A method for improving corner cracks and middle cracks of slab
By setting up a dual temperature control interval for the bent section and straightening section during the casting production process and optimizing the cooling structure, the problem of cracks in the corners and intermediate sections of the slab is solved, and the uniformity of the casting billet temperature and significant reduction of cracks are achieved. Improve product quality and equipment life.
Patent Information
- Application Number
- CN202210018325.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-01-07
AI Technical Summary
The existing technology is difficult to effectively solve the problems of cracks in the corners and intermediates of the slabs, especially in the production process of casting. The existing methods such as weak-cold and strong-cold technologies have problems such as equipment wear, nozzle blockage, and uneven temperature, resulting in casting. The quality of the blank deteriorates.
By setting the dual temperature control intervals of the bent section and the straightening section, the inlet to outlet temperature of the bent section is controlled at a temperature above 900°C, the low temperature target control interval is set at a temperature below 750°C, and the trunnion is added to the bent section and " The gap of the U-shaped seat is set, the second cold partition of the straightening section is optimized, the nozzle adjustment ratio and liquid steel composition are optimized, and the temperature uniformity of the casting billet is controlled.
The incidence of slab corners and intermediate cracks is significantly reduced, the angle crack rate of casting billet is reduced to below 0.25%, and the intermediate crack level is reduced from above 2.5 to ≤0.5, which improves the surface quality and equipment service life of casting billets.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of steelmaking, and in particular relates to a method for improving corner cracks and middle cracks of a slab, and more specifically to a method for improving corner cracks and middle cracks of a slab based on dual-temperature process control of the corners of the casting slab. Background Art
[0002] The main mechanisms for transverse cracks in corners are: 1) Coarsening of austenite grains at the oscillation marks on the corners of the slab reduces the high-temperature plasticity of the steel; 2) During the phase transformation, second-phase particles (such as AlN, Nb(C,N), VN, and BN) precipitate at the austenite grain boundaries, increasing their brittleness; and 3) During operation, the slab is subjected to bending (compression on the inner arc and tension on the outer arc), straightening (tension on the inner arc and compression on the outer arc), and bulging. Since the slab is in its low-temperature brittle zone (750-900°C), if the strain caused by tensile stress exceeds the allowable strain, cracks will form. Research has found that transverse cracks in slab corners are one of the main causes of edge defects on the rolled product surface. The mechanism for the generation of intermediate cracks is due to bulging strain, dislocation strain, and repeated temperature regeneration during the production process.
[0003] The main solutions of the existing technology are: 1) weak cooling is used in the secondary cooling of continuous casting to reduce the longitudinal and transverse temperature unevenness of the slab, especially to prevent overcooling of the edge, that is, the "hot running method"; 2) the method of strengthening the cooling of the slab edge is adopted, and nozzles are added to the edge of the slab to strengthen the cooling, so that the edge temperature drops below 750℃, reducing the cracks at the corners of the slab, that is, the "cold running method"; 3) the method of using a chamfered crystallizer. The secondary cooling weak cooling method is widely used in China to control the cracks in the corners of the slab. For example, Baosteel has proposed measures to improve the transverse cracks in the corners of the slab by analyzing the factors affecting the cracks in the corners of the slab, namely, weakening the cooling of the crystallizer and the distribution of the secondary cooling water, and improving the corners of the slab so that the temperature of the corners of the slab is higher than 900℃ and enters the straightening zone (see Figure 1 ), after implementing the above measures, the cracks on the edge of the steel plate have been reduced to a certain extent, however, this problem has not been completely solved yet, and the use of weak cooling is not conducive to the control of cracks in the middle of the billet. The high temperature operation of the continuous casting roller aggravates the wear of the continuous casting roller and increases the friction with the billet. The long-term operation of the secondary cooling nozzle