Composition for dissolving polishing particles and cleaning method using the same
By using sulfur-containing organic acids, fluorine-containing ionic compounds and solvent compositions after chemical mechanical polishing, the problem of residual polishing particles is solved, efficient dissolution and removal of polishing particles is achieved, and damage to semiconductor devices is reduced, and more Excellent cleaning effect.
Patent Information
- Application Number
- CN202111289645.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-06
- Filing Date
- 2021-11-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-11-02
AI Technical Summary
After the chemical mechanical polishing (CMP) process, polished particles remain on the surface of the semiconductor device and are difficult to completely remove, resulting in scratches and quality problems during subsequent processing. Existing cleaning methods such as hydrofluoric acid treatment may lead to surface defects.
A composition, including sulfur-containing organic acids, fluorine-containing ionic compounds and solvents, is used to dissolve polished particles and by-products, and efficient dissolution and removal of polished particles is achieved by adjusting the proportion and temperature conditions of the composition.
The composition can reduce the turbidity change rate to -80 to -99% in 15 minutes at 60°C, effectively remove polished particles and by-products, reduce damage to semiconductor devices, and replace traditional hydrogen peroxide mixture cleaning solution , providing better cleaning results.
Smart Images

Figure BDA0003334212510000101 
Figure BDA0003334212510000111 
Figure BDA0003334212510000112
Abstract
Description
Technical Field
[0001] The present invention relates to a composition for dissolving polishing particles and a cleaning method using the same, and more particularly, to a composition for dissolving polishing particles and a cleaning method using the same, wherein the composition for dissolving polishing particles can be used as a cleaning liquid for cleaning a substrate after chemical mechanical polishing (CMP). Background Art
[0002] Chemical Mechanical Polishing (CMP) is a process for removing any material from the surface of a semiconductor device, where the surface is polished by physical processes (e.g., polishing) and chemical processes (e.g., oxidation or chelation). In its most basic form, CMP involves applying a CMP slurry (e.g., a solution of an active compound and polishing particles) to a polishing pad, which polishes the surface of a semiconductor wafer to achieve removal, flattening, and polishing processes. During the polishing of the wafer in the CMP process, the polishing particles included in the CMP slurry solution tend to aggregate with each other. Due to this aggregation of polishing particles, even if the CMP process is completed, a large number of particles with a size of several μm or more may remain on the wafer, and defects such as scratches on the wafer surface may be caused by the above particles during subsequent processing. Therefore, after performing the CMP process, a cleaning process is required to remove contaminants such as aggregated particles from the wafer surface.
[0003] After performing a polishing process using polishing particles such as silicon dioxide slurry or ceria slurry, a cleaning process is required to remove polishing debris, polishing particles, organic residues or by-products remaining on the surface of the substrate. In addition, in order to cope with the next generation of semiconductor process technology, the requirements for the research and development of new cleaning processes and equipment are becoming increasingly higher.
[0004] The cleaning process for cleaning a semiconductor wafer on which a CMP process is performed may include a cleaning method using a brush to scrub (scrubbing) and a chemical cleaning method using a cleaning solution. The method of scrubbing with a brush is used to remove pollutants adsorbed on the wafer, such as CMP slurry and CMP residues, and a brush is used when deionized water (DI water) is sprayed on the wafer, thereby mechanically removing the adsorbed pollutants. However, if only a mechanical method using a brush is used, pollutants (such as CMP slurry and CMP residues) may not be completely removed, and may often remain, so it is difficult to perform subsequent processes. After the CMP process, it is necessary to use a cleaning solution formed by a chemical material to completely remove the pollutants remaining on the wafer through an additional cleaning process, and then perform subsequent processes.
[0005] Among cleaning processes using a cleaning liquid, liquid phase cleaning is effective in removing metal contamination, and is generally treated using HPM, SPM, ozone water, DHF, etc. It is difficult to completely remove metal contaminants using HPM and SPM, but DHF is being widely used.
