Negative electrode for rechargeable lithium battery and rechargeable lithium battery including the same
By using the hierarchical structure of linear conductive materials and dot-shaped conductive materials in the negative electrode of rechargeable lithium batteries, the structural rupture problem caused by volume expansion of the negative electrode active material during charging and discharging is solved, and the cycle life and high of the battery are significantly improved. Magnification characteristics.
Patent Information
- Application Number
- CN202111367862.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-19
- Filing Date
- 2021-11-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-11-18
AI Technical Summary
The negative electrode active materials of existing rechargeable lithium batteries are prone to structural rupture due to volume expansion during charging and discharging, which affects the battery's cycle life and high-magnification characteristics.
The negative electrode structure consisting of a current collector, a first negative electrode active material layer and a second negative electrode active material layer are adopted, wherein the first negative electrode active material layer contains a linear conductive material, and the second negative electrode active material layer contains a dot-shaped conductive material, and by reasonable Layer thickness and material combinations are used to suppress volume expansion and maintain structural integrity.
It effectively suppresses the volume expansion of the negative electrode active material, improves the cycle life of the battery and the high-rate charging and discharging performance, and significantly improves the energy density and capacity retention rate of the battery.
Smart Images

Figure CN114520315B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode for a rechargeable lithium battery and a rechargeable lithium battery including the negative electrode. Background Art
[0002] Recently, with the rapid popularization of electronic devices using batteries (such as mobile phones, notebook computers and electric vehicles), the demand for small, lightweight and relatively high-capacity rechargeable lithium batteries is rapidly increasing. Recently, since rechargeable lithium batteries have a lighter weight and a high energy density, they have attracted attention as a driving power source for portable devices. Therefore, research on improving the performance of rechargeable lithium batteries is actively studied.
[0003] The rechargeable lithium battery includes positive and negative electrodes including an active material capable of intercalating and deintercalating lithium ions and an electrolyte, and generates electric energy due to oxidation and reduction reactions when lithium ions are intercalated and deintercalated in the positive and negative electrodes.
[0004] For the positive active material of the rechargeable lithium battery, transition metal compounds such as lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide are mainly used. As the negative active material, crystalline carbon or amorphous carbon such as natural graphite and artificial graphite is used, or silicon-based active materials are used.
[0005] Recently, in order to improve the energy density of rechargeable lithium batteries, a thick negative electrode active material layer is prepared, and in particular, a negative electrode active material layer using two layers of silicon-based active materials has been tried. However, in this case, cracking of the negative electrode structure caused by volume expansion and formation of the silicon-based active material may occur during charging and discharging.
[0006] The above information disclosed in this Background section is only for enhancement of understanding of the background of the invention and therefore it may contain information that does not form the prior art that is already known in this country to a person of ordinary skill in the art. Summary of the invention
[0007] One embodiment provides a negative electrode for a rechargeable lithium battery exhibiting excellent high-rate characteristics and cycle-life characteristics.
[0008] Another embodiment provides a rechargeable lithium battery including a negative electrode.
[0009] One embodiment provides a negative electrode comprising: a current collector; a first negative active material layer disposed on the current collector and comprising a first negative active material and a linear conductive material; and a second negative active material layer disposed on one side of the first negative active material layer and comprising a second negative active material.
[0010] The linear conductive material may be carbon nanotubes, carbon fibers, carbon nanofibers, or a combination thereof.
[0011] The second negative electrode active material layer may further include dot-shaped conductive materials.
[0012] The dot-shaped conductive material may be carbon black, superconductive acetylene black, Ketjen black, acetylene black, crystalline carbon, or a combination thereof.
[0013] The first negative electrode active material or the second negative electrode active material may be a Si-carbon composite, graphite, or a combination thereof. In addition, the first negative electrode active material or the second negative electrode active material may further include crystalline carbon.
[0014] The thickness of the second negative active material layer may be about 1% to about 75% based on the total thickness of the first negative active material layer and the second negative active material layer.
[0015] Another embodiment provides a rechargeable lithium battery including a negative electrode, a positive electrode, and an electrolyte.
[0016] The negative active material according to one embodiment may exhibit excellent high rate characteristics and cycle life characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a schematic diagram showing the structure of a negative electrode for a rechargeable lithium battery according to an embodiment.
[0018] Figure 2 is a schematic diagram showing the structure of a rechargeable lithium battery according to an embodiment.
[0019] Figure 3A and Figure 3B is a SEM photograph of the first negative electrode active material layer according to Example 1.
[0020] Figure 4 is a SEM photograph of the second negative electrode active material layer according to Example 1.