with a small amount of water can easily lead to nozzle blockage. The blockage of the nozzle makes the billet temperature uneven, deteriorates the billet quality, and creates a vicious cycle. Foreign countries and Northeastern University at home have designed a strong cooling device for the high-temperature cooling zone of the billet, and adjusted the secondary cooling water distribution to make the corner of the billet undergo a rapid phase transformation in the high-temperature zone, so that the corner of the billet is quickly cooled to the temperature where the transformation from austenite to ferrite is completed (the cooling rate reaches 5-7℃ / s), so that the precipitates are dispersed in the crystal. On this basis, the temperature of the billet corner in the subsequent cooling process is controlled to keep the temperature of the billet corner below 750℃ (about Ar3 temperature), which refines the grain structure of the billet corner, makes the billet corner temperature enter the straightening zone at a low temperature, and improves the billet corner cracking (see Figure 2 However, this technology places extremely high demands on the equipment precision of the continuous casting machine. To match this technology, foreign casting machines have developed new continuous bending and straightening curves for straight-arc continuous casting machines. The arc accuracy of the bending and straightening sections can reach ±0.1mm, while the arc accuracy of conventional slab casting machines can only be controlled within ±0.3mm. Therefore, the application of strong cooling technology to conventional domestic slab casting machines will inevitably exacerbate the corner cracks of the castings. In addition, due to the low casting temperature and increased strength, the bending and straightening reaction force during the casting process increases, which can easily lead to damage to the continuous casting equipment and reduce the equipment service life. In recent years, major domestic steel companies have paid extensive attention to and tried large chamfered mold technology, which is also based on improving the two-dimensional heat transfer of the corners of the billet, increasing the corner temperature and improving the corner cracking of the billet. Since the technology is not yet very mature, the use of this technology in actual continuous casting production is likely to cause longitudinal cracks in the corners of the billet, and even steel leakage accidents. In addition, due to the unreasonable crystallizer taper compensation system, the crystallizer copper plate is severely worn, the service life of the crystallizer is reduced by about 35% to 45%, and the production efficiency is reduced by about 40%. Summary of the Invention
[0004] In view of this, the object of the present invention is to provide a method for improving slab corner cracks and middle cracks. The method provided by the present invention can achieve a better effect of improving slab cracks.
[0005] The present invention provides a method for improving corner cracks and middle cracks of a slab, comprising:
[0006] Two temperature control intervals are set for the slab corner temperature.
[0007] Preferably, the two temperature control intervals include:
[0008] Temperature control range from the bend section inlet to the bend section outlet;
[0009] A low temperature target control range is set in the straightening section of the continuous casting machine.
[0010] Preferably, the temperature control range from the inlet to the outlet of the bending section is higher than 900°C.
[0011] Preferably, the low temperature target control range of the straightening section of the continuous casting machine is set to be lower than 750°C.
[0012] Preferably, the method for improving slab corner cracks and middle cracks further comprises:
[0013] Set the gap between the bending section trunnion and the "U" shaped seat.
[0014] Preferably, the gap is 0.2-0.7 mm.
[0015] Preferably, the method for improving slab corner cracks and middle cracks further comprises:
[0016] Set up the secondary cooling zone in the straightening section.
[0017] Preferably, the first of the two cooling zones comprises a sector;
[0018] The second sub-zone of the secondary cooling sub-zone includes two sector segments.
[0019] Preferably, the nozzle adjustment ratio of the secondary cooling zone is 18-22.
[0020] Preferably, the method for improving slab corner cracks and middle cracks further comprises:
[0021] Molten steel composition control;
[0022] The molten steel composition control includes:
[0023] The mass content of C in the molten steel is ≤0.50wt%; the mass content of Si is ≤0.50%; the mass content of Mn is ≤2.0%; the mass content of P is ≤0.020%; the mass content of S is ≤0.020%; the mass content of Al is ≤0.050%; the mass content of B is ≤0.0020%; and the total mass content of Nb, V and Ti is ≤0.20%.
