Adhesive film

By introducing a photothermal conversion layer and a multifunctional epoxy resin into the adhesive film, efficient bonding and separation of the flexible substrate and the hard support is achieved, and the process complexity and damage problems in the prior art are solved, reducing costs and Maintain stability under high temperature and high vacuum conditions.

CN114555355BActive Publication Date: 2024-11-013M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080072799.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-18
Filing Date
2020-10-13
Publication Date
2024-11-01
Estimated Expiration
2040-10-13

Smart Images

  • Figure CN114555355B_ABST
    Figure CN114555355B_ABST
Patent Text Reader

Abstract

The present invention relates to an adhesive film, the adhesive film comprising: an adhesive layer; a light-to-heat conversion layer, the light-to-heat conversion layer comprising a light absorber and a thermally decomposable resin; and an adhesive base film layer, the adhesive base film layer being arranged between the adhesive layer and the light-to-heat conversion layer, wherein the adhesive base film layer comprises a multifunctional epoxy resin, a binder resin, a curing agent and a curing catalyst. The adhesive film according to the present invention can simplify the processing process of a substrate and prevent damage to the substrate and a circuit or element formed on the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] The present invention relates to an adhesive film, and more particularly, to an adhesive film disposed between a substrate to be processed and a carrier during processing of the substrate.

[0002] In various fields, it is generally preferred to use a thin substrate or a flexible substrate. In the process of forming such a thin substrate or using a flexible substrate, a process of bonding the substrate to a hard carrier and then separating the substrate from the hard carrier after the processing of the substrate is completed has been proposed.

[0003] For example, in the field of quartz devices, it is preferred to reduce the thickness of quartz wafers in order to increase the oscillation frequency. Specifically, in the semiconductor industry, efforts are being made to further reduce the thickness of semiconductor wafers for high-density manufacturing by chip lamination technology and to reduce the thickness of semiconductor packages.

[0004] The thickness reduction is performed by performing so-called back grinding on the semiconductor wafer on the surface opposite to the surface having the pattern-formed circuit. In order to reduce the thickness, a method has been proposed in which the bottom surface of the wafer is ground and transferred while the wafer is firmly fixed on a hard carrier with an adhesive, and then the wafer is separated from the hard carrier. By supporting the wafer using a hard carrier, it is possible to prevent the wafer from being cracked during back grinding and transfer, and to process the wafer to a thin thickness level.

[0005] On the other hand, for example, a flexible display device capable of enhancing aesthetic functions and imparting multi-functions in use has been developed, and at this time, a flexible substrate is preferably used. The flexible display device is expected to become a next-generation display device that replaces portable computers, electronic newspapers or smart cards, and printed media such as books, newspapers, and magazines. Due to the enhanced aesthetic functions, reduced thickness, and reduced weight of such a display device, a variety of materials are required, and various flexible substrates are applied and used. For example, thin film metal sheets, plastics, etc. can be used as flexible substrates.

[0006] However, due to its good bending characteristics, the flexible substrate is difficult to apply to existing display device manufacturing equipment designed for glass or quartz substrates. For example, there is a limitation that it is difficult to transport by rail equipment or robots or store in a box.

[0007] Therefore, the flexible substrate is bonded to a hard carrier before forming an element, the carrier supports the flexible substrate while the element is formed on the flexible substrate, and the carrier is separated from the flexible substrate after the element is formed on the substrate. Therefore, even if a flexible substrate is used, a flexible display device in which elements are stably formed can be provided.

[0008] However, this method has a problem in that it is complicated and increases cost and time due to the addition of processes of applying an adhesive between the substrate and the hard carrier, curing the adhesive, etc. In addition, in the process of separating the substrate from the hard carrier after substrate processing, there is a problem that the wafer or the substrate itself is damaged, or the circuit of the wafer and the elements of the flexible substrate are damaged. Summary of the invention

[0009] An object of the present invention is to provide an adhesive film capable of maintaining high adhesion during a processing process and capable of easily peeling a substrate fixed on a carrier from the carrier after the processing process. Therefore, in the present invention, it is possible to prevent the substrate and an element or circuit formed on the substrate from being damaged and broken due to physical force when the substrate is separated from the carrier.

[0010] Another object of the present invention is to provide an adhesive film that can prevent damage to a substrate to be processed and an element or circuit formed on the substrate due to excellent heat resistance and excellent light shielding effect, and the adhesive film is particularly used even in a process requiring high vacuum / high heat resistance of 250° C. or higher. More specifically, the present invention can be applied to a process that requires ramping at a very fast speed, or a process that excludes the ramping process itself and exposes a material to a high temperature at once so that the thermal shock applied to the material is significant.

[0011] Still another object of the present invention is to provide an adhesive film capable of reducing cost and time by simplifying the process of fixing a substrate to be processed on a carrier and peeling the substrate from the carrier.

[0012] In order to solve the problems in the above-mentioned prior art, the adhesive film of the present invention includes: an adhesive layer; a light-to-heat conversion layer, the light-to-heat conversion layer including a light absorber and a thermally decomposable resin; and an adhesive base film layer, the adhesive base film layer being arranged between the adhesive layer and the light-to-heat conversion layer, wherein the adhesive base film layer includes a multifunctional epoxy resin, a binder resin, a curing agent and a curing catalyst.

[0013] The adhesive layer may be a silicone-based adhesive layer.

[0014] The thermally decomposable resin may include two acrylic resins having a -COOH or -OH functional group and different weight average molecular weights.

[0015] The adhesive-based film layer may have adhesion to both the adhesive layer and the light-to-heat conversion layer.

[0016] The curing agent may be a phenolic curing agent.

[0017] The binder resin may be an elastomer resin having a weight average molecular weight of 500,000 to 1,500,000.

[0018] The binder resin may be an acryl-based or rubber-based elastomeric resin.

[0019] The binder resin may have an epoxy group in the chain.

[0020] The adhesive-based film layer may further include a filler.

[0021] The filler may include at least one selected from the group consisting of TiO2, silica, copper powder, alumina, and carbon black.

[0022] The weight ratio of the binder resin to the epoxy resin of the adhesive base film layer may be 25:75 to 55:45.

[0023] According to the adhesive film of the present invention, high adhesion can be maintained during the processing process, and the substrate fixed on the carrier can be easily peeled off from the carrier after the processing process. Therefore, it is possible to prevent the substrate and the components or circuits formed on the substrate from being damaged and broken due to physical force when the substrate is separated from the carrier. In addition, the adhesive film according to the present invention has excellent heat resistance and excellent light shielding effect, and specifically, can even be used in processes requiring high vacuum / high heat resistance of 250°C or higher. In addition, according to the adhesive film of the present invention, cost and time can be reduced by simplifying the process of fixing the substrate to be processed on the carrier and peeling the substrate from the carrier. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a cross-sectional view of an adhesive film according to the present invention.

[0025] FIG. 2A to FIG. 2C : is a view showing a process of treating a substrate using the adhesive film according to the present invention. DETAILED DESCRIPTION

[0026] The advantages and features of the present invention and methods for achieving them will be apparent from the embodiments described in detail below with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments, but may be implemented in various different forms. The embodiments are provided only to complete the disclosure of the present invention and fully provide the scope of the present invention to those of ordinary skill in the art to which the present invention belongs, and the present invention will be limited only by the scope of the appended claims.

