A method for removing (Ni, Pt) Al coating by chemical solution corrosion
Through the combination of chemical solution corrosion and sandblasting treatment, the (Ni,Pt)Al coating on nickel-based single crystal high-temperature alloy was successfully removed, solving the problem of coating removal and achieving high performance of re-coated coating and economic benefits extend the service life of the engine blades.
Patent Information
- Application Number
- CN202011269891.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-11-13
AI Technical Summary
The prior art is difficult to effectively remove the (Ni,Pt)Al coating on nickel-based single crystal high-temperature alloys, resulting in a shortening of the life of the matrix alloy and lack of investigation of the matrix state and the performance of the recoating coating after removal.
Using chemical solution corrosion method, the coating was removed in a 45-75℃ water bath using a mixed solution of H2O, HCl, CH3COOH, C6H8O7·H2O. The oxide film and corrosion products were removed in a tangential small pressure sand blasting treatment to ensure the clean surface of the substrate. Prepare to recoat.
Fast and simple coating removal is achieved, ensuring good service performance of the recoated coating, reducing costs, and supporting secondary utilization of the blades and extended engine life.
Smart Images

Figure HDA0002777340660000011 
Figure HDA0002777340660000012 
Figure HDA0002777340660000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of surface treatment of high-temperature protective coatings, in particular to a method for removing (Ni, Pt)Al coatings by chemical solution corrosion. Background Art
[0002] (Ni,Pt)Al coating has excellent comprehensive resistance to high-temperature oxidation and thermal corrosion, and is one of the commonly used commercial coatings for aircraft engines and marine gas turbines. The modification of Pt significantly improves the oxidation resistance of the coating. The coating continuously generates α-Al2O3 by consuming Al, preventing the oxidative atmosphere from oxidizing the base alloy and slowing down the oxidation rate. However, when the coating is exposed to an oxidizing environment for a long time, with the mutual diffusion of elements, the continuous consumption of Al elements, the phase change from β-NiAl to γ'-Ni3Al caused by the decrease in Al content, and the plastic deformation of the coating, the oxide film peels off and the coating degrades until it eventually fails. The nickel-based single crystal high-temperature alloy substrate is relatively expensive. If the failed (Ni,Pt)Al coating can be effectively removed and then coated with (Ni,Pt)Al coating, the base alloy can be effectively utilized and its life can be maximized, which will be of great significance and economic value. If the unqualified or failed coating is removed and a new coating is applied under the premise of ensuring the original performance of the single crystal / directional alloy blade substrate, the blade can be reused again, the service life of the substrate can be extended, and the engine blade can be reused, which is of great significance for the overhaul and life extension of the engine. Foreign countries have imposed strict technical blockades on coating stripping and re-coating technologies. At present, domestic research is mostly focused on the exploration of coating stripping processes, and little attention is paid to the performance evaluation of re-coating coatings. The research on the stripping of (Ni, Pt) Al coatings lacks the surface substrate state after stripping and the performance of the re-coating coating. Summary of the invention
[0003] The purpose of the present invention is to provide a method for removing (Ni, Pt)Al coating by chemical solution corrosion, wherein the substrate after the coating is removed can be re-coated, and the re-coated coating meets the service requirements, thereby realizing the secondary utilization of workpieces such as blades.
[0004] The technical solution of the present invention is:
[0005] A method for removing (Ni, Pt)Al coating by chemical solution corrosion, the specific steps of the method are as follows:
[0006] (1) Pretreatment: The (Ni, Pt) Al coated workpiece with an oxide film after use is subjected to tangential low-pressure sandblasting to remove the non-conductive oxide film on the coating surface; the tangential pressure of the sandblasting is 0.2-0.4 MPa, the sandblasting medium is 200-mesh glass beads, and the angle between the sandblasting direction and the workpiece plane is 30-60°;
[0007] (2) Removing the coating by chemical corrosion: the stripping solution used is a mixed solution of H2O, HCl, CH3COOH, and C6H8O7·H2O. The workpiece is placed in the mixed solution, the water bath heating temperature is 45-75°C, and the stripping time is 30-60 minutes;
[0008] (3) Post-treatment: Sandblasting is used to remove corrosion products attached to the surface in preparation for re-coating of a new (Ni, Pt)Al coating; the sandblasting pressure is 0.2-0.4 MPa, and the sandblasting medium is 240 mesh corundum sand.
