Porous silicon composite material filled with zinc oxide nanowires and preparation method thereof
By growing zinc oxide nanowires in porous silicon pores, the problems of poor response of zinc oxide materials and gaps in nanowire growth technology are solved, the photocatalytic performance and application prospects are improved, and the high efficiency of zinc oxide nanowire-filled porous silicon composite materials is achieved. preparation.
Patent Information
- Application Number
- CN202210036107.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-01-13
AI Technical Summary
In the existing technology, defects such as poor response of zinc oxide materials in the visible light band and rapid recombination of photogenerated carriers limit the improvement of its photocatalytic efficiency, and the growth of zinc oxide nanowires cannot be achieved in porous silicon pores.
Using porous silicon as the substrate, the porous silicon microstructure is prepared by electrochemical anodization. The zinc oxide seed layer is prepared by combining vacuum filtration and sol-gel method. Zinc oxide nanowires are grown using the oil bath method to form zinc oxide nanowire filling. porous silicon composite materials.
The uniform growth of zinc oxide nanowires in porous silicon pores is achieved, the optical performance and light absorption capacity are improved, and the application prospects of zinc oxide in the optical field are broadened. The operation is simple and the cost is low.
Smart Images

Figure CN114522676B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite material preparation, and particularly relates to a porous silicon composite material filled with zinc oxide nanowires and a preparation method thereof. Background Art
[0002] In recent years, with the rapid advancement of industrialization, environmental pollution has become an increasingly serious problem. In many industrial activities, such as textile, pulp, dye and bleaching industries, the lack of appropriate post-treatment processes often causes various refractory organic pollutants to pollute natural water bodies, thereby destroying the sustainability of the environment and causing highly toxic damage to humans and ecosystems. Traditional environmental purification methods, such as adsorption, filtration separation, oxidation, etc., not only have the disadvantages of high cost, low efficiency and secondary pollution, but are also ineffective in degrading many pollutants. Photocatalytic environmental purification technology is one of the advanced oxidation technologies. Its essence is an advanced technology that uses photocatalysts to oxidize and decompose organic pollutants, bacteria or viruses into non-toxic organic products such as carbon dioxide and water under light induction. Zinc oxide is a semiconductor material with a band gap of 3.2eV. Under ultraviolet light excitation, the generated electrons and holes react with oxygen molecules and water molecules to generate superoxide radicals and hydroxyl radicals, respectively, so it has strong catalytic oxidation. At the same time, due to its good biocompatibility and low cost, it is used as a commonly used photocatalytic material. With the development of nano-engineering technology, compared with traditional zinc oxide, nano zinc oxide has a smaller particle size, larger specific surface area, and higher surface energy, making it easier to combine with organic matter, so it has greater potential for application in the field of photocatalysis.
[0003] Photocatalytic efficiency is one of the key indicators for evaluating the performance of photocatalysts. However, zinc oxide materials have defects such as poor response in the visible light band and rapid recombination of photogenerated carriers, which inhibit the further improvement of their photocatalytic efficiency. Semiconductor-based heterostructures are considered to be an effective prototype to overcome these problems. Semiconductor-based heterostructures composed of two or more semiconductor materials have various advantages, including a wide light absorption spectrum range, utilizing the strength of a single material, optimizing photogenerated charge separation or recombination, enhancing new photophysical effects, improving photocatalytic activity, and good stability to photocorrosion. Therefore, zinc oxide can be coupled with another semiconductor with an appropriate band gap to overcome the recombination problem of photogenerated charge carriers. At present, the light absorption band of zinc oxide has been further broadened by doping with transition metal or non-metal ions, depositing precious metals or nanocarbon materials, and coupling with other semiconductors. Crystalline silicon material is a semiconductor material that responds to visible light and can obtain a high absorption coefficient in the 300nm to 1100nm band. Therefore, by combining zinc oxide with crystalline silicon material, it will help zinc oxide materials to obtain photocatalytic oxidation effects in a wide spectral region.
