A vertical structure ultraviolet light emitting diode and its preparation and mass transfer method
By designing vertical structure and epitaxial layer in ultraviolet light emitting diodes, combining electrochemical corrosion and metal hot press bonding methods, the problem of small application range and huge transfer area is solved, and the light extraction efficiency and application range are improved.
Patent Information
- Application Number
- CN202210201728.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-03-03
AI Technical Summary
The application range of existing ultraviolet light emitting diodes is small and the huge transfer area is limited, especially the power conversion efficiency of ultraviolet light emitting diodes with wavelengths less than 350nm is low, and the traditional huge transfer method cannot achieve the preparation of large-area vertical structures.
UV LED design with vertical structure, including substrate, buffer layer, current expansion layer, sacrificial layer, current barrier layer, UV LED array and bonded metal, is prepared by epitaxial structure and electrochemical corrosion methods, combined with metal hot pressing bonds Together, achieve huge transfers.
It improves light extraction efficiency, broadens the application range of ultraviolet light emitting diodes, realizes large-area vertical structure preparation and huge transfer, simplifies the process and reduces costs.
Smart Images

Figure CN114583030B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ultraviolet light emitting diodes, and in particular to a vertical structure ultraviolet light emitting diode and a preparation method and a mass transfer method thereof. Background Art
[0002] UV LEDs based on group III nitride semiconductor materials have a wide range of application needs in water disinfection, medical and health care, UV curing and phototherapy. UV LEDs are considered to be an ideal choice to replace traditional UV light sources such as mercury lamps due to their small size, easy integration, mercury-free and environmentally friendly, and adjustable emission wavelength.
[0003] However, the power conversion efficiency of UV LEDs with wavelengths less than 350nm is less than 10%, which seriously limits their widespread application. One of the main factors limiting power conversion efficiency is light extraction efficiency. In addition, the stripping technology used in the traditional mass transfer method cannot achieve large-area vertical structure UV LED mass transfer, and the existing bonding technology has problems such as complexity and high cost that need to be solved. Summary of the invention
[0004] The purpose of the present invention is to provide a vertical structure ultraviolet light emitting diode and its preparation and mass transfer method to solve the problems of small application range and limited mass transfer area of ultraviolet light emitting diodes in the prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] A vertically structured ultraviolet light emitting diode comprises a substrate, a buffer layer, a current spreading layer, a first current blocking layer, a sacrificial layer, a second current blocking layer, a plurality of ultraviolet LED arrays, a second bonding metal and a heterogeneous substrate arranged in sequence from bottom to top;
[0007] The ultraviolet LED array includes an LED target layer, a Pd electrode and a first bonding metal which are arranged in sequence from bottom to top; the LED target layer and the Pd electrode are deposited with a SiO2 layer.
[0008] Optionally, the LED target layer includes an n-type layer, an active region, an electron blocking layer, a p-type superlattice layer and a cap layer which are sequentially arranged from bottom to top.
[0009] A method for preparing a vertically structured ultraviolet light emitting diode, comprising:
[0010] A buffer layer, a current spreading layer, a first current blocking layer, a sacrificial layer, a second current blocking layer and an LED target layer are sequentially deposited on the surface of the substrate to obtain an epitaxial structure;
[0011] Etching an array pattern on the epitaxial structure to obtain an epitaxial array;
[0012] depositing a Pd electrode on the epitaxial array;
[0013] Depositing a SiO2 layer on the surface of the epitaxial structure including the Pd electrode;
[0014] Opening holes in the SiO2 layer of the epitaxial array to obtain an epitaxial array with holes;
[0015] depositing a first bonding metal on the epitaxial array of openings;
[0016] The epitaxial array after depositing the first bonding metal is bonded to a heterogeneous substrate to obtain a vertical structure ultraviolet light emitting diode.
[0017] Optionally, etching an array pattern on the epitaxial structure to obtain an epitaxial array specifically includes:
[0018] Performing patterning processing on the epitaxial structure by using photoresist to obtain a processed epitaxial structure;
[0019] An array pattern is etched on the processed epitaxial structure by a plasma method to obtain an epitaxial array; the etching depth reaches the n-type layer of the LED target layer.