[0009] In the method for removing (Ni, Pt)Al coating by chemical solution corrosion, in step (1), the base alloy of the workpiece is a nickel-based directionally solidified high-temperature alloy or a nickel-based single crystal high-temperature alloy.
[0010] In the method for removing (Ni, Pt)Al coating by chemical solution corrosion, in step (1), the (Ni, Pt)Al coating has a normalized nominal composition range of Al 38-50, Ni 40-55, Pt 2-10, Cr 1-5, and Co 1-5, calculated in atomic percentage.
[0011] In the method for removing (Ni, Pt)Al coating by chemical solution corrosion, in step (1), the thickness of the (Ni, Pt)Al coating including the interdiffusion zone is 30 to 70 μm.
[0012] In the method for removing (Ni, Pt)Al coating by chemical solution corrosion, in step (1), the thickness of the oxide film of the (Ni, Pt)Al coating after use is 1 to 5 μm.
[0013] The method for removing (Ni, Pt)Al coating by chemical solution corrosion is as follows: the composition of the removal solution is as follows by weight percentage: HCl 25-30%, CH3COOH 5-10%, C6H8O7·H2O 15-20%, H2O 40-50%.
[0014] The design idea of the present invention is:
[0015] The present invention provides a method for completely removing the (Ni, Pt)Al coating without affecting the service performance of the re-coated coating. The (Ni, Pt)Al coating reacts with the corrosive solution, and the coating is mainly removed by corrosion along the grain boundary.
[0016] The advantages and beneficial effects of the present invention are:
[0017] 1. The present invention uses a chemical method to remove the coating, which has a fast removal speed and is easy to operate.
[0018] 2. The present invention uses a chemical method to remove the coating, and then the coating has good service performance.
[0019] 3. The coating can be removed thoroughly and cleanly by the present invention, with low cost, and can be used to realize large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is the cross-sectional morphology of the coating after oxidation sandblasting.
[0021] Figure 2 The surface and cross-sectional morphologies of coatings with different stripping times are shown in Figure 1. (a) Cross-sectional morphology of coating with stripping time of 15 min, (b) Cross-sectional morphology of coating with stripping time of 30 min, (c) Cross-sectional morphology of coating with stripping time of 45 min, (d) Cross-sectional morphology of coating with stripping time of 100 min, (e) Surface morphology of coating with stripping time of 15 min, (f) Surface morphology of coating with stripping time of 30 min, (g) Surface morphology of coating with stripping time of 45 min, and (h) Surface morphology of coating with stripping time of 100 min.
[0022] Figure 3 The surface (a, b) and cross-sectional (c, d) morphologies of a coating (a, c) prepared once and a re-coated coating (b, d) are shown.
[0023] Figure 4 The cross-sectional morphologies of the once prepared coating (a) and the re-coated coating (b) after cyclic oxidation at 1100°C for 300 h.
[0024] Figure 5 The kinetic curves of cyclic oxidation of the coating prepared once and re-coated at 1100℃ are shown in the figure. The horizontal axis Number of cycles represents (number of cycles), and the vertical axis Δw (Mass Gain) represents the oxidation weight gain (mg / cm 2 ). DETAILED DESCRIPTION
[0025] In the specific implementation process, the present invention has determined a method suitable for removing the (Ni, Pt) Al coating by chemical solution corrosion, and the process flow is: pre-treating the (Ni, Pt) Al coating with an oxide film to remove the stable oxidation products on the surface; stripping the coating by chemical solution corrosion; post-treating the sample after stripping the coating to remove the corrosion products attached to the surface in preparation for re-coating a new coating. It is characterized by: (1) The corrosion solution used for stripping the coating is composed of H2O, HCl, C6H8O7·H2O, and CH3COOH; (2) When stripping the coating, the water bath temperature is 45-75°C and the removal time is 30-60 minutes.
[0026] The present invention is further described in detail below through examples and drawings.
[0027] Example 1
[0028] In this embodiment, a coating is prepared on a substrate, and then the coating after service simulation is corroded and removed by a chemical solution.