[0027] The shapes, sizes, ratios, angles, quantities, etc. shown in the drawings for describing the embodiments of the present invention are exemplary, and therefore the present invention is not limited to the details shown in the drawings. Throughout the specification, the same reference numerals represent the same parts. In addition, when describing the present invention, when it is determined that a detailed explanation of known related art may unnecessarily obscure the subject matter of the present invention, its detailed description will be omitted.

[0028] When the terms "including", "having" and the like are used in this specification, other contents besides the described details may be added unless the expression "only" is used. When a component is expressed in the singular form, the component includes the plural form unless otherwise specifically stated.

[0029] Unless expressly stated otherwise, parts should be interpreted as including the margin of error.

[0030] When describing a positional relationship, when terms such as "on", "above", "below" and "next" are used to describe the positional relationship between two parts, one or more other parts may also be positioned between the two parts, unless the expression "immediately" or "directly" is used.

[0031] The respective features of the embodiments of the present invention may be partially or entirely bonded or combined with each other, and may be technically interlocked or driven in various ways.

[0032] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. The following embodiments are provided as examples so as to fully convey the essence of the present invention to those skilled in the art. Therefore, the present invention is not limited to the embodiments to be described below and may also be implemented in different forms.

[0033] Figure 1 is a cross-sectional view of an adhesive film according to an embodiment of the present invention. Figure 1 , the adhesive film according to the embodiment of the present invention includes a first liner 110 , a light-to-heat conversion layer 120 , an adhesive base film layer 130 , an adhesive layer 140 , and a second liner 150 , which are sequentially laminated.

[0034] The adhesive film of the present invention is in the form of a film and is formed by directly bonding the light-to-heat conversion layer 120 and the adhesive layer 140 to both surfaces of the adhesive base film layer 130 formed in the form of a film. That is, in the adhesive film of the present invention, the adhesive base film layer 130 is used as a support film and is formed into a structure having multiple layers without a hard base film such as a PI film or a PEN film. In the process of processing the substrate later, the adhesive layer 140 is bonded to the substrate, and the light-to-heat conversion layer 120 is bonded to the hard support.

[0035] In more detail, the light-to-heat conversion layer 120 is divided when irradiated with radiation energy such as laser, and can be separated from the carrier without damaging the substrate or elements or circuits on the substrate.

[0036] The light-to-heat conversion layer 120 includes a light absorber and a thermally decomposable resin. Radiant energy applied to the light-to-heat conversion layer 120 in the form of laser light or the like is absorbed by the light absorber and converted into thermal energy. The generated thermal energy rapidly increases the temperature of the light-to-heat conversion layer 120, and the temperature reaches the thermal decomposition temperature of the thermally decomposable resin (organic component) in the light-to-heat conversion layer 120, thereby causing thermal decomposition of the resin. The gas generated by the thermal decomposition forms a pore layer (such as a space) in the light-to-heat conversion layer 120, and the light-to-heat conversion layer 120 is divided into two parts, and therefore, the carrier and the substrate are separated from each other.

[0037] The light absorber can absorb radiation energy and convert the absorbed radiation energy into heat energy. In addition, the light absorber can block light to prevent the substrate from being damaged by laser or the like.

[0038] Although the light absorber varies depending on the wavelength of the laser, examples of light absorbers that can be used include carbon black, graphite powder, fine metal powders (such as iron, aluminum, copper, nickel, cobalt, manganese, chromium, zinc and tellurium), metal oxide powders (such as black titanium oxide) and dyes and pigments (such as aromatic diamino-based metal complexes, aliphatic diamine-based metal complexes, aromatic dithiol-based metal complexes, hydroxythiophenol-based metal complexes, square acid-based compounds, cyanine-based dyes, methine-based dyes, naphthoquinone-based dyes and anthraquinone-based dyes). The light absorber may be in the form of a film, including a vapor-deposited metal film.

[0039] Among these light absorbers, carbon black is particularly useful, and the reason is that carbon black significantly reduces the force required to separate the substrate from the support after irradiation and accelerates the separation.

[0040] The particle size of the light absorber in the light-to-heat conversion layer 120 may be about 20 nm to about 2000 nm, preferably about 50 nm to about 1000 nm, and more preferably about 100 nm to about 350 nm.

[0041] When the particle size of the light absorber is less than about 20 nm, dispersion is difficult, and the smaller the particle size, the larger the surface area, so that a large amount of light absorber cannot be loaded and the loading content is limited. In addition, when the particle size of the light absorber is greater than about 2000 nm, the laser blocking performance is reduced, and the laser segmentation performance of the light-to-heat conversion layer 120 is reduced. In addition, as the particle size of the light absorber increases, the film-forming property is reduced, the dispersion stability after dispersion is reduced, and the time required until the rough solution is formed and coated should be short.

[0042] The light absorber in the light-to-heat conversion layer 120 may be contained in an amount of about 5 wt % to about 80 wt %, preferably about 10 wt % to about 60 wt %, and more preferably about 20 wt % to about 50 wt %, based on the total weight of the light-to-heat conversion layer 120 .

[0043] When the content of the light absorber is less than about 5 wt %, separation by laser is difficult. In addition, when the content of the light absorber is greater than about 80 wt %, after the light-to-heat conversion layer 120 is split by the laser, a portion of the light-to-heat conversion layer 120 separated by the laser remains on the surface of the adhesive base film layer 130, and at this time, the adhesion becomes very low due to the high carbon content. In this case, there is a problem that in the process of removing the adhesive base film layer 130 and the adhesive layer 140 with the removal tape later, the adhesive base film layer 130 is not well bonded to the removal tape, and therefore it is difficult to remove it. In addition, as the content of the light absorber increases, the adhesion on the surface of the light-to-heat conversion layer 120 becomes too low, and therefore it is difficult to laminate with the carrier and the dispersion of the light absorber is uneven.

[0044] The thermally decomposable resin in the light-to-heat conversion layer 120 includes an acrylic resin. Preferably, the acrylic resin includes a monomer selected from the group consisting of methyl methacrylate (MMA), hydroxyethyl methacrylate (HEMA), ethyl acrylate (EA), butyl acrylate (BA), acrylonitrile (AN), and a combination thereof. Preferably, the acrylic resin may be selected from a combination of at least three of methyl methacrylate (MMA), hydroxyethyl methacrylate (HEMA), ethyl acrylate (EA), butyl acrylate (BA), and acrylonitrile (AN). The acrylic resin may have a suitable molecular weight, Tg, heat resistance, and functional group.

[0045] The content of the acrylic resin may be about 5 wt % to about 80 wt %, preferably about 15 wt % to about 60 wt %, and more preferably about 40 wt % to about 60 wt %, based on the total weight of the light-to-heat conversion layer 120. When the content of the acrylic resin is less than about 5 wt %, the film-forming property is reduced, it is difficult to control the thickness of the light-to-heat conversion layer 120, and the adhesion of the surface of the light-to-heat conversion layer 120 is too low to be laminated with a carrier. In addition, when the content of the acrylic resin is greater than about 80 wt %, physical force is largely required when dividing the light-to-heat conversion layer 120 after laser irradiation, it is difficult to separate the substrate from the carrier, and damage to the substrate or an element or circuit formed on the substrate may occur.

[0046] The acrylic resin preferably includes two types of acrylic resins having different weight average molecular weights, more preferably a high molecular weight acrylic resin and a low molecular weight acrylic resin. The high molecular weight acrylic resin allows the light-to-heat conversion layer 120 to have excellent heat resistance, and the low molecular weight acrylic resin improves the adhesion of the light-to-heat conversion layer 120 and facilitates film formation.

