Artificial hair fibers and hair accessories
By using a resin composition of a polycondensation polymer and a cross-linking agent in artificial hair fibers, the problem of knot generation and excessive gloss during the stretching process is solved, achieving the effect of less knots and moderate gloss, and improving The fineness and heat resistance of the fiber.
Patent Information
- Application Number
- CN202080070517.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Existing artificial hair fibers are prone to uneven stretching during the stretching process, resulting in nodules, which affects the touch and gloss. If the gloss is too high, it is easy to be identified as artificial hair.
Fiberization is carried out using a resin composition containing a polycondensation polymer and a cross-linking agent. Cross-linking improves the interweaving of molecular chains, inhibits the formation of knots, reduces gloss by appropriately forming unevenness on the surface, and optimizes the stretching and heat treatment of the fiber to control Single fiber and gloss.
The fiber for artificial hair with fewer knots and moderate gloss has been realized. The fineness and heat resistance of the fiber have been improved, and the gloss has been reduced, making it easier to maintain a semi-glossy to semi-glossy state.
Smart Images

Figure BDA0003584217820000141 
Figure BDA0003584217820000201 
Figure BDA0003584217820000202
Abstract
Description
Technical Field
[0001] The present invention relates to fibers for artificial hair, hair accessories, and the like. Background Art
[0002] Artificial hair fibers (fibers for artificial hair) can be used for wigs, hairpieces, hair extensions, etc. Patent Document 1 below discloses artificial hair fibers obtained by fiberizing a resin composition containing a polyamide resin and a bromine flame retardant.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2011-246844 Summary of the invention
[0006] Problems to be solved by the invention
[0007] In the above-mentioned Patent Document 1, artificial hair fibers are produced by stretching unstretched yarns formed by melt spinning. In this case, the yarns are not stretched uniformly during stretching, and knots are formed on the stretched yarns. When knots are present in the artificial hair fibers, there are problems such as poor touch.
[0008] One aspect of the present invention aims to provide a fiber for artificial hair having few knots. Another aspect of the present invention aims to provide a hair accessories including such a fiber for artificial hair.
[0009] Means for solving problems
[0010] One aspect of the present invention relates to a fiber for artificial hair comprising a polycondensation polymer and a crosslinking agent.
[0011] Another aspect of the present invention relates to a hair accessories including the above-mentioned fiber for artificial hair.
[0012] Effects of the Invention
[0013] According to one aspect of the present invention, a fiber for artificial hair having few knots can be provided. According to another aspect of the present invention, a hair accessories including such a fiber for artificial hair can be provided. DETAILED DESCRIPTION
[0014] Hereinafter, embodiments of the present invention will be described in detail.
[0015] "Above A" in the numerical range refers to A and the range exceeding A. "Below A" in the numerical range refers to A and the range below A. In the numerical range described in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of other stages. In the numerical range described in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. "A or B" means that as long as it contains either A and B, it can also contain both. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. In the case where there are multiple substances equivalent to each component in the composition, unless otherwise specified, the content of each component in the composition refers to the total amount of the multiple substances present in the composition. The term "process" is not only an independent process, but also included in this term as long as the desired effect of the process can be achieved even if it cannot be clearly distinguished from other processes. "(Meth) acrylic acid" refers to at least one of acrylic acid and its corresponding methacrylic acid. The same is true for other similar expressions such as "(meth) acrylic acid".
[0016] The fiber for artificial hair according to the present embodiment contains a polycondensation polymer and a crosslinking agent. The fiber for artificial hair according to the present embodiment can be used as artificial hair or can be used to obtain artificial hair.
[0017] The inventors of the present application have conducted intensive research and found that by fibrillating a resin composition containing a polycondensation polymer and a crosslinking agent (e.g., a resin composition containing a base resin containing a polycondensation polymer and a crosslinking agent), a fiber for artificial hair in which the generation of knots is suppressed can be obtained. The fiber for artificial hair involved in the present embodiment is a fiber for artificial hair with fewer knots when subjected to a stretching treatment. In the fiber for artificial hair involved in the present embodiment, it is presumed that the crosslinking of the polycondensation polymer and the crosslinking agent increases the interweaving of molecular chains, thereby suppressing the generation of knots. However, the main reason for fewer knots is not limited to this main reason.
[0018] However, since the conventional artificial hair fibers have too high a gloss compared to human hair, there is a problem that they are easily recognized as artificial hair. Therefore, for artificial hair fibers, sometimes less gloss is required. The artificial hair fibers involved in the present embodiment may be artificial hair fibers with less gloss. It is speculated that in the artificial hair fibers involved in the present embodiment, by using a polycondensation polymer and a crosslinking agent together, unevenness (undesirableness to the extent of not forming a tumor) can be appropriately formed on the surface of the fiber, thereby reducing the gloss. However, the main reason for the low gloss is not limited to this main reason. In the artificial hair fibers involved in the present embodiment, gloss is not easily generated, so it is easy to maintain a state of semi-gloss to seven-point gloss.
[0019] The fiber for artificial hair involved in the present embodiment may be a resin composition containing a polycondensation polymer and a crosslinking agent. The resin composition may contain a base resin containing a polycondensation polymer and a crosslinking agent, or may be obtained by melt-kneading a mixture containing a polycondensation polymer and a crosslinking agent. The fiber for artificial hair involved in the present embodiment may be composed of a fiber formed by a resin composition containing a polycondensation polymer and a crosslinking agent, or may be composed of a fiber formed by melt-deforming a resin composition containing a polycondensation polymer and a crosslinking agent. The fiber for artificial hair involved in the present embodiment may be a fiber after a stretching treatment (an artificial hair fiber composed of a fiber formed by stretching a resin composition), or may be an unstretched fiber (unstretched yarn). The fiber for artificial hair involved in the present embodiment may be an unstretched fiber obtained by spinning a resin composition containing a polycondensation polymer and a crosslinking agent, or may be a fiber obtained by stretching the unstretched fiber. Each of the polycondensation polymer and the crosslinking agent may be used alone or in combination of two or more.