[0006] After performing a CMP process using a ceria CMP slurry, hydrofluoric acid is often used for cleaning to remove ceria particles remaining on the substrate surface as polishing particles. Due to the extremely high solubility of thermal oxide films when cleaning with hydrofluoric acid, scratches or surface defects may occur, which may affect the post-cleaning process and may result in reduced yield and quality of semiconductor devices. Summary of the invention
[0007] Technical issues to be solved
[0008] The object of the present invention is to solve the above-mentioned problems, namely to provide a composition for dissolving polishing particles, which comprises a sulfur-containing organic acid to dissolve and remove the polishing slurry, polishing particles, debris derived from the polishing particles, polishing by-products, etc. remaining after the polishing process, and minimize defects.
[0009] Another object of the present invention is to provide a cleaning method using the composition for dissolving polishing particles according to the present invention after a polishing process.
[0010] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by ordinary technicians in this field through the following description.
[0011] Technical methods to solve problems
[0012] According to an embodiment of the present invention, a composition for dissolving polishing particles comprises: a sulfur-containing organic acid; a fluorine-containing ion compound; and a solvent, wherein the turbidity change reduction rate (%) measured at 60° C. for 15 minutes is -80 to -99.
[0013] According to an embodiment of the present invention, the sulfur-containing organic acid may account for 1 wt % to 10 wt % of the composition for dissolving polishing particles.
[0014] According to one embodiment of the present invention, the sulfur-containing organic acid may include at least one selected from the group consisting of sulfoxylic acid (RSOH), sulfurous acid (RSO(OH)), organic sulfonic acid (RS(=0)2-OH), thiosulfonic acid (RSO2SH)) and thiocarboxylic acid (RC(S)OH).
[0015] According to an embodiment of the present invention, the organic sulfonic acid may include at least one selected from the group consisting of alkane sulfonic acid, alkanol sulfonic acid, sulfosuccinic acid and aromatic sulfonic acid.
[0016] According to an embodiment of the present invention, the fluorine ion compound may account for 2 wt % to 10 wt % of the composition for dissolving polishing particles.
[0017] According to an embodiment of the present invention, the fluorine-containing ion compound may be an ionic fluoride compound.
[0018] According to an embodiment of the present invention, the fluorine-containing ion compound may include at least one selected from the group consisting of ammonium fluoride, ammonium bifluoride, ammonium fluoroborate, ammonium silico fluoride, aminobenzotrifluoride, tetramethylammonium fluoride, tetraethylammonium fluoride, tetrabutylammonium difluorotriphenylsilicate, tetrabutylammonium fluoride and benzyltrimethylammonium fluoride.
[0019] According to one embodiment of the present invention, the composition further includes at least one sulfur-containing compound selected from the group consisting of thiosulfuric acid (H2S2O3), sulfuric acid (Sulfuric acid), sulfide (Sulfide), disulfide (RSS-R'), hydrogen sulfide (H2S), sulfur trioxide (SO3), aminosulfonic acid (Sulfamic acid), mercaptan (R-SH) and sulfonate, and the sulfur-containing compound can account for 5 weight % to 15 weight % of the composition for dissolving polishing particles.
[0020] According to an embodiment of the present invention, the mass ratio of the sulfur-containing compound to the sulfur-containing organic acid may be 2:1 to 5:1.
[0021] According to one embodiment of the present invention, the sulfonate may include at least one selected from the group consisting of alkylsulfonate, arylsulfonate, alkylarylsulfonate, alkylethersulfonate, polystyrenesulfonate, alkanesulfonate, α-olefinsulfonate, dodecylbenzenesulfonate and alkylbenzenesulfonate.
[0022] The composition for dissolving polishing particles can be used for cleaning after polishing a semiconductor device wafer, wherein the semiconductor device includes at least one film selected from the group consisting of a silicon nitride film, a silicon oxide film, a polysilicon film, and a silicon film.
[0023] According to an embodiment of the present invention, the composition for dissolving polishing particles can dissolve residual polishing particles after polishing is performed using a slurry for chemical mechanical polishing (CMP) containing the polishing particles.
[0024] According to an embodiment of the present invention, the polishing particles may include cerium dioxide.
[0025] The cleaning method according to an embodiment of the present invention comprises the following steps: after chemical mechanical polishing of a semiconductor device wafer, cleaning the semiconductor device wafer using the composition for dissolving polishing particles according to the present invention.
[0026] According to an embodiment of the present invention, the semiconductor device wafer may include at least one film selected from the group consisting of a silicon nitride film, a silicon oxide film, a polysilicon film, and a silicon film.