[0047] At this time, the Tg (glass transition temperature) of the high molecular weight acrylic resin is 0° C. to 10° C., and the Tg of the low molecular weight acrylic resin may be -10° C. to 0° C. When the Tg of the high molecular weight acrylic resin is higher than 10° C. and the Tg of the low molecular weight acrylic resin is higher than 0° C., the heat resistance of the light-to-heat conversion layer 120 may be improved, but the surface adhesiveness may be reduced. On the other hand, when the Tg of the high molecular weight acrylic resin is lower than 0° C. and the Tg of the low molecular weight acrylic resin is lower than -10° C., the bonding performance may be improved, but the heat resistance may be reduced.

[0048] The weight average molecular weight of the high molecular weight acrylic resin may be about 400,000 g / mol to about 15,000,000 g / mol, preferably about 500,000 g / mol to about 1,200,000 g / mol, and more preferably about 700,000 g / mol to about 1,000,000 g / mol. When the weight average molecular weight of the high molecular weight acrylic resin is less than about 400,000 g / mol, the heat resistance of the light-to-heat conversion layer 120 is reduced, and when the weight average molecular weight thereof is greater than about 15,000,000 g / mol, coating of the light-to-heat conversion layer 120 and mixing of the crude solution are not easy.

[0049] The weight average molecular weight of the low molecular weight acrylic resin may be about 50,000 g / mol to about 600,000 g / mol, preferably about 100,000 g / mol to about 500,000 g / mol, and more preferably about 400,000 g / mol to about 500,000 g / mol. When the weight average molecular weight of the low molecular weight acrylic resin is less than about 50,000 g / mol, the heat resistance of the light-to-heat conversion layer 120 is reduced, and when the weight average molecular weight thereof is greater than about 600,000 g / mol, the lamination performance of the light-to-heat conversion layer 120 is deteriorated.

[0050] The weight ratio of the high molecular weight acrylic resin to the low molecular weight acrylic resin may be about 1:4 to about 4:1, preferably about 1:3 to about 3:1, and more preferably about 1:2 to about 2:1. When the content of the low molecular weight acrylic resin is significantly less than the content of the high molecular weight acrylic resin, the lamination performance of the light-to-heat conversion layer 120 is deteriorated. In addition, when the content of the high molecular weight acrylic resin is significantly less than the content of the low molecular weight acrylic resin, the heat resistance of the light-to-heat conversion layer 120 is reduced, and after laser irradiation, the adhesion on the divided surface of the light-to-heat conversion layer 120 is strong, and therefore, a physically large force is required for separation.

[0051] The heat-decomposable resin has a -COOH or -OH functional group. Preferably, the heat-decomposable resin includes an acrylic resin having a -COOH or -OH functional group. The light-to-heat conversion layer 120 including a heat-decomposable resin having a -COOH or -OH functional group is not a pressure-sensitive adhesive type. By having a -COOH or -OH functional group, the light-to-heat conversion layer can be bonded to a carrier by hydrogen bonding, and for example, can be bonded to a silanol group on a glass surface of a carrier made of glass by hydrogen bonding. At this time, hydrogen bonding provides initial adhesion for bonding the adhesive layer to the carrier, and due to the heat generated in the process after the bonding process, the adhesion between the light-to-heat conversion layer 120 and the carrier is greatly increased.

[0052] The -COOH or -OH functional group may have an acid value of at least about 1 mgKOH / g, preferably at least about 5 mgKOH / g. The lamination performance of the light-to-heat conversion layer 120 is based on the -COOH or -OH functional group. When the acid value of the -COOH or -OH functional group is lower than about 1 mgKOH / g, the lamination performance deteriorates. The upper limit of the acid value of -COOH or -OH is not a problem. However, due to the chemical structure, the -COOH or -OH functional group may have an acid value of preferably about 1 mgKOH / g to about 50 mgKOH / g, more preferably about 1 mgKOH / g to about 30 mgKOH / g, and most preferably about 10 mgKOH / g to about 20 mgKOH / g.

[0053] The light-to-heat conversion layer 120 may further include an inorganic filler. The inorganic filler plays a role in preventing the light-to-heat conversion layer 120 from re-adhesion after being separated due to the formation of a void layer caused by thermal decomposition of the thermally decomposable resin. Therefore, after processing the substrate, when the light-to-heat conversion layer 120 is irradiated with laser and separated, the physical force required to separate the substrate and the carrier can be further reduced.

[0054] The inorganic filler may be selected from the group consisting of SiO2, Al2O3, TiO2 and combinations thereof. Specifically, in the case of TiO2, there is an additional light shielding effect on the substrate.

[0055] The particle size of the inorganic filler in the light-to-heat conversion layer 120 may be about 20 nm to about 2000 nm, preferably about 50 nm to about 1000 nm, and more preferably about 100 nm to about 350 nm. When the particle size of the inorganic filler is less than about 20 nm, the dispersion of the inorganic filler is not easy during film preparation, and there is a limit to the amount of inorganic filler that can be loaded. In addition, when the particle size of the inorganic filler is greater than about 2000 nm, the film-forming property is reduced and the dispersion durability after dispersion is reduced.

[0056] The content of the inorganic filler in the light-to-heat conversion layer 120 may be about 4 wt % to about 60 wt %, preferably about 5 wt % to about 50 wt %, and more preferably about 5 wt % to about 30 wt %, based on the total weight of the light-to-heat conversion layer 120. When the content of the inorganic filler is less than about 4 wt %, after the separation process by laser irradiation, the adhesion of the separated surface is high, and therefore, the light-to-heat conversion layer 120 may be re-bonded over time. In addition, when the content of the inorganic filler is greater than about 60 wt %, the adhesion of the light-to-heat conversion layer 120 is too low to be laminated on a carrier, which is difficult, the film-forming property is reduced, and the dispersion is uneven.

[0057] The light-to-heat conversion layer 120 may further include a dispersant. Based on the total weight of the light-to-heat conversion layer 120, the content of the dispersant may be from about 0.1 wt % to about 10 wt %, preferably from about 0.1 wt % to about 7 wt %, and more preferably from about 0.1 wt % to about 5 wt %. When the content of the dispersant is less than about 0.1 wt %, the dispersibility of the light absorber and the inorganic filler in the light-to-heat conversion layer 120 may be reduced, and the dispersion durability after dispersion may also be reduced. In addition, when the content of the dispersant is greater than about 10 wt %, the heat resistance of the light-to-heat conversion layer 120 deteriorates, the additive to be added decomposes at high temperature, and the weight loss increases.

[0058] The thickness of the light-to-heat conversion layer 120 is about 1 μm to about 30 μm, preferably about 3 μm to about 20 μm, and more preferably about 5 μm to about 15 μm. When the thickness of the light-to-heat conversion layer 120 is less than about 1 μm, the upper adhesive layer may directly affect the material, and the laser shielding performance may be deteriorated due to the light absorber. In addition, when the thickness of the light-to-heat conversion layer 120 is greater than about 30 μm, after laser irradiation, many adhesive residues may remain on the carrier.

