heating furnace 143 is configured to heat to form a temperature gradient in which the temperature decreases / increases from the upper container 141c toward the lower container 141b of the main container 141. Thus, a temperature gradient is formed in the thickness direction of the object 1 to be processed.
[0258] like Fig.12 As shown, the heating furnace 143 includes: a main heating chamber 143c, which can heat the processed object 1 to a temperature above 1000°C and below 2300°C; a preparatory chamber 143a, which can preheat the processed object to a temperature above 500°C; a high melting point container 142, which can accommodate the main container 141; and a moving device 143b (moving platform), which can move the high melting point container 142 from the preparatory chamber 143a to the main heating chamber 143c.
[0259] The main heating chamber 143c is formed into a regular hexagon in a planar cross-sectional view, and a high melting point container 142 is arranged inside the main heating chamber 143c. A heater 143d (mesh heater) is arranged inside the main heating chamber 143c. In addition, a multi-layer heat-reflecting metal plate (not shown) is fixed to the side wall or the top of the main heating chamber 143c. The multi-layer heat-reflecting metal plate is configured to reflect the heat of the heater 143d toward the approximate center of the main heating chamber 143c.
[0260] The heater 143d is installed in the main heating chamber 143c so as to surround the high melting point container 142 storing the processed object. At this time, by installing a plurality of heat reflecting metal plates outside the heater 143d, the temperature can be increased within the temperature range of 1000°C to 2300°C.
[0261] The heater 143d may be, for example, a resistance heating heater or a high-frequency induction heating heater.
[0262] The heater 143d may also be configured to form a temperature gradient in the high melting point container 142. The heater 143d may be configured to have a plurality of heaters disposed on the upper side (or the lower side), for example. In addition, the heater 143d may also be configured to have a width that increases as it moves toward the upper side (or the lower side). Alternatively, the heater 143d may also be configured to increase the power supplied as it moves toward the upper side (or the lower side).
[0263] The main heating chamber 143c is connected with: a vacuum forming valve 143f for exhausting the main heating chamber 143c; an inert gas injection valve 143e for introducing inert gas into the main heating chamber 143c; and a vacuum gauge 143g for measuring the vacuum degree in the main heating chamber 143c.
[0264] The vacuum forming valve 143f is connected to a vacuum pump (not shown) for exhausting the main heating chamber 143c to evacuate the inside. By means of the vacuum forming valve 143f and the vacuum pump, the vacuum degree in the main heating chamber 143c can be adjusted to preferably 10Pa or less, more preferably 1.0Pa or less, and most preferably 10Pa or less. -3 Pa or less. As the vacuum pump, a turbomolecular pump can be exemplified.
[0265] The inert gas injection valve 143e is connected to an inert gas supply source (not shown). -5 Up to 10 4 An inert gas is introduced into the main heating chamber 143c within the range of Pa. Ar or the like can be selected as the inert gas.
[0266] The inert gas injection valve 143e is a doping gas supply device capable of supplying a doping gas into the main body container 141. That is, by selecting a doping gas (for example, N2 or the like) as the inert gas, the doping concentration of the growth layer 10 can be increased.
[0267] The preparatory chamber 143a is connected to the main heating chamber 143c and is configured to be able to move the high melting point container 142 through the moving device 143b. In addition, the preparatory chamber 143a of this embodiment is configured to be able to increase the temperature by utilizing the residual heat of the heater 143d of the main heating chamber 143c. For example, when the main heating chamber 143c is heated to 2000°C, the preparatory chamber 143a is heated to about 1000°C, and a degassing treatment of the object to be treated (the object to be treated 1, the main container 141, the high melting point container 142, etc.) can be performed.
[0268] The moving device 143b is configured to be able to place the high melting point container 142 thereon and to be able to move between the main heating chamber 143c and the preliminary chamber 143a.
[0269] Since the transportation between the main heating chamber 143c and the preparatory chamber 143a by the moving device 143b is completed in about 1 minute at the shortest, the temperature rise / fall of 1.0 to 1000°C / min can be achieved. Therefore, since rapid temperature rise and rapid temperature fall can be performed, the surface shape without low-temperature growth history during temperature rise and temperature fall can be observed.