[0020] The single fineness of the fiber for artificial hair according to the present embodiment is preferably in the following range after the stretching treatment. The single fineness is preferably 20 dtex or more, and more preferably 35 dtex or more. The single fineness is preferably 100 dtex or less, and more preferably 80 dtex or less. From such a viewpoint, the single fineness is preferably 20 to 100 dtex, and more preferably 35 to 80 dtex.
[0021] The single fineness of the fiber for artificial hair according to the present embodiment is preferably 300 dtex or less, and more preferably 200 dtex or less when not stretched, from the viewpoint that the stretching ratio can be reduced to obtain a fine-fine fiber for artificial hair and the fiber for artificial hair after the stretching treatment is less likely to have gloss.
[0022] Examples of polycondensation polymers include polyamide resins (polyamides), polyesters, etc. The fiber for artificial hair according to the present embodiment may not contain polyester. From the perspective of facilitating the reduction of knots and the perspective of facilitating the reduction of gloss, the polycondensation polymer preferably includes a polyamide resin.
[0023] Examples of polyamide resins include aliphatic polyamides, aromatic polyamides, and polyamides such as semi-aromatic polyamides having a skeleton obtained by polycondensation of aliphatic diamines and aromatic dicarboxylic acids. Examples of aliphatic polyamides include polyamide 6 (nylon 6), polyamide 66 (nylon 66), polyamide 12 (nylon 12), polyamide 6 / 66 (nylon 6 / 66), and polyamide 6 / 12 (nylon 6 / 12). Examples of aromatic polyamides include poly(m-xylylene adipamide) (nylon MXD6). Examples of semi-aromatic polyamides include polyamide 6T (nylon 6T), polyamide 9T (nylon 9T), and polyamide 10T (nylon 10T).
[0024] Examples of the polyester include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polycyclohexanedimethylene terephthalate.
[0025] Based on the total mass of the fiber for artificial hair, the content of the polycondensation polymer is preferably in the following range. From the viewpoint of being easy to reduce knots and gloss with good balance, the content of the polycondensation polymer is preferably 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, more than 50% by mass, 60% by mass or more, 65% by mass or more, 67% by mass or more, 68% by mass or more, or 69% by mass or more. From the viewpoint of being easy to reduce knots and gloss with good balance, the content of the polycondensation polymer is preferably 95% by mass or less, 90% by mass or less, 80% by mass or less, 75% by mass or less, 74% by mass or less, 73% by mass or less, 72% by mass or less, 71% by mass or less, or 70% by mass or less. From such a viewpoint, the content of the polycondensation polymer is preferably 10 to 95% by mass, 50 to 90% by mass, or 60 to 90% by mass. The content of the polycondensation polymer may be 70% by mass or more, 71% by mass or more, 72% by mass or more, 73% by mass or more, or 74% by mass or more. The content of the polycondensation polymer may be 69% by mass or less, or 68% by mass or less. From the same viewpoint, the content of the polyamide resin is preferably within the above ranges based on the total mass of the fiber for artificial hair.
[0026] As a crosslinking agent, a compound that can react with the terminal functional group (e.g., amino group) of the polycondensation polymer can be used. The crosslinking agent has a functional group that participates in crosslinking. As such a functional group, a carboxyl group, a maleic anhydride group, etc. can be cited. As a crosslinking agent, a compound that does not belong to the polycondensation polymer can be used.
[0027] The crosslinking agent may have various monomers as monomer units (monomer unit = structural unit. The same applies below), and may have monomer units derived from various monomers. Examples of such monomers include aromatic vinyl compounds, maleimide compounds (compounds having a maleimide group), maleic acid compounds, olefin hydrocarbons (ethylene, propylene, butene, etc.), (meth)acrylates (methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, etc.), unsaturated dicarboxylic acids (itaconic acid, citraconic acid, aconitic acid, etc.), unsaturated dicarboxylic acid anhydrides (itaconic anhydride, citraconic anhydride, aconitic anhydride, etc. Maleic anhydride (anhydrous maleic acid) is excluded), vinyl acetate, vinyl carboxylic acid ((meth)acrylic acid, etc.), (meth)acrylamide, etc. The monomers may be used alone or in combination of two or more.
[0028] From the viewpoint of facilitating reduction of knots, facilitating reduction of gloss, and facilitating improvement of the hue of the crosslinking agent and the fiber for artificial hair (facilitating suppression of yellowing), the crosslinking agent preferably has an aromatic vinyl compound as a monomer unit, and more preferably has a monomer unit derived from an aromatic vinyl compound.
[0029] As the aromatic vinyl compound, there can be mentioned styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, ethylstyrene, p-tert-butylstyrene, α-methylstyrene, α-methyl-p-methylstyrene and other styrene compounds. From the viewpoint of being easy to further reduce knots, easy to further reduce the gloss, and the viewpoint of making the hue of the crosslinking agent and the artificial hair fiber more effective, the aromatic vinyl compound preferably contains styrene. Aromatic vinyl compounds (styrene compounds, etc.) can be used alone or in combination of two or more.
[0030] Examples of the maleimide compound include maleimide; N-alkyl maleimides such as N-methylmaleimide, N-butylmaleimide, and N-cyclohexylmaleimide; aromatic maleimides such as N-phenylmaleimide, N-chlorophenylmaleimide, N-methylphenylmaleimide, N-methoxyphenylmaleimide, and N-tribromophenylmaleimide. From the viewpoint of facilitating the reduction of knots, from the viewpoint of facilitating the reduction of gloss, and from the viewpoint of high effect of improving the heat resistance of the crosslinking agent and the fiber for artificial hair, the maleimide compound preferably contains at least one selected from the group consisting of maleimide and N-phenylmaleimide. The maleimide compound can be used alone or in combination of two or more.