[0027] Effects of the Invention
[0028] The present invention can provide a composition for dissolving polishing particles, the composition comprising a sulfur-containing organic acid to dissolve and remove the polishing slurry, polishing particles, debris from the polishing particles, polishing byproducts, etc. remaining after the polishing process, and minimize defects. In addition, the composition for dissolving polishing particles according to the present invention can be used as a cleaning liquid for removing and cleaning polishing contaminants, and in particular, can be used as a cleaning liquid that can replace sulfuric acid peroxide mixture (SPM, Sulfuric acid peroxide mixture). DETAILED DESCRIPTION
[0029] The embodiments of the present invention are described in detail below. In the process of describing the present invention, when it is judged that the specific description of the relevant known functions or structures unnecessarily confuses the gist of the present invention, the detailed description thereof is omitted. In addition, the terms used in this specification are used to accurately express the preferred embodiments of the present invention, and may vary according to the intention of the user or the user or the conventions in the technical field described in the present invention. Therefore, the definition of this term should be defined according to the overall content of this specification.
[0030] In the overall specification, when it is stated that a certain component is “on” other components, it not only refers to the case where the certain component contacts other components, but also includes the case where other components exist between the two components.
[0031] Throughout the specification, when it is stated that a certain part “includes” a certain constituent element, it does not mean that other constituent elements are excluded and other constituent elements may be included.
[0032] Hereinafter, the composition for dissolving polishing particles of the present invention and the cleaning method using the same will be specifically described with reference to Examples. However, the present invention is not limited to the above Examples.
[0033] The present invention relates to a composition for dissolving polishing particles. According to an embodiment of the present invention, the composition for dissolving polishing particles may include: a sulfur-containing organic acid; a fluorine-containing ion compound; and a solvent.
[0034] According to an embodiment of the present invention, the sulfur-containing organic acid may be an organic acid having sulfur and / or sulfur-containing functional groups in the molecule, and may be used as a dissolving activator to dissolve polishing byproducts, such as residual polishing liquid, polishing debris or particles, etc. The sulfur-containing organic acid may account for 1 wt % to 10 wt % of the composition for dissolving polishing particles, and when the content is less than the above range, dissolution may not be performed; when it exceeds the above range, chemical materials may be precipitated, or solubility may be reduced.
[0035] As an example of the present invention, the sulfur-containing organic acid may include at least one selected from the group consisting of sulfurous acid (Sulfenic acid, RSOH), sulfurous acid (Sulfinic acid, RSO(OH)), organic sulfonic acid (Sulfonic acid, RS(=0)2-OH), thiosulfonic acid (Thiosulfonic acid, (RSO2SH)) and thiocarboxylic acid (Thiocarboxylic acid, RC(S)OH). Here, R may be selected from hydrogen, substituted or unsubstituted hydrocarbons (e.g., alkyl groups having 1 to 20 carbon atoms, substituted or unsubstituted aryl groups having 6 to 30 carbon atoms, and substituted or unsubstituted aralkyl groups) (e.g., benzyl, phenyl, tolyl, naphthyl, etc.) and esters, but is not limited thereto, and will be described in detail below. The substitution may be substituted from at least one of hydroxyl (-OH), halogen, carboxyl (-COOH), alkyl groups having 1 to 10 carbon atoms, and aryl groups having 6 to 10 carbon atoms. The salt may be an inorganic salt or an organic salt, for example, a sodium salt, a potassium salt, a magnesium salt or an ammonium salt.
[0036] As an example of the present invention, the organic sulfonic acid may include at least one selected from the group consisting of alkane sulfonic acid, alkanol sulfonic acid, sulfosuccinic acid and aromatic sulfonic acid. As an example of the present invention, the alkane sulfonic acid may be CnH 2n+1 SO3H (for example, n=1 to 20), and for example, methanesulfonic acid, ethanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, 1-butanesulfonic acid, 2-butanesulfonic acid, pentanesulfonic acid, and the like may be mentioned.