[0020] Optionally, depositing a Pd electrode on the epitaxial array specifically includes:
[0021] Performing patterning processing on the epitaxial array by using photoresist to obtain a processed epitaxial array;
[0022] Etching the processed epitaxial array by a plasma method to form a pattern smaller than a single pattern of the array;
[0023] A Pd electrode is deposited on the pattern by electron beam evaporation.
[0024] Optionally, the step of opening holes in the SiO2 layer of the epitaxial array to obtain the epitaxial array with holes specifically includes:
[0025] Performing a patterning process on the SiO2 layer of the epitaxial array by using a photoresist to obtain a processed SiO2 layer of the epitaxial array;
[0026] A plasma method is used to open holes in the SiO2 layer of the processed epitaxial array to obtain an epitaxial array with holes.
[0027] Optionally, depositing a first bonding metal on the epitaxial array of openings specifically includes:
[0028] A first bonding metal is deposited on the epitaxial array of openings by electron beam evaporation.
[0029] Optionally, the step of bonding the epitaxial array after depositing the first bonding metal to a foreign substrate to obtain a vertically structured ultraviolet light emitting diode may also include:
[0030] Performing patterning on the n-type layer using a photoresist to obtain a processed n-type layer;
[0031] The processed n-type layer is etched by a plasma method to expose the sacrificial layer; the etching depth reaches the sacrificial layer.
[0032] Optionally, bonding the epitaxial array after depositing the first bonding metal to a foreign substrate to obtain a vertically structured ultraviolet light emitting diode specifically includes:
[0033] Depositing a second bonding metal on the foreign substrate by electron beam evaporation;
[0034] The epitaxial array after the first bonding metal is deposited and the heterogeneous substrate after the second bonding metal is evaporated are fixed by a fixture and placed in an oven for heating.
[0035] A method for mass transfer of vertically structured ultraviolet light emitting diodes, comprising:
[0036] The vertically structured ultraviolet light emitting diode prepared above is placed in an electrolytic cell device, and the sacrificial layer is corroded by an electrochemical etching method to release the epitaxial array, thereby obtaining an array device of vertically structured ultraviolet light emitting diodes.
[0037] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:
[0038] The present invention grows an epitaxial structure with a sacrificial layer on a substrate and prepares an ultraviolet light emitting diode array by a photolithography process, thereby obtaining an ultraviolet light emitting diode with a vertical structure, thereby improving the light extraction efficiency; at the same time, through a metal hot pressing bonding method combined with electrochemical corrosion stripping samples, a large-area mass transfer of ultraviolet light emitting diodes with a vertical structure can be achieved, which greatly broadens the application range of ultraviolet light emitting diodes with a vertical structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0040] Figure 1 A schematic diagram of the structure of a vertical structure ultraviolet light emitting diode provided by the present invention;
[0041] Figure 2 A schematic diagram of the epitaxial structure of a vertical ultraviolet light emitting diode provided by the present invention;
[0042] Figure 3 A schematic diagram of the epitaxial structure of a vertical structure ultraviolet light emitting diode provided by the present invention;
[0043] Figure 4 A flow chart of a method for preparing a vertical structure ultraviolet light emitting diode provided by the present invention;
[0044] Figure 5 It is a schematic diagram of electrochemical stripping in an embodiment of the present invention;
[0045] Figure 6 Schematic diagram of an array device of vertically structured ultraviolet light-emitting diodes after transfer in an embodiment of the present invention. DETAILED DESCRIPTION
[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] The purpose of the present invention is to provide a vertical structure ultraviolet light emitting diode and its preparation and mass transfer method to solve the problems of small application range and limited mass transfer area of ultraviolet light emitting diodes in the prior art.
[0048] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0049] Figure 1 The schematic diagram of the structure of the vertical ultraviolet light emitting diode provided by the present invention is as follows: Figure 1 As shown, a vertical structure ultraviolet light emitting diode includes a substrate, a buffer layer, a current spreading layer, a first current blocking layer, a sacrificial layer, a second current blocking layer, a plurality of ultraviolet LED arrays, a second bonding metal and a heterogeneous substrate arranged in sequence from bottom to top.
[0050] The ultraviolet LED array includes an LED target layer, a Pd electrode and a first bonding metal which are arranged in sequence from bottom to top; the LED target layer and the Pd electrode are deposited with a SiO2 layer.