[0021] Figure 5A and Figure 5B is a SEM photograph of the first negative electrode active material layer according to Comparative Example 1.
[0022] Figure 6 is a graph showing the discharge capacity of the half-cells of Example 1 and Comparative Example 1 at each discharge rate.
[0023] Figure 7 is a graph showing the charge capacity of the half-cells of Example 1 and Comparative Example 1 at each charge rate.
[0024] Figure 8 It shows that Figure 7FIG. 5 is a graph showing the retention rates obtained after charging and discharging under the charging and discharging conditions of FIG. DETAILED DESCRIPTION
[0025] Hereinafter, embodiments are described in detail. However, these embodiments are only examples, the present invention is not limited thereto, and the present invention is defined by the scope of the claims.
[0026] A negative electrode for a rechargeable lithium battery according to one embodiment includes: a negative electrode collector; a first negative electrode active material layer disposed on the negative electrode collector; and a second negative electrode active material layer disposed on the first negative electrode active material layer.
[0027] The first negative electrode active material layer may include a first negative electrode active material and a linear conductive material, and the second negative electrode active material layer may include a second negative electrode active material. In addition, the second negative electrode active material layer may further include a dot conductive material.
[0028] Therefore, when a linear conductive material is used in the first negative electrode active material layer as the lower layer in contact with the negative electrode current collector, the volume expansion of the negative electrode can be effectively suppressed during charging and discharging. Specifically, when the second negative electrode active material layer as the upper layer in contact with the separator can also include a dot-shaped conductive material, this effect can be further improved.
[0029] Since the linear conductive material positioned on the lower layer acts as a matrix for holding the negative electrode active material, this volume expansion suppression can be achieved. In addition, the structure of the negative electrode active material can be well maintained during charge and discharge, so a long cycle life can be exhibited.
[0030] In addition, the linear conductive material can increase the distance of mobile electrons so that all negative electrode active materials positioned on the lower portion of the negative electrode active material layer participate in charge and discharge, and thus, high rate charge and discharge performance can be improved.
[0031] The dot-shaped conductive material can be in contact with the negative electrode active material over a large area in the negative electrode active material layer, and thus can improve high rate characteristics.
[0032] If a linear conductive material and a dot-shaped conductive material are mixed and used in one layer, such effects of using a linear conductive material in the lower part and using the linear conductive material together with the dot-shaped conductive material may not be sufficiently obtained. That is, when a linear conductive material and a dot-shaped conductive material are used together in one layer, the respective effects of the dot-shaped conductive material and the linear conductive material may not be sufficiently obtained. In addition, if a linear conductive material is used in the second negative electrode active material layer which is an upper layer in contact with the separator, and a dot-shaped conductive material is used in the first negative electrode active material layer which is a lower layer in contact with the negative electrode current collector, the volume expansion of the negative electrode active material layer is likely to occur during charge and discharge, and the dot-shaped conductive material may not sufficiently function as a negative electrode conductive material that imparts conductivity between the negative electrode active materials.
[0033] The linear conductive material may be carbon nanotubes, carbon fibers, carbon nanofibers, or a combination thereof. The carbon nanotubes may be single-walled carbon nanotubes, double-walled carbon nanotubes, multi-walled carbon nanotubes, or a combination thereof.
[0034] The linear conductive material may have an average length of about 30 μm to about 100 μm, about 30 μm to about 80 μm, or about 30 μm to about 50 μm. The linear conductive material may have a width of about 10 nm to about 40 nm, about 10 nm to about 30 nm, or about 10 nm to about 20 nm. The average length of the linear conductive material means not only a complete straight line length, but also a distance corresponding to the long axis of the linear conductive material in the negative active material layer. When a linear conductive material having such an average length and width is used, the linear conductive material can easily contact the negative active material.
[0035] The point-shaped conductive material may be carbon black, superconductive acetylene black (denkablack), Ketjen black, acetylene black, crystalline carbon or a combination thereof. The crystalline carbon may be artificial graphite, natural graphite or a combination thereof. The particle size of the point-shaped conductive material may be about 1 nm to about 100 nm, about 10 nm to about 80 nm or about 20 nm to about 60 nm.
[0036] The first negative electrode active material may be the same as or different from the second negative electrode active material, and may be a Si-carbon composite, graphite, or a combination thereof. According to one embodiment, when the negative electrode active material includes a Si-carbon composite, the advantages of using a linear conductive material in the first negative electrode active material layer and a dot conductive material in the second negative electrode active material layer can be effectively obtained. This is because the volume expansion of the Si-carbon composite is greater than that of crystalline carbon during charge and discharge.