[0037] As an example of the present invention, the alkanol sulfonic acid can be composed of C m H 2m+1 -CH(OH)-C p H 2p -SO3H (for example, m=0 to 10, p=1 to 10), and for example, it can be 2-hydroxyethane-1-sulfonic acid (hydroxyethanesulfonic acid), 2-hydroxypropane-1-sulfonic acid (2-propanolsulfonic acid), 3-hydroxypropane-1-sulfonic acid, 2-hydroxybutane-1-sulfonic acid, 2-hydroxypentane-1-sulfonic acid, 1-hydroxypropane-2-sulfonic acid, 4-hydroxybutane-1-sulfonic acid and 2-hydroxyhexane-1-sulfonic acid, etc.
[0038] As an example of the present invention, the aromatic sulfonic acid may be benzenesulfonic acid, alkylbenzenesulfonic acid, aminobenzenesulfonic acid, nitrobenzenesulfonic acid, sulfobenzoic acid, hydroxybenzenesulfonic acid, toluenesulfonic acid, phenolsulfonic acid, naphthalenesulfonic acid, alkylnaphthalenesulfonic acid, naphtholsulfonic acid, xylenesulfonic acid, cresolsulfonic acid, sulfosalicylic acid (5-sulfosalicylic acid), polystyrenesulfonic acid, diphenylamine-4-sulfonic acid, etc. Here, the alkyl group may be selected from 1 to 20 carbon atoms.
[0039] As an example of the present invention, the sulfur-containing organic acid may be of two or more types. The ratio of the first compound to the second compound may be 1 to 10: 1 to 10; or 1 to 5: 1 to 5 (w / w), or the ratio of the first compound, the second compound and the third compound may be 1 to 10: 1 to 10: 1 to 10; or 1 to 5: 1 to 5: 1 to 5 (w / w).
[0040] As an example of the present invention, the composition for dissolving polishing particles may further include a sulfur-containing compound to further activate the dissolution of the polishing particles.
[0041] As an example of the present invention, the sulfur-containing compound may account for 5 to 15 weight % of the composition for dissolving polishing particles. When its content is less than 5 weight %, the dissolution activity of the polishing particles may not be increased; when it exceeds 20 weight %, the semiconductor substrate may be affected to cause defects, and the solution may precipitate, or an addition reaction may occur.
[0042] As an example of the present invention, the sulfur-containing compound may include thiosulfuric acid (H2S2O3), sulfuric acid (Sulfuric acid), sulfide (Sulfide), disulfide (Bisulfide, RSS-R'), hydrogen sulfide (H2S), sulfur trioxide (SO3), aminosulfonic acid (Sulfamicacid), mercaptan (Mercaptan, R-SH), sulfate (Sulfate), sulfonate (Sulfonate, R-SO3 -, R-SO3-R') and at least one selected from the group consisting of its salts and its anhydrides. Here, R and R' may be selected from hydrogen, substituted or unsubstituted hydrocarbons (e.g., alkyl groups having 1 to 20 carbon atoms, substituted or unsubstituted aryl groups having 6 to 30 carbon atoms, and substituted or unsubstituted aralkyl groups) (e.g., benzyl, phenyl, tolyl, naphthyl, etc.) and esters, but are not limited thereto, and will be described in detail below. The substitution may be substituted from at least one of hydroxyl (-OH), carboxyl (-COOH), alkyl groups having 1 to 10 carbon atoms, and aryl groups having 6 to 10 carbon atoms. The salt may be an inorganic salt or an organic salt, for example, a sodium salt, a potassium salt, a magnesium salt, an ammonium salt, etc.
[0043] As an example of the present invention, the sulfonate may be a salt or ester of the sulfonic acid, for example, an alkyl sulfonate, an aryl sulfonate, an alkyl aryl sulfonate, an alkyl ether sulfonate, a polystyrene sulfonate, an alkane sulfonate, an α-olefin sulfonate, a dodecyl benzene sulfonate, an alkyl benzene sulfonate, etc. Here, the alkyl and alkane may be selected from 1 to 20 carbon atoms, and the aryl may be selected from 6 to 30 carbon atoms.
[0044] As an example of the present invention, the sulfur-containing compound may be of two or more types. The ratio of the first compound to the second compound may be 1 to 10: 1 to 10; or 1 to 5: 1 to 5 (w / w), or the ratio of the first compound, the second compound and the third compound may be 1 to 10: 1 to 10: 1 to 10; or 1 to 5: 1 to 5: 1 to 5 (w / w).