[0024] The present invention solves the defects of corner cracks and middle cracks in the production process of slab continuous casting, and improves the surface quality of the product. The present invention changes the temperature control strategy of the corner of the slab, which is different from the existing "hot running method" and "cold running method" control. Because the roller spacing in the bending section of the slab is small, the bulging stress of the slab is relatively small. The cooling intensity in this area is reduced to make the temperature of the corner of the slab out of the bending section in the high temperature section, avoiding the influence of the bending stress in the bending area to cause corner cracks and middle cracks; increasing the cooling intensity of the arc section makes the temperature of the slab entering the straightening area enter the low temperature zone, which not only effectively reduces the middle cracks of the slab, but also avoids the corner of the slab from entering the brittle zone of steel in the straightening area, avoiding the occurrence of corner cracks (see Figure 4 ); Simultaneously, by optimizing the positioning parameters of the bending section, the cooling zoning of the straightening zone, and the nozzle parameters, the stress conditions and temperature uniformity of the corners of the slab were improved. The method provided by the present invention significantly improved the control of corner and center cracks in the slab, with the corner crack rate below 0.25%. Furthermore, by increasing the cooling intensity of the curved section, reducing the bulging of the slab in the curved section, lowering the bulging stress of the curved section, and reducing the reheating of the slab, the center cracking of the slab was also significantly improved, with the level of center cracks in the slab being reduced from above 2.5 to ≤ 0.5. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the temperature control diagram of the corner of the casting billet using the existing "heating method";
[0026] Figure 2 This is the temperature control diagram of the corner of the billet using the existing "cold running method" technology;
[0027] Figure 3 Schematic diagram of the gap between the curved section trunnion and the "U"-shaped seat in the present invention;
[0028] Figure 4 This is the temperature control diagram of the corner of the casting billet in the present invention;
[0029] Figure 5 The left figure is the cooling zone of the prior art, and the right figure is the cooling zone of the present invention;
[0030] Figure 6 The left picture shows a corner crack and the right picture shows a corner crack-free slab prepared in an embodiment of the present invention.
[0031] Figure 7 Comparison diagram of the corner crack defects of the castings prepared in the embodiment of the present invention and the comparative example before and after improvement;
[0032] Figure 8 Comparison of the middle cracks of high-carbon steel slabs prepared in Example 1 and Comparative Example 1 before and after improvement. The upper figure is the slab prepared in Comparative Example 1, and the lower figure is the slab prepared in Example 1.
[0033] Figure 9 Comparison of the middle cracks of the boron-containing steel slabs prepared in Example 2 of the present invention and Comparative Example 2 before and after improvement. The upper figure is the slab prepared in Comparative Example 2, and the lower figure is the slab prepared in Example 2.
[0034] Figure 10 3 and 4. These are comparison diagrams of the microalloyed steel ingots prepared in Example 3 of the present invention and Comparative Example 3 before and after improvement of the middle cracks. The upper diagram is the ingot prepared in Comparative Example 3, and the lower diagram is the ingot prepared in Example 3. DETAILED DESCRIPTION
[0035] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0036] The present invention provides a method for improving corner cracks and middle cracks of a slab, comprising:
[0037] Two temperature control intervals are set for the corner temperature of the casting billet.
[0038] In the present invention, the setting of two temperature control intervals for the corner temperature of the casting billet preferably includes:
[0039] Temperature control range from the bend section inlet to the bend section outlet;
[0040] A low temperature target control range is set in the straightening section of the continuous casting machine.
[0041] In the present invention, since the roller spacing in the bending section of the billet is small, the bulging stress of the billet is relatively small, and the cooling intensity is reduced in this area, so that the temperature of the billet corner exiting the bending section is in a higher temperature range.
[0042] In the present invention, the temperature control range from the bend section inlet to the bend section outlet is preferably higher than 900°C, more preferably 900-1000°C, and most preferably 950°C. Figure 4 shown.
[0043] In the present invention, by increasing the cooling intensity of the arc segment, the temperature of the arc segment entering the straightening zone is brought into the low temperature zone, which can not only effectively reduce the middle cracks of the ingot, but also avoid the corners of the ingot entering the brittle zone of the steel in the straightening zone, thereby avoiding the occurrence of corner cracks.
[0044] In the present invention, the low temperature target control range of the straightening section of the continuous casting machine is preferably set to be lower than 750°C, more preferably 680-750°C, more preferably 700-730°C, and most preferably 710-720°C; Figure 4 shown.
[0045] In the present invention, the method for improving slab corner cracks and middle cracks preferably further comprises:
[0046] Set the gap between the bending section trunnion and the "U" shaped seat.
[0047] In the present invention, the gap between the bending section trunnion and the "U" shaped seat is controlled within a reasonable range to improve the stress of the billet during the bending process, avoid excessive stress and corner crack defects, such as Figure 3 shown.
[0048] In the present invention, the gap is preferably 0.2 to 0.7 mm, more preferably 0.3 to 0.6 mm, and most preferably 0.4 to 0.5 mm.
[0049] In the present invention, the method for improving slab corner cracks and middle cracks preferably further comprises:
[0050] Set up the secondary cooling zone in the straightening section.