[0051] In practical applications, the substrate, the buffer layer, the current spreading layer, the first current blocking layer, the sacrificial layer, the second current blocking layer and the LED target layer constitute an epitaxial structure, such as Figure 2 and Figure 3 As shown, the buffer layer is used to relieve the stress caused by lattice mismatch during the growth of the heterogeneous substrate; the current spreading layer is 4.25 μm and its doping concentration is 2.0×10 18 cm -3 , which is convenient for the expansion of current and provides the sacrificial layer with the current required for the reaction; the thickness of the sacrificial layer is 130nm and its doping concentration is 2.0×10 19 cm -3 , used to react with oxalic acid solution to peel off the LED target layer from the substrate; - -Al 0.5 Ga 0.5 N is used as the first current blocking layer and the second current blocking layer, and its doping concentration is 0.5×10 18 cm -3 , which is used to prevent the current from diffusing to the epitaxial structure, confine the current to the sacrificial layer, and accelerate the reaction rate.
[0052] The LED target layer includes an n-type layer, an active region, an electron blocking layer, a p-type superlattice layer and a cap layer which are arranged in sequence from bottom to top. In this embodiment, 730nm n-Al0.5Ga0.5N is used as the n-type layer to provide electron carriers; InGaN / AlGaN MQWs is used as the active region to determine the wavelength of the luminescence peak; 20-30nm Al0.75Ga0.25N is used as the electron blocking layer to block excess electrons from entering the p-type layer and improve the luminescence efficiency; 200nm p-AlGaN is used as the p-type superlattice layer to provide hole carriers; 20nm p-GaN is used as the cap layer to provide Ga vacancies, which helps to form ohmic contact with the electrode.
[0053] Figure 4 The flowchart of the method for preparing the vertical structure ultraviolet light emitting diode provided by the present invention is as follows: Figure 4 As shown, the method for preparing the vertical structure ultraviolet light emitting diode includes:
[0054] Step 401: depositing a buffer layer, a current spreading layer, a first current blocking layer, a sacrificial layer, a second current blocking layer and an LED target layer in sequence on the surface of a substrate to obtain an epitaxial structure.
[0055] In practical applications, the AlN / AlGaN superlattice nucleation layer (buffer layer) and current spreading layer are grown on the AlN / sapphire substrate (substrate) by MOCVD. 0.5 Ga 0.5 N is used as the current spreading layer, Si is doped, and the doping concentration is 2.0×10 18 cm-3 Next, the first current blocking layer, the sacrificial layer and the second current blocking layer are grown. The first current blocking layer is n - -Al 0.5 Ga 0.5 N, Si doping, doping concentration is 0.5×10 18 cm -3 , thickness is 240nm, heavily doped sacrificial layer (sacrificial layer) is n + -Al 0.37 Ga 0.63 N, Si doping, doping concentration is 2×10 19 cm -3 , with a thickness of 130nm and a second current blocking layer of n - -Al 0.5 Ga 0.5 N, Si doping, doping concentration is 0.5×10 18 cm -3 , with a thickness of 240nm, where the current blocking layer is used to limit the current and enhance the corrosion rate; finally, the LED target layer, n-Al 0.5 Ga 0.5 The N n-type layer is Si-doped with a doping concentration of 2.0×10 18 cm -3 ; The composition of the active region of InGaN / AlGaN MQWs is adjustable; the average Al concentration of the p-type superlattice layer p-AlGaN is 50%, and the Mg doping concentration is 7×10 19 ; The p-GaN cap layer is doped with Mg, and the Mg doping concentration is 3×10 19 .
[0056] Step 402: etching an array pattern on the epitaxial structure to obtain an epitaxial array.
[0057] In a specific implementation, the step 402 specifically includes:
[0058] A patterning process is performed on the epitaxial structure by using a photoresist to obtain a processed epitaxial structure.
[0059] The array pattern is etched on the treated epitaxial structure by a plasma method to obtain an epitaxial array; the etching depth is to the n-type layer n-Al of the LED target layer; 0.5 Ga 0.5 N.
[0060] In practical applications, the above-mentioned epitaxial structure is cleaned by a standard cleaning process, and a mask of an array pattern of any size and shape is designed. After spin coating of photoresist, exposure treatment is performed using a mask and ultraviolet photolithography technology, and the pattern is dried after development. Any array pattern is used as a mask and an array pattern is etched by a plasma etching (ICP) method to obtain an array pattern. In this embodiment, a circular array with a diameter of 80 μm and a pitch of 20 μm is finally obtained, and the etching depth is 0.4 to 0.6 μm.