[0045] As an example of the present invention, the fluorine-containing ion compound can be used as an etchant and a reduction catalyst to help polishing particles remaining after the polishing process, byproducts derived from the polishing particles, etc., dissolve in water in the form of hydrates.
[0046] As an example of the present invention, the fluorine ion compound may account for 2 wt % to 10 wt % of the composition for dissolving polishing particles, and when its content is less than 2 wt %, hydrates may not be generated; and when it exceeds 10 wt %, the semiconductor substrate may be affected to cause defects.
[0047] As an example of the present invention, the fluorine-containing ion compound may be an ionic fluoride compound. The fluorine-containing ion compound may include at least one selected from the group consisting of ammonium fluoride, ammonium bifluoride, ammonium fluoroborate, ammonium silico fluoride, aminobenzotrifluoride, tetramethylammoniumfluoride, tetraethylammoniumfluoride, tetrabutylammonium difluorotriphenylsilicate, tetrabutylammoniumfluoride, and benzyltrimethylammoniumfluoride.
[0048] As an example of the present invention, the mass ratio of the sulfur-containing compound to the sulfur-containing organic acid may be 2: 1 to 5: 1. As an example of the present invention, the mass ratio (w / w) of the sulfur-containing organic acid to the fluorine-containing ion compound may be 1: 1 to 1: 15. That is, when the sulfur-containing organic acid and the fluorine-containing ion compound are included in the above mass ratio range, excellent solubility of the polishing particles and their byproducts can be obtained, and damage to the semiconductor substrate can be minimized.
[0049] According to one embodiment of the present invention, the solvent may include water and / or an organic solvent. The solvent in the composition may be used to dissolve and / or disperse other components in the composition. Preferably, the solvent does not include impurities that inhibit the effects of other components as much as possible. Specifically, the solvent may include ion exchange water, or pure water, ultrapure water, deionized water or distilled water, wherein the ion exchange water uses an ion exchange resin to remove impurity ions, and then removes foreign matter therefrom through a filter.
[0050] As an example of the present invention, the pH value of the composition may be in the range of 2 to 7. When the pH is within the above pH range, and when a substrate on which CMP is performed (e.g., a wafer for processing a semiconductor device using the composition) is treated, contaminants such as polishing particles, organic materials, and impurities remaining in the cleaning process may be sufficiently removed, thereby minimizing defects.
[0051] As an example of the present invention, the dissolution and removal performance of the composition relative to polishing particles, debris derived from polishing particles, and polishing by-products can be confirmed based on the change in turbidity. For example, at room temperature (rt) to 80°C; 50°C to 70°C or about 60°C, the turbidity change reduction rate (%) measured for 15 minutes in a mixed solution including the composition and any one of polishing particles, debris derived from polishing particles, and polishing by-products can be -80 to -99.
[0052] According to one embodiment of the present invention, the composition can be used to clean polishing particles on the surface of a substrate after a CMP process or a substrate on which foreign matter originating from polishing particles adheres and / or remains. For example, the substrate can be a substrate for a semiconductor device, such as a silicon substrate, a sapphire substrate, a quartz substrate, a glass substrate, a ceramic substrate, etc.
[0053] As an example of the present invention, the semiconductor device wafer may include at least one film selected from the group consisting of silicon nitride film, silicon oxide film, polysilicon film and silicon film, and the film may be used as a polishing object film or a polishing stop film in a polishing process.
[0054] As an example of the present invention, the composition can be used to remove defects, residues and contaminants on the surface of a wafer of a polished semiconductor device, and can be used to dissolve and / or remove polishing process residues (e.g., polishing particles, foreign matter derived from polishing particles) after a CMP process.
[0055] As an example of the present invention, the residue may be polishing particles of CMP polishing slurry, materials derived from polishing particles, chemical materials present in CMP slurry, byproducts of CMP polishing slurry, carbon-rich particles, polishing pad particles, brush-off particles, equipment materials, metals and metal oxides, etc. For example, it may be used to dissolve and / or remove polishing particles of CMP slurry including polishing particles and / or debris and particles derived from the polishing particles.
