Method for manufacturing SiC wafer with residual stress control

By using dopants to adjust stress during the silicon carbide wafer manufacturing process, the wafer warping problem is solved, and the stable production of large-size silicon carbide wafers and the manufacturing of electronic devices are achieved.

CN114561705BActive Publication Date: 2024-11-29STMICROELECTRONICS SRL
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111421201.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-11-29
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

Silicon carbide wafers have a tendency to warp during manufacturing, especially in large-sized wafers, which make them unable to be used to manufacture electronic devices.

Method used

By forming a first SiC layer in the same reaction chamber and growing a second SiC layer thereon, the dopant vapor phase precursor with different electrical conductivity is introduced into the reaction chamber to generate stresses of the relative stresses, thereby adjusting the residual stress of the wafer , ensure the flatness and stability of the wafer. The specific steps include forming a first SiC layer on the support, removing the support, and growing a second SiC layer on the first SiC layer, adjusting the stress by a CVD process and dopant injection.

Benefits of technology

The stable manufacturing of large-size silicon carbide wafers is achieved, warping is avoided, and the suitability and quality of the wafer is ensured, especially in wafers of 6 inches and above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114561705B_ABST
    Figure CN114561705B_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure relate to a method for manufacturing a SiC wafer with residual stress control. A method for manufacturing a SiC wafer includes the following steps: introducing a support into a reaction chamber; forming a first SiC layer on the support; separating the support from the first SiC layer; growing a second SiC layer on the first SiC layer, including introducing a vapor-phase precursor of a first dopant having a first conductivity into the reaction chamber to generate a first stress in the second SiC layer; and introducing a vapor-phase precursor of a second dopant having a second conductivity opposite to the first conductivity into the reaction chamber to generate a second stress in the second SiC layer, the second stress being opposite to the first stress and balancing the first stress. The SiC wafer is therefore free from the influence of warping.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a process for producing SiC wafers with residual stress control. Background Art

[0002] As is well known, semiconductor devices are usually manufactured using silicon wafers. However, silicon carbide wafers (SiC) have become increasingly popular, at least in part due to the favorable chemical and physical properties of SiC. For example, silicon carbide generally has a wider band gap than silicon. Therefore, even with a relatively small thickness, SiC has a higher breakdown voltage than silicon and can therefore be advantageously used in high voltage applications, such as power devices.

[0003] Silicon carbide can exist in different crystal forms or polytypes. The most common polytypes are the cubic polytype (3C-SiC polytype), the hexagonal polytype (4H-SiC and 6H-SiC polytypes) and the rhombohedral polytype (15R-SiC polytype). Of these, the 3C-SiC cubic polytype is currently the object of intensive research, thanks to its unique properties compared to other wafer polytypes. For example, in general, 3C-SiC wafers have a smaller trap density at the SiO2 / 3C-SiC interface and a greater channel electron mobility. Other properties that make 3C-SiC interesting include the on-resistance R on This is particularly useful for devices operating at 650V and above.

[0004] However, the manufacturing of silicon carbide wafers is more complicated than that of silicon wafers, and there are currently no 3C-SiC substrates on the market.

[0005] In particular, the applicant has found that silicon carbide wafers have a tendency to warp, which makes them practically unusable for the manufacture of electronic devices. This phenomenon is more pronounced in large-sized wafers, especially those with a size exceeding 6 inches. Summary of the invention

[0006] The present disclosure provides various embodiments of a production process or a manufacturing method for a silicon carbide wafer, which overcomes the disadvantages of the known technology and enables the manufacturing of silicon carbide wafers even of large sizes.

[0007] According to the present disclosure, a production process or a manufacturing method of a silicon carbide wafer is provided.

[0008] In at least one embodiment, a process for producing a silicon carbide (SiC) wafer performed in the same reaction chamber is provided, the method comprising: forming a first SiC layer on a support; separating the support from the first SiC layer; and growing a second SiC layer on the first SiC layer. Growing the second SiC layer comprises: introducing a precursor of a gas phase of a first dopant having a first conductivity into the reaction chamber to generate a first stress in the second SiC layer; and introducing a precursor of a gas phase of a second dopant having a second conductivity opposite to the first conductivity into the reaction chamber to generate a second stress opposite to the first stress in the second SiC layer; and at least partially removing the support from the seed SiC layer.