[0031] Examples of the maleic acid compound include maleic acid and maleic acid derivatives. Examples of the maleic acid derivative include maleic anhydride, maleate salts (e.g., sodium maleate), maleate esters (e.g., maleic acid alkyl esters such as methyl maleate), etc. From the perspective of facilitating the reduction of knots and the perspective of facilitating the reduction of gloss, the maleic acid compound preferably includes maleic anhydride.
[0032] As the cross-linking agent, maleimide polymers (maleimide polymers), epoxy-modified polymers (except compounds equivalent to maleimide polymers), maleic acid polymers (except epoxy-modified polymers or compounds equivalent to maleimide polymers), etc. can be cited. The cross-linking agent can be a form containing maleimide polymers, a form containing epoxy-modified polymers, or a form containing maleic acid polymers. Each of maleimide polymers, epoxy-modified polymers, and maleic acid polymers can be used alone or in combination of two or more.
[0033] From the viewpoint of facilitating reduction of knots and from the viewpoint of facilitating reduction of gloss, the crosslinking agent preferably comprises at least one selected from the group consisting of maleimide polymers, epoxy-modified polymers, and maleic acid polymers. From the viewpoint of facilitating further reduction of gloss, it preferably comprises at least one selected from the group consisting of maleimide polymers and maleic acid polymers, and more preferably comprises a maleimide polymer.
[0034] The maleimide polymer has a maleimide compound as a monomer unit (maleimide monomer unit), and may have a monomer unit derived from a maleimide compound. By using a maleimide polymer, it is easy to improve the heat resistance of the fiber for artificial hair. The monomer unit of the maleimide compound can be obtained by polymerizing a raw material containing a maleimide compound, or by polymerizing an unsaturated dicarboxylic acid anhydride in advance, reacting a group derived from the unsaturated dicarboxylic acid anhydride with ammonia or a primary amine, and converting the group derived from the unsaturated dicarboxylic acid anhydride (post-imidization method) to obtain it. As the maleimide polymer, a maleimide homopolymer (homopolymer of a maleimide compound) or a maleimide copolymer (copolymer of a maleimide compound) can be used.
[0035] The content of the monomeric unit of the maleimide compound in the maleimide polymer is preferably in the following range based on the total mass of the maleimide polymer. From the viewpoint of easily achieving the improvement of the heat resistance of the maleimide polymer and the fiber for artificial hair, the content of the monomeric unit of the maleimide compound is preferably 35% by mass or more, and more preferably 37% by mass or more. From the viewpoint of easily obtaining good impact strength of the maleimide polymer and the fiber for artificial hair, the content of the monomeric unit of the maleimide compound is preferably 50% by mass or less, and more preferably 45% by mass or less. From such a viewpoint, the content of the monomeric unit of the maleimide compound is preferably 35 to 50% by mass, and more preferably 37 to 45% by mass.
[0036] The maleimide copolymer has a compound different from the maleimide compound as a monomer unit. The maleimide copolymer can be obtained by copolymerizing a raw material containing a maleimide compound and a monomer other than the maleimide compound, or by copolymerizing an unsaturated dicarboxylic acid anhydride in advance, reacting a group derived from the unsaturated dicarboxylic acid anhydride with ammonia or a primary amine, and converting the group derived from the unsaturated dicarboxylic acid anhydride (post-imidization method). As a compound different from the maleimide compound, various monomers mentioned above in relation to the crosslinking agent can be used.
[0037] From the viewpoint of being easy to reduce knots, the viewpoint of being easy to reduce gloss, and the viewpoint of being easy to improve the hue of the maleimide copolymer and the fiber for artificial hair (easy to suppress yellowing), the maleimide copolymer preferably has an aromatic vinyl compound as a monomer unit, and preferably has a monomer unit derived from an aromatic vinyl compound. As the aromatic vinyl compound, the styrene compounds mentioned above with respect to the crosslinking agent can be used. From the viewpoint of being easier to reduce knots, the viewpoint of being easier to reduce gloss, and the viewpoint of having a higher effect of improving the hue of the maleimide copolymer and the fiber for artificial hair, the aromatic vinyl compound preferably contains styrene.
[0038] The content of the monomer unit of the aromatic vinyl compound in the maleimide copolymer is preferably in the following range based on the total mass of the maleimide copolymer. From the viewpoint of easily obtaining a good hue of the maleimide copolymer and the fiber for artificial hair, the content of the monomer unit of the aromatic vinyl compound is preferably 40% by mass or more, and more preferably 45% by mass or more. From the viewpoint of easily obtaining a good heat resistance of the maleimide copolymer and the fiber for artificial hair, the content of the monomer unit of the aromatic vinyl compound is preferably 60% by mass or less, and more preferably 55% by mass or less. From such a viewpoint, the content of the monomer unit of the aromatic vinyl compound is preferably 40 to 60% by mass, and more preferably 45 to 55% by mass.
[0039] The maleimide copolymer preferably has an unsaturated dicarboxylic acid anhydride as a monomer unit, preferably a monomer unit derived from an unsaturated dicarboxylic acid anhydride. In this case, the monomer unit of the unsaturated dicarboxylic acid anhydride reacts with other polymers having amino or alcohol groups at the end, and the effect as a compatibilizer of the polymer is easily obtained.