[0051] In the present invention, the first partition of the secondary cooling partition preferably includes one sector; and the second partition of the secondary cooling partition preferably includes two sector.
[0052] In the present invention, by changing one partition corresponding to three sectors to corresponding to two sectors, the cooling uniformity of the corner of the billet in the straightening zone is improved, and the corner crack defect of the billet caused by repeated temperature recovery in the straightening zone is avoided. Figure 5 As shown, the secondary cooling zone consisting of the three fan-shaped segments SEG6, SEG7, and SEG8 (left picture) is reset to zone 7 consisting of SEG6 and zone 8 consisting of the straightening segments, namely SEG7 and SEG8 (right picture), and the cooling pipelines, pneumatic control valves, pressure transmitters, and electromagnetic flowmeters are reset.
[0053] In the present invention, the nozzle adjustment ratio of the secondary cooling zone is preferably adjusted from 7.0 to 18-22, more preferably 19-21, and most preferably 20.
[0054] In the present invention, the method for improving slab corner cracks and middle cracks preferably further comprises:
[0055] Control of molten steel composition.
[0056] In the present invention, the steel liquid composition control preferably includes: the mass content of C in the steel liquid is ≤0.50wt%; the mass content of Si is ≤0.50%; the mass content of Mn is ≤2.0%; the mass content of P is ≤0.020%; the mass content of S is ≤0.020%; the mass content of Al is ≤0.050%; the mass content of B is ≤0.0020%; and the total mass content of Nb, V and Ti is ≤0.2%.
[0057] In the present invention, the method for improving slab corner cracks and middle cracks preferably includes:
[0058] Before the continuous casting machine is put into operation, the clearance between the bending section trunnion and the "U" seat and the secondary cooling nozzle are confirmed;
[0059] After the converter completes the smelting of any steel grade, it is poured into the continuous casting machine after the composition and temperature meet the requirements;
[0060] After the molten steel passes through the continuous casting machine crystallizer and cools and solidifies into a shell with a certain thickness, it is pulled out from the crystallizer outlet;
[0061] Set the cooling temperature of each cooling zone, especially ensure that the temperature of the bending zone is higher than 900℃ and the temperature of the straightening zone is lower than 750℃;
[0062] After the billet passes through the cooling of the bending zone, the arc zone, the straightening zone and the horizontal zone, a completely solidified billet is formed.
[0063] In the present invention, the method for confirming the gap between the bending section trunnion and the "U"-shaped seat preferably includes:
[0064] Use a feeler gauge to check the gap between the bent section trunnion and the "U" seat, and use a special tool to adjust it until the gap is controlled between 0.2 and 0.7 mm.
[0065] In the present invention, the method for confirming the secondary cooling nozzle preferably includes:
[0066] Use visual inspection to check the water spray height, angle and atomization degree of the secondary cooling nozzle, focusing on SEG7, SEG8 ( Figure 5 (As shown in the right picture) Check and confirm the secondary cooling nozzle in the straightening area.
[0067] In the present invention, the water flow rate of the SEG7 zone (first zone) is preferably 160-200 L / min, more preferably 170-190 L / min, and most preferably 180 L / min; the water flow rate of the SEG8 zone (second zone) is preferably 7-11 L / min, more preferably 8-10 L / min, and most preferably 9 L / min; it is ensured that under the conditions of maximum and minimum water flow rates, the water spray height can reach the surface of the ingot, the water spray width covers the ingot, the atomization effect is good, and the secondary cooling nozzles that do not meet the requirements are replaced.
[0068] The present invention has no special restrictions on the composition of the steel. Those skilled in the art can use steel with appropriate composition according to actual needs. The steel can be high carbon steel, boron-containing steel or micro-alloyed steel, etc. The content range of C, Si, Mn, P, S, Al, B, Nb, V and Ti in the steel can meet the above-mentioned steel liquid composition control requirements.
[0069] The present invention has no particular limitation on the smelting method. Those skilled in the art can adopt a suitable smelting method according to actual conditions to obtain molten steel with qualified composition and temperature.
[0070] In the present invention, the pulling speed is preferably 0.9 to 1.8 m / min, more preferably 1.0 to 1.6 m / min, more preferably 1.1 to 1.4 m / min, and most preferably 1.3 m / min.