[0004] Porous silicon is a porous skeleton structure formed by nano-silicon atom clusters. It can be divided into microporous, mesoporous and macroporous porous silicon according to the pore size. Macroporous porous silicon has micron-level pores and a large specific surface area, which can provide a larger space for the attachment and growth of nano zinc oxide. However, most of the composite structures of nano zinc oxide and silicon materials currently use silicon wafers as the substrate. Among the few zinc oxide nanostructures based on porous silicon, the zinc oxide nanostructures are all grown on the surface of porous silicon, and there are no reports on ZnO nanorods grown in the pores of porous silicon. Summary of the invention
[0005] In view of the above technical problems, the present invention provides a porous silicon composite material filled with zinc oxide nanowires and a preparation method thereof, wherein zinc oxide nanowires are prepared in the pores of porous silicon to achieve rapid preparation of the porous silicon composite material filled with zinc oxide nanowires. The method has simple steps and can efficiently prepare the porous silicon composite material filled with zinc oxide nanowires. The method is simple to operate, low in cost, and greatly improves the optical properties of zinc oxide.
[0006] The present invention uses porous silicon as a substrate and combines it with zinc oxide material. The structure can significantly improve the light absorption capacity of porous silicon. The present invention uses an electrochemical positive etching method to prepare a porous silicon microstructure on a single crystal silicon substrate; prepares a zinc ion sol for preparing a zinc oxide seed layer; uses a vacuum filtration method and a sol-gel method to prepare a zinc oxide seed layer on porous silicon; and uses an oil bath method to grow zinc oxide nanowires on the porous silicon after the seed layer is prepared. The method is simple to operate, highly safe, and low in cost. It greatly improves the optical properties of zinc oxide and broadens its application prospects in the optical field. The present invention fills the technical gap in preparing zinc oxide nanowires in porous silicon pores.
[0007] The technical solution of the present invention is: a method for preparing a porous silicon composite material filled with zinc oxide nanowires, comprising the following steps:
[0008] Solution preparation: preparing an electrochemical etching solution, wherein the electrochemical etching solution comprises hydrofluoric acid HF, dimethylformamide DMF, anhydrous ethanol and deionized water, and the hydrofluoric acid HF, dimethylformamide DMF, anhydrous ethanol and deionized water are mixed in a certain proportion; preparing a seed layer solution, wherein the seed layer solution comprises zinc acetate dihydrate, ethanol and diethanolamine; preparing a zinc oxide nanowire growth solution, wherein the growth solution comprises zinc nitrate hexahydrate and hexamethylenetetramine;
[0009] Electrochemical etching: placing a square silicon wafer into a container containing the electrochemical etching solution, applying a constant current for electrochemical etching, and obtaining porous silicon;
[0010] Preparation of seed layer: placing the porous silicon into a seed layer solution, using vacuum filtration combined with a sol-gel method, drying, and annealing to prepare a zinc oxide seed layer on the pore walls of the porous silicon to obtain a porous silicon-zinc oxide seed layer;
[0011] Preparation of zinc oxide nanowires: vertically placing the porous silicon-zinc oxide seed layer into the zinc oxide nanowire growth solution, and performing an oil bath reaction to obtain a porous silicon composite material filled with zinc oxide nanowires.
[0012] In the above scheme, the hydrofluoric acid HF, dimethylformamide DMF, anhydrous ethanol and deionized water are mixed in a volume ratio of 3:5:3:3.
[0013] In the above scheme, the molar concentration of zinc acetate in the zinc acetate dihydrate, ethanol and diethanolamine solution is 0.5 mol / L, ethanol is used as the solvent, and the molar ratio of diethanolamine to zinc ions in the solution is fixed at 1.
[0014] In the above scheme, the molar concentrations of the zinc nitrate hexahydrate and hexamethylenetetramine are 0.02 mol / L-0.1 mol / L.
[0015] In the above scheme, the corrosion current of the electrochemical corrosion is 40-60mA / cm 2 , the corrosion time is 5-8min.
[0016] In the above scheme, the low speed of the sol-gel method of the sizing machine in the preparation of the seed layer is 300-500 r / min, and the high speed is 3000-4000 r / min.
[0017] In the above scheme, the drying temperature in the preparation of the seed layer is 150° C. and the drying time is 20 min. The annealing temperature is 500° C. and the annealing time is 1 h.
[0018] In the above scheme, the oil bath reaction temperature in the preparation of zinc oxide nanowires is 85-100° C. and the reaction time is 3-6 hours.
[0019] Furthermore, in the preparation of the zinc oxide nanowires, the oil bath reaction temperature is 95° C. and the reaction time is 4 h.