[0037] The Si-carbon composite may include a composite comprising Si particles and a first carbon-based material. The first carbon-based material may be amorphous carbon or crystalline carbon. An example of a composite may include a core in which Si particles are mixed with a second carbon-based material and a third carbon-based material surrounding the core. The second carbon-based material and the third carbon-based material may be the same or different from each other and may be amorphous carbon or crystalline carbon.
[0038] The amorphous carbon may be pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, burned coke, carbon fiber, or a combination thereof, and the crystalline carbon may be artificial graphite, natural graphite, or a combination thereof.
[0039] The particle size of the Si particles may be about 10 nm to about 30 μm, and according to one embodiment, may be about 10 nm to about 1000 nm, and according to another embodiment, may be about 20 nm to about 150 nm. When the particle size of the Si particles is within the range, volume expansion caused during charge and discharge can be suppressed, and disconnection of the conductive path due to rupture of the particles can be prevented.
[0040] In the specification, the particle size may be the average particle size of the particles. Here, the average particle size may represent the particle size (D50) measured by cumulative volume. As used herein, when no definition is otherwise provided in the specification, such a particle size (D50) represents the particle diameter of which the cumulative volume is about 50% by volume in the particle distribution.
[0041] The average particle size (D50) can be measured by a method known to those of ordinary skill in the art, for example, by a particle size analyzer or by a transmission electron microscope photo or a scanning electron microscope photo. Alternatively, a dynamic light scattering measurement device is used for data analysis, and the number of particles is counted for each particle size range. Thus, the average particle size (D50) value can be easily obtained by calculation.
[0042] When the Si-carbon composite includes Si particles and a first carbon-based material, the amount of the Si particles may be about 30 wt % to about 70 wt %, and according to one embodiment, may be about 40 wt % to about 50 wt %. The amount of the first carbon-based material may be about 70 wt % to about 30 wt %, and according to one embodiment, may be about 60 wt % to about 50 wt %. When the amounts of the Si particles and the first carbon-based material fall within the range, high capacity characteristics may be exhibited.
[0043] If the Si-carbon composite includes a core in which Si particles and a second carbon-based material are mixed and a third carbon-based material surrounding the core, the third carbon-based material may be present with a thickness of about 5 nm to about 100 nm. In addition, based on the total weight of the Si-carbon composite, the amount of the third carbon-based material may be about 1 wt% to about 50 wt%, based on the total weight of the Si-carbon composite, the amount of the Si particles may be about 30 wt% to about 70 wt%, and based on the total weight of the Si-carbon composite, the amount of the second carbon-based material may be about 20 wt% to about 69 wt%. In the case where the amounts of the Si particles, the third carbon-based material and the second carbon-based material meet the range, the discharge capacity may be excellent and the capacity retention rate may be improved.
[0044] In one embodiment, the first negative electrode active material or the second negative electrode active material may further include crystalline carbon, which may be artificial graphite, natural graphite, or a combination thereof.
[0045] If the first negative electrode active material or the second negative electrode active material further includes crystalline carbon, the mixing ratio of the crystalline carbon and the Si-carbon composite may be about 1: 1 to about 20: 1 by weight, about 1: 1 to about 19: 1 by weight, or about 1.5: 1 to about 19: 1 by weight. When the mixing ratio of the crystalline carbon and the Si-carbon composite is within the range, the volume expansion of the negative electrode active material may be effectively suppressed, and the conductivity may also be improved.
[0046] In one embodiment, the thickness of the second negative electrode active material layer may be about 1% to about 75% based on the total thickness of the first negative electrode active material layer and the second negative electrode active material layer. When the thickness of the second negative electrode active material layer is within the range, the linear conductive material exists between the negative electrode active materials or between the negative electrode active material and the negative electrode current collector to be connected to each other, that is, the contact area between each other can be well controlled, and thus electron transport can also be improved.
[0047] In the first negative active material layer, the amount of the linear conductive material may be about 0.1 wt % to about 5 wt %, about 0.1 wt % to about 3 wt % or about 0.1 wt % to about 2 wt % based on the total 100 wt % of the first negative active material layer.
[0048] In addition, if the second negative active material layer further includes a dot-shaped conductive material, the amount of the dot-shaped conductive material may be about 0.5 wt % to about 5 wt %, about 0.5 wt % to about 3 wt % or about 0.5 wt % to about 2 wt % based on the total 100 wt % of the second negative active material layer.