[0071] In the present invention, in the secondary cooling process, the amount of cooling water is preferably automatically adjusted according to the physical properties of the steel type and the drawing speed to ensure the realization of the process temperature.
[0072] In the present invention, the prepared qualified slab is preferably sent to a steel rolling mill for rolling.
[0073] In the steel production process, the quality of continuous casting billets, especially the corner cracks and middle cracks of the billets, has an important impact on the surface quality and performance of the products. In order to meet customers' increasingly stringent requirements for quality, the present invention provides a method for improving the corner cracks and middle cracks of slabs based on dual-temperature process control of the billet corners. Without increasing the cost, the corner cracks and middle cracks of the billets are improved, thereby improving both product quality and operating efficiency.
[0074] The present invention balances the bending section's gravity and the billet drawing force by providing a gap between the bending section's trunnion and the "U"-shaped seat. A dual-target temperature segmented control strategy for corner temperature control reduces corner defects while significantly improving central cracking. By dividing the straightening zone into secondary cooling zones, the temperature of the corners of the billet entering the straightening zone is more uniform, eliminating corner cracks caused by repeated reheating at the corners. The method provided by the present invention significantly improves corner crack control in steel slabs produced by continuous slab casting, reducing the corner crack rate to below 0.25% and the central crack level from above 2.5 to ≤0.5.
[0075] The continuous casting machine used in the following embodiments of the present invention is provided by MCC SEDI, which is a straight arc continuous casting machine with continuous bending and straightening.
[0076] Example 1
[0077] The continuous casting machine is used to prepare medium-high carbon steel ingots, and the composition of medium-high carbon steel is:
[0078] Steel Type C(2) Si(2) Mn(2) P(3) S(3) <![CDATA[Al S (3)]]> Medium and high carbon steel (wt%) ≤0.48 ≤0.30 0.50~1.30 ≤0.020 ≤0.010 ≤0.020
[0079] The continuous casting machine is set up so that the gap between the east trunnion and the U-shaped seat of the bending section is measured with a feeler gauge to be 0.2 mm, and the gap between the west trunnion and the U-shaped seat is measured with a feeler gauge to be 0.3 mm.
[0080] The casting speed during the casting process is 1.1m / min~1.4m / min, and the tundish temperature is 1535℃~1545℃;
[0081] The target temperature of the corner of the billet in the bending zone was set at 910°C, and the actual temperature measured by an infrared temperature gun was 900°C to 908°C. The target temperature of the corner of the billet in the straightening zone was set at 730°C, and the actual temperature of the corner of the billet at the entrance of the straightening zone was 727°C to 734°C using an infrared temperature gun. The actual temperature of the corner of the billet at the exit of the straightening zone was 720°C to 732°C, and there was no temperature recovery at the corner of the billet.
[0082] The straightening zone consists of two sectors ( Figure 5 The nozzle adjustment ratio is 20.
[0083] Comparative Example 1
[0084] The medium-high carbon steel ingot of Example 1 was prepared using a continuous casting machine:
[0085] There is no control requirement for the clearance between the bending section trunnion and the "U"-shaped seat;
[0086] During the casting process, the pulling speed is 0.9m / min~1.1m / min, and the tundish temperature is 1540℃~1550℃;
[0087] The target temperature of the corner of the billet is always set above 850℃, and the temperature of the billet in the straightening zone is measured by an infrared temperature gun and ranges from 870℃ to 911℃;
[0088] The straightening area consists of three fan-shaped segments (SEG6, 7, 8, Figure 5 As shown in the left figure), the nozzle adjustment ratio is 7, and the temperature fluctuation of the corner of the billet is ±20℃.
[0089] Example 2
[0090] The continuous casting machine is used to prepare the boron-containing steel ingot, and the composition of the boron-containing steel is:
[0091] Steel Type C(2) Si(2) Mn(2) P(3) S(3) <![CDATA[Al S (3)]]> B(4) Boron-containing steel (wt%) ≤0.20 ≤0.30 0.30~0.90 ≤0.020 ≤0.010 ≤0.025 ≤0.0020
[0092] The continuous casting machine is set up so that the gap between the east trunnion and the U-shaped seat of the bending section is measured with a feeler gauge to be 0.5 mm, and the gap between the west trunnion and the U-shaped seat is measured with a feeler gauge to be 0.6 mm.