[0009] In at least one embodiment, a method is provided, the method comprising: forming a seed silicon carbide (SiC) layer on a substrate in a reaction chamber, the seed SiC layer having a thickness of less than 10 nm; at least partially removing the substrate from the first SiC layer; and forming a second SiC layer on the first SiC layer, the forming of the second SiC layer comprising: generating a first stress in the second SiC layer by introducing a vapor-phase precursor of a first dopant having a first conductivity into the reaction chamber; and generating a second stress opposite to the first stress in the second SiC layer by introducing a vapor-phase precursor of a second dopant having a second conductivity opposite to the first conductivity into the reaction chamber.

[0010] In at least one embodiment, a method includes: forming a seed silicon carbide (SiC) layer on a semiconductor substrate in a reaction chamber at a first temperature, the seed SiC layer having a first thickness; removing at least a portion of the semiconductor substrate from the first SiC layer by heating the reaction chamber to a second temperature higher than the first temperature, the second temperature being higher than a melting temperature of the semiconductor substrate and lower than a melting temperature of the first SiC layer; and forming a second SiC layer on the first SiC layer, the second SiC layer having a second thickness greater than the first thickness, the forming the second SiC layer including: generating a first stress in the second SiC layer by introducing a precursor in a gas phase of a first dopant having a first conductivity into the reaction chamber; and generating a second stress opposite to the first stress in the second SiC layer by introducing a precursor in a gas phase of a second dopant having a second conductivity opposite to the first conductivity into the reaction chamber. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] For a better understanding of the present disclosure, embodiments thereof will now be described, by way of non-limiting examples only, with reference to the accompanying drawings, in which:

[0012] Figures 1 to 6 An embodiment of a production process or a manufacturing process of a silicon carbide wafer, in particular a 3C-SiC wafer, is shown. DETAILED DESCRIPTION

[0013] Figure 1-3 The steps are of known type and are described here for completeness and to facilitate understanding of the present disclosure.

[0014] exist Figure 1-6 In the present invention, the production process or manufacturing method of the silicon carbide wafer is described with reference to an apparatus 10 for chemical vapor deposition (CVD) growth, which includes a reaction chamber 24, which defines a closed space, and the chemical reaction of the growth and doping of the SiC wafer is carried out in the closed space. The apparatus 10 includes a heater (not shown), an inlet conduit 16 and an outlet conduit 18. The apparatus 10 also includes a support 20 (also called a "base") and a container 22, which is, for example, cup-shaped. The support 20 and the container 22 are located inside the reaction chamber 24. The heater is configured to heat the reaction chamber 24 and the things contained inside the reaction chamber 24 (for example, the support 20, the container 22, the gas, the substrate, the wafer or other objects or substances). The inlet conduit 16 provides a fluid path from the environment outside the apparatus 10 toward the reaction chamber 24, and can be used to introduce precursors and gases into the reaction chamber 24. The outlet conduit 18 provides a fluid path from the reaction chamber 24 toward the outside of the apparatus 10. It can also be used to discharge the reaction gas formed in the reaction chamber 24 to the outside. The support 20 is arranged on the container 22 and in the reaction chamber 24. The support 20 constitutes a platform for receiving and holding a substrate or wafer within the reaction chamber 24. Specifically, as described below, a silicon substrate is arranged on the support 20 during the manufacture of a SiC wafer.

[0015] The above-mentioned type of device etc. can be implemented as described in US2018 / 090350, for example, which describes a base formed by a plurality of rods having an inclined shape or facing downward. In addition, patent document numbered US2020 / 144047 describes a device similar to device 10 and provided with a base that can be used to implement the present disclosure.

[0016] In detail, Figure 1 In the embodiment of the present invention, a substrate 58 of a first material (here a silicon substrate) is placed in the reaction chamber 24 and precisely located in the base 48 of the support 20. The substrate 58 is inserted into the base 48.

[0017] The substrate 58 has a thickness as small as possible to match the brittle characteristics. For example, the thickness of the substrate 58 may be at least 60-70 μm, in particular between 200 μm and 300 μm.

[0018] The substrate 58 generally has a crystalline structure. In addition, in this step, the reaction chamber 24 is at room temperature.