[0049] When the amounts of the linear conductive material and the dot-shaped conductive material fall within the ranges respectively, the effects of using the linear conductive material and the dot-shaped conductive material can be more increased.
[0050] In one embodiment, when the first negative electrode active material layer includes a linear conductive material and the second negative electrode active material layer includes a dot-shaped conductive material, the amount of the linear conductive material may be about 20 wt% to about 50 wt% based on the total 100 wt% of the linear conductive material and the dot-shaped conductive material included in the negative electrode. Therefore, even if the linear conductive material is used in an amount of at least 20 wt%, the structure of the negative electrode active material layer can be well maintained, so that the volume expansion during charging and discharging can be effectively prevented to improve the battery performance. In addition, the linear conductive material can be used to the maximum extent in the same amount as the dot-shaped conductive material, and here, the effect associated with the high rate characteristics using the linear conductive material can also be improved.
[0051] In the first negative electrode active material layer, the amount of the first negative electrode active material may be about 95 wt % to about 99.5 wt % based on the total 100 wt % of the first negative electrode active material layer. In the second negative electrode active material layer, the amount of the second negative electrode active material may be about 95 wt % to about 99.5 wt % based on the total 100 wt % of the second negative electrode active material layer.
[0052] In addition, the first negative electrode active material layer may further include a binder. When the first negative electrode active material layer further includes a binder, the first negative electrode active material layer may include about 94 wt % to about 98.5 wt % of the first negative electrode active material, about 0.5 wt % to 5 wt % of the negative electrode conductive material (linear conductive material), and about 1 wt % to about 5.5 wt % of the binder, based on the total weight of the first negative electrode active material layer.
[0053] The second negative electrode active material layer may further include a binder. When the second negative electrode active material layer further includes a binder, the second negative electrode active material layer may include about 94 wt % to about 98.5 wt % of the second negative electrode active material, about 0.5 wt % to 5 wt % of the negative electrode conductive material (dot conductive material), and about 1 wt % to about 5.5 wt % of the binder, based on the total weight of the second negative electrode active material layer.
[0054] The binder improves the binding properties between the negative electrode active material particles and between the negative electrode active material particles and the negative electrode current collector. The binder includes a non-aqueous binder, an aqueous binder, or a combination thereof.
[0055] The non-aqueous binder may be ethylene propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0056] The aqueous binder can be styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber (ABR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polymers containing ethylene oxide, polyvinyl pyrrolidone, polypropylene, polyepichlorohydrin, polyphosphazene, ethylene propylene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol or a combination thereof.
[0057] When the negative electrode binder is an aqueous binder, a cellulose compound may also be used as a thickener to provide viscosity. The cellulose compound includes one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, and their alkali metal salts. The alkali metal may be Na, K, or Li. Based on 100 parts by weight of the negative electrode active material, such a thickener may be included in an amount of about 0.1 parts by weight to about 3 parts by weight.
[0058] The negative electrode current collector may include one selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0059] When referring to Figure 1 When the negative electrode is shown, the negative electrode 1 according to one embodiment includes a negative current collector 3, a first negative active material layer 5, and a second negative active material layer 7. The first negative active material layer 5 includes a first negative active material 5a and a linear conductive material 5b, and the second negative active material layer 7 includes a second negative active material 7a and a dot conductive material 7b.
[0060] Another embodiment provides a rechargeable lithium battery including a negative electrode, a positive electrode, and an electrolyte.
[0061] The positive electrode may include a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector.
[0062] The positive electrode active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions. Specifically, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. More specifically, a compound represented by one of the following chemical formulas may be used: Li a A 1-b X b D 2 (0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a E1-b X b O 2-c D c (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05);Li a HAVE BEEN 2-b X b O 4-c D c (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05);Li a Ni 1-b- c Co b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α≤2);Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);Li a Ni 1-b-c Co b X c O 2-α T 2 (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Mr b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α≤2);Li a Ni 1-b- c Mr b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Mr b X c O 2-α T 2 (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni b HAVE BEEN c G d O 2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1);Li a Nor b Co c Mn d G e O 2 (0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0.001≤e≤0.1);Li a Nor b Co c Al d G e O 2 (0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0≤e≤0.1);Li a NiG b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a CoG b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-b G b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 2 G b O 4 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-g G g MONTH 4 (0.90≤a≤1.8,0≤g≤0.5);QO 2 ;QS 2 ;LiQS 2 ;V 2 O 5 ;LiV 2 O 5 ;LiZO 2 ;LiLevel 4 ;The (3-f) J 2 (MONTH 4 ) 3 (0≤f≤2);Li (3-f) Fe 2 (MONTH 4 ) 3 (0≤f≤2);Li a FePO4 (0.90≤a≤1.8).