[0270] In addition, Fig.12 In the embodiment, the preliminary chamber 143a is disposed below the main heating chamber 143c, but the present invention is not limited thereto and the preliminary chamber 143a may also be disposed in any direction.
[0271] The moving device 143b according to this embodiment is a moving stage for placing the high melting point container 142. The contact portion between the moving stage and the high melting point container 142 becomes a heat propagation path. Thus, a temperature gradient can be formed in the high melting point container 142 so that the contact portion side between the moving stage and the high melting point container 142 becomes a low temperature side.
[0272] In the heating furnace 143 of the present embodiment, since the bottom of the high melting point container 142 is in contact with the moving stage, the temperature gradient is set so that the temperature decreases from the upper container 142b toward the lower container 142a of the high melting point container 142.
[0273] By changing the position of the contact portion between the moving stage and the high melting point container 142, the direction of the temperature gradient can be set to any direction. For example, in the case where the moving stage is suspended and the contact portion is set at the top of the high melting point container 142, heat escapes in the upward direction. Therefore, the temperature gradient is set so that the temperature rises from the upper container 142b of the high melting point container 142 toward the lower container 142a. In addition, it is desirable that the temperature gradient is formed along the thickness direction of the processed body 1 and the SiC raw material 4. In addition, as described above, the temperature gradient can also be formed according to the structure of the heater 143d.
[0274] The vapor pressure environment of the gaseous species containing the Si element in the heating furnace 143 according to the present embodiment is formed by using the high melting point container 142 and the Si vapor supply material. For example, any method that can form a vapor pressure environment of the gaseous species containing the Si element around the main container 141 can be adopted in one embodiment of the present invention.
[0275] The high melting point container 142 is preferably configured to include a high melting point material having a melting point that is equal to or higher than the melting point of the material constituting the main body container 141 .
[0276] The high melting point container 142 can be exemplified by: C as a general heat-resistant component, W, Re, Os, Ta, Mo as high melting point metals, Ta9C8, HfC, TaC, NbC, ZrC, Ta2C, TiC, WC, MoC as carbides, HfN, TaN, BN, Ta2N, ZrN, TiN as nitrides, HfB2, TaB2, ZrB2, NB2, TiB2 as borides, SiC polycrystals, etc.
[0277] like Fig.12 As shown, the high melting point container 142 is a fitting container including an upper container 142b and a lower container 142a that can fit together, like the main container 141, and is configured to accommodate the main container 141. A small gap 43 is formed at the fitting portion between the upper container 142b and the lower container 142a, and it is configured to be possible to exhaust (evacuate) the inside of the high melting point container 142 through the gap 43.
[0278] The high melting point container 142 has a Si vapor supply material capable of supplying a vapor pressure of a gaseous species including the Si element into the high melting point container 142 .
[0279] The Si vapor supply material may be any material as long as it generates Si vapor in the high melting point container 142 during the heat treatment, and examples thereof include solid Si (Si particles such as Si wafers or Si powder) or Si compounds.
[0280] In addition, the Si vapor supply material is, for example, a thin film covering the inner wall of the high melting point container 142 .
[0281] When the high melting point container 142 is a metal compound such as TaC, the Si vapor supply material is, for example, a silicide material of metal atoms and Si atoms constituting the high melting point container 142 .
[0282] The high-melting-point container 142 can maintain the vapor pressure environment of the gas-phase species containing Si elements in the main container 141 by having a Si vapor supply material on its inner side. It can be understood that this is because the vapor pressure of the gas-phase species containing Si elements in the main container 141 is balanced with the vapor pressure of the gas-phase species containing Si elements outside the main container 141.
[0283] This specification will explain the effects of the present invention with reference to Reference Examples 1 to 3.
[0284] 《Reference Example 1》
[0285] Under the following conditions, the SiC single-crystal substrate E10 was placed in the main container 141, and the main container 141 was placed in the high-melting-point container 142.