[0019] Once the substrate 58 is positioned in the support 20, the reaction chamber 24 is sealed and heated to a first temperature by a heater. For example, the first temperature may be between 450°C and 550°C. A first pressure level is also set inside the reaction chamber 24, for example, at 8.10 -5 Ba to 12.10 -5 Between Pakistan.

[0020] After the reaction chamber 24 has been heated to the first temperature, it is brought to a second temperature higher than the first temperature. For example, the second temperature may be between 1050° C. and 1150° C. A second pressure level higher than the first pressure level, for example between 75 mbar and 125 mbar, is also provided inside the reaction chamber 24 .

[0021] During the remainder of the process, reaction chamber 24 is maintained at the second pressure level.

[0022] After the reaction chamber 24 has been heated to the second temperature, the substrate 58 is immersed in hydrogen (H2). The hydrogen is introduced into the reaction chamber 24 through the inlet conduit 16. In addition, the substrate 58 is activated by introducing hydrochloric acid (HCl) into the reaction chamber 24 through the inlet conduit 16.

[0023] Then, the reaction chamber 24 is heated by the heater to a third temperature higher than the second temperature. For example, the third temperature is between 1340°C and 1400°C.

[0024] Reference again Figure 1 , when the reaction chamber 24 is brought to the third temperature or after it has reached the third temperature, a carbon-based precursor is introduced into the reaction chamber 24 through the inlet conduit 16. The carbon-based precursor carbonizes the surface silicon atoms of the substrate 58 to form a thin SiC layer, in particular a 3C-SiC layer. In one or more embodiments, the thin SiC layer has a thickness of less than 10 nm and in some embodiments is a few nanometers. This step is also referred to as "slope carbonization". As will be discussed below, the thin SiC layer acts as a seed for growing another thicker SiC layer (in particular a 3C-SiC polytype).

[0025] When the reaction chamber 24 is at the third temperature, the silicon-based precursor is added to the carbon-based precursor in the reaction chamber 24. Thus, the first SiC layer 60 begins to epitaxially grow from the thin SiC layer, such as Figure 2 This step is usually defined as “heteroepitaxial growth”. The first SiC layer 60 is the seed layer mentioned above.

[0026] Next, a melting process is performed. Specifically, the melting process is performed by maintaining the H2 flow in the reaction chamber 24 through the inlet conduit 16, and the reaction chamber 24 is heated by the heater to a fourth temperature, which is higher than or equal to the melting temperature of the substrate 58 and lower than the melting temperature of the first SiC layer 60. For example, the fourth temperature is between 1550°C and 1650°C. Therefore, Figure 3 As shown, the substrate 58 is melted (at Figure 3 66) and is deposited in the container 22 to be collected by the absorbent material 33 (e.g., a sponge material).

[0027] Reaction chamber 24 may be maintained at the fourth temperature until all of substrate 58 is removed from first SiC layer 60 or until a small or thin remnant portion 70 of substrate 58 remains on support 20 (remnant portion 70 of substrate 58 is then removed by an etching process).

[0028] exist Figure 4 In the process, the silicon and carbon-based precursors are introduced into the reaction chamber 24 through the inlet conduit 16. Then, the thickness of the first SiC layer 60 continues to grow or the second SiC layer 68 begins to grow on the first SiC layer 60 (for example, by a CVD process). This step is generally referred to as "homoepitaxial growth". The silicon and carbon-based precursors can be provided during the melting step of the substrate 58. Alternatively, the silicon and carbon-based precursors are provided after the melting process of the substrate 58 is completed.

[0029] When the second SiC layer 68 reaches the desired thickness, the flow of the silicon and carbon-based precursors is stopped. Any possible reaction gases in the reaction chamber 24 are removed from the reaction chamber 24 through the outlet conduit 18 .

[0030] refer to Figure 5 In the case where the SiC wafer contains residual portions 70 of the substrate 58, these can be removed by an etching process during or at the end of the growth of the second SiC layer 68. In this case, an etching chemical such as hydrochloric acid (HCl) (particularly in gaseous form) is introduced into the reaction chamber 24 via the inlet conduit 16, which serves to remove the residual portions 70, which are then exhausted from the reaction chamber 24 via the outlet conduit 18.