[0040] Based on the total mass of the maleimide polymer, the content of the monomer unit of the unsaturated dicarboxylic anhydride in the maleimide polymer is preferably in the following range. From the viewpoint of reducing knots and gloss with good balance, and the viewpoint that the monomer unit of the unsaturated dicarboxylic anhydride reacts with other polymers having amino or alcohol groups at the end, it is easier to obtain the effect of the compatibilizer for the polymer, the content of the monomer unit of the unsaturated dicarboxylic anhydride is preferably 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, 0.8% by mass or more, 1% by mass or more, 1.2% by mass or more, 1.5% by mass or more, 2% by mass or more, 3% by mass or more, 5% by mass or more, or 6% by mass or more. From the viewpoint of reducing knots and gloss with good balance, and the viewpoint of being easy to obtain excellent thermal stability, the content of the monomer unit of the unsaturated dicarboxylic anhydride is preferably 10% by mass or less, 8% by mass or less, or 6% by mass or less. From such a viewpoint, the content of the monomer unit of the unsaturated dicarboxylic anhydride is preferably 0.1 to 10% by mass, 0.5 to 10% by mass, or 0.5 to 6% by mass. The content of the monomer unit of the unsaturated dicarboxylic anhydride may be 5% by mass or less, 3% by mass or less, 2% by mass or less, or 1.5% by mass or less. The content of the monomer unit of the unsaturated dicarboxylic anhydride may be 0.5 to 5% by mass.
[0041] Specific examples of maleimide polymers include styrene-maleimide copolymers, maleimide-maleic anhydride copolymers, styrene-maleimide-maleic anhydride copolymers, etc. From the perspective of facilitating the reduction of knots and the perspective of facilitating the reduction of gloss, the maleimide polymer preferably includes a styrene-maleimide-maleic anhydride copolymer.
[0042] When the crosslinking agent contains a maleimide polymer, the content of the maleimide polymer is preferably 80% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more, or 99% by mass or more, based on the total mass of the crosslinking agent (the total mass of the crosslinking agent contained in the fiber for artificial hair. The same shall apply hereinafter). The crosslinking agent may be substantially composed of a maleimide polymer (substantially 100% by mass of the crosslinking agent is a maleimide polymer).
[0043] Examples of the epoxy-modified polymer include a polymer having an epoxy group at the end of the main chain and / or a side chain of a (meth)acrylic polymer, i.e., an epoxy-modified (meth)acrylic polymer, and a polymer having an epoxy group at the end of the main chain and / or a side chain of a polyolefin, i.e., an epoxy-modified polyolefin. The epoxy-modified polymer may be used alone or in combination of two or more.
[0044] The epoxy-modified (meth)acrylic polymer has a (meth)acryloyl group. The epoxy-modified polyolefin has an olefinic hydrocarbon as a monomer unit, and may have a monomer unit derived from an olefinic hydrocarbon.
[0045] From the viewpoint of being easy to reduce knots, the viewpoint of being easy to reduce gloss, and the viewpoint of being easy to improve the hue of the epoxy-modified polymer and the fiber for artificial hair (easy to suppress yellowing), the epoxy-modified polymer preferably has an aromatic vinyl compound as a monomer unit, and preferably has a monomer unit derived from an aromatic vinyl compound. As the aromatic vinyl compound, the styrene-based compounds mentioned above in connection with the crosslinking agent can be used. From the viewpoint of being easier to reduce knots, the viewpoint of being easier to reduce gloss, and the viewpoint of having a higher effect of improving the hue of the epoxy-modified polymer and the fiber for artificial hair, the aromatic vinyl compound preferably contains styrene.
[0046] When the crosslinking agent includes an epoxy-modified polymer, the content of the epoxy-modified polymer is preferably 80% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more, or 99% by mass or more, based on the total mass of the crosslinking agent. Alternatively, the crosslinking agent may be substantially composed of the epoxy-modified polymer (substantially 100% by mass of the crosslinking agent is the epoxy-modified polymer).
[0047] The maleic acid polymer has at least one maleic acid compound selected from the group consisting of maleic acid and maleic acid derivatives as a monomer unit, and may have a monomer unit from a maleic acid compound. As a maleic acid derivative, the maleic acid derivative described above with respect to a cross-linking agent can be used. From the viewpoint of reducing knots and gloss with good balance, the maleic acid compound preferably includes maleic anhydride (the maleic acid polymer is preferably a copolymer of a skeleton of maleic anhydride introduced into the molecule, i.e., a maleic anhydride-modified polymer). From the viewpoint of reducing knots and gloss with good balance, the maleic acid polymer preferably has a polyalkylene chain (e.g., a polypropylene chain).
[0048] Specific examples of maleic acid polymers include styrene-maleic anhydride copolymers; maleic anhydride-modified polyalkylenes (e.g. maleic anhydride-modified polypropylene); maleic anhydride-grafted polymers; terpolymers such as ethylene-acrylate-maleic anhydride copolymers and ethylene-vinyl acetate-maleic anhydride copolymers, and the like.
[0049] The equivalent weight of the functional group involved in the crosslinking in the crosslinking agent is preferably in the following range. From the viewpoint of reducing the knot and gloss with good balance, the equivalent weight of the functional group is preferably 0.1 meq / g or more, 0.2 meq / g or more, 0.3 meq / g or more, 0.4 meq / g or more, 0.45 meq / g or more, 0.48 meq / g or more, 0.5 meq / g or more, 0.6 meq / g or more, 0.7 meq / g or more, 0.8 meq / g or more, 0.9 meq / g or more, 1 meq / g or more, 1.2 meq / g or more, 1.4 meq / g or more, 1.5 meq / g or more, 1.8 meq / g or more, 2 meq / g or more, 2.5 meq / g or more, 3 meq / g or more, or 3.5 meq / g or more. From the viewpoint of reducing knots and gloss with good balance, the equivalent of the functional group is preferably 5 meq / g or less, 4 meq / g or less, 3.5 meq / g or less, 3 meq / g or less, 2.5 meq / g or less, 2 meq / g or less, 1.8 meq / g or less, 1.5 meq / g or less, 1.4 meq / g or less, 1.2 meq / g or less, 1 meq / g or less, 0.7 meq / g or less, 0.6 meq / g or less, 0.5 meq / g or less, 0.48 meq / g or less, 0.45 meq / g or less, 0.4 meq / g or less, 0.3 meq / g or less, or 0.2 meq / g or less. From such a viewpoint, the equivalent of the functional group is preferably 0.1 to 5 meq / g.