[0029] First, a (Ni,Pt)Al coating was prepared on the second-generation nickel-based single crystal high-temperature alloy (N5):
[0030] (1) Using wire cutting equipment, nickel-based single crystal high-temperature alloy rods were cut into Φ15 mm × 2 mm disc-shaped specimens, and a circular hole with a diameter of about 1.7 mm was cut on the edge of each specimen to facilitate sample hanging in subsequent experiments.
[0031] (2) The sample was first ground with 400-grit sandpaper, then sandblasted with 240-mesh white corundum, and then boiled in a 50 g / L NaOH aqueous solution for 10 min. Finally, it was ultrasonically cleaned with a mixed solution of alcohol and acetone (volume ratio of 1:1) for 20 min.
[0032] (3) The sample was subjected to Pt electroplating, vacuum interdiffusion, and high-temperature low-activity vapor deposition aluminum in turn. The aluminum diffusion time was 5 hours, and a 40-70 μm thick (Ni, Pt)Al coating (including the interdiffusion zone) was obtained; its nominal composition in atomic percentage was: Al49.43, Cr 1.23, Co 1.93, Ni 43.16, Pt 4.25.
[0033] In order to simulate the service environment of the coating and accelerate the failure of the coating, the sample with the (Ni, Pt)Al coating was placed in a muffle furnace for oxidation at 1100℃ for 300h. Then the sample with the (Ni, Pt)Al coating was taken out, and a stable and dense oxide film with a thickness of 2μm was formed on the surface.
[0034] Pre-treatment of the sample after simulated service: The sample after service is subjected to tangential low-pressure sandblasting to remove the dense and stable oxide film of the coating. The tangential pressure of sandblasting is 0.3MPa, the sandblasting medium is glass sand, and the angle between the sandblasting direction and the sample plane is 45°. Figure 1 As shown in the figure, the cross-sectional morphology of the coating after oxidation and sandblasting to remove the oxide film is shown in the figure. Figure 1 It can be seen that the oxide scale is completely removed after sandblasting, and the residual thickness of the (Ni, Pt)Al coating is about 68 μm, that is, the (Ni, Pt)Al coating to be removed is about 68 μm.
[0035] The composition of the stripping solution is as follows by weight percentage: HCl 25-30%, CH3COOH 5-10%, C6H8O7·H2O 15-20%, and H2O 40-50%.
[0036] After the oxide film is removed, the sample is cleaned and the (Ni, Pt) Al coating can be removed in the removal solution. The specific process is as follows:
[0037] First, dissolve C6H8O7·H2O in deionized water, pour in HCl and CH3COOH solution, and stir evenly. Then use a constant temperature water bath to control the temperature at 55°C during the reaction. Figure 2 As shown in the figure, the surface and cross-sectional morphology of the samples at different times in the corrosion solution are Figure 2 It can be seen from the surface that the dissolution method is mainly through corrosion along the grain boundaries. Figure 2 It can be seen from the cross section that with the extension of immersion time, the coating gradually dissolves. After the sample is immersed in the corrosive solution for 15 minutes, it can be seen that the outer layer of the coating is basically removed, and its interdiffusion zone is still retained; after 30 minutes, there are still trace residues in the interdiffusion zone of the coating; after 45 minutes, the coating is completely removed; when the time is extended to 100 minutes, although the thickness of the coating is removed to the maximum, it is seen that the substrate surface is over-corroded. Based on the above analysis, when the removal is 45 minutes, it can be seen that the coating is completely removed and its surface is relatively flat, but the needle-shaped TCP phase can be seen in the single crystal substrate. The coating is removed best and the loss to the substrate is small.
[0038] After the coating is removed, the sample is sandblasted to remove the corrosion products attached to the surface in preparation for re-coating. The sandblasting pressure is 0.3MPa, and the sandblasting medium is 240 mesh corundum sand.
[0039] Example 2
[0040] In this example, the coating was re-coated on the sample after the (Ni, Pt)Al coating was removed in Example 1.