[0059] The light-to-heat conversion layer 120 is formed in the form of a thin film on the adhesive base film layer 130. When the light-to-heat conversion layer 120 is directly applied to the carrier and formed in the form of a liquid, if the viscosity is low, the thickness thereof is less than about 1 μm, so that the thickness cannot be sufficiently thick. Therefore, it is difficult to fully use the light absorber capable of shielding the laser, and it is difficult to prevent the laser from damaging the substrate.

[0060] In the present invention, the light-to-heat conversion layer 120 may be directly applied to a carrier and formed in a liquid form, and after being formed into a film form by separate application, the light-to-heat conversion layer 120 may be bonded to the adhesive base film layer 130 through a thermal lamination process.

[0061] When the light-to-heat conversion layer 120 according to the present invention is formed in the form of a film, its thickness is easily controlled and may be more advantageous in protecting the substrate and circuits or elements formed thereon. In addition, the adhesion of the light-to-heat conversion layer 120 to the carrier may be 150 gf / 25 mm to 1600 gf / 25 mm.

[0062] Meanwhile, the adhesive layer 140 is used to fix the substrate. After the substrate and the carrier are separated by decomposition of the light-to-heat conversion layer 120, a substrate having the adhesive layer 140 thereon is obtained. Therefore, the adhesive layer 140 should be easily separated from the substrate by peeling or the like. The adhesive layer 140 is in the form of a film formed on the adhesive base film layer 130, and is not a photocurable adhesive directly applied to the substrate.

[0063] The adhesive layer 140 may be a silicon-based adhesive layer. Preferably, the adhesive of the silicon-based adhesive layer may include a radical-curable organic silicon-based adhesive.

[0064] In substrate processing, especially in semiconductor processing, an adhesive film having excellent stability under high temperature and high vacuum conditions is required. However, in the case of an acrylic adhesive layer, for example, the temperature limit of heat resistance is 230°C, and if the process is performed at a higher temperature or the process lasts for a long time, the adhesive may melt and flow. In addition, since acrylic adhesives and the like have high CTE but low modulus and are flexible, acrylic adhesives and the like may move according to the deformation of the material at high temperature. Therefore, there is a problem that the heat resistance of acrylic adhesives is not sufficient for high temperature / high vacuum processes, and the adhesion under conditions such as high temperature is poor.

[0065] On the other hand, the silicone-based adhesive layer has excellent stability and excellent heat resistance at high temperatures. In addition, since the silicone-based adhesive layer is softer than an adhesive layer made of another material (e.g., an acrylic adhesive layer), the lamination performance is excellent when bonding hard materials such as substrates and carriers.

[0066] In addition, the soft nature of the silicon-based adhesive layer allows the adhesive layer 140 to be gently removed when peeling after the substrate processing process is completed, and damage to the components on the substrate can be prevented. In addition, after the substrate processing process is completed, high temperatures can be used when peeling the adhesive layer 140 so that no residue remains on the substrate.

[0067] The adhesive layer 140 may include a curing agent. Preferably, the curing agent may be a benzoyl peroxide (BPO) curing agent. More preferably, the benzoyl peroxide (BPO) curing agent may be di(2,4-dichlorobenzoyl) peroxide or dibenzoyl peroxide. For example, the benzoyl peroxide (BPO) curing agent may be used in a powder form or a paste form.

[0068] The curing agent may be contained in the adhesive layer 140 in an amount of about 1 wt % to about 4 wt %, preferably about 1 wt % to about 3 wt %, and more preferably about 2 wt % to about 3 wt %, based on the total weight of the adhesive layer 140 .

[0069] When the content of the curing agent is less than about 1 wt %, the reactivity may be deteriorated. In addition, when the content of the curing agent is greater than about 4 wt %, the excess curing agent may not react and unreacted curing agent may remain, and after curing and drying, the transparency and roughness of the surface of the adhesive layer 140 may be reduced.

[0070] The adhesive layer 140 may further include an additive. The additive is used to remove moisture in the silicone-based adhesive layer 140. That is, the additive removes moisture in the adhesive layer 140 to improve the curing efficiency of the adhesive layer 140, thereby further improving the heat resistance of the adhesive layer 140.

[0071] Preferably, the additive may be TiO2. For example, in the case of Al2O3, SiO2, etc., the dispersibility is weak, and thus a dispersant is required. However, in the case of a silicone-based adhesive layer, since an aromatic solvent is used as a solvent, it is difficult to use as most of the dispersants, and when a dispersant is added, the heat resistance of silicone may be deteriorated due to the dispersant.

[0072] In the case of TiO2, dispersibility is very excellent, and TiO2 is a filler that can be applied without a special dispersant. In addition, moisture and the like can be removed to prevent the curing reaction from being reduced due to moisture during the radical reaction of silicon.

[0073] The size of the additive in the adhesive layer 140 is about 100 nm to about 500 nm, preferably about 200 nm to about 400 nm, and more preferably about 200 nm to about 300 nm.

[0074] When the size of the additive is less than about 100 nm, dispersibility is reduced and the amount that can be loaded is limited. In addition, when the size of the additive is greater than about 500 nm, there may be problems in that the additive may precipitate over time after dispersion and the surface roughness is not good when the resin is coated.

[0075] The additive may be contained in adhesive layer 140 in an amount of about 1 wt % to about 10 wt %, preferably about 1 wt % to about 8 wt %, and more preferably about 1 wt % to about 5 wt %, based on the total weight of adhesive layer 140 .

[0076] When the content of the additive is less than about 1% by weight, it is difficult to show the effect of the additive. In addition, when the content of the additive is greater than about 10% by weight, problems may occur on the surface of the adhesive layer 140. The thickness of the adhesive layer 140 is about 5 μm to about 100 μm, preferably about 5 μm to about 70 μm, and more preferably about 10 μm to about 60 μm. When the thickness of the adhesive layer 140 is less than about 5 μm, when the device is severely deformed due to low adhesion, interlayer peeling may occur. In addition, when the thickness of the adhesive layer 140 is greater than about 100 μm, the drying efficiency is reduced when the adhesive layer 140 is formed, and there is a possibility of solvent residue, and the cohesion of the adhesive layer 140 is reduced, and therefore residues may remain. Due to the soft nature of the adhesive layer 140, it may be difficult to fix the adhesive layer 140 during the substrate processing process.

[0077] On the other hand, when the adhesive layer 140 is a silicone-based adhesive layer, the light-to-heat conversion layer 120 includes an acrylic component, making it difficult to directly coat the light-to-heat conversion layer 120 between the silicone-based material and the acrylic material. Specifically, due to the low surface energy of the silicone-based adhesive, the light-to-heat conversion layer 120 may not be coated on the silicone-based adhesive layer 140. On the contrary, due to the high curing temperature of the silicone-based adhesive, the adhesion of the light-to-heat conversion layer 120 is reduced, and the adhesive layer 140 may not be coated on the light-to-heat conversion layer 120.

[0078] In addition, a supporting film layer for supporting the light-to-heat conversion layer 120 and the adhesive layer 140 is required.

[0079] In order to support the light-to-heat conversion layer 120 and the adhesive layer 140, solid films such as PI films have been designed. However, the PI film has high rigidity and modulus, but generally exhibits a CTE greater than the CTE of a carrier or substrate such as a wafer. Therefore, when the PI film is exposed to high temperatures, wrinkling, distortion, warping, etc. may occur. Due to the wrinkling, distortion, and warping of the PI film, the irregular surface may affect substrate processing, and processing defects may occur.