[0050] When the cross-linking agent includes a maleic acid polymer, the content of the maleic acid polymer is preferably 80% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more, or 99% by mass or more, based on the total mass of the cross-linking agent. Alternatively, the cross-linking agent may be substantially composed of a maleic acid polymer (substantially 100% by mass of the cross-linking agent is a maleic acid polymer).
[0051] The content of the crosslinking agent is preferably in the following ranges based on the total mass of the fiber for artificial hair. From the viewpoint of reducing knots and gloss with good balance, the content of the crosslinking agent is preferably 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, 0.7% by mass or more, or 0.75% by mass or more. From the viewpoint of reducing knots and gloss with good balance, the content of the crosslinking agent is preferably 50% by mass or less, less than 50% by mass, 45% by mass or less, 40% by mass or less, 35% by mass or less, 30% by mass or less, 25% by mass or less, 20% by mass or less, 15% by mass or less, 10% by mass or less, 9% by mass or less, 8% by mass or less, or 7.5% by mass or less. From such a viewpoint, the content of the crosslinking agent is preferably 0.1 to 50% by mass. From the same viewpoint, the content of the maleimide polymer, the content of the epoxy-modified polymer, or the content of the maleic acid polymer is preferably in the above ranges based on the total mass of the fiber for artificial hair.
[0052] The content of the crosslinking agent can be adjusted according to the type of the crosslinking agent, and can be in the following ranges based on the total mass of the fiber for artificial hair in consideration of the balance between the knot and the gloss. The content of the crosslinking agent can be 0.8% by mass or more, 1% by mass or more, 1.5% by mass or more, 1.8% by mass or more, 2% by mass or more, 2.5% by mass or more, 3% by mass or more, 3.5% by mass or more, 4% by mass or more, 4.5% by mass or more, 5% by mass or more, 5.5% by mass or more, 6% by mass or more, 6.5% by mass or more, or 7% by mass or more. The content of the crosslinking agent can be 7% by mass or less, 6.5% by mass or less, 6% by mass or less, 5.5% by mass or less, 5% by mass or less, 4.5% by mass or less, 4% by mass or less, 3.5% by mass or less, 3% by mass or less, 2.5% by mass or less, 2% by mass or less, 1.8% by mass or less, 1.5% by mass or less, 1% by mass or less, 0.8% by mass or less, or 0.75% by mass or less. From the same viewpoint, the content of the maleimide polymer, the content of the epoxy-modified polymer, or the content of the maleic acid polymer based on the total mass of the fiber for artificial hair may be within the above-mentioned respective ranges.
[0053] Based on the total amount of the polycondensation polymer and the crosslinking agent, the content of the crosslinking agent is preferably in the following range. From the perspective of reducing knots and gloss with good balance, the content of the crosslinking agent is preferably 0.1% by mass or more, 0.5% by mass or more, or 1% by mass or more. From the perspective of reducing knots and gloss with good balance, the content of the crosslinking agent is preferably 90% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, less than 50% by mass, 45% by mass or less, 40% by mass or less, 35% by mass or less, 30% by mass or less, 25% by mass or less, 20% by mass or less, 15% by mass or less, or 10% by mass or less. From such a viewpoint, the content of the crosslinking agent is preferably 0.1 to 90% by mass. From the same viewpoint, based on the total amount of the polycondensation polymer and the crosslinking agent, the content of the maleimide polymer, the content of the epoxy-modified polymer, or the content of the maleic acid polymer is preferably in the above-mentioned respective ranges.
[0054] The content of cross-linking agent can be adjusted according to the type of cross-linking agent, taking into account the balance of knot, gloss, etc., the total amount of polycondensation polymer and cross-linking agent as a benchmark can be the following range. The content of cross-linking agent can be more than 1.5 mass %, more than 2 mass %, more than 2.5 mass %, more than 3 mass %, more than 4 mass %, more than 5 mass %, more than 6 mass %, more than 7 mass %, more than 7.5 mass %, more than 8 mass % or more than 10 mass %. The content of cross-linking agent can be less than 8 mass %, less than 7.5 mass %, less than 7 mass %, less than 6 mass %, less than 5 mass %, less than 4 mass %, less than 3 mass %, less than 2.5 mass %, less than 2 mass %, less than 1.5 mass % or less than 1 mass %. From the same viewpoint, based on the total amount of polycondensation polymer and cross-linking agent, the content of maleimide polymer, the content of epoxy-modified polymer or the content of maleic acid polymer can be the above-mentioned each range.
[0055] The product XY (X·Y=X×Y) of the ratio X [mass %] of the content of the crosslinking agent relative to the total amount of the polycondensation polymer and the crosslinking agent and the equivalent Y [meq / g] of the functional group participating in the crosslinking in the crosslinking agent is preferably in the following range. When the polycondensation polymer is a maleimide polymer, the following range is more preferred. From the viewpoint of facilitating the inhibition of the formation of knots and the viewpoint of facilitating the reduction of gloss, the product XY is preferably 1.8 or more, 1.9 or more, 2 or more, 2.2 or more, 2.3 or more, 2.5 or more, 3 or more, 3.3 or more, 3.5 or more, 4 or more, 4.2 or more, 4.5 or more, or 4.6 or more. From the viewpoint of facilitating the inhibition of the formation of knots, the viewpoint of facilitating the reduction of gloss, and the viewpoint of facilitating the obtaining of excellent spinning properties and processability, the product XY is preferably 10 or less, 8 or less, or 7 or less. From such a viewpoint, the product XY is preferably 1.8 to 10, or 2 to 7. The product XY may be 4.65 or more, 4.7 or more, 4.8 or more, 4.9 or more, 5 or more, 6 or more, or 7 or more. The product XY may be 6 or less, 5 or less, 4.9 or less, 4.8 or less, 4.7 or less, 4.65 or less, 4.6 or less, 4.5 or less, 4.2 or less, 4 or less, 3.5 or less, 3.3 or less, 3 or less, 2.5 or less, 2.3 or less, 2.2 or less, 2 or less, 1.9 or less, or 1.8 or less.