[0286] <SiC single-crystal substrate E10>
[0287] Polymorphism: 4H-SiC
[0288] Substrate size: Width (10 mm), length (10 mm), thickness (0.3 mm)
[0289] Off-axis direction and off-axis angle: 4° off in the <11-20> direction
[0290] Growth surface: (0001) crystal plane
[0291] Presence or absence of MSB: None
[0292] Separation layer or strain layer: None
[0293] Material: SiC polycrystal
[0294] Container size: Diameter (60 mm), height (4.0 mm)
[0295] Distance between the SiC single-crystal substrate E10 and the SiC material: 2.0 mm
[0296] Si / C atomic ratio in the container: 1 or less
[0297] Material: TaC
[0298] Container size: Diameter (160 mm), height (60 mm)
[0299] Si vapor supply material (Si compound): TaSi2
[0300] Under the following conditions, the SiC single-crystal substrate E10 set under the above conditions was heat-treated.
[0301] Heating temperature: 1700 °C
[0302] Heating time: 300min
[0303] Temperature gradient: 1.0℃ / mm
[0304] Growth rate: 5.0nm / min
[0305] Vacuum degree of main heating chamber 143c: 10 -5 Pa
[0306] Fig.13 This is an explanatory diagram of a method for obtaining the conversion rate from BPD to other defects / dislocations (TED, etc.) in the growth layer E11.
[0307] Fig.13 (a) in FIG. 1 shows a state where the growth layer E11 is grown by a heating step. In this heating step, the BPD present in the SiC single crystal substrate E10 is transformed into TED with a certain probability. Therefore, unless 100% transformation is performed, TED and BPD exist mixedly on the surface of the growth layer E11.
[0308] Fig.13 (b) in the figure shows the condition of defects in the growth layer E11 confirmed by using the KOH dissolution etching method. The KOH dissolution etching method is a method in which the SiC single crystal substrate E10 is immersed in a dissolved salt (KOH, etc.) heated to about 500°C, an etching pit is formed at the dislocation or defect portion, and the type of dislocation is determined based on the size / shape of the etching pit. By this method, the number of BPDs present at the surface of the growth layer E11 is evaluated.
[0309] Fig.13 (c) shows the state where the growth layer E11 is removed after KOH dissolution etching. In this method, after being flattened to the depth of the etching pit by mechanical polishing, CMP, etc., the growth layer E11 is removed by thermal etching to expose the surface of the SiC single crystal substrate E10.
[0310] Fig.13 (d) shows a state where defects in the SiC single crystal substrate E10 were confirmed using a KOH dissolution etching method for the SiC single crystal substrate E10 from which the growth layer E11 was removed. This method evaluated the number of BPDs present on the surface of the SiC single crystal substrate E10.
[0311] according to Fig.13 The series of sequences shown in FIG. 1 and FIG. 2 show the number of BPDs present at the surface of the growth layer E11 (refer to Fig.13 (b)) and the number of BPDs present on the surface of SiC single crystal substrate E10 ( Fig.13 By comparing with (d) in the figure, the BPD transformation rate from BPD to other defects / dislocations through heat treatment can be obtained.
[0312] The number of BPDs present on the surface of the growth layer E11 in Reference Example 1 was approximately 0 / cm 2 , and the number of BPDs present on the surface of the SiC single crystal substrate E10 was 1000 / cm 2 . That is, it can be understood that by placing the SiC single crystal substrate E10 having no MSB on the surface in a quasi-closed space with a Si / C atomic ratio of 1 or less and heating it, BPDs are reduced / removed.
[0313] In Reference Example 1, it can be understood that since a SiC-C equilibrium vapor pressure environment is formed in the main container 141, the Si / C atomic ratio in the main container 141 is 1 or less, and thus BPDs can also be reduced / removed in the growth step S1.
[0314] 《Reference Example 2》
[0315] Under the following conditions, the SiC single crystal substrate E10 was placed in the main container 141, and the main container 141 was placed in the high melting point container 142.
[0316] <SiC single crystal substrate E10>
[0317] Polymorph: 4H-SiC
[0318] Substrate size: horizontal width (10 mm), vertical width (10 mm), thickness (0.3 mm)
[0319] Off-axis direction and off-axis angle: 4° off in the <11-20> direction
[0320] Growth surface: (0001) crystal plane
[0321] Presence or absence of MSB: Yes
[0322] Material: SiC polycrystal
[0323] Container size: diameter (60 mm), height (4.0 mm)
[0324] Distance between the SiC single crystal substrate E10 and the SiC material: 2.0 mm
[0325] Si vapor supply source: Si wafer
[0326] Si / C atomic ratio in the container: More than 1
[0327] By placing the Si wafer together with the SiC single crystal substrate in the main container 141, the Si / C atomic ratio in the container exceeds 1.