[0061] Step 403: depositing a Pd electrode on the epitaxial array.
[0062] In a specific implementation, the step 403 specifically includes:
[0063] A patterning process is performed on the epitaxial array using photoresist to obtain a processed epitaxial array.
[0064] A plasma method is used to perform etching on the processed epitaxial array to form a pattern smaller than a single pattern of the array.
[0065] A Pd electrode is deposited on the pattern by electron beam evaporation.
[0066] An electrode array slightly smaller than the above-mentioned array pattern is obtained by secondary photolithography based on the above-mentioned circular array using an overlay process. The electrode array can also use masks of different shapes and sizes. In this embodiment, the final electrode array is a circular array with a diameter of 75μm and a spacing of 25μm. A 50nm Pd electrode is evaporated by electron beam evaporation (EBL) as a p-type electrode, and annealed at 550℃ for 1min to realize the preparation of a vertical structure light-emitting diode, which is convenient for subsequent electrical, thermal and other performance tests of the device.
[0067] Step 404: Deposit a SiO2 layer on the surface of the epitaxial structure including the Pd electrode.
[0068] In practical applications, 10-20 nm SiO2 is deposited on the entire epitaxial array surface using atomic layer deposition (ALD). 10-20 nm SiO2 is deposited on the entire epitaxial structure surface as an insulating layer to protect the sample, passivate the edge, and reduce device leakage.
[0069] Step 405: opening holes in the SiO2 layer of the epitaxial array to obtain an epitaxial array with holes.
[0070] In a specific implementation, the step 405 specifically includes:
[0071] The SiO2 layer of the epitaxial array is patterned by using photoresist to obtain the processed SiO2 layer of the epitaxial array.
[0072] A plasma method is used to open holes in the SiO2 layer of the treated epitaxial array to obtain an epitaxial array with holes. A small hole much smaller than the array pattern is opened in the SiO2 layer of the epitaxial array to expose the p-type electrode for easy deposition of bonding metal.
[0073] Step 406: Depositing a first bonding metal on the epitaxial array of openings.
[0074] In a specific implementation, the step 406 specifically includes:
[0075] A first bonding metal is deposited on the epitaxial array of openings by electron beam evaporation.
[0076] In actual applications, a window is opened on the surface of the SiO2 layer above the epitaxial array to expose the p-type electrode. In this embodiment, the window size is 10μm×10μm. After the window is opened, the photolithography process is used again to etch out an array pattern that overlaps with the device array. After patterning, the first bonding metal Ti / Au (10 / 300nm) is deposited using electron beam evaporation (EBL) to increase contact with the p-type electrode and facilitate the subsequent bonding process of the device to achieve mass transfer.
[0077] Step 407: Bonding the epitaxial array after depositing the first bonding metal to a foreign substrate to obtain a vertically structured ultraviolet light emitting diode.
[0078] In a specific implementation, the step 407, before further comprising:
[0079] The n-type layer is patterned by using a photoresist to obtain a processed n-type layer.
[0080] The treated n-type layer is etched by plasma method to expose the sacrificial layer. The etched pattern is larger than the array pattern and the etching depth reaches the sacrificial layer to enhance the conductivity of the sacrificial layer, protect the epitaxial structure and facilitate the subsequent mass transfer process.
[0081] In practical applications, after the first bonding metal is deposited, the photoresist is washed off, and the epitaxial array is used for overlay again. After the epitaxial structure is spin-coated with photoresist, a circular array mask with a diameter of 85 μm and a spacing of 15 μm and ultraviolet photolithography is used for exposure processing, and after development, it is dried. The pattern is used as a mask and a plasma etching (ICP) method is used to etch a table with a diameter of 85 μm and a spacing of 15 μm. The etching depth is 1.2 to 1.5 μm. At this time, the epitaxial structure is as follows Figure 3 shown.
[0082] In a specific embodiment, bonding the epitaxial array after depositing the first bonding metal to a foreign substrate to obtain a vertically structured ultraviolet light-emitting diode specifically includes:
[0083] The second bonding metal is deposited on the foreign substrate by electron beam evaporation.
[0084] The epitaxial array after the first bonding metal is deposited and the heterogeneous substrate after the second bonding metal is evaporated are fixed by a fixture and placed in an oven for heating.
