Method and equipment for the rhythmic deposition of perovskite thin films

By employing an alternating deposition and pause method, the problem of insufficient diffusion of AX material in perovskite thin film preparation was solved, enabling highly reliable and repeatable continuous large-area production and forming high-quality ABX3 thin films.

CN114583060BActive Publication Date: 2026-11-17HANGZHOU MICROQUANTA SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202011387375.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-01
Publication Date
2026-11-17
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

In the prior art, the continuous deposition method of perovskite thin films is not suitable for the preparation of vapor phase perovskite thin films. This results in the inability of AX material to fully enter the interior of BX2 material for reaction, and the formed perovskite thin film has problems such as BX2 residue or AX excess, abnormal stoichiometry, and lattice distortion.

Method used

The perovskite thin film rhythmic deposition production method is adopted. By alternating deposition and pause, the precursor AX material is gradually diffused into the precursor BX2 film to fully react and form the ABX3 film. The rhythmic deposition production equipment is used to achieve continuous large-area production.

Benefits of technology

This improves reaction speed and reliability, ensures high repeatability of perovskite films, and facilitates continuous large-area production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114583060B_ABST
    Figure CN114583060B_ABST
Patent Text Reader

Abstract

This invention relates to a rhythmic deposition method and equipment for perovskite thin films, comprising: placing a substrate containing a pre-prepared perovskite precursor BX2 film into a deposition reaction chamber to evaporate and deposit the precursor AX material; pausing the deposition process after a certain time to allow sufficient time for the AX material deposited on the surface of the precursor BX2 film to diffuse into the film and form perovskite ABX3 crystals; repeating the deposition process after a pause; and repeating this alternating deposition and pause process multiple times to ensure that the AX material penetrates the interior of the BX2 film and reacts fully with it, resulting in ABX3 perovskite crystals with no BX2 material residue or abundant AX material. The rhythmic deposition process continues until a perovskite ABX3 film of a predetermined thickness is obtained. This invention also discloses equipment for using this method. This invention enables continuous large-area production of perovskite thin films and features high reliability and repeatability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of perovskite solar cell module preparation technology, and specifically relates to a method and equipment for rhythmic deposition of perovskite thin films. Background Technology

[0002] The light-absorbing layer in a perovskite solar cell structure is a film formed from organometal halide perovskite materials. The forming processes for this film are mainly divided into two categories: solution methods and vapor-phase methods. Solution methods are simple in terms of both methods and equipment, and have made some progress in large-area fabrication. However, due to the extremely high requirements for solution formulation and the complex and difficult-to-control crystallization process during the transformation of the solution into a solid film, it is easily affected by the external environment, resulting in poor process repeatability. Therefore, further in-depth research is needed before it can be applied on a large scale in production. Vapor-phase methods mainly include dual-source co-evaporation and chemical vapor deposition. Because perovskite films prepared by vapor-phase methods have good crystal quality, uniformity, and controllable performance, they can be mass-produced and therefore have great potential in the industrialization of perovskite solar cells. They have already been widely used in the industrial production of traditional thin-film solar cells, such as copper indium gallium selenide (CIGS) and cadmium telluride (CdTe) thin-film solar cells. In addition, another method suitable for the fabrication of perovskite solar cells is the solution-assisted vapor phase method. This method combines the solution method with the vapor phase method, which takes advantage of the convenience of the solution method while retaining the high quality of the uniform thin film of the vapor phase method.