[0020] A porous silicon composite material filled with zinc oxide nanowires is prepared by utilizing the method for preparing the porous silicon composite material filled with zinc oxide nanowires.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention realizes the preparation of zinc oxide nanowires in porous silicon pore walls for the first time. At the same time, performance tests show that the structure grows uniformly and has good crystallinity. Optical performance tests show that the structure has higher light absorption performance. The method has simple steps, convenient operation, low preparation cost, and can quickly and efficiently prepare porous silicon composite materials filled with zinc oxide nanowires. It provides technical support for the rapid preparation of zinc oxide nanostructures on porous silicon substrates and has great application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of a porous silicon zinc oxide seed layer and a macroporous silicon-zinc oxide nanowire composite structure prepared in one embodiment of the present invention.
[0024] Figure 2 This is an XRD characterization diagram of the macroporous silicon-zinc oxide nanowire composite structure prepared according to one embodiment of the present invention.
[0025] Figure 3 It is a reflection spectrum diagram of the porous silicon zinc oxide seed layer and macroporous silicon-zinc oxide nanowire composite structure prepared according to one embodiment of the present invention.
[0026] Figure 4 It is an absorption spectrum diagram of the porous silicon zinc oxide seed layer and macroporous silicon-zinc oxide nanowire composite structure prepared according to one embodiment of the present invention. DETAILED DESCRIPTION
[0027] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0028] The method for preparing the porous silicon composite material filled with zinc oxide nanowires of the present invention comprises the following steps:
[0029] Material selection: Select p-type single crystal silicon with a crystal orientation of
[100] , cut the sample and clean it;
[0030] Solution preparation: preparing an electrochemical etching solution, wherein the electrochemical etching solution comprises hydrofluoric acid HF, dimethylformamide DMF, anhydrous ethanol and deionized water, and the hydrofluoric acid HF, dimethylformamide DMF, anhydrous ethanol and deionized water are mixed in a certain proportion; preparing a seed layer solution, wherein the seed layer solution comprises zinc acetate dihydrate, ethanol and diethanolamine; preparing a zinc oxide nanowire growth solution, wherein the growth solution comprises zinc nitrate hexahydrate and hexamethylenetetramine;
[0031] Electrochemical etching: placing a square silicon wafer into a container containing the electrochemical etching solution, applying a constant current for electrochemical etching, and obtaining porous silicon;
[0032] Preparation of seed layer: placing the porous silicon into a seed layer solution, selecting zinc acetate dihydrate as the zinc source for the seed layer, using vacuum filtration combined with a sol-gel method, drying, and annealing to prepare a zinc oxide seed layer on the porous silicon pore wall, thereby obtaining a porous silicon-zinc oxide seed layer;
[0033] Preparation of zinc oxide nanowires: vertically placing the porous silicon-zinc oxide seed layer into the zinc oxide nanowire growth solution, and performing an oil bath reaction to obtain a porous silicon composite material filled with zinc oxide nanowires.
[0034] Preferably, the hydrofluoric acid HF, dimethylformamide DMF, anhydrous ethanol and deionized water are mixed in a volume ratio of 3:5:3:3.
[0035] Preferably, the molar concentration of zinc acetate in the zinc acetate dihydrate, ethanol and diethanolamine solution is 0.5 mol / L, ethanol is used as the solvent, and the molar ratio of diethanolamine to zinc ions in the solution is fixed at 1.
[0036] Preferably, the molar concentration of the zinc nitrate hexahydrate and hexamethylenetetramine is 0.02 mol / L-0.1 mol / L.
[0037] Preferably, the corrosion current of the electrochemical corrosion is 40-60 mA / cm 2 , the corrosion time is 5-8min.
[0038] Preferably, in the preparation of the seed layer, the low speed of the sol-gel method of the sizing machine is 300-500 r / min, and the high speed is 3000-4000 r / min.
[0039] Preferably, the drying temperature in the preparation of the seed layer is 150° C. and the drying time is 20 min. The annealing temperature is 500° C. and the annealing time is 1 h.
[0040] Preferably, in the preparation of the zinc oxide nanowires, the oil bath reaction temperature is 85-100° C. and the reaction time is 3-6 h.
[0041] Preferably, in the preparation of the zinc oxide nanowires, the oil bath reaction temperature is 95° C. and the reaction time is 4 h. Specific embodiment:
[0043] A method for preparing a porous silicon composite material filled with zinc oxide nanowires, taking macroporous silicon as an example in this embodiment, comprises the following steps:
[0044] Material selection: Select P-type silicon wafer, which is
[100] crystalline P-type single crystal silicon with a resistivity of 10-20Ω / cm 2 , with a thickness of 525μm, and the silicon wafer is cut into 1.6m×1.6m square silicon wafers using a diamond tool.