[0063] In the above chemical formula, A is selected from Ni, Co, Mn and combinations thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements and combinations thereof; D is selected from O, F, S, P and combinations thereof; E is selected from Co, Mn and combinations thereof; T is selected from F, S, P and combinations thereof; G is selected from Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V and combinations thereof; Q is selected from Ti, Mo, Mn and combinations thereof; Z is selected from Cr, V, Fe, Sc, Y and combinations thereof; and J is selected from V, Cr, Mn, Co, Ni, Cu and combinations thereof.
[0064] The compound may have a coating layer located on the surface, or may be mixed with another compound having a coating layer. The coating layer may include at least one coating element compound selected from the group consisting of an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compound used for the coating layer may be amorphous or crystalline. The coating element included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating layer may be provided by using these elements in the compound in a manner that does not adversely affect the properties of the positive active material. For example, the method may include any coating method (such as spraying, dipping, etc.), but since it is well known in the art, it is not described in more detail.
[0065] In the positive electrode, the amount of the positive active material may be about 90 wt % to about 98 wt % based on the total weight of the positive active material layer.
[0066] In an embodiment, the positive electrode active material layer may further include a binder and a positive electrode conductive material. Here, the binder and the positive electrode conductive material may be included in an amount of about 1 wt % to about 5 wt % based on the total weight of the positive electrode active material layer.
[0067] The binder improves the bonding properties between the positive electrode active material particles and between the positive electrode active material particles and the positive electrode current collector. Examples of the binder may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0068] The positive electrode conductive material is included to provide electrode conductivity. Any electrically conductive material can be used as the positive electrode conductive material unless it causes a chemical change. Examples of the positive electrode conductive material may include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials of metal powder or metal fiber, including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0069] The positive electrode current collector may use Al, but is not limited thereto.
[0070] The electrolyte includes a non-aqueous organic solvent and a lithium salt.
[0071] The nonaqueous organic solvent serves as a medium for transporting ions participating in the electrochemical reaction of the battery.
[0072] The non-aqueous organic solvent may include a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent, or an aprotic solvent.
[0073] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, decanoic acid lactone, caprolactone, etc. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. Ketone solvents include cyclohexanone, etc. Alcohol solvents include ethanol, isopropanol, etc. Examples of aprotic solvents include: nitriles, such as R-CN (wherein R is a C2 to C20 straight chain, branched or cyclic hydrocarbon, or may include a double bond, an aromatic ring or an ether bond); amides, such as dimethylformamide; dioxolanes, such as 1,3-dioxolane; cyclopentane sulfone, etc.
[0074] The non-aqueous organic solvent may be used alone or in a mixture. When the non-aqueous organic solvent is used in a mixture, the mixing ratio may be controlled according to desired battery performance.
[0075] The carbonate solvent may include a mixture of cyclic carbonate and linear carbonate. The cyclic carbonate and linear carbonate are mixed together in a volume ratio of about 1:1 to about 1:9. When the mixture is used as an electrolyte, it can have enhanced performance.
[0076] The organic solvent may further include an aromatic hydrocarbon solvent and a carbonate solvent. The carbonate solvent and the aromatic hydrocarbon solvent may be mixed together in a volume ratio of about 1:1 to about 30:1.
[0077] The aromatic hydrocarbon solvent may be an aromatic hydrocarbon compound represented by Chemical Formula 1.
[0078] [Chemical formula 1]
[0079]
[0080] In Chemical Formula 1, R 1 To R 6 are the same or different and are selected from hydrogen, halogen, C1 to C10 alkyl, halogenated alkyl and combinations thereof.
[0081] Specific examples of aromatic hydrocarbon solvents can be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, , 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0082] The electrolyte may further include vinylene carbonate, an ethylene carbonate-based compound represented by Chemical Formula 2, or propane sultone as an additive for improving cycle life.
[0083] [Chemical formula 2]
[0084]
[0085] In chemical formula 2, R 7 and R 8 are the same or different and may each independently be hydrogen, halogen, cyano (CN), nitro (NO 2 ) or fluorinated C1 to C5 alkyl, provided that R 7 and R 8 At least one of them is a halogen, a cyano (CN), a nitro (NO 2 ) or a fluorinated C1 to C5 alkyl group, and R 7 and R 8 Not at the same time hydrogen.
[0086] Examples of ethylene carbonate compounds may include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. The amount of the additive for improving cycle life characteristics may be used within an appropriate range.