[0093] The casting speed during the casting process is 1.1m / min~1.6m / min, and the tundish temperature is 1545℃~1555℃;
[0094] The target temperature of the corner of the billet in the bending zone was set at 900℃, and the actual temperature measured using an infrared temperature gun was 902℃~915℃; the target temperature of the corner of the billet in the straightening zone was set at 750℃, and the actual temperature of the corner of the billet at the entrance of the straightening zone was 745℃~755℃ using an infrared temperature gun, and the actual temperature of the corner of the billet at the exit of the straightening zone was 740℃~748℃, and there was no temperature recovery at the corner of the billet.
[0095] The straightening zone consists of two sectors ( Figure 5 The nozzle adjustment ratio is 20.
[0096] Comparative Example 2
[0097] The boron-containing steel ingot of Example 2 was prepared using a continuous casting machine:
[0098] There is no control requirement for the clearance between the bending section trunnion and the "U"-shaped seat;
[0099] During the casting process, the pulling speed is 0.9m / min~1.1m / min, and the tundish temperature is 1560℃~1570℃;
[0100] The target temperature of the corner of the billet is always set above 850℃, and the temperature range of the billet in the straightening area is measured by an infrared temperature gun and is 870℃~920℃;
[0101] The straightening area consists of three fan-shaped segments (SEG6, 7, 8, Figure 5 Left figure), the nozzle adjustment ratio is 7, and the temperature fluctuation of the corner of the billet is ±25℃.
[0102] Example 3
[0103] The microalloyed steel ingot is prepared by continuous casting machine. The composition of microalloyed steel is:
[0104]
[0105] The continuous casting machine is set up so that the gap between the east trunnion and the U-shaped seat of the bend is measured with a feeler gauge to be 0.3mm, and the gap between the west trunnion and the U-shaped seat is measured with a feeler gauge to be 0.35mm.
[0106] The casting speed during the casting process is 1.0m / min~1.3m / min, and the tundish temperature is 1540℃~1550℃;
[0107] The target temperature of the corners of the billet in the bending zone was set at 920°C, and the actual temperature measured by an infrared temperature gun was 925°C to 930°C. The target temperature of the corners of the billet in the straightening zone was set at 700°C, and the actual temperature of the corners of the billet at the entrance of the straightening zone was 690°C to 705°C using an infrared temperature gun. The actual temperature of the corners of the billet at the exit of the straightening zone was 686°C to 703°C, and there was no temperature recovery at the corners of the billet.
[0108] The straightening zone consists of two sectors ( Figure 5 The nozzle adjustment ratio is 20.
[0109] Comparative Example 3
[0110] A continuous casting machine was used to prepare the microalloyed steel ingot with the composition of Example 3:
[0111] There is no control requirement for the clearance between the bending section trunnion and the "U"-shaped seat;
[0112] During the casting process, the pulling speed is 0.9m / min~1.1m / min, and the tundish temperature is 1545℃~1555℃;
[0113] The target temperature of the corner of the billet is always set to be higher than 850℃, and the temperature of the billet in the straightening area is measured by an infrared temperature gun and is between 845℃ and 915℃.
[0114] The straightening area consists of three fan-shaped segments (SEG6, 7, 8, Figure 5 Left figure), the nozzle adjustment ratio is 7, and the temperature fluctuation of the corner of the billet is ±25℃.
[0115] Performance testing
[0116] Inspection of casting corner cracks
[0117] The ingots prepared in the embodiments of the present invention and the comparative examples were flame cut and soaked in concentrated hydrochloric acid to remove the iron oxide scale. The ingot corners were then visually inspected for cracks. Figure 6 As shown, the left picture is a picture of the ingot with corner cracks, and the right picture is a picture without corner cracks.
[0118] Long-term production practice was carried out using the methods of the embodiments of the present invention and the comparative examples. Before the improvement (Comparative Example 1), 824,000 tons of medium-high carbon steel were produced with a corner crack defect rate of 1.34%, and after the improvement (Example 1), 1.456 million tons of medium-high carbon steel were produced with a corner crack defect rate of 0.01%; before the improvement (Comparative Example 2), 344,000 tons of boron-containing steel were produced with a corner crack defect rate of 7.96%, and after the improvement (Example 2), 101,000 tons of boron-containing steel were produced with a corner crack defect rate of 0.17%; before the improvement (Comparative Example 3), 201,000 tons of microalloyed steel were produced with a corner crack defect rate of 4.24%, and after the improvement (Example 3), 197,000 tons of microalloyed steel were produced with a corner crack defect rate of 0.25%; the method provided by the present invention reduces the corner crack defect rate of different steel grades to below 0.25%, such as Figure 7 shown.