[0080] In addition, in the case of using a rigid base film such as a PI film, there is a problem that a silicone primer needs to be processed on the PI film. Therefore, there is a problem that the process increases and the cost and time increase.

[0081] Furthermore, an additional adhesive layer is required to bond the PI film with the light-to-heat conversion layer 120 , and thus, there are problems in that the overall thickness of the film increases and the structure is complicated.

[0082] In order to solve these problems, in the present invention, the adhesive base film layer 130 is formed between the light-to-heat conversion layer 120 and the adhesive layer 140 to support the light-to-heat conversion layer 120 and the adhesive layer 140 and to bond the light-to-heat conversion layer 120 and the adhesive layer 140. That is, the adhesive base film layer 130 of the present invention can reduce or prevent problems caused by a rigid base film. Specifically, due to the low modulus compared to the PI film, the adhesive base film layer 130 expands or contracts according to the thermal behavior of the material or carrier to prevent problems such as wrinkling, distortion, and warping.

[0083] In addition, when the adhesive base film layer 130 is used instead of the rigid film, the light-to-heat conversion layer 120, the adhesive base film layer 130 and the adhesive layer 140 are all flexible layers made of adhesive materials to form an adhesive film. Therefore, the adhesive film itself exhibits flexibility, and thus is more conducive to lamination with a carrier and a substrate, and exhibits high adhesion.

[0084] The adhesive base film layer 130 includes an epoxy resin. Preferably, the adhesive base film layer 130 includes a multifunctional epoxy resin. More preferably, the multifunctional epoxy resin may be a novolac epoxy resin or a dicyclopentadiene epoxy resin. The multifunctional epoxy resin may increase chemical resistance by achieving a high crosslinking density.

[0085] The adhesive base film layer 130 has chemical resistance to a solvent (eg, methyl ethyl ketone (MEK) and ethyl acrylate (EA)) used for the light-to-heat conversion layer 120 and a solvent (eg, toluene and xylene) used for the adhesive layer 140 .

[0086] Furthermore, even at high temperatures, the adhesive base film layer does not expand or contract between the light-to-heat conversion layer 120 and the adhesive layer 140. Specifically, even at the curing temperature of the silicone-based adhesive layer 140, physical rigidity is maintained without contraction or expansion.

[0087] Furthermore, the adhesive base film layer 130 has a CTE and modulus suitable for the process and does not exhibit physical changes during subsequent substrate handling.

[0088] In addition, the adhesive-based film layer 130 including the epoxy resin has adhesiveness to both the light-to-heat conversion layer 120 and the adhesive layer 140 which are not bonded to each other, and has hardness capable of supporting the two layers.

[0089] In addition, the adhesive base film layer 130 itself has adhesiveness, and in the manufacturing process, instead of the process of forming and laminating separate film layers, the light-to-heat conversion layer 120 and the adhesive layer 140 are directly coated and cured on the adhesive base film layer 130, and therefore, the interlayer adhesiveness between the adhesive base film layer 130 and the light-to-heat conversion layer 120 and between the adhesive base film layer 130 and the adhesive layer 140 is very high. Therefore, the adhesive base film layer 130 has excellent heat resistance and excellent process stability even under high temperature and high vacuum processes.

[0090] In addition, the adhesive base film layer 130 includes a binder resin. Such a binder resin allows a layer including an epoxy resin to be film-formed.

[0091] The binder resin may be an elastomer resin. Preferably, the binder resin may have a glass transition temperature Tg of at least 0° C. or higher. The binder resin having such a glass transition temperature may allow the adhesive base film layer 130 to have excellent heat resistance.

[0092] The binder resin may be an acryl or rubber-based elastomeric resin. The binder resin may include a rubber-based or acrylic polymer. For example, the binder resin may include acrylonitrile butadiene rubber (NBR) or styrene butadiene rubber (SBR).

[0093] Preferably, when the binder resin includes NBR, the binder resin may include 30 wt % or more of an acrylonitrile group based on the total weight of the binder resin. In this case, the binder resin may be easily dissolved in a solvent.

[0094] Preferably, when the binder resin includes an acrylic polymer, the acrylic polymer may include at least two or three monomers selected from the group consisting of ethyl acrylate (EA), hydroxyethyl methacrylate (HEMA), hydroxyethyl acrylate (HEA), butyl acrylate (BA), poly(methyl methacrylate) (PMMA), acrylonitrile (AN) and combinations thereof.

[0095] The binder resin has a weight average molecular weight (Mw) of about 500,000 to about 1,500,000, more preferably about 700,000 to about 1,000,000, more preferably 800,000 to 1,000,000. The binder resin having a high molecular weight has heat resistance of the adhesive base film layer 130 .

[0096] When the weight average molecular weight of the binder resin is less than about 500,000, the chemical resistance and heat resistance of the adhesive base film layer 130 may be insufficient. In addition, when the weight average molecular weight of the binder resin is greater than about 1,500,000, there is a problem that the adhesive base film layer 130 is difficult to form a film and it is difficult to apply the adhesive base film layer because the binder resin is not easily dissolved in a solvent.

[0097] In addition, the binder resin may have an epoxy group in its chain. The chain of the binder resin has an epoxy group, thereby improving the compatibility of the epoxy resin and the binder resin.

[0098] At this time, preferably, the weight ratio of the binder resin to the epoxy resin of the adhesive base film layer may be 25:75 to 55:45. That is, when the total weight of the epoxy resin and the binder resin is 100 parts by weight, the content of the epoxy resin is 30 to 60 parts by weight, and the content of the binder resin is 40 to 70 parts by weight. The weight ratio of the binder resin to the epoxy resin of the adhesive base film layer is preferably 30:70 to 50:50, more preferably 40:60.

[0099] When the total weight of the epoxy resin and the binder resin is 100 parts by weight and the amount of the epoxy resin is less than 30 parts by weight, the chemical resistance is reduced and the rigidity of the binder resin film layer is insufficient, so that the subsequent coating of the light-to-heat conversion layer and the adhesive layer may be difficult. In addition, when the epoxy resin is greater than 60 parts by weight, the chemical resistance and rigidity are excellent, but the binder resin film layer is brittle and may be difficult to use as a supporting film layer.

[0100] In addition, the adhesive-based film layer 130 including the epoxy resin has adhesiveness to both the light-to-heat conversion layer 120 and the adhesive layer 140 which are not bonded to each other, and has hardness capable of supporting the two layers.

[0101] The adhesive base film layer 130 may include a curing agent. Preferably, a phenolic curing agent may be included. Generally, amines and isocyanates may be considered as curing agents for epoxy resins, but the problem is that these curing agents are difficult to form films. The adhesive base film layer 130 may be formed into a film by using a phenolic curing agent as a curing agent and appropriately controlling the curing rate.

[0102] The adhesive base film layer 130 may include a curing catalyst. The amount of the curing catalyst used allows the adhesive base film layer 130 to have chemical resistance to methyl ethyl ketone (MEK), ethyl acrylate (EA), toluene, and xylene and maintain heat resistance. For example, the curing catalyst may be imidazole.

[0103] In addition, the adhesive base film layer 130 may further include a filler. For example, the filler may include at least one selected from the group consisting of TiO2, silica, copper powder, alumina, and carbon black.

[0104] The filler may additionally prevent shrinkage and expansion of the adhesive base film layer 130. Furthermore, after the substrate treatment process is completed, when light is irradiated to the light-to-heat conversion layer 120, there is an additional light shielding effect on the substrate.