[0087] The lithium salt dissolved in the non-aqueous organic solvent supplies lithium ions to the battery, enables the basic operation of the rechargeable lithium battery, and improves the transport of lithium ions between the positive electrode and the negative electrode. Examples of the lithium salt include those selected from LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiN(SO 2 C 2 F 5 ) 2 、Li(CF 3 SO 2 ) 2 N、LiN(SO 3 C 2 F 5 ) 2 、Li(FSO 2 ) 2 N(Lithium bis(fluorosulfonyl)imide: LiFSI), LiC 4 F 9 SO 3 、LiClO 4 、LiAlO 2 、LiAlCl 4 、LiPO 2 F 2 、LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 )(wherein x and y are natural numbers, for example, integers from 1 to 20), lithium difluoro(bisoxalato)phosphate, LiCl, LiI, LiB(C 2 O 4 ) 2 At least one supporting salt of lithium bis(oxalate)borate: LiBOB) and lithium difluoro(oxalate)borate (LiDFOB). The concentration of the lithium salt may range from about 0.1 M to about 2.0 M. When the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to optimal electrolyte conductivity and viscosity.
[0088] According to the type of rechargeable lithium battery, the separator may be provided between the positive electrode and the negative electrode. The separator may use polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer thereof having two or more layers, and may be a mixed multilayer (such as a polyethylene / polypropylene double-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, a polypropylene / polyethylene / polypropylene three-layer separator, etc.).
[0089] Figure 2 is an exploded perspective view of a rechargeable lithium battery according to an embodiment. The rechargeable lithium battery according to an embodiment is illustrated as a prismatic battery, but is not limited thereto and may include batteries of various shapes such as a cylindrical battery, a pouch-type battery, and the like.
[0090] Reference Figure 2 , the rechargeable lithium battery 100 according to the embodiment may include an electrode assembly 40 manufactured by winding a separator 30 disposed between a positive electrode 10 and a negative electrode 20, and a case 50 accommodating the electrode assembly 40. An electrolyte (not shown) may be impregnated in the positive electrode 10, the negative electrode 20, and the separator 30.
[0091] Hereinafter, comparative examples and examples of the present invention are described. However, these examples should not be interpreted as limiting the scope of the invention in any sense.
[0092] Example 1
[0093] 97.1wt% of graphite and Si-carbon composite (86wt% of graphite, 14wt% of Si-carbon composite) as negative electrode active materials, 0.3wt% of carbon nanotubes (average length: 30μm to 50μm, width: 10nm to 20nm) as linear conductive materials, 0.9wt% of carboxymethyl cellulose and 1.7wt% of styrene-butadiene rubber were mixed in water to prepare a first negative electrode active material layer slurry. Here, the Si-carbon composite uses a Si-carbon composite including a core containing artificial graphite and silicon particles and a soft carbon coating layer coated on the core. The soft carbon coating layer has a thickness of 20nm, and the silicon particles have an average particle size D50 of 100nm.
[0094] 96.4 wt % of graphite as a negative electrode active material, 1.0 wt % of superconductive acetylene black (average particle size: 30 nm to 40 nm) as a dot conductive material, 0.9 wt % of carboxymethyl cellulose and 1.7 wt % of styrene-butadiene rubber were mixed in water to prepare a second negative electrode active material layer slurry.
[0095] The first negative electrode active material layer slurry and the second negative electrode active material layer slurry are simultaneously coated on the copper foil current collector and dried. The coating process is performed to directly coat the first negative electrode active material layer slurry on the copper foil current collector.
[0096] Thereafter, the obtained product was pressed to prepare a negative electrode in which a first negative electrode active material layer having a thickness of 54 μm and a second negative electrode active material layer having a thickness of 44 μm were formed.
[0097] Comparative Example 1
[0098] 96.4wt% of graphite and Si-carbon composite (86wt% of graphite, 14wt% of Si-carbon composite) as negative electrode active materials, 1.0wt% of superconductive acetylene black (average particle size: 30nm to 40nm) as dot conductive material, 0.9wt% of carboxymethyl cellulose and 1.7wt% of styrene-butadiene rubber were mixed in water to prepare the first negative electrode active material layer slurry. Here, the Si-carbon composite uses a Si-carbon composite including a core containing artificial graphite and silicon particles and a soft carbon coating layer coated on the core. The soft carbon coating layer has a thickness of 20nm, and the silicon particles have an average particle size D50 of 100nm.