[0119] Inspection of cracks in the middle of the ingot
[0120] The cross section of the ingot prepared in the embodiment and the comparative example was cut into a 200 mm thick, 700 to 1300 mm wide, and 180 mm long low-magnification sample, which was processed on a grinder, polished, and corroded with concentrated hydrochloric acid to test the level of the middle crack in the cross section of the ingot. The inspection standard was implemented in accordance with the "YB / T 4003-2016 Continuous Casting Steel Slab Macrostructure Defect Rating Chart". The test results showed that the middle crack in the medium and high carbon steel ingot was reduced from the highest level of 3.0 to the elimination of the middle crack. Figure 8 As shown in the figure, the cracks in the middle of the boron-containing steel ingot are reduced from the highest level 2.5 to level 0.5. Figure 9 As shown in the figure, the cracks in the microalloyed steel ingot are reduced from the highest level 1.0 to level 0.5. Figure 10 shown.
[0121] The present invention provides a method for improving cracks at the corners and middle cracks of slabs based on dual-temperature process control of the corners of the slabs. The method improves product quality without increasing costs. Compared with traditional process control methods (weak cooling and strong cooling), the method has the following advantages: compared with the weak cooling technology, the method improves the repeated warming of the corners of the continuous casting slabs, reduces nozzle blockage and cracking of the continuous casting rollers, and reduces the defect rate of cracks at the corners of the slabs. At the same time, the internal quality of the slabs is improved and the middle crack defects are improved; compared with the strong cooling technology, the process requirements are more adaptable to the precision of the casting machine, the maintenance costs of the nozzles, energy media, and equipment precision are reduced, the bending and straightening reaction forces in the production process are reduced, the quality of the slabs is improved, and the service life of the equipment is increased; the temperature in the length direction of the slabs is more uniform, and the internal and external quality of the slabs is excellent.
[0122] Although the present invention has been described and illustrated with reference to specific embodiments of the present invention, these descriptions and illustrations do not limit the present invention. It will be clearly understood by those skilled in the art that, without departing from the true spirit and scope of the present invention as defined by the appended claims, various changes may be made to make specific circumstances, materials, compositions of matter, substances, methods or processes suitable for the object, spirit and scope of the present application. All such modifications are intended to be within the scope of the appended claims. Although the methods disclosed herein have been described with reference to specific operations performed in a specific order, it will be understood that these operations may be combined, subdivided or reordered to form equivalent methods without departing from the teachings of the present invention. Therefore, unless otherwise indicated herein, the order and grouping of operations are not limitations of the present application.
Claims
1. A method for improving corner cracks and middle cracks of a slab, comprising: Two temperature control intervals are set for the corner temperature of the casting billet; The two temperature control intervals include: Temperature control interval from the bend section inlet to the bend section outlet; The low temperature target control range is set in the straightening section of the continuous casting machine; The temperature control range from the inlet of the bending section to the outlet of the bending section is 900-1000°C, and the low temperature target control range of the straightening section of the continuous casting machine is set to 680-750°C; The method for improving the corner cracks and middle cracks of the slab also includes: Setting a secondary cooling zone of the straightening section, wherein the first zone of the secondary cooling zone includes one sector segment, the second zone of the secondary cooling zone includes two sector segments, and the nozzle adjustment ratio of the secondary cooling zone is 18-22; The method for improving the corner cracks and middle cracks of the slab also includes: Molten steel composition control; The molten steel composition control includes: The mass content of C in the molten steel is ≤0.50wt%; the mass content of Si is ≤0.50%; the mass content of Mn is ≤2.0%; the mass content of P is ≤0.020%; the mass content of S is ≤0.020%; the mass content of Al is ≤0.050%; the mass content of B is ≤0.0020%; the total mass content of Nb, V and Ti is ≤0.20%.
2. The method according to claim 1, characterized in that The method for improving the corner cracks and middle cracks of the slab also includes: Set the gap between the bending section trunnion and the "U" shaped seat.
3. The method according to claim 2, characterized in that The gap is 0.2~0.7mm.