[0085] In practical applications, electron beam evaporation (EBL) is used to evaporate the second bonding metal Ti / Au (10 / 300nm) on the foreign substrate. In this embodiment, Si is used as the foreign substrate. The epitaxial structure and the foreign substrate are fixed with a stainless steel clamp, and a bonding stress of 50MPa is applied. The structure is heated at 300℃ in an oven for 2h. The vertical structure ultraviolet light-emitting diode is finally obtained. Figure 1 shown.
[0086] The present invention also includes a method for mass transfer of vertically structured ultraviolet light-emitting diodes, which includes placing the vertically structured ultraviolet light-emitting diodes prepared above in an electrolytic cell device, utilizing the difference in conductivity of the epitaxial structure, adopting an electrochemical corrosion method, directionally corroding the sacrificial layer, releasing the epitaxial array, and obtaining an array device of vertically structured ultraviolet light-emitting diodes, thereby realizing mass transfer of vertically structured ultraviolet light-emitting diodes.
[0087] In practical applications, vertically structured ultraviolet light-emitting diodes are stripped and transferred by electrochemical corrosion. The electrolytic cell device includes a constant voltage source and a reaction electrolytic cell, wherein the epitaxial structure sample is used as the anode, the platinum sheet electrode is used as the cathode, the electrolyte is 0.3Mol / L oxalic acid solution, the voltage is 10V, the corrosion time is 1 to 2 hours, and the spin-coated silver paste is used as the contact electrode of the epitaxial wafer. During the corrosion process, the epitaxial structure is immersed in the oxalic acid solution as much as possible, and the cathode is the platinum sheet. The reaction schematic diagram is shown in FIG. Figure 5 shown.
[0088] After electrochemical corrosion, the vertically structured ultraviolet light-emitting diodes were cleaned with deionized water to remove the oxalic acid solution remaining on the surface of the vertically structured ultraviolet light-emitting diodes, thereby achieving mass transfer of the ultraviolet light-emitting diodes.
[0089] like Figure 6 As shown, a photolithography process is used to plate an n-type electrode on the transferred array device, and an overlay process is used to photolithography the required n-type electrode array pattern on the top of the peeled array. After patterning, Al / Ti / Au (100 / 20 / 30nm) is evaporated using electron beam evaporation (EBL), and vacuum annealing is performed at 550°C to form an ohmic contact to facilitate vertical current injection.
[0090] In the prior art, the power conversion efficiency of ultraviolet light-emitting diodes with a wavelength less than 350nm is less than 10%, which seriously limits their widespread application. One of the main factors limiting the power conversion efficiency is the light extraction efficiency. The present invention proposes a method to improve this efficiency through a thin film flip chip design. By designing an epitaxial layer with a special structure, utilizing the conductivity difference between the epitaxial structures, and using a specific electrochemical stripping method, the ultraviolet LED device substrate can be removed, a vertical structure ultraviolet light-emitting diode can be prepared, vertical current injection and surface roughening can be achieved, and the light extraction efficiency can be improved.
[0091] The present invention adopts a unique process, adopts the MOCVD method to grow an epitaxial structure with a sacrificial layer, uses a photolithography process to prepare an ultraviolet light-emitting diode array, and uses an electrochemical corrosion method to prepare a vertical structure ultraviolet light-emitting diode; at the same time, through the metal hot pressing bonding method, combined with electrochemical corrosion to peel off the sample, it is possible to achieve a mass transfer of vertical structure ultraviolet light-emitting diodes, which greatly broadens the scope of use of ultraviolet light-emitting diodes. At the same time, since the composition of the target layer is adjustable, the wavelength range of the ultraviolet light-emitting diode is adjustable, the shape and size of the array are adjustable, and the selection range of heterogeneous substrates is wide, it has very excellent characteristics in terms of device heat dissipation, current injection, etc., which greatly improves the scope of application of the method. The present invention is simple to operate, low in cost, and highly repeatable, and has broad application prospects in the development, heterogeneous integration, and mass transfer of semiconductor ultraviolet light-emitting diodes.