[0056] As an example of the present invention, the polishing particles of the chemical mechanical polishing slurry may include at least one selected from the group consisting of metal oxides, metal oxides coated with organic or inorganic substances, and metal oxides in a colloidal state, and the metal oxide may include at least one selected from the group consisting of silicon dioxide, ceria, zirconium oxide, aluminum oxide, titanium dioxide, barium titanate, germanium oxide, manganese oxide and magnesium oxide, preferably, ceria.
[0057] As an example of the present invention, the polishing particles may include single-sized particles ranging from 10 nm to 200 nm or mixed particles having two or more different sizes ranging from 10 nm to 200 nm.
[0058] The present invention relates to a composition for dissolving polishing particles and a cleaning method using the same. According to one embodiment of the present invention, the cleaning method may include the following steps: after chemical mechanical polishing of a semiconductor device wafer, using the composition for dissolving polishing particles of the present invention to clean the semiconductor device wafer.
[0059] Hereinafter, the present invention will be described in detail with reference to the following examples and comparative examples. However, the technical concept of the present invention is not limited thereto.
[0060] Example 1
[0061] A composition including 1 wt % to 10 wt % of methane sulfonic acid and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0062] Example 2
[0063] A composition including 1 wt % to 10 wt % of methane sulfonic acid (containing 10 times the content of Example 1) and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0064] Example 3
[0065] A composition including 1 wt % to 10 wt % of p-toluene sulfonic acid and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0066] Example 4
[0067] A composition including 1 wt % to 10 wt % of p-toluene sulfonic acid (10 times the content of Example 3) and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0068] Example 5
[0069] A composition including 1 wt % to 10 wt % of methane sulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0070] Example 6
[0071] A composition including 1 wt % to 10 wt % of methane sulfonic acid and 5-sulfosalicylic acid, 5 wt % to 15 wt % of sulfamic acid (methane sulfonic acid:5-sulfosalicylic acid:sulfamic acid=1:1:3 (w / w)), and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0072] Example 7
[0073] A composition including 1 wt % to 10 wt % of methane sulfonic acid, 5 wt % to 15 wt % of sulfamic acid (methane sulfonic acid:sulfamic acid=1:2 (w / w)), and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0074] Example 8
[0075] A composition including 1 wt % to 10 wt % of polystyrene sulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0076] Example 9
[0077] A composition including 1 wt % to 10 wt % of methane sulfonic acid, 5 wt % to 15 wt % of sulfuric acid, and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0078] Example 10
[0079] A composition including 1 wt % to 10 wt % of methane sulfonic acid (6 times that of Example 7), 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0080] Embodiment 11
[0081] A composition including 1 wt % to 10 wt % of methane sulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride (1.1 to 1.5 times that of Example 7) was prepared.
[0082] Example 12
[0083] A composition including 1 wt % to 10 wt % of ethylsulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0084] Embodiment 13
[0085] A composition including 1 wt % to 10 wt % of benzene sulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride is prepared.
[0086] Embodiment 14
[0087] A composition including 1 wt % to 10 wt % of methane sulfonic acid and 5-sulfosalicylic acid (MSA:SSA=1:1 (w / w)) and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0088] Embodiment 15
[0089] A composition including 1 wt % to 10 wt % of methane sulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 1 wt % to 10 wt % of ammonium fluoride was prepared.
[0090] Example 16
[0091] A composition including 1 wt % to 10 wt % of methane sulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride (5 times that of Example 15) was prepared.
[0092] Embodiment 17
[0093] A composition including 1 wt % to 10 wt % of methane sulfonic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride (7 times that of Example 15) was prepared.
[0094] Embodiment 18
[0095] A composition including 1 wt % to 10 wt % of 5-sulfosalicylic acid, 5 wt % to 15 wt % of sulfamic acid, and 2 wt % to 10 wt % of ammonium fluoride was prepared.
[0096] Comparative Example 1
[0097] Commercially available sulfuric acid peroxide mixture (SPM, Sulfuric Peroxide Mixture) cleaning solution.
[0098] Comparative Example 2
[0099] A cleaning solution comprising phosphoric acid and hydrogen peroxide (3:1 (w / w), based on weight %).