[0328] Material: TaC
[0329] Container size: diameter 160mm x height 60mm
[0330] Si vapor supply material (Si compound): TaSi2
[0331] The SiC single crystal substrate E10 set under the above conditions was heat-treated under the following conditions.
[0332] Heating temperature: 1800℃
[0333] Heating time: 60min
[0334] Temperature gradient: 1.0℃ / mm
[0335] Growth rate: 68nm / min
[0336] Vacuum degree of main heating chamber 143c: 10 -5 Pa
[0337] Fig.14 This is a SEM image of the surface of the SiC single crystal substrate E10 before the growth of the growth layer E11. Fig.14 (a) is a SEM image observed at ×1000 magnification. Fig.14 (b) is a SEM image observed at ×100,000 magnification. It can be understood that MSB is formed on the surface of the SiC single crystal substrate E10 before the growth of the growth layer E11, and steps with a height of 3.0 nm or more are arranged with an average platform width of 42 nm. In addition, the step height was measured by AFM.
[0338] Fig.15 This is a SEM image of the surface of the SiC single crystal substrate E10 after the growth of the growth layer E11. Fig.15 (a) is a SEM image observed at ×1000 magnification. Fig.15 (b) is a SEM image observed at ×100,000 magnification.
[0339] It can be understood that no MSB is formed at the surface of the growth layer E11 of Reference Example 2, and steps of 1.0 nm (full cell) are regularly arranged with a terrace width of 14 nm. In addition, the step height was measured by AFM.
[0340] Therefore, it can be understood that the growth layer E11 in which the MSB is decomposed is formed by placing the SiC single crystal substrate E10 having the MSB on the surface in a quasi-closed space having a Si / C atomic ratio exceeding 1 and heating it.
[0341] In Reference Example 2, since the Si vapor supply source is set so that the Si / C atomic ratio in the main body container 141 exceeds 1, a SiC-Si equilibrium vapor pressure environment is formed in the main body container 141. Therefore, it can be understood that the MSB on the surface of the SiC single crystal substrate can be decomposed even in the growth step S1.
[0342] 《Reference Example 3》
[0343] Fig.16 It is a graph showing the relationship between the heating temperature and the growth rate obtained by the method for manufacturing a SiC single crystal substrate according to the present invention. The horizontal axis of the graph is the inverse of the temperature, and the vertical axis of the graph represents the growth rate logarithmically. The result obtained by setting the SiC single crystal substrate E10 in a space (in the main container 141) where the Si / C atomic number ratio exceeds 1 and growing the growth layer E11 on the SiC single crystal substrate E10 is indicated by the ○ mark. In addition, the result obtained by setting the SiC single crystal substrate E10 in a space (in the main container 141) where the Si / C atomic number ratio is less than 1 and growing the growth layer E11 on the SiC single crystal substrate E10 is indicated by the × mark.
[0344] In addition, Fig.16 In the curve graph, the thermodynamic calculation results of the growth of the SiC substrate in the SiC-Si equilibrium vapor pressure environment are represented by the dotted line (Arrhenius diagram), and the thermodynamic calculation results of the growth of the SiC substrate in the SiC-C equilibrium vapor pressure environment are represented by the double-dotted line (Arrhenius diagram).
[0345] In this method, under the condition that the vapor pressure environment between the SiC raw material and the SiC substrate becomes a SiC-C equilibrium vapor pressure environment or a SiC-C equilibrium vapor pressure environment, the chemical potential difference or the temperature gradient is used as the growth driving force to grow the SiC single crystal substrate E10. The chemical potential difference can be exemplified by the partial pressure difference of the gas phase species generated on the surface of the SiC polycrystal and the SiC single crystal.