[0056] The artificial hair fiber of this embodiment may contain additives other than the polycondensation polymer and the crosslinking agent. Examples of the additives include flame retardants, flame retardant aids, colorants (pigments, dyes, etc.), microparticles, heat-resistant agents, light stabilizers, fluorescent agents, antioxidants, antistatic agents, plasticizers, lubricants, and the like.
[0057] The fiber for artificial hair involved in this embodiment may contain a flame retardant. From the viewpoint of facilitating the reduction of gloss, the flame retardant preferably includes a bromine-based flame retardant (a flame retardant containing bromine atoms). The content of the flame retardant is preferably 3 to 30 parts by mass, more preferably 5 to 30 parts by mass, and further preferably 10 to 28 parts by mass relative to 100 parts by mass of the total of the polycondensation polymer and the crosslinking agent. In addition, the content of the flame retardant may also exceed 30 parts by mass relative to 100 parts by mass of the polycondensation polymer (e.g., polyamide resin).
[0058] As the bromine-based flame retardant, there can be cited brominated phenol condensates, brominated polystyrene resins, brominated benzyl acrylate flame retardants, brominated epoxy resins, brominated phenoxy resins (excluding components equivalent to brominated epoxy resins), brominated polycarbonate resins, bromine-containing triazine compounds, and the like. From the viewpoint of excellent balance of drip resistance, processability, transparency of the raw yarn, etc. of the artificial hair fiber, the viewpoint of easy reduction of knots, and the viewpoint of easy reduction of gloss, the flame retardant preferably contains a compound having a structure represented by the following formula (1) (bromine-based flame retardant), and more preferably contains a brominated epoxy resin having a structure represented by the following formula (1). When the artificial hair fiber involved in the present embodiment contains a compound having a structure represented by formula (1), from the viewpoint of improving the dispersibility of the flame retardant, the crosslinking agent preferably has an aromatic vinyl compound (e.g., styrene) as a monomer unit. As the aromatic vinyl compound, the styrene-based compounds described above with respect to the crosslinking agent can be used.
[0059] [Chemical formula 1]
[0060]
[0061] [n represents an integer greater than or equal to 1.]
[0062] The method for producing the fiber for artificial hair according to the present embodiment comprises a spinning step of spinning a composition containing a polycondensation polymer and a crosslinking agent. According to the method for producing the fiber for artificial hair according to the present embodiment, the fiber for artificial hair according to the present embodiment can be obtained.
[0063] In the spinning step, a filament containing a polycondensation polymer and a crosslinking agent can be obtained. In the spinning step, the composition containing a polycondensation polymer and a crosslinking agent can be melt-spun (melt-deformed). The fiber for artificial hair can be produced by melt spinning under appropriate temperature conditions corresponding to the type of the polycondensation polymer by a conventional melt spinning method.
[0064] The melt viscosity of the polycondensation polymer (for example, polyamide resin) measured at 300°C and a shear rate of 2400 [1 / s] is preferably in the following range. From the viewpoint of facilitating the reduction of knots and the viewpoint of facilitating the reduction of gloss, the melt viscosity of the polycondensation polymer is preferably 50 Pa·s or more, more preferably 60 Pa·s or more, further preferably 70 Pa·s or more, and particularly preferably 75 Pa·s or more. From the viewpoint of facilitating the reduction of knots and the viewpoint of facilitating the reduction of gloss, the melt viscosity of the polycondensation polymer is preferably 300 Pa·s or less, more preferably 250 Pa·s or less, further preferably 200 Pa·s or less, particularly preferably 140 Pa·s or less, extremely preferably 120 Pa·s or less, very preferably 100 Pa·s or less, and further preferably 80 Pa·s or less. From such a viewpoint, the melt viscosity of the polycondensation polymer is preferably 50 to 300 Pa·s.
[0065] The method for producing the fiber for artificial hair according to the present embodiment may include a mixing step of mixing the polycondensation polymer and the crosslinking agent to obtain a composition before the spinning step. In the mixing step, the melt viscosity of the polycondensation polymer is preferably within the above range.
[0066] Before the spinning step, the method for producing the fiber for artificial hair according to the present embodiment may include a kneading step of melt-kneading the composition containing the polycondensation polymer and the cross-linking agent. As the device for melt-kneading, various common kneaders may be used. As the kneader, single-screw extruders, twin-screw extruders, rollers, Banbury mixers, kneaders, etc. may be cited. From the viewpoint of adjusting the kneading degree and the simplicity of operation, twin-screw extruders are preferred.
[0067] The method for producing the fiber for artificial hair according to the present embodiment may include a stretching step of stretching the yarn (unstretched yarn) obtained in the spinning step after the spinning step.
[0068] From the viewpoint of easily showing the strength of the fiber, the stretching ratio in the stretching process is preferably 1.5 times or more, and more preferably 2.0 times or more. From the viewpoint of not easily causing the breakage of the fiber during the stretching process, the stretching ratio is preferably 5.0 times or less, and more preferably 4.0 times or less. From such a viewpoint, the stretching ratio is preferably 1.5 to 5.0 times, and more preferably 2.0 to 4.0 times.