[0031] Thus, a SiC wafer 72 is obtained. The diameter of the SiC wafer 72 is between 2 inches and 12 inches, and in some embodiments, is equal to or substantially equal to 6 inches.

[0032] SiC wafer 72 may be used, for example, as a substrate for fabricating electronic devices (eg, by growing additional layers thereon and / or performing steps of dopant implantation and activation, photolithography, etc.).

[0033] According to one aspect of the present disclosure, Figure 4During the step of , doping of SiC layer 68 is performed during the CVD growth step. This aspect of the present disclosure is Figure 6 In the description, the Figure 6 Reappeared Figure 4 steps.

[0034] The doping here has the dual function of setting the desired value of the resistivity of the wafer 72 according to the subsequent steps of forming the electronic components, and adjusting the net stress value to which the SiC wafer 72 is subjected at the end of the manufacturing steps.

[0035] Specifically, in one embodiment of the present disclosure, the doping process of the second SiC layer 68 is performed by simultaneously providing two different dopant species in a CVD growth process, wherein one dopant species is N-type and one dopant species is P-type; for example, the dopant species is provided by aluminum atoms by using a gas phase precursor, such as using nitrogen (N2) for N-type doping, and using trimethylaluminum, TMA or Al2(CH3)6 for P-type doping.

[0036] The Applicant has found that by appropriately calibrating the concentrations of N and P dopants in the SiC wafer 72 (or equivalently, the doses of dopants or precursors introduced into the reaction chamber), it is possible to adjust the tensile and compressive stresses of the SiC wafer 72. In fact, the compressive and tensile stresses act in directions orthogonal to the plane defined by the surface of the SiC wafer 72 and tend to bend it in directions opposite to each other. The N-type doping performed by N2 enables the stress in the compressive direction to be adjusted (it acts in a first direction), while the P-type doping performed by TMA enables the stress in the tensile direction to be adjusted (it acts in a second direction, which is parallel to and opposite to the first direction).

[0037] The applicant has found that the desired stress balance can be obtained by introducing the precursors in the gas phase into the reaction chamber 24 at flow rates in sccm (standard cubic centimeters per minute) in the following proportions: Given a nitrogen flow rate equal to "x" sccm, selected according to the desired N-type doping to be obtained in the SiC wafer 72, the flow rate "y" of TMA is between 0.01% and 1% of the value of x. For example, considering an internal volume of about 2100 cm 3 For the reaction chamber 24, the value of x may be in the range of 500 to 1800 sccm, and the value of y may be in the range of 0.1 to 5 sccm, which are selected so as to conform to the above ratio.

[0038] Obviously, the flow rate values ​​expressed in sccm may vary depending on the size of the reaction chamber used and / or the desired dopant concentration at the SiC wafer 72 level.

[0039] In order to balance the stress of the wafer layer, the applicant has confirmed that the concentration of N-type dopant (N2) can be set at 10 18 Atom / cm 3 Up to 10 20 Atom / cm 3 The P-type dopant (Al) concentration can be set within the range of 10 17 Atom / cm 3 Up to 10 19 Atom / cm 3 More specifically, the applicant has demonstrated that it is possible to obtain a substantially flat wafer 72 having a 2·10 19 Atom / cm 3 Until June 10 19 Atom / cm 3 N-type dopant concentration in the range of 1.5·10 18 Atom / cm 3 Until July 10 18 Atom / cm 3 The stress balance using the above values ​​is particularly effective for 3C-SiC.

[0040] The concentration of the dopant can generally be varied depending on the electrical requirements of the wafer manufactured therefrom. For example, to obtain an N-type net doping of 10 18 Atom / cm 3 (For example, in 1×10 18 Up to 10×10 18 Atom / cm 3 The concentration of N dopant measured at the level of the wafer 72 is between 4·10 18 To 1.5·10 19 Atom / cm 3 and the concentration of dopant P (aluminum) measured at the wafer 72 level is higher than 10 17 Atom / cm 3 (e.g. 1.10 18 Atom / cm 3 ) and less than 10 19 Atom / cm 3 (For example, 8.10 18 Atom / cm 3 ).