[0099] According to the same composition as the first negative electrode active material layer slurry, 96.4wt% of graphite as a negative electrode active material, 1.0wt% of superconductive acetylene black (average particle size: 30nm to 40nm) as a point conductive material, 0.9wt% of carboxymethyl cellulose and 1.7wt% of styrene-butadiene rubber were mixed in water to prepare a second negative electrode active material layer slurry.
[0100] The first negative electrode active material layer slurry and the second negative electrode active material layer slurry are simultaneously coated on the copper foil current collector and dried. The coating process is performed to directly coat the first negative electrode active material layer slurry on the copper foil current collector.
[0101] Thereafter, the obtained product was pressed to prepare a negative electrode in which a first negative electrode active material layer having a thickness of 49 μm and a second negative electrode active material layer having a thickness of 49 μm were formed.
[0102] Comparative Example 2
[0103] 97.1wt% of graphite and Si-carbon composite (86wt% of graphite, 14wt% of Si-carbon composite) as negative electrode active materials, 0.3wt% of carbon nanotubes (average length: 30μm to 50μm, width: 10nm to 20nm) as linear conductive materials, 0.9wt% of carboxymethyl cellulose and 1.7wt% of styrene-butadiene rubber were mixed in water to prepare a first negative electrode active material layer slurry. Here, the Si-carbon composite uses a Si-carbon composite including a core containing artificial graphite and silicon particles and a soft carbon coating layer coated on the core. The soft carbon coating layer has a thickness of 20nm, and the silicon particles have an average particle size D50 of 100nm.
[0104] 97.1 wt % of graphite and Si-carbon composite (86 wt % of graphite, 14 wt % of Si-carbon composite) as negative electrode active materials, 0.3 wt % of carbon nanotubes (average length: 30 μm to 40 μm, width: 10 nm to 20 nm) as linear conductive materials, 0.9 wt % of carboxymethyl cellulose and 1.7 wt % of styrene-butadiene rubber were mixed in water to prepare a second negative electrode active material layer slurry.
[0105] The first negative electrode active material layer slurry and the second negative electrode active material layer slurry are simultaneously coated on the copper foil current collector and dried. The coating process is performed to directly coat the first negative electrode active material layer slurry on the copper foil current collector.
[0106] Thereafter, the obtained product was pressed to prepare a negative electrode in which a first negative electrode active material layer having a thickness of 49 μm and a second negative electrode active material layer having a thickness of 49 μm were formed.
[0107] Comparison Example 3
[0108] 96.4wt% of graphite and Si-carbon composite (86wt% of graphite, 14wt% of Si-carbon composite) as negative electrode active materials, 1.0wt% of superconductive acetylene black (average particle size: 30nm to 40nm) as dot conductive material, 0.9wt% of carboxymethyl cellulose and 1.7wt% of styrene-butadiene rubber were mixed in water to prepare the first negative electrode active material layer slurry. Here, the Si-carbon composite uses a Si-carbon composite including a core containing artificial graphite and silicon particles and a soft carbon coating layer coated on the core. The soft carbon coating layer has a thickness of 20nm, and the silicon particles have an average particle size D50 of 100nm.
[0109] 97.1 wt % of graphite and Si-carbon composite (86 wt % of graphite, 14 wt % of Si-carbon composite) as negative electrode active materials, 0.3 wt % of carbon nanotubes (average length: 30 μm to 50 μm, width: 10 nm to 20 nm) as linear conductive materials, 0.9 wt % of carboxymethyl cellulose and 1.7 wt % of styrene-butadiene rubber were mixed in water to prepare a second negative electrode active material layer slurry.
[0110] The first negative electrode active material layer slurry and the second negative electrode active material layer slurry are simultaneously coated on the copper foil current collector and dried. The coating process is performed to directly coat the first negative electrode active material layer slurry on the copper foil current collector.
[0111] Thereafter, the obtained product was pressed to prepare a negative electrode in which a first negative electrode active material layer having a thickness of 49 μm and a second negative electrode active material layer having a thickness of 49 μm were formed.
[0112] Experimental Example 1) SEM measurement
[0113] Regarding the negative electrode according to Example 1, a SEM photograph of one side of the negative electrode active material layer was measured. The SEM photograph of the first negative electrode active material layer is shown in FIG. Figure 3A and Figure 3B and the SEM photograph of the second negative electrode active material layer is shown in Figure 4 middle.
[0114] Figure 3A is the area of artificial graphite, and Figure 3B is the area of Si-carbon composite, so it can be clearly seen that both figures present linear conductive materials. In addition, from Figure 4 It can be clearly shown that dot-shaped conductive materials exist in the second negative electrode active material layer.