[0069] The stretching treatment can be carried out by a two-step method in which the undrawn yarn is temporarily wound on a bobbin and then stretched in a process discontinuous with the spinning process, or by a direct spinning stretching method in which the undrawn yarn is not wound on a bobbin but stretched in a process continuous with the spinning process. The stretching treatment can be carried out by a single-stage stretching method in which the undrawn yarn is stretched to a target stretching ratio once, or by a multi-stage stretching method in which the undrawn yarn is stretched to a target stretching ratio by two or more stretchings. By such a stretching treatment, it is easy to obtain a drawn yarn with a fineness of less than 100 dtex, and it is easy to increase the tensile strength of the fiber.
[0070] The temperature of the stretching treatment is preferably 90 to 120° C. When the temperature is 90° C. or higher, it is easy to ensure sufficient fiber strength and less likely to break. When the temperature is 120° C. or lower, it is easy to obtain a suitable feel of the fiber (it is easy to suppress the feel of the fiber from becoming a smooth plastic-like feel).
[0071] After the stretching step, the method for producing the fiber for artificial hair according to the present embodiment may include a heat treatment step of heat-treating (annealing) the yarn obtained in the stretching step (stretched yarn). The heat treatment step can reduce the heat shrinkage of the stretched yarn.
[0072] The heat treatment temperature is preferably 150° C. or higher, more preferably 160° C. or higher, further preferably 170° C. or higher, and particularly preferably 180° C. or higher. The heat treatment temperature is preferably 200° C. or lower. The heat treatment may be performed continuously after the stretching treatment, or may be performed at intervals after temporary winding.
[0073] The hair accessories according to the present embodiment include the artificial hair fibers according to the present embodiment. The hair accessories according to the present embodiment are articles that can be worn on the head and can be in the form of being formed of the artificial hair fibers according to the present embodiment (for example, a fiber bundle of the artificial hair fibers). Examples of the hair accessories include wigs, hairpieces, and hair extensions.
[0074] Example
[0075] Hereinafter, the present invention will be specifically described using Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0076] <Production of Undrawn Yarn>
[0077] The polycondensation polymer is dried and the moisture absorption rate is adjusted to less than 1000 ppm. A total of 100 parts by mass of the polycondensation polymer and the crosslinking agent (the crosslinking agent shown in Tables 1 to 3), 27.5 parts by mass of the flame retardant, 2.3 parts by mass of the flame retardant aid, 1.4 parts by mass of the colorant A, 0.6 parts by mass of the colorant B, 0.2 parts by mass of the colorant C, 0.2 parts by mass of the antioxidant A, 0.2 parts by mass of the antioxidant B, and 1.1 parts by mass of the lubricant are mixed to obtain a mixture. For the "total of 100 parts by mass of the polycondensation polymer and the crosslinking agent", for example, in Example 1, 92.5 parts by mass of the polycondensation polymer and 7.5 parts by mass of the crosslinking agent are used, and in Comparative Example 1, no crosslinking agent is used but 100 parts by mass of the polycondensation polymer is used. In the table, "content (X)" represents the content of the crosslinking agent based on the total amount of the polycondensation polymer and the crosslinking agent, "equivalent (Y)" represents the equivalent of the functional groups in the crosslinking agent that participate in the crosslinking, and "product XY" represents the product of content (X) and equivalent (Y).
[0078] The details of the materials used in Examples and Comparative Examples are as follows: The content of maleic anhydride refers to the content of the monomer unit of maleic anhydride in the maleimide polymer.
[0079] (Condensation Polymer)
[0080] Polyamide resin: polyamide 66, manufactured by Asahi Kasei Corporation, trade name "Leona 1300 301", melt viscosity 75 Pa·s (measured at 300° C., shear rate 2400 [1 / s])
[0081] (Crosslinking agent)
[0082] [Maleimide polymer]
[0083] Crosslinking agent A: styrene-maleimide-maleic anhydride copolymer, manufactured by Denka Co., Ltd., trade name "MS-L2A", maleic anhydride content 6.0 mass%
[0084] Crosslinking agent B: styrene-maleimide-maleic anhydride copolymer, manufactured by Denka Co., Ltd., trade name "MS-NB", maleic anhydride content 1.5 mass%
[0085] [Epoxy modified polymer]
[0086] Crosslinking agent C: Epoxy-modified acrylic-styrene polymer, manufactured by Toagosei Co., Ltd., trade name "ARUFONUG 4070"
[0087] Crosslinking agent D: Epoxy-modified acrylic-styrene polymer, manufactured by Toagosei Co., Ltd., trade name "ARUFONUG 4035"
[0088] Crosslinking agent E: Epoxy-modified acrylic-styrene polymer, manufactured by BASF Japan Ltd., trade name "Joncryl ADR 4368C"
[0089] [Maleic acid polymer]
[0090] Crosslinking agent F: Maleic anhydride-modified polypropylene, manufactured by Sanyo Chemical Industries, Ltd., trade name "UMEX 1010"
[0091] Crosslinking agent G: Maleic anhydride-modified polypropylene, manufactured by Sanyo Chemical Industries, Ltd., trade name "UMEX 1001"
[0092] Crosslinking agent H: Maleic anhydride-modified polypropylene, manufactured by Riken Vitamin Co., Ltd., trade name "Rikeeido MG-670P"
[0093] Crosslinking agent I: Maleic anhydride-modified polypropylene, manufactured by Riken Vitamin Co., Ltd., trade name "Rikeeido MG-400P"
[0094] Crosslinking agent J: Maleic anhydride-modified polypropylene, manufactured by Riken Vitamin Co., Ltd., trade name "Rikeeido MG-250P"
[0095] (Other additives)
[0096] Flame retardant: Brominated epoxy resin, manufactured by Sakamoto Pharmaceutical Industry Co., Ltd., trade name "SRT-20000"
[0097] Flame retardant additive: Suzuyu Chemical Co., Ltd., trade name "S-370DE"
[0098] Colorant A: Made by Saika Chemical Industry Co., Ltd., trade name "SPUNDYE NGS BK-35"
[0099] Colorant B: manufactured by Saika Chemical Industry Co., Ltd., trade name "PA7-4089 Red"
[0100] Colorant C: manufactured by Saika Chemical Industry Co., Ltd., trade name "PA7-4092 Yellow"
[0101] Antioxidant A: manufactured by BASF Japan Ltd., trade name "Irganox 1098"
[0102] Antioxidant B: manufactured by BASF Japan Ltd., trade name "Irgafos 168"
[0103] Lubricant: Nitto Kasei Kogyo Co., Ltd., trade name "CS-8CP"
[0104] use The mixture was kneaded by a twin-screw extruder to obtain raw material pellets for spinning. Next, the raw material pellets were dried to adjust the moisture absorption rate to less than 1000 ppm. The raw material pellets were melt-kneaded by a twin-screw extruder at a barrel set temperature of 280°C. The gear pump was used to adjust the discharge rate to a constant level, and the melt was spun vertically from a die with a hole diameter of 0.5 mm / root at a temperature of 295°C. The undrawn yarn (undrawn artificial hair fiber) was wound at a constant speed by a tractor set at a position 2m directly below the nozzle. The single fineness of the undrawn yarn was 145 dtex.