[0041] In at least one embodiment, the above-described manufacturing process is performed in the same reaction chamber 24, in particular without removing the manufactured product (i.e., SiC wafer 72 and its intermediate product, which is formed by a stack of two or more of substrate 58, layer 60, and layer 68) from reaction chamber 24. Applicants have found that in the case where SiC wafer 72 (or its intermediate product) is removed from reaction chamber 24 during an intermediate step of manufacturing, there is a high risk of damage to SiC wafer 72 (or its intermediate product). In particular, if reference is made to Figures 2 to 4 If any stack formed is removed from reaction chamber 24 to perform the step of removing substrate 58 (e.g., using a delamination process), such stack is most likely to break or crack during the removal process. Figure 3 The process of melting the substrate 58 in the reaction chamber 24 is discussed, and if necessary, by referring to Figure 4 The etching step in question completes the process without the layers 60 and 68 being damaged and the resulting SiC wafer 72 showing no cracks or other physical damage.

[0042] Finally, it is evident that modifications and variations may be made to the apparatus and methods described and illustrated herein without departing from the scope of the present disclosure.

[0043] For example, the teachings of the present disclosure are also applicable to obtaining a net P-type doping on a SiC wafer by balancing the effects of stress by introducing N-type dopants.

[0044] Furthermore, for N-type doping, dopant species alternative to nitrogen, such as phosphorus (P), may be used; for P-type doping, dopant species alternative to aluminum, such as boron (B), may be used.

[0045] A method for manufacturing a silicon carbide, SiC, wafer can be summarized as comprising the following steps: introducing a support (20) into a reaction chamber (24); forming a first SiC layer (60) on the support (20); separating the support (20) from the first SiC layer (60); growing a second SiC layer (68) on the first SiC layer (60) until a desired thickness is reached, wherein the step of growing the second SiC layer (68) comprises at least partially and simultaneously performing the following operations: introducing a vapor-phase precursor of a first dopant having a first conductivity (N) into the reaction chamber (24) to generate a first stress in the second SiC layer (68); and introducing a vapor-phase precursor of a second dopant having a second conductivity (P) opposite to the first conductivity (N) into the reaction chamber (24) to generate a second stress opposite to the first stress in the second SiC layer (68).

[0046] The precursor of the first dopant may be nitrogen N2.

[0047] The precursor of the second dopant may be trimethylaluminum TMA.

[0048] The precursor of the second dopant may be introduced into the reaction chamber (24) at a flow rate (expressed in sccm) having a value between 0.01% and 1% of the flow rate (expressed in sccm) of the precursor of the first dopant.

[0049] The above precursor of the first dopant can be introduced into the reaction chamber (24) to generate a concentration of 10 18 Atom / cm 3 The first dopant of the order of 10 17 Atom / cm 3 Up to 10 19 Atom / cm 3 A second dopant between.

[0050] The first conductivity may be N-type, the second conductivity may be P-type, the first stress may be compressive, and the second stress may be tensile.

[0051] The step of forming the first SiC layer (60) may include at least partially simultaneously performing the following sub-steps: introducing the above-mentioned precursor of the first dopant in a gas phase into the reaction chamber (24); and introducing the above-mentioned precursor of the second dopant in a gas phase into the reaction chamber (24).

[0052] The material of the first layer and the second layer ( 60 ′, 60 ″) may be 3C—SiC.

[0053] The step of growing the second material may include performing CVD growth in the presence of the above-mentioned precursor of the first dopant and the above-mentioned precursor of the second dopant.

[0054] The wafer may have a diameter of 6 inches.

[0055] The various embodiments described above can be combined to provide other embodiments. Based on the above detailed description, these and other changes can be made to the embodiments. In general, in the appended claims, the terms used should not be interpreted as limiting the claims to the specific embodiments disclosed in the specification and claims, but should be interpreted as including all possible embodiments to which such claims are entitled and the full range of their equivalents. Therefore, the claims are not limited by this disclosure.