[0105] The adhesive base film layer 130 may be prepared and aged for a predetermined period of time. For example, aging may be performed for about 4 days. Thus, the reaction of the epoxy resin is completely terminated, and the light-to-heat conversion layer 120 and the adhesive layer 140 are later formed on the adhesive base film layer 130, or stability is improved during substrate processing.

[0106] The thickness of the adhesive base film layer 130 is about 10 μm to about 50 μm, preferably about 20 μm to about 40 μm, and more preferably about 20 μm to about 30 μm. When the thickness of the adhesive layer 140 is less than about 10 μm, it is difficult to obtain physically sufficient strength, it may be difficult to support the light-to-heat conversion layer 120 and the adhesive layer 140, and it may be affected by the shrinkage that occurs during the curing of the adhesive layer. In addition, when the thickness of the adhesive base film layer 130 is greater than about 50 μm, the solvent is difficult to evaporate during coating, irregular holes may be formed on the film surface, and when the solvent remains, the solvent may affect the physical properties of the adhesive film.

[0107] The first gasket 110 and the second gasket 150 are used to support and protect the adhesive layer 140 and the light-to-heat conversion layer 120, respectively. When the adhesive film is used, the first gasket 110 and the second gasket 150 are removed.

[0108] The first gasket 110 and the second gasket 150 may be silicon-coated polyethylene terephthalate (PET), but are not limited thereto, and are sufficient as a material capable of supporting and protecting the adhesive layer 140 and the light-to-heat conversion layer 120 .

[0109] A method of manufacturing an adhesive film according to an embodiment of the present invention is as follows.

[0110] The adhesive base film layer 130 is formed on the first liner. Thereafter, the second liner may be laminated on the adhesive base film layer 130 in a roll-to-roll method.

[0111] Thereafter, while the second liner is removed, the silicone-based adhesive layer 140 may be directly formed on the adhesive base film layer 130 , and the third liner may be laminated on the adhesive layer 140 .

[0112] Subsequently, while removing the first liner, the light-to-heat conversion layer 120 may be directly formed on the other surface of the adhesive base film layer 130, and the fourth liner may be laminated on the light-to-heat conversion layer 120. That is, in this process, the fourth liner on the light-to-heat conversion layer 120 and the third liner on the adhesive layer 140 correspond to Figure 1The first gasket 110 and the second gasket 150 are provided.

[0113] However, the manufacturing process of the adhesive film of the present invention is not limited thereto, and a method of forming the light-to-heat conversion layer 120 and the adhesive layer 140 in the form of films on both surfaces of the adhesive base film layer 130 , respectively, is sufficient.

[0114] When a liquid adhesive material and a liquid photothermal conversion material are used between a substrate and a carrier, a process of forming a photothermal conversion layer by applying and curing the photothermal conversion material on the carrier and a process of forming an adhesive layer by applying and curing the adhesive material on the substrate to be processed are respectively required. Thereafter, a process of bonding the adhesive layer and the photothermal conversion layer under vacuum is required. That is, when a liquid material is used, a coating time, a curing time, and a bonding time are required.

[0115] On the other hand, in the case of using the film-form adhesive film according to the present invention, it is sufficient to remove the first liner and attach the adhesive layer to the substrate, and to remove the second liner and attach the light-to-heat conversion layer to the carrier. Therefore, according to the present invention, the time required for the process can be significantly reduced, and the cost required for the application process, the curing process, the vacuum process, etc. can be reduced.

[0116] FIG. 2A to FIG. 2C : is a view showing a process of treating a substrate using the adhesive film according to the present invention.

[0117] refer to Figure 2A , in the adhesive film according to the present invention, the first liner is removed and the light-to-heat conversion layer 120 is attached to the carrier 200, and the second liner is removed and the adhesive layer 140 is attached to the substrate 300. At this time, it is preferred to perform the process at about 40° C. to about 80° C. so that the adhesion between the light-to-heat conversion layer 120 and the carrier 200 is increased.

[0118] The carrier 200 is a material capable of transmitting radiation energy such as laser used in the present invention, and is required to maintain the substrate 300 in a flat state and prevent the substrate 300 from being broken during handling and transfer. Preferably, the carrier 200 is hard and transmissive.

[0119] The transmittance of the carrier 200 is not limited unless it prevents radiation energy from being transmitted into the light-to-heat conversion layer 120 so as to enable decomposition of the light-to-heat conversion layer 120. However, the transmittance is preferably, for example, about 50% or more.

[0120] Furthermore, in order to prevent the substrate from being deformed during processing, it is preferred that the carrier 200 has sufficiently high rigidity, and the bending strength of the carrier 200 is preferably 2×10 -3 (Pa·m 3 ) or more, more preferably 3×10 -2(Pa·m 3 ) or higher.

[0121] Furthermore, in order to prevent damage due to thermal history that may occur during processes performed on the substrate, it is preferred that the carrier 200 has sufficient heat resistance, and the heat deflection temperature of the carrier 200 is preferably 550° C. or higher, more preferably 700° C. or higher.

[0122] The carrier 200 may be, for example, glass. In addition, in order to improve the adhesive strength to the adjacent layers such as the light-to-heat conversion layer 120, the carrier 200 may be surface-treated with an adhesive or the like, if necessary.

[0123] Thereafter, after fixing the substrate 300 and the carrier 200 with the adhesive film including the light-to-heat conversion layer 120 , the adhesive base film layer 130 , and the adhesive layer 140 interposed therebetween, the substrate 300 is processed.

[0124] The substrate 300 is a substrate that is fixed to the carrier 200 and processed and then separated from the carrier 200 , and may be, for example, a wafer or a substrate for a flexible display device.

[0125] For example, the substrate 300 may include a semiconductor wafer such as silicon and gallium arsenide, a crystal wafer, sapphire, or glass. The circuit surface of the substrate 300 may be bonded to the adhesive layer 140. Thereafter, the surface of the substrate 300 not bonded to the adhesive layer 140 may be ground by a grinder or the like to be processed into a thin substrate.

[0126] As another example, the substrate 300 may be an epoxy resin molded wafer. The molded surface of the substrate 300 may be bonded to the adhesive layer 140, and then the substrate may be processed into a completed substrate by performing a predetermined process for connecting a circuit to the surface of the substrate 300 that is not bonded to the adhesive layer 140.

[0127] On the other hand, for another example, the substrate 300 may be a plastic or metal film as a flexible substrate, etc. For example, the substrate 300 may be PI. However, the present invention is not limited thereto, and a material having a flexible property may be sufficient as a material that can be used as a substrate of a flexible display device.

[0128] For example, the "processing" may include a process of forming an element layer on the substrate 300. Although not shown, the element layer is composed of a plurality of thin film layers and electrical elements, and more specifically, may include a thin film transistor including a gate electrode, a semiconductor layer, a source electrode, and a drain electrode.

[0129] The flexible display device may be any one selected from the group consisting of an organic light emitting diode display, a liquid crystal display, and an electrophoretic display. However, the flexible display device is not limited thereto and may include all flexible display devices using a flexible substrate.

[0130] refer to Figure 2B , after a desired degree of processing, the carrier 200 and the processed substrate 300 are separated from each other by irradiating laser 400. The laser 400 is irradiated from the carrier 200 side.