[0105] <Production of Evaluation Fiber>
[0106] The undrawn yarn was drawn at 100°C and then annealed at 180°C to obtain an evaluation fiber (drawn fiber for artificial hair) having a single fineness of 66 dtex. The drawing ratio was 2.3 times, and the relaxation rate during annealing was 6.8%. The relaxation rate during annealing was a value calculated as "(rotation speed of the take-up roll during annealing) / (rotation speed of the delivery roll during annealing)".
[0107] <Evaluation of Evaluation Fiber>
[0108] The number of knots and gloss were evaluated using the above-mentioned evaluation fibers. The details of each evaluation are as follows. The measurement results are shown in Tables 1 to 3.
[0109] (Number of knots)
[0110] The number of knots observed on 50 evaluation fibers of 1 m in length was measured. Here, a "knot" is a nodular portion that bulges outward in a nodular manner in the radial direction, and is a portion whose maximum diameter is 1.2 times or more the minimum diameter in an area within a range of ±10 mm from the maximum diameter in the fiber length direction. The values in Tables 1 to 3 are the total number of knots observed on 50 evaluation fibers.
[0111] (luster)
[0112] The glossiness is evaluated by measuring the glossiness. The glossiness is measured using a goniophotometer (goniophotometer) GP-700 manufactured by Murakami Color Research Laboratory Co., Ltd. First, a reference fiber (Luxeena, a polyamide-based artificial hair fiber manufactured by Denka Co., Ltd., hue #613T) is placed on a sample stand, the sensitivity adjustment counter value (COARSE) is set to 718, the sensitivity adjustment counter value (FINE) is set to 737, and the incident angle is set to 45°. The incident light intensity, the gain of the detector, etc. are adjusted so that the reflected light intensity at a light receiving angle of 45° is 80% of the detection limit of the device. After that, the evaluation fiber is placed on the sample stand, and the reflected light intensity is measured by changing the light receiving angle from 10° to 80°. And the maximum value of the reflected light intensity relative to the detection limit of the device is obtained as the glossiness [unit: %]. The smaller the glossiness value, the better.
[0113] [Table 1]
[0114] [Table 2]
[0115] [Table 3]
[0116] From the results shown in Tables 1 to 3, it can be seen that, compared with Comparative Example 1 in which no crosslinking agent was used, the generation of knots in the fiber was suppressed in Examples 1 to 21 in which a polycondensation polymer and a crosslinking agent were used in combination. In addition, it can be seen that the gloss of the fiber in Examples 1 to 21 was lower than that in Comparative Example 1. In particular, when a maleimide copolymer was used as a crosslinking agent (Examples 1 to 6), it was found that the gloss of the fiber tended to be lower than when an epoxy-modified polymer or a maleic acid-based polymer was used as a crosslinking agent (Examples 7 to 21).
Claims
1. A fiber for artificial hair, comprising a polycondensation polymer and a crosslinking agent, The polycondensation polymer comprises a polyamide resin, The content of the polyamide resin is 65% by mass or more based on the total mass of the fiber for artificial hair, The cross-linking agent comprises a maleimide polymer, The product of a ratio X [mass %] of the content of the crosslinking agent to the total amount of the polycondensation polymer and the crosslinking agent and an equivalent Y [meq / g] of functional groups participating in crosslinking in the crosslinking agent is 1.8 or more.
2. The fiber for artificial hair according to claim 1, wherein The product of a ratio X [mass %] of the content of the crosslinking agent to the total amount of the polycondensation polymer and the crosslinking agent and an equivalent Y [meq / g] of functional groups participating in crosslinking in the crosslinking agent is 2 or more.
3. The fiber for artificial hair according to claim 1, wherein The content of the polyamide-based resin is 65 to 90% by mass based on the total mass of the fiber for artificial hair.
4. The fiber for artificial hair according to any one of claims 1 to 3, wherein The crosslinking agent comprises an epoxy-modified polymer.
5. The fiber for artificial hair according to any one of claims 1 to 3, wherein The cross-linking agent includes a maleic acid-based polymer.
6. The fiber for artificial hair according to any one of claims 1 to 3, further comprising a compound having a structure represented by the following formula (1): The crosslinking agent has an aromatic vinyl compound as a monomer unit, [Chemical formula 1] n represents an integer of 1 or greater.
7. A hair accessories comprising the fiber for artificial hair according to any one of claims 1 to 6.
Citation Information
Patent Citations
Fiber for artificial hair
JP2011246844A
Fiber for polyester-based artificial hair and headdress product
CN104271821A
Polyamide-based fiber for artificial hair having exceptional dripping resistance upon combustion
CN107148227A
Fiber for artificial hair
CN109068780A
Yarn substitute for hair
JP1988243317A