Claims

1. A process for producing silicon carbide SiC wafers performed in the same reaction chamber, include: forming a first SiC layer on the support member on the support member; separating the support member from the first SiC layer; as well as growing a second SiC layer on the first SiC layer, Wherein growing the second SiC layer comprises: introducing a vapor-phase precursor of a first dopant having a first conductivity into the reaction chamber to generate a first stress in the second SiC layer; introducing into the reaction chamber a vapor-phase precursor of a second dopant having a second conductivity opposite to the first conductivity to generate a second stress in the second SiC layer opposite to the first stress; and removing at least partially the support from the seed SiC layer, The first electrical conductivity is N-type, the second electrical conductivity is P-type, the first stress is compressive, and the second stress is tensile. 2 . The process according to claim 1 , wherein at least partially removing the support is performed by at least partially melting the support in the reaction chamber.

3. The process of claim 2, further comprising completely removing the support member by etching a remaining portion of the support member in the reaction chamber. 4 . The process of claim 2 , wherein melting is performed by heating the reaction chamber to a temperature equal to or greater than a melting temperature of the support and less than a melting temperature of the first SiC layer.

5. The process according to claim 1, in, The thickness of the second SiC layer is greater than that of the first SiC layer. The process of claim 1 , wherein the first SiC layer is a 3C-SiC layer.

7. The process of claim 1, wherein the second SiC layer is a 3C-SiC layer.

8. The process of claim 1, wherein the precursor of the first dopant is nitrogen (N 2 ).

9. The process of claim 1, wherein the precursor of the second dopant is trimethylaluminum (TMA).

10. The process of claim 1 , wherein the precursor of the second dopant is introduced into the reaction chamber at a flow rate, expressed in sccm, having a value between 0.01% and 1% of the flow rate, expressed in sccm, of the precursor of the first dopant.

11. The process of claim 1 , wherein the precursor of the first dopant is introduced into the reaction chamber to generate a concentration of the first dopant in the second SiC layer that is an order of magnitude greater than a corresponding concentration of the second dopant.

12. The process of claim 1 , wherein the precursor of the first dopant is introduced into the reaction chamber to generate a concentration of 2·10 19 Atom / cm 3 Until June 10 19 Atom / cm 3 The first dopant, and The precursor of the second dopant is introduced into the reaction chamber to generate a concentration of 1.5·10 18 Atom / cm 3 Until July 10 18 Atom / cm 3 The second dopant between.

13. The process according to claim 1, wherein the forming of the first SiC layer include: introducing the precursor of the first dopant in the gas phase into the reaction chamber; as well as The precursor of the second dopant in the vapor phase is introduced into the reaction chamber.

14. The process of claim 1, wherein for growing the first SiC layer, the precursor of the first dopant in gas phase and the precursor of the second dopant in gas phase are introduced into the reaction chamber simultaneously or during respective time intervals that at least partially overlap.

15. The process of claim 1, wherein for growing the second SiC layer, the precursor of the first dopant in gas phase and the precursor of the second dopant in gas phase are introduced into the reaction chamber simultaneously or during respective time intervals that at least partially overlap.

16. The process of claim 1, wherein the second SiC layer is grown include: CVD growth is performed in the presence of the precursor of the first dopant and the precursor of the second dopant.

17. The process of claim 1 wherein the wafer has a diameter of 6 inches.

18. The process of claim 1 wherein the support is a silicon substrate.

19. A method, include: forming a seed silicon carbide (SiC) layer on a substrate in a reaction chamber, the seed SiC layer having a thickness of less than 10 nm; at least partially removing the substrate from the first SiC layer; as well as Forming a second SiC layer on the first SiC layer, wherein forming the second SiC layer comprises: generating a first stress in the second SiC layer by introducing a vapor-phase precursor of a first dopant having a first conductivity into the reaction chamber; as well as generating a second stress opposite to the first stress in the second SiC layer by introducing into the reaction chamber a vapor-phase precursor of a second dopant having a second conductivity opposite to the first conductivity, The first electrical conductivity is N-type, the second electrical conductivity is P-type, the first stress is compressive, and the second stress is tensile.

Citation Information

Patent Citations

  • Apparatus for manufacturing a silicon carbide wafer

    US20180090350A1

  • Apparatus and method for manufacturing a wafer

    US20200144047A1

  • Method of manufacturing semiconductor device

    CN104465392A

  • Silicon carbide epitaxial wafer, and manufacturing method thereof

    JP2019151543A

  • Method for manufacturing a silicon carbide wafer and respective equipment

    US20130157448A1