[0003] In traditional vapor-phase deposition processes for thin-film solar cells, the deposition of the coating material is continuous. Generally, the deposition module enters the deposition area via a conveyor, where the coating material is continuously deposited. After the deposition reaction is complete, it is removed by the conveyor. However, this process is not suitable for the preparation of perovskite thin films via vapor-phase deposition, especially for solution-assisted vapor-phase deposition. The main reason is that in the perovskite formation process using solution-assisted vapor-phase deposition, a BX2 thin film is typically formed first. Then, AX vapor is obtained through evaporation, reaching the surface of the BX2 film and diffusing into BX2 to react and form ABX3. During this process, after AX reaches the BX2 surface, two kinetic processes occur: diffusion and reaction. These two processes are interdependent; for AX to fully react with BX2, these two kinetic processes must be carefully balanced. However, if the AX material is continuously evaporated, due to the unique properties of AX material vapor, it cannot fully penetrate into the internal reaction of the BX2 material, resulting in the formation of a dense perovskite on the surface of BX2. Consequently, the formed perovskite film either contains BX2 material residue deep within it (because the AX material cannot diffuse in), or has an excess of AX material on its surface. Therefore, we propose an intermittent deposition method that effectively solves this problem, allowing AX to fully penetrate into the internal reaction of BX2.

[0004] The lateral uniform growth of perovskite crystals is intermittent. Continuous deposition of the corresponding material can lead to overgrowth or abnormal stoichiometry, which does not conform to the stoichiometry of perovskite ABX3 type materials, causing problems such as lattice distortion and deformation. Therefore, it is necessary to control the rhythm of the deposition process. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a method and equipment for the rhythmic deposition of perovskite thin films, which enables continuous large-area production of perovskite thin films and has the characteristics of high reliability and repeatability.

[0006] This invention is achieved by providing a method for rhythmic deposition of perovskite thin films, comprising the following processes: The substrate to be deposited, which has been pre-prepared with a BX2 precursor thin film containing perovskite precursor material, is placed in the deposition reaction chamber to evaporate and deposit the precursor material AX. The deposition continues for a certain period of time and then pauses, allowing sufficient time for the precursor material AX deposited on the surface of the precursor BX2 thin film to diffuse into the precursor BX2 thin film and form perovskite ABX3 crystals. After pausing for a period of time, the deposition is carried out again. This process of deposition and pausing is repeated rhythmically and repeatedly, allowing the AX material to enter the interior of the BX2 thin film and react fully with the BX2 material, thereby obtaining ABX3 perovskite crystals with no BX2 material residue or with excess AX material. The deposition duration and pausing time are preset until a perovskite ABX3 thin film of the set thickness is obtained, at which point the rhythmic deposition process ends. Among them, precursor BX2 is a metal halide material, precursor AX is an organohalide powder material, and A is a methylamino group CH3NH3. + , Ethylamino group CH3CH2NH3 + , Methamidinyl CH(NH2)2 + Ethylamidinyl CH3C(NH2)2 + Na + K + 、Rb + and Cs + The cation is any one of the monovalent cations, B is any one of the divalent metal cations of lead, tin, tungsten, copper, zinc, gallium, germanium, arsenic, selenium, rhodium, palladium, silver, cadmium, indium, antimony, osmium, iridium, platinum, gold, mercury, thallium, bismuth, and polonium, and X is any one of the monovalent anions of iodine, bromine, chloride, and astatine.

[0007] This invention is implemented as follows, and also provides a perovskite thin film rhythmic deposition production equipment, including a deposition reaction chamber. The deposition reaction chamber has two types of functional zones: a deposition functional zone and a reaction functional zone. The deposition functional zone includes one or more deposition sections, each containing at least two consecutively arranged unit deposition stations. An evaporation source is provided in each unit deposition station, and the precursor AX material powder to be evaporated is placed in the evaporation source. The reaction functional zone includes one or more reaction sections, each containing at least two consecutively arranged unit reaction stations. No evaporation source is provided in each unit reaction station. The deposition sections and reaction sections are spaced apart from each other. The deposition reaction chamber is connected to a vacuum pump via a pipeline. A heating device is also provided in the deposition reaction chamber for heating the substrate to be deposited, on which a pre-prepared perovskite precursor BX2 thin film containing BX2 material has been prepared. Among them, precursor BX2 is a metal halide material, precursor AX powder is an organohalide powder material, and A is a methylamino group CH3NH3. + , Ethylamino group CH3CH2NH3 +, Methamidinyl CH(NH2)2 + Ethylamidinyl CH3C(NH2)2 + Na + K + 、Rb + and Cs + The cation is any one of the monovalent cations, B is any one of the divalent metal cations of lead, tin, tungsten, copper, zinc, gallium, germanium, arsenic, selenium, rhodium, palladium, silver, cadmium, indium, antimony, osmium, iridium, platinum, gold, mercury, thallium, bismuth, and polonium, and X is any one of the monovalent anions of iodine, bromine, chloride, and astatine.