[0092] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0093] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A vertical structure ultraviolet light emitting diode, characterized in that: The device comprises a substrate, a buffer layer, a current spreading layer, a first current blocking layer, a sacrificial layer, a second current blocking layer, a plurality of ultraviolet LED arrays, a second bonding metal and a heterogeneous substrate which are sequentially arranged from bottom to top; The ultraviolet LED array comprises an LED target layer, a Pd electrode and a first bonding metal arranged in sequence from bottom to top; the LED target layer and the Pd electrode are deposited with a SiO2 layer; The LED target layer comprises an n-type layer, an active region, an electron blocking layer, a p-type superlattice layer and a cap layer which are sequentially arranged from bottom to top.
2. A method for preparing a vertically structured ultraviolet light-emitting diode, characterized in that: The method for preparing the vertical structure ultraviolet light emitting diode comprises: A buffer layer, a current spreading layer, a first current blocking layer, a sacrificial layer, a second current blocking layer and an LED target layer are sequentially deposited on the surface of the substrate to obtain an epitaxial structure; Etching an array pattern on the epitaxial structure to obtain an epitaxial array; depositing a Pd electrode on the epitaxial array; Depositing a SiO2 layer on the surface of the epitaxial structure including the Pd electrode; Opening holes in the SiO2 layer of the epitaxial array to obtain an epitaxial array with holes; depositing a first bonding metal on the epitaxial array of openings; The epitaxial array after depositing the first bonding metal is bonded to a foreign substrate to obtain the vertical structure ultraviolet light emitting diode as claimed in claim 1.
3. The method for preparing a vertically structured ultraviolet light emitting diode according to claim 2, characterized in that: The etching of an array pattern on the epitaxial structure to obtain an epitaxial array specifically includes: Performing patterning processing on the epitaxial structure by using photoresist to obtain a processed epitaxial structure; An array pattern is etched on the processed epitaxial structure by a plasma method to obtain an epitaxial array; the etching depth reaches the n-type layer of the LED target layer.
4. The method for preparing a vertically structured ultraviolet light emitting diode according to claim 3, characterized in that: The depositing of the Pd electrode on the epitaxial array specifically comprises: Performing patterning processing on the epitaxial array by using photoresist to obtain a processed epitaxial array; Etching the processed epitaxial array by a plasma method to form a pattern smaller than a single pattern of the array; A Pd electrode is deposited on the pattern by electron beam evaporation.
5. The method for preparing a vertically structured ultraviolet light emitting diode according to claim 2, characterized in that: The step of opening holes in the SiO2 layer of the epitaxial array to obtain an epitaxial array with holes specifically includes: Performing a patterning process on the SiO2 layer of the epitaxial array by using a photoresist to obtain a processed SiO2 layer of the epitaxial array; A plasma method is used to open holes in the SiO2 layer of the processed epitaxial array to obtain an epitaxial array with holes.
6. The method for preparing a vertically structured ultraviolet light emitting diode according to claim 2, characterized in that: The step of depositing a first bonding metal on the epitaxial array of the openings specifically comprises: A first bonding metal is deposited on the epitaxial array of openings by electron beam evaporation.
7. The method for preparing a vertically structured ultraviolet light emitting diode according to claim 3, characterized in that: The method further comprises bonding the epitaxial array after depositing the first bonding metal to a heterogeneous substrate to obtain a vertically structured ultraviolet light-emitting diode, and the method further comprises: Performing patterning on the n-type layer using a photoresist to obtain a processed n-type layer; The processed n-type layer is etched by a plasma method to expose the sacrificial layer; the etching depth reaches the sacrificial layer.
8. The method for preparing a vertically structured ultraviolet light emitting diode according to claim 2, characterized in that: The step of bonding the epitaxial array after depositing the first bonding metal to a foreign substrate to obtain a vertically structured ultraviolet light emitting diode specifically includes: Depositing a second bonding metal on the foreign substrate by electron beam evaporation; The epitaxial array after the first bonding metal is deposited and the heterogeneous substrate after the second bonding metal is evaporated are fixed by a fixture and placed in an oven for heating.
9. A method for mass transfer of vertically structured ultraviolet light emitting diodes, characterized in that: include: The vertical structure ultraviolet light emitting diode prepared by the preparation method of the vertical structure ultraviolet light emitting diode described in any one of claims 2-8 is placed in an electrolytic cell device, and the sacrificial layer is corroded by an electrochemical corrosion method to release the epitaxial array to obtain an array device of the vertical structure ultraviolet light emitting diode.