[0100] Comparative Example 3
[0101] A composition including 0.1 wt % to 10 wt % of methane sulfonic acid and 5 wt % to 20 wt % of sulfuric acid was prepared.
[0102] * In the examples and comparative examples, the solvent is a residual amount or an appropriate amount of deionized water.
[0103] [Table 1]
[0104]
[0105]
[0106] Observe the change of turbidity (NTU_%)
[0107] In order to verify the dissolution performance of the cerium oxide particles of the cleaning solutions prepared in the examples and comparative examples, each cleaning solution was added to a solution containing 0.01 wt% of cerium oxide slurry, and stirred at room temperature 60°C and 80°C for 1 minute to 15 minutes, respectively, and then the turbidity change was observed using a turbidity change evaluation device (HACH 2100Q). The results are shown in Table 2. The turbidity change was based on a solution containing 0.01 wt% of cerium oxide slurry (turbidity: 169).
[0108] [Table 2]
[0109]
[0110]
[0111] It can be seen from Table 2 that the composition according to the present invention becomes excellent in the solubility of the ceria particles according to the change of turbidity in the process of dissolving the ceria particles. In addition, it can be confirmed that in the cleaning process after the CMP process of the semiconductor device substrate, the solubility of the ceria particles is better than the solubility of the SPM, and therefore, it can be applied to the SPM cleaning step of the cleaning process after the CMP process, or can be used for a cleaning solution that can replace SPM. In addition, considering the dissolution and removal performance of the ceria particles shown in Table 2, in the cleaning method using a brush module in the cleaning process after the CMP process, it is expected that the composition according to the present invention can be used to remove polishing particles and byproducts derived therefrom, residues of the CMP process, etc.
[0112] In summary, the embodiments are described through limited embodiments, and a person skilled in the art can make various modifications and variations to the above description. For example, the described techniques are performed in a different order from the described methods, and / or the described constituent elements are combined or combined in a different form from the described methods, or the same effect can be obtained by replacing or replacing with other constituent elements or equivalents. Therefore, other embodiments, other embodiments, and equivalents of the scope of the claims all belong to the scope of the patent claims.
Claims
1. A composition for dissolving polishing particles, characterized in that: include: Sulfur-containing organic acids; Fluoride-containing compounds; and Solvents, Also includes sulfur compounds, The sulfur-containing organic acid includes at least one selected from the group consisting of methanesulfonic acid, p-toluenesulfonic acid, 5-sulfosalicylic acid, polystyrenesulfonic acid, ethylsulfonic acid and benzenesulfonic acid. The fluorine-containing ion compound is ammonium fluoride, The sulfur-containing compound is aminosulfonic acid, The sulfur-containing organic acid accounts for 1 wt % to 10 wt % of the composition for dissolving polishing particles. The sulfur-containing compound accounts for 5 wt % to 15 wt % of the composition for dissolving polishing particles. The fluorine ion compound accounts for 2 wt % to 10 wt % of the composition for dissolving polishing particles. The mass ratio of the sulfur-containing organic acid to the fluorine-containing ion compound is 1:1 to 1:15, The mass ratio of the sulfur-containing compound to the sulfur-containing organic acid is 2:1 to 5:1, The turbidity change reduction rate measured at 60°C for 15 minutes is -80% to -99%. The composition for dissolving polishing particles dissolves the remaining polishing particles after polishing is performed using a slurry for chemical mechanical polishing containing the polishing particles.
2. The composition for dissolving polishing particles according to claim 1, characterized in that: The composition for dissolving polishing particles is used for cleaning after polishing a semiconductor device wafer, wherein the semiconductor device wafer includes at least one film selected from the group consisting of a silicon nitride film, a silicon oxide film, a polysilicon film, and a silicon film.
3. The composition for dissolving polishing particles according to claim 1, characterized in that: The polishing particles include ceria.
4. A cleaning method, characterized in that: The following steps are involved: After chemical mechanical polishing of a semiconductor device wafer, the semiconductor device wafer is cleaned using the composition for dissolving polishing particles according to any one of claims 1 to 3.
5. The cleaning method according to claim 4, characterized in that: The semiconductor device wafer includes at least one film selected from the group consisting of a silicon nitride film, a silicon oxide film, a polysilicon film, and a silicon film.