[0131] The light absorber of the light-to-heat conversion layer 120 absorbs the radiation energy of the laser 400 and converts the absorbed energy into heat energy. The generated heat energy rapidly increases the temperature of the light-to-heat conversion layer 120, and the temperature causes the decomposition of the thermally decomposable resin in the light-to-heat conversion layer 120. The gas generated by the thermal decomposition forms a pore layer in the light-to-heat conversion layer 120, and the light-to-heat conversion layer 120 is divided into two parts, and thus, the carrier 200 and the processed substrate 300 are separated from each other.

[0132] The thermally decomposable resin in the light-to-heat conversion layer 120 is decomposed by the irradiation of the laser 400 to form cracks inside the layer, thereby separating the light-to-heat conversion layer itself. The air (gas) generated by the decomposition of the resin is eventually introduced between the two layers to separate the two layers. Therefore, in order to facilitate the introduction of air, it is preferred to perform the irradiation of the laser 400 from the edge of the light-to-heat conversion layer 120 to the inside of the light-to-heat conversion layer 120.

[0133] To use the laser 400 from the edge of the light-to-heat conversion layer 120 , a method of applying the laser 400 while linearly reciprocating from the edge may be employed, or alternatively, a method of spirally irradiating the laser 400 from the edge to the center, such as a record player, may be employed.

[0134] Laser 400 is typically a laser having a wavelength of about 300 nm to about 11,000 nm, preferably about 300 nm to about 2,000 nm, and specific examples thereof include a YAG laser emitting light at a wavelength of 1,064 nm, a YAG laser generating a second harmonic at a wavelength of 532 nm, and a semiconductor laser having a wavelength of 780 nm to 1,300 nm.

[0135] refer to Figure 2C , after removing the carrier 200, the adhesive base film layer 130 and the adhesive layer 140 on the processed substrate 300 are removed. In order to remove the adhesive base film layer 130 and the adhesive layer 140, it is preferred to use a removal tape 500 having stronger adhesion to the adhesive base film layer 130 than between the processed substrate 200 and the adhesive layer 140.

[0136] The removal tape 500 is disposed to be adhered to the adhesive base film layer 130 and then peeled off together with the adhesive base film layer 130 and the adhesive layer 140 to remove the adhesive base film layer 130 and the adhesive layer 140 from the processed substrate 300 .

[0137] Although not clearly shown in the drawings, a portion of the light-to-heat conversion layer 120 may remain after the light-to-heat conversion layer 120 is divided on the adhesive base film layer 130. When the removal tape 500 is used, the remaining portion is also removed together.

[0138] Meanwhile, although not shown in the figure, after removing the carrier 200, the adhesive base film layer 130 and the adhesive layer 140 may be removed using a removal solution. Preferably, the adhesive base film layer 130 and the adhesive layer 140 in which the light-to-heat conversion layer is partially retained may be immersed in the removal solution to remove the adhesive base film layer 130 and the adhesive layer 140. Preferably, the adhesive layer 140 may be immersed in the removal solution for about 10 seconds to 60 seconds.

[0139] Additionally, the removal solution may contain trans-1,2-dichloroethylene and a hydrofluoroether.

[0140] When the size or area of ​​the processed substrate 200 is large, it may be difficult to remove the adhesive base film layer 130 and the adhesive layer 140 at one time with the removal tape 500. However, when the removal solution is used, it is advantageous to remove the adhesive base film layer 130 and the adhesive layer 140 having a large area. In addition, no additional external physical force is required, and there is an effect of removing the adhesive base film layer 130 and the adhesive layer 140 in a short time without residue.

[0141] The processing method of the substrate according to the present invention is environmentally friendly because no solvent is required when the substrate is processed by using the prepared adhesive film. In addition, when the prepared adhesive film is used, the exposure of the carrier and the substrate to heat and UV is reduced when the substrate is processed, thereby preventing additional damage.

[0142] In addition, the process of directly applying and curing the adhesive material or the photothermal conversion material on the carrier or substrate can be omitted, and thus the process is simplified, thereby reducing the cost and time of the process. In addition, the processing method is conducive to forming an adhesive layer and a photothermal conversion layer of uniform thickness, and can also be used to process large-area substrates.

[0143] Hereinafter, the present invention will be described in more detail by experimental examples, but the following experimental examples are only intended to illustrate the present invention and are not intended to limit the present invention. That is, the embodiments of the present invention can be modified in various forms, and the scope of the present invention should not be interpreted as being limited by the experimental examples described below.

[0144] Example

[0145] Preparation Example

[0146] Preparation Example 1-Preparation of Adhesive Base Film Layer

[0147] Prepare 40g of solvent (MEK / EA). Add 11g of epoxy resin and 9g of phenolic resin curing agent to the solvent. The ratio of epoxy resin to phenolic resin curing agent is 1:1 based on equivalent weight. Stir the solution at 30RPM for 15 minutes using a stirrer to completely dissolve the solid epoxy resin and phenolic resin.

[0148] 80 g of solid content of elastomer resin was further added to the solution. The solution was stirred well at 30 RPM for 30 minutes using the same stirrer to form an epoxy resin / elastomer mixture.

[0149] 0.1 g of imidazole as a curing catalyst was aliquoted in a separate container, and then 10 g of a solvent (MEK / EA) was further added to completely dissolve.

[0150] Add the dissolved imidazole solution to the prepared epoxy / elastomer mixture. Stir the solution at 30 RPM for 15 minutes using the same stirrer.

[0151] The prepared solution was degassed using a vacuum pump and a vacuum dryer for 30 minutes to form a mixture. Thereafter, the mixture was filtered using a 250-300 mesh filter.

[0152] The filtered solution was coated on a PET liner, and both 50 μm thick surfaces of the liner were subjected to anti-adhesive treatment with silicone. Coating was performed on a tight anti-adhesive surface. Drying and curing were performed at 130° C. for 2 minutes, and the thickness of the coated film after drying was 25 μm. The coated film was wound in the form of a roll and prepared.

[0153] The prepared adhesive base film layer was aged in an aging oven at 45° C. for 4 days.

[0154] Preparation Example 2 - Preparation of Adhesive Layer

[0155] 80 g of solvent (toluene / xylene) was prepared. Benzoyl peroxide (BPO) (Pergan) was added to the solvent. The amount added was 3.5 wt % compared to the solid content of the free radical curable silicone resin added later. BPO was stirred at 10 RPM for 15 minutes using a stirrer to completely dissolve.

[0156] 100 g of silicone resin Q2-7406 (Dow Corning, 56.5 wt%) was added to the dissolved BPO solution and stirred again for 30 minutes in the same manner. The solution was degassed for 30 minutes using a vacuum pump and a vacuum dryer to form a mixture. Thereafter, the mixture was filtered using a 250-300 mesh filter.

[0157] The filtered solution was coated on the adhesive base film layer prepared in Preparation Example 1. After drying at 180° C. for 2 minutes, the filtered solution was coated to have a coated film thickness of 30 μm. After the coated film was dried, a fluorine-treated 50 μm release PET liner was bonded and then wound in a roll form for preparation.