[0346] Here, when the partial pressure difference of the vapor generated from the SiC raw material (transport source) and the SiC substrate (transport destination) is taken as the growth amount, the SiC growth rate is calculated by the following formula 1.
[0347] [Formula 1]
[0348]
[0349] Here, T is the temperature of the SiC raw material side, m i For gas phase species (Si x C y ) is the molecular weight, and k is the Boltzmann constant. In addition, P 输送源i -P输送目的地i This is the amount of growth that causes SiC to precipitate when the raw material gas becomes supersaturated, and the raw material gas may include SiC, Si2C, or SiC2.
[0350] Therefore, the dotted line is the result of thermodynamic calculation when SiC single crystal is grown using SiC polycrystal as raw material in a vapor pressure environment when SiC (solid) and Si (liquid phase) are in phase equilibrium through the gas phase. Specifically, the result is obtained by thermodynamic calculation under the following conditions (i) to (iv) using formula 1.
[0351] (i) is the SiC-Si equilibrium vapor pressure environment with constant volume;
[0352] (ii) The growth driving force is the temperature gradient in the main container 141 and the vapor pressure difference (chemical potential difference) between the SiC polycrystal and the SiC single crystal;
[0353] (iii) The raw material gas is SiC, Si2C, SiC2;
[0354] (iv) The adsorption coefficient of the raw material to the step of the SiC single crystal substrate E10 is 0.001.
[0355] In addition, the double-dotted dashed line is the result of thermodynamic calculation when SiC single crystal is grown using SiC polycrystal as raw material in a vapor pressure environment when SiC (solid phase) and C (solid phase) are in phase equilibrium through the gas phase. Specifically, this result is obtained by thermodynamic calculation under the following conditions (i) to (iv) using formula 1.
[0356] (i) is the SiC-C equilibrium vapor pressure environment with constant volume;
[0357] (ii) The growth driving force is the temperature gradient in the main container 141 and the vapor pressure difference (chemical potential difference) between the SiC polycrystal and the SiC single crystal;
[0358] (iii) The raw material gas is SiC, Si2C, SiC2;
[0359] (iv) The adsorption coefficient of the raw material to the step of the SiC single crystal substrate E10 is 0.001.
[0360] In addition, the data of each chemical species used in the thermodynamic calculation adopted the values of the JANAF thermochemical table.
[0361] According to the Fig.16From the curve graph, it can be understood that the result (○ mark) obtained by setting the SiC single crystal substrate E10 in a space (in the main container 141) where the Si / C atomic number ratio exceeds 1 and growing the growth layer E11 on the SiC single crystal substrate E10 is consistent with the thermodynamic calculation results of SiC growth in the SiC-Si equilibrium vapor pressure environment. In addition, it can be understood that the result (× mark) obtained by setting the SiC single crystal substrate E10 in a space (in the main container 141) where the Si / C atomic number ratio is less than 1 and growing the growth layer E11 on the SiC single crystal substrate E10 is consistent with the thermodynamic calculation results of SiC growth in the SiC-C equilibrium vapor pressure environment.
[0362] It can be understood that, under the SiC-Si equilibrium vapor pressure environment, a growth rate of 1.0 μm / min or more is achieved at a heating temperature of 1960°C. In addition, it can be understood that a growth rate of 2.0 μm / min or more is achieved at a heating temperature of 2000°C or more. On the other hand, it can be understood that, under the SiC-C equilibrium vapor pressure environment, a growth rate of 1.0 μm / min or more is achieved at a heating temperature of 2000°C or more. In addition, it can be understood that a growth rate of 2.0 μm / min or more is achieved at a heating temperature of 2030°C or more.
[0363] According to the present invention, a high-quality SiC semiconductor device can be provided in which the growth step S1 , the device formation step S2 , and the separation step S3 are combined.