[0045] Cleaning samples: Place the cut square silicon wafers in beakers containing deionized water, alcohol, and acetone in turn and perform ultrasonic cleaning for 10 minutes to remove oil stains and impurities on the square silicon wafers.
[0046] Solution preparation: Preparation of electrochemical etching solution: Use a pipette to take out 6 ml of HF, 10 ml of DMF, 6 ml of anhydrous ethanol and 6 ml of deionized water respectively on a workbench with a fume hood and put them into a plastic measuring cylinder to prepare the electrochemical etching solution; Prepare the seed layer solution: Use zinc acetate dihydrate (99.5% purity, Zn(CH3COO)2·2H2O) as the main provider of zinc element, use ethanol as solvent and diethanolamine (HN(CH2CH2OH)2, DEA) as sol stabilizer. In the preparation of sol, first weigh 0.1 mol of zinc acetate dihydrate and dissolve it in a beaker containing 0.2 L of anhydrous ethanol to form a 0.5 M zinc acetate-ethanol solution. The prepared solution was vigorously stirred on a magnetic stirrer for half an hour. After the stirring was completed, the diethanolamine solution was slowly added to keep the molar ratio of diethanolamine in the solution to zinc ions in the solution fixed at 1; Preparation of zinc oxide nanowire growth solution: 0.008 mol of hexamethylenetetramine and zinc nitrate hexahydrate were weighed separately, poured into a beaker containing 100 ml of deionized water, and the mixed solution was placed in an ultrasonic cleaner for a period of time to fully mix it, and the concentration of the mixed solution was configured to be 0.08 mol / L.
[0047] Electrochemical corrosion: Set the corrosion parameters and place the cleaned square silicon wafer into an anodizing device filled with electrolyte for electrochemical anodic corrosion. The corrosion current is 40mA / cm 2 , corrosion time 5min.
[0048] Cleaning of corroded samples: Take out the prepared samples with clamps and carefully rinse the corroded area with deionized water for 3 minutes. Blow dry the silicon wafer with nitrogen and seal it for subsequent testing.
[0049] Preparation of zinc oxide seed layer: Soak the prepared porous silicon sample in the sol liquid, and filter it in a vacuum device to allow the liquid to fully enter the porous silicon pores until no bubbles are generated. After the solution has completed penetration, use a glue-spinning table to slick the sample at a speed of 400r / min for 15s to evenly disperse the solution on the sample surface, and then increase the speed to 3000r / min for 40s to thin the sol attached to the pores. Then put the glue-coated sample into a horizontal temperature drying oven at 150°C and dry it for 20 minutes. After repeating this process twice, put the sample into a tubular furnace and anneal it at 500°C for 1h to complete the preparation of the zinc oxide seed layer.
[0050] Preparation of macroporous silicon-zinc oxide nanowires: The porous silicon sample with the prepared seed layer was vertically immersed in the mixed solution and placed in a 95°C oil bath for reaction for 4 hours. After the reaction, it was taken out, the surface was rinsed with deionized water, and then placed in a drying oven at 60°C for drying for 12 hours.
[0051] A porous silicon composite material filled with zinc oxide nanowires is prepared by utilizing the method for preparing the porous silicon composite material filled with zinc oxide nanowires.
[0052] Result analysis:
[0053] The obtained porous silicon composite material filled with zinc oxide nanowires was subjected to morphology testing. Figure 1 (a) shows the morphology of porous silicon for preparing zinc oxide seed layer. It can be seen that zinc oxide nanoparticles are evenly covered on the inner wall and the bottom of the pores of the porous silicon. Figure 1 (b) is a cross-sectional view, and (c) is a surface view, showing the morphology of zinc oxide nanowires prepared in porous silicon pores. It can be seen that the zinc oxide nanowires grow vertically on the zinc oxide seed layer. The zinc oxide nanowires are uniform in size and evenly distributed. The length of the zinc oxide nanowires is about 500nm and the diameter is about 100nm.