[0041] A (Ni, Pt) Al coating was prepared on a second-generation nickel-based single crystal high-temperature alloy (N5), and the coating was removed after oxidation in a muffle furnace at 1100° C. for 300 h. The specific operation method was the same as that in Example 1. Then, the (Ni, Pt) Al coating was re-coated. The specific method was as follows:
[0042] (1) The sandblasted sample was ultrasonically cleaned in a mixed solution of acetone and alcohol (volume ratio of 1:1) for 20 min to remove surface oil stains and set aside;
[0043] (2) The sample was subjected to Pt electroplating, vacuum interdiffusion and high temperature low activity vapor deposition aluminum in turn. The aluminum infiltration time was 4 hours, and a 40-45 μm thick (Ni, Pt)Al coating was obtained for annealing. After annealing, its nominal composition in terms of atomic percentage was: Al 38.84, Cr 4.74, Co 4.70, Ni 41.76, Pt 9.96.
[0044] The obtained (Ni, Pt)Al coating is placed in a vacuum annealing furnace for annealing to eliminate the pores in the coating. Figure 3 As shown in the figure, the microscopic morphology of the coating prepared once and the coating re-coated is Figure 3 It can be seen from (a)-(b) that there is almost no significant difference in the surface microstructure of the coating prepared once and the coating re-coated. Both are composed of "ridges" formed by grain boundaries and "grooves" formed within the grains. Figure 3 From the cross-sectional morphology (c)-(d), it can be seen that both coatings are dense and continuous; the thickness of the re-coated coating is slightly thicker than that of the once-prepared coating. There are some needle-like TCP phases in the matrix of the re-coated coating sample. This is formed by the mutual diffusion of elements during the pre-service simulated oxidation, which causes the refractory elements dissolved in the γ phase to precipitate.
[0045] The re-coated coating and the primary prepared coating obtained in this example were subjected to cyclic oxidation at 1100°C. Figure 4 As shown in FIG. 1 , the microscopic cross-sectional morphology of the primary coating and the re-coated coating obtained in this embodiment after cyclic oxidation at 1100° C. for 300 hours. Figure 4 (a)-(b) shows that the oxide films of the two coatings are dense and continuous, and the oxide film thickness of the re-coated coating is slightly lower than that of the coating prepared once. Figure 5 As shown in FIG. 1 , the 1100°C cyclic oxidation kinetic curves of the once prepared coating and the re-coated coating obtained in this example. Figure 5 It can be seen that the oxidation kinetics of the two coatings conform to the parabolic law. It can be seen that the re-coated coating still has good high-temperature oxidation resistance, meets the coating service requirements, and can be used to achieve large-scale production.
Claims
1. A method for removing (Ni, Pt)Al coating by chemical solution corrosion, characterized in that: The specific steps of this method are as follows: (1) Pretreatment: The (Ni, Pt) Al coated workpiece with an oxide film after use is subjected to tangential low-pressure sandblasting to remove the non-conductive oxide film on the coating surface; the tangential pressure of sandblasting is 0.2~0.4 MPa, the sandblasting medium is 200 mesh glass beads, and the angle between the sandblasting direction and the workpiece plane is 30~60°; In step (1), the (Ni, Pt)Al coating has a normalized nominal composition range of Al 38-50, Ni 40-55, Pt 2-10, Cr 1-5, Co 1-5, in terms of atomic percentage; (2) Removing the coating by chemical corrosion: the stripping solution used is a mixed solution of H2O, HCl, CH3COOH, and C6H8O7•H2O. The workpiece is placed in the mixed solution, the water bath heating temperature is 45~75℃, and the stripping time is 30~60min. (3) Post-treatment: sandblasting to remove corrosion products attached to the surface in preparation for re-coating of a new (Ni, Pt) Al coating; the sandblasting pressure is 0.2~0.4MPa, and the sandblasting medium is 240 mesh corundum sand; In step (1), the thickness of the oxide film of the (Ni,Pt)Al coating after use is 1-5 μm; The composition of the stripping solution is as follows by weight percentage: HCl 25-30%, CH3COOH 5-10%, C6H8O7•H2O 15-20%, H2O 40-50%.
2. The method for removing (Ni, Pt)Al coating by chemical solution corrosion according to claim 1, characterized in that: In step (1), the base alloy of the workpiece is a nickel-based directionally solidified high-temperature alloy or a nickel-based single crystal high-temperature alloy.
3. The method for removing (Ni, Pt)Al coating by chemical solution corrosion according to claim 1, characterized in that: In step (1), the thickness of the (Ni, Pt)Al coating including the interdiffusion zone is 30-70 μm.