[0364] Description of Reference Numerals
[0365] 1 Processed object
[0366] 1a Back surface
[0367] 4 SiC raw materials
[0368] 4a Main surface
[0369] 10 Growth layer
[0370] 11 Original substrate
[0371] 12 SiC semiconductor device formed on growth layer 10
[0372] 23 Insulation film
[0373] 43 Gap
[0374] 101a Steps
[0375] 101b Platform
[0376] 102a Steps
[0377] 102b Platform
[0378] 103a Steps
[0379] 103b Platform
[0380] 111 Substrate
[0381] 141 Main container
[0382] 141a Setting utensils
[0383] 141b Lower container
[0384] 141c Upper container
[0385] 142 High Melting Point Container
[0386] 142a Lower container
[0387] 142b Upper container
[0388] 143 Heating furnace
[0389] 143a Preparation Room
[0390] 143b Mobile Device
[0391] 143c Main heating chamber
[0392] 143d Heater
[0393] 143e Inert gas injection valve
[0394] 143f Vacuum forming valve
[0395] 143g Vacuum Gauge
[0396] 211 Circuit Pattern
[0397] 220 Drift Area
[0398] 221 Well region
[0399] 222 Contact area
[0400] 226 Low concentration area
[0401] 230 Insulation film
[0402] 240 Gate electrode
[0403] 241 Source electrode
[0404] 242 Drain electrode
[0405] 244 Anode Electrode
[0406] 245 cathode electrode
[0407] 300 Separation Layer
[0408] 301 Crystal dislocation
[0409] 302 Damage Area
[0410] 311 Light Source
[0411] 312 Converging device
[0412] E10 SiC single crystal substrate
[0413] E11 Growth layer
[0414] S1 Growth Step
[0415] S11 Epitaxial growth step
[0416] S12 Bunch Decomposition Steps
[0417] S2 Device Formation Steps
[0418] S21 Composition steps
[0419] S22 doping step
[0420] S23 Insulation film forming step
[0421] S24 Electrode Formation Step
[0422] S3 separation step
[0423] S31 Separation layer forming step
[0424] S32 Stripping Step
[0425] S4 Etching Step
[0426] W1 Platform Length
[0427] W2 Platform Length
[0428] W3 Platform Length
Claims
1. A method for manufacturing a SiC semiconductor device, comprising: A growth step of forming a growth layer on a workpiece including a SiC single crystal; a device forming step of forming at least a portion of a SiC semiconductor device in the growth layer; as well as a separation step of separating at least a portion of the SiC semiconductor device from the object to be processed, The growth step comprises: placing the object to be processed in a main body container composed of a material containing SiC polycrystal and heating it, thereby forming a first growth layer having a bunched surface; and then placing the object to be processed and a Si vapor supply source in a main body container composed of a material containing SiC polycrystal and heating it, thereby forming a second growth layer on the surface of the first growth layer, wherein the second growth layer has a surface that terminates at a step having a height of a full unit cell.
2. The manufacturing method according to claim 1, wherein: The growth step heat-treats the object to be processed in an atmosphere containing Si element and C element.
3. The manufacturing method according to claim 2, wherein: The growth step heat-treats the object to be processed in a quasi-enclosed space where the SiC material is exposed.
4. The manufacturing method according to claim 1, wherein: The device forming step performs a patterning step of forming a circuit pattern on the second growth layer.
5. The manufacturing method according to claim 1, wherein: The device forming step performs a doping step of introducing dopant atoms into the second growth layer.
6. The manufacturing method according to claim 1, wherein: The device forming step performs an insulating film forming step of introducing an insulating film into the second growth layer.
7. The manufacturing method according to claim 1, wherein: The device forming step performs an electrode forming step of forming an electrode on the second growth layer.
8. The manufacturing method according to claim 1, wherein: The separation step includes: a separation layer forming step of forming a separation layer inside the processed body including the first growth layer and the second growth layer; and a stripping step of stripping a portion of the processed body including the first growth layer and the second growth layer starting from the separation layer.
9. The manufacturing method according to claim 8, wherein: The separation layer forming step forms the separation layer by irradiating the object with laser light so that the inner part becomes a focus.
10. The manufacturing method according to claim 1, wherein: An etching step of performing heat treatment on the object to be processed in an atmosphere containing Si element and C element and etching the object to be processed is performed.
11. The manufacturing method according to claim 10, wherein: The etching step heat-treats the object to be processed in a quasi-enclosed space where the SiC material is exposed.
12. The manufacturing method according to claim 10 or 11, wherein: The method includes the separation step, the etching step and the growth step in sequence.