[0115] In addition, the SEM photograph of the negative electrode of Comparative Example 1 shows Figure 5A and Figure 5B In. Figure 5A and Figure 5B As shown in , dot-shaped conductive materials are distributed in the Si-carbon composite and artificial graphite in Comparative Example 1.
[0116] Experimental Example 2) Rate Performance Measurement
[0117] *Half-cell manufacturing
[0118] Using the negative electrodes of Example 1 and Comparative Example 1, a lithium metal counter electrode, and an electrolyte, a half-cell was fabricated.
[0119] As the electrolyte, 1 M LiPF 6 A mixed solvent of ethylene carbonate and diethyl carbonate (50:50 volume ratio).
[0120] The half-cell was operated as follows: charging and discharging to 4.25V at 0.2C and discharging to 2.8V at 0.2C for four times, charging and discharging to 4.25V at 0.2C and discharging to 2.8V at 0.5C for three times, charging and discharging to 4.25V at 0.2C and discharging to 2.8V at 1.0C for three times, charging and discharging to 4.25V at 0.2C and discharging to 2.8V at 1.5C for three times, and charging and discharging to 4.25V at 0.2C and discharging to 2.8V at 2.0C for two times. In addition, after charging at each C rate, it was charged to 0.05C at constant voltage (CV). The discharge capacity at each C rate was measured, and the results are shown in Figure 6 middle.
[0121] The half-cell was operated as follows: charging and discharging at 0.2C to 4.25V and discharging at 0.2C for four times, charging and discharging at 0.5C to 4.25V and discharging at 0.2C for three times, charging and discharging at 1C to 4.25V and discharging at 0.2C for three times, charging and discharging at 1.5C to 4.25V and discharging at 0.2C for three times, and charging and discharging at 2C to 4.25V and discharging at 0.2C for two times. In addition, after charging at each C rate, it was charged to 0.05C at constant voltage (CV). The charge capacity at each C rate was measured, and the results are shown in Figure 7 middle.
[0122] like Figure 6 and Figure 7 As shown in , the rate performance of the half-cell including the negative electrode according to Example 1 is higher than that of Comparative Example 1, and in particular, exhibits excellent high-rate characteristics.
[0123] When Figure 7 When charging and discharging are performed under the conditions of , the ratio of the last charge capacity to the first charge capacity at each C rate is determined. The results of the retention rate are shown in Figure 8 In. Figure 8 As shown in , at a high rate of 1.0 C or higher, the charge capacity retention rate of the half-cell including the negative electrode of Example 1 is excellent compared to Comparative Example 1.
[0124] While the present invention has been described in conjunction with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.
Claims
1. A negative electrode for a rechargeable lithium battery, the negative electrode include: current collector; a first negative electrode active material layer, disposed on one side of the current collector and comprising a first negative electrode active material and a linear conductive material, but excluding a dot-shaped conductive material; as well as A second negative electrode active material layer is provided on one side of the first negative electrode active material layer and includes a second negative electrode active material and a dot-shaped conductive material, in: The linear conductive material is carbon nanotubes, carbon fibers or a combination thereof. The dot-shaped conductive material is carbon black, crystalline carbon, or a combination thereof, and The first negative electrode active material or the second negative electrode active material is Si-carbon composite, graphite or a combination thereof.
2. The negative electrode for a rechargeable lithium battery according to claim 1, in: The thickness of the second negative electrode active material layer is 1% to 75% of the total thickness of the first negative electrode active material layer and the second negative electrode active material layer.
3. The negative electrode for a rechargeable lithium battery according to claim 1, in: The linear conductive material is carbon nanotube, carbon nanofiber or a combination thereof.
4. The negative electrode for a rechargeable lithium battery according to claim 1, in: The dot-shaped conductive material is superconductive acetylene black, Ketjen black, crystalline carbon or a combination thereof.
5. The negative electrode for a rechargeable lithium battery according to claim 1, in: The dot-shaped conductive material is Ketjen black, acetylene black, crystalline carbon or a combination thereof.
6. A rechargeable lithium battery, the rechargeable lithium battery include: The negative electrode according to any one of claims 1 to 5; Positive electrode; as well as Electrolytes.
Citation Information
Patent Citations
Silicon-carbon negative electrode and preparation method thereof, and lithium ion battery
CN106560943A
Lithium ion battery negative electrode plate and preparation method thereof
CN107528044A
High-rate lithium battery negative plate and lithium battery
CN111799451A
Cited By
Anode for secondary battery and lithium secondary battery including anode
US20240274800A1