[0054] Figure 2 This is the X-ray diffraction pattern of macroporous silicon-zinc oxide nanowires. The peak positions of the spectrum correspond to the zinc oxide standard card (JCPDS.No.89-0510), indicating that zinc oxide nanowires are successfully grown in the porous silicon pores and are in good crystallization condition. Figure 3 This is the reflectivity result diagram of porous silicon zinc oxide film and macroporous silicon-zinc oxide nanowire. It can be seen that the reflectivity of macroporous silicon-zinc oxide nanowire is lower and the absorption of sunlight is significantly improved. Figure 4 Figure 2 is the absorption spectrum of porous silicon zinc oxide film and macroporous silicon-zinc oxide nanowire. It can be seen that macroporous silicon-zinc oxide nanowire has higher light absorption effect in the ultraviolet light band.
[0055] It can be seen from the specific embodiments that the method of the present invention can realize the preparation of macroporous silicon composite materials filled with zinc oxide nanowires, and has important application prospects. In this embodiment, an electrochemical etching solution, a zinc oxide seed layer solution and a zinc oxide nanowire growth solution are configured to electrochemically anodically corrode the silicon wafer, prepare a zinc oxide seed layer on the porous silicon pore wall, and prepare zinc oxide nanowires on the porous silicon pore wall. The prepared macroporous silicon composite material filled with zinc oxide nanowires has good optical properties. The method is simple to operate, the required equipment cost is low and the time is short, and it is suitable for large-scale and rapid preparation of macroporous silicon-zinc oxide nanowire composite structures.
[0056] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a porous silicon composite material filled with zinc oxide nanowires, characterized in that: The following steps are involved: Solution preparation: preparing an electrochemical etching solution, wherein the electrochemical etching solution comprises hydrofluoric acid (HF), dimethylformamide (DMF), anhydrous ethanol, and deionized water, wherein the hydrofluoric acid (HF), dimethylformamide (DMF), anhydrous ethanol, and deionized water are mixed in a certain proportion; preparing a seed layer solution, wherein the seed layer solution comprises zinc acetate dihydrate, ethanol, and diethanolamine; and preparing a zinc oxide nanowire growth solution, wherein the growth solution comprises zinc nitrate hexahydrate and hexamethylenetetramine; Electrochemical etching: placing a square silicon wafer into a container containing the electrochemical etching solution, applying a constant current to perform electrochemical etching to obtain porous silicon; Preparation of seed layer: placing the porous silicon into the seed layer solution, using vacuum filtration combined with sol-gel method, drying, and annealing to form a zinc oxide seed layer on the pore wall of the porous silicon to obtain a porous silicon-zinc oxide seed layer; Preparation of zinc oxide nanowires: vertically placing the porous silicon-zinc oxide seed layer into the zinc oxide nanowire growth solution, and reacting in an oil bath to obtain a porous silicon composite material filled with zinc oxide nanowires; The hydrofluoric acid HF, dimethylformamide DMF, anhydrous ethanol and deionized water are mixed in a volume ratio of 3:5:3:3; The molar concentration of zinc acetate in the zinc acetate dihydrate, ethanol and diethanolamine solution is 0.5 mol / L, ethanol is used as the solvent, and the molar ratio of diethanolamine to zinc ions in the solution is fixed at 1:1; The molar concentration of the zinc nitrate hexahydrate and the hexamethylenetetramine is 0.02 mol / L-0.1 mol / L; The corrosion current of the electrochemical corrosion is 40-60 mA / cm 2 , corrosion time is 5-8min; In the preparation of the zinc oxide nanowires, the oil bath reaction temperature is 85-100° C., and the reaction time is 3-6 hours.
2. The method for preparing a porous silicon composite material filled with zinc oxide nanowires according to claim 1, characterized in that: In the preparation of the seed layer, the low speed of the sol-gel method spinner is 300-500 r / min, and the high speed is 3000-4000 r / min.
3. The method for preparing a porous silicon composite material filled with zinc oxide nanowires according to claim 1, characterized in that: In the preparation of the seed layer, the drying temperature is 150° C., the drying time is 20 min, the annealing temperature is 500° C., and the annealing time is 1 h.
4. The method for preparing a porous silicon composite material filled with zinc oxide nanowires according to claim 1, wherein: In the preparation of the zinc oxide nanowires, the oil bath reaction temperature is 95° C. and the reaction time is 4 h.
5. A porous silicon composite material filled with zinc oxide nanowires, characterized in that: The porous silicon composite material filled with zinc oxide nanowires is prepared by the method for preparing a porous silicon composite material filled with zinc oxide nanowires according to any one of claims 1 to 4.