[0008] This invention is implemented as follows, and also provides a method for depositing perovskite thin films on substrates using the perovskite thin film rhythmic deposition production equipment as described above, comprising the following steps: Step 1: Add precursor AX powder material to the evaporation source of each deposition station in the deposition reaction chamber, adjust the vacuum degree of the deposition reaction chamber, and start the heating device. Step 2: Place the substrate to be deposited, which has been pre-prepared with a BX2 precursor film containing perovskite precursor material, into the sample loading chamber and transfer it into the deposition reaction chamber. The substrate to be deposited passes through the deposition station and the reaction station in sequence, and finally, a perovskite ABX3 film with complete reaction is obtained on the substrate.

[0009] Compared with the prior art, the rhythmic deposition production method and equipment for perovskite thin films of the present invention adopts an alternating arrangement of deposition and reaction stations when depositing precursor AX material on the surface of precursor BX2 thin film. This allows the precursor AX material to gradually diffuse into the precursor BX2 thin film for full reaction, generating perovskite ABX3 thin film. This not only improves the reaction speed but also has high reliability and repeatability, facilitating continuous large-area production of perovskite thin films. Attached Figure Description

[0010] Figure 1 This is a schematic diagram showing the relationship between the thickness of the perovskite formed by the reaction and the reaction kinetic coefficient. Figure 2 This is a schematic diagram of the structural principle of the perovskite thin film rhythmic deposition production method and equipment of the present invention, Example 1; Figure 3 for Figure 1 Cross-sectional view of the evaporation crucible; Figure 4 This is a schematic diagram of the structural principle of Example 2 of the perovskite thin film rhythmic deposition production method and equipment of the present invention; Figure 5 This is a schematic diagram of the structural principle of Example 3 of the perovskite thin film rhythmic deposition production method and equipment of the present invention. Detailed Implementation

[0011] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.

[0012] A preferred embodiment of the rhythmic deposition method for producing perovskite thin films of the present invention includes the following processes: A substrate containing a pre-prepared BX2 precursor film is placed in a deposition chamber to evaporate and deposit the AX precursor material. Deposition continues for a certain time, then pauses to allow sufficient time for the AX precursor material deposited on the BX2 film surface to diffuse into the film and form ABX3 perovskite crystals. After a pause, deposition resumes. This alternating deposition and pause process is repeated rhythmically to ensure the AX material penetrates the BX2 film and reacts fully with it, resulting in ABX3 perovskite crystals with no BX2 residue or abundant AX material. The deposition duration and pause times are preset until a perovskite ABX3 film of the desired thickness is obtained, at which point the rhythmic deposition process ends.

[0013] Among them, precursor BX2 is a metal halide material, and precursor AX is an organohalide powder material; A is methylamino group CH3NH3. + , Ethylamino group CH3CH2NH3 + , Methamidinyl CH(NH2)2 + Ethylamidinyl CH3C(NH2)2 + Na + K + 、Rb + and Cs + The cation is any one of the monovalent cations, B is any one of the divalent metal cations of lead, tin, tungsten, copper, zinc, gallium, germanium, arsenic, selenium, rhodium, palladium, silver, cadmium, indium, antimony, osmium, iridium, platinum, gold, mercury, thallium, bismuth, and polonium, and X