[0158] Preparation Example 3-Preparation of light-to-heat conversion layer

[0159] 6 wt% of carbon black having a particle size of 240 nm (Cancarb), 4 wt% of titanium dioxide having a particle size of 240 nm (Huntsman), and 1 wt% of a dispersant (BYK Chemie Japan Co., Ltd.) were added to 75 wt% of methyl ethyl ketone (MEK, Samchun Chemical Co., Ltd.), and dispersed for 30 minutes using an ultrasonic disperser to prepare a solution in which a light absorber was dispersed. 7 wt % of a high molecular weight acrylic polymer elastomer replacing PSA having a weight average molecular weight of 1,000,000 g / mol and containing 10 mgKOH / g or more COOH / OH functional groups, and 7 wt % of a low molecular weight acrylic polymer elastomer replacing PSA having a weight average molecular weight of 500,000 g / mol and containing 5 mgKOH / g or more COOH / OH functional groups are mixed and stirred with a stirrer for 30 minutes to prepare a thermally decomposable resin. The thermally decomposable resin is added to the solution dispersed with a light absorber, and then stirred for another 20 minutes. Then, methyl ethyl ketone (MEK) is added so that the mixture has a viscosity suitable for coating (200 CPS to 5,000 CPS).

[0160] The solution was coated on the adhesive base film layer prepared in Preparation Example 1. However, the adhesive layer was coated on the opposite surface of the coated surface and the PET liner of the adhesive base film layer was removed before coating. After drying at 90° C. for 1 minute, the solution was coated to have a coated film thickness of 10 μm and dried.

[0161] Thereafter, the adhesive film was aged in an oven at 45° C. for 15 hours to complete the adhesive film.

[0162] Example

[0163] In Preparation Example 1, an adhesive film was prepared by applying the type and content of each component as shown in the following table. The components and content of each example are shown in Table 1 below.

[0164] [Table 1]

[0165]

[0166] *Indications are not the invention.

[0167] The materials used in the above table are as follows.

[0168] Multifunctional epoxy resin: YDCN-500-4P (KUKDO), YDCN-500-8P (KUKDO), KDCP-100 (KUKDO), KDCP-150 (KUKDO) and KDCP-200 (KUKDO).

[0169]

[0170] Bifunctional epoxy resin: YD-011 (Guodu Chemical), YD-012 (Guodu Chemical), YD-017 (Guodu Chemical)

[0171]

[0172] Crystalline epoxy resin: YX4000H (Mitsubishi Chemical Corporation), YSLV-80XY (Nippon Steel & Sumitomo Metal), or YSLV-120TE (Nippon Steel & Sumitomo Metal)

[0173]

[0174] Core-shell epoxy resin: MX-136 (Kaneka), MX-138 (Kaneka), B-tough-A3 (Croda), YP-50 (Kudo Chemical)

[0175] Curing agent (phenolic novolac resin): KPH-2001 (Kolon), TD2131 (DIC Corporation), MEH-7800-SS (MEIWA), MEH-7800-4S (MEIWA), MEH-800-SSKC (MEIWA)

[0176] Elastomer (Mw: 300,000 to 1,000,000): NBR (acrylonitrile 40%, Kumho Petrochemical), WS-023 (Nagase Chemtex), SG-708-6 (Nagase Chemical), SG-P3-TEA (Nagase Chemical)

[0177] Curing catalyst (imidazole): 2PZ-CN (Shikoku), 2PZ-PW (Shikoku), 2PHZ-PW (Shikoku)

[0178] Packing: CUSP03 (JoinM), CUSP05 (JoinM), Sterlling1120 (Cabot), Thermax N990 (Cancab), TR72 (Huntsman) and TR92 (Huntsman), R972, SO31R

[0179] Dispersants: BYK111 (BYK Japan Co., Ltd.), DISPERBYK-161 (BYK Japan Co., Ltd.), BYK2131 (BYK Japan Co., Ltd.), BYK2150 (BYK Japan Co., Ltd.), KD6 (Croda), KD8 (Croda), KD9 (Croda)

[0180] The experimental results of Examples 1 to 9 are shown in Table 2 below.

[0181] [Table 2]

[0182]

[0183] Referring to Table 2, in Example 1 where no binder resin is applied, it is confirmed that the epoxy resin alone is very brittle, difficult to coat, and cannot form a film by itself. In addition, even in the absence of a ratio of a multifunctional epoxy resin as in Example 9, the film is very brittle and does not form a film. In addition, in Examples 2 and 3 that do not include an epoxy resin, the chemical resistance is insufficient, and therefore, when the light-to-heat conversion layer is coated, the adhesive-based film layer dissolves. In addition, as in Example 7, it is confirmed that even if an epoxy resin is included, when the multifunctional epoxy resin is too little, the hardness of the epoxy resin is low, and therefore, the film does not have sufficient chemical resistance in a solvent such as methyl ethyl ketone (MEK).

[0184] On the other hand, referring to Examples 4 and 5, when a filler was additionally included, rigidity could be imparted to the film and shrinkage could be suppressed.

[0185] Although the embodiments according to the present invention have been described above, they are only examples, and those skilled in the art will appreciate that various modifications and equivalent embodiments may be implemented thereby. Therefore, the protection scope of the present invention should be understood to include not only the following claims, but also their equivalents.

[0186] Description of Figure Numbers

[0187] 110: first liner, 120: light-to-heat conversion layer, 130: adhesive base film layer, 140: adhesive layer, 150: second liner, 200: carrier, 300: substrate, 400: laser, 500: removal tape.

Claims

1. An adhesive film, comprising: an adhesive layer, the adhesive layer being a silicon-based adhesive layer; A light-to-heat conversion layer, the light-to-heat conversion layer comprising a light absorber and a thermally decomposable resin, wherein the thermally decomposable resin comprises an acrylic resin, the thickness of the light-to-heat conversion layer is 1 μm to 30 μm, the content of the light absorber is 5 wt % to 80 wt % based on the total weight of the light-to-heat conversion layer, and the content of the acrylic resin is 5 wt % to 80 wt % based on the total weight of the light-to-heat conversion layer; as well as an adhesive base film layer, the adhesive base film layer having a thickness of 10 μm to 50 μm and disposed between the adhesive layer and the light-to-heat conversion layer, The adhesive base film layer comprises a multifunctional epoxy resin, a binder resin, a curing agent and a curing catalyst, the binder resin has a weight average molecular weight of 500,000 to 1,500,000, and when the total weight of the multifunctional epoxy resin and the binder resin is 100 parts by weight, the content of the multifunctional epoxy resin is 30 parts by weight to 60 parts by weight, and the content of the binder resin is 40 parts by weight to 70 parts by weight, and The adhesive layer, the light-to-heat conversion layer, and the adhesive-based film layer are flexible layers, the multifunctional epoxy resin is a novolac epoxy resin or a dicyclopentadiene epoxy resin, and the binder resin is an elastomer resin. 2 . The adhesive film according to claim 1 , wherein the thermally decomposable resin comprises two acrylic resins having a —COOH or —OH functional group and different weight average molecular weights. 3 . The adhesive film according to claim 1 , wherein the adhesive base film layer has adhesion to both the adhesive layer and the light-to-heat conversion layer. The adhesive film according to claim 1 , wherein the curing agent is a phenolic curing agent. 5 . The adhesive film according to claim 1 , wherein the binder resin is an acryl-based or rubber-based elastomer resin. The adhesive film according to claim 1 , wherein the binder resin has an epoxy group in a chain. The adhesive film according to claim 1 , wherein the adhesive base film layer further comprises a filler. 8 . The adhesive film according to claim 7 , wherein the filler comprises at least one selected from the group consisting of TiO 2 , silica, copper powder, alumina, and carbon black. 9 . The adhesive film according to claim 1 , wherein the curing catalyst of the adhesive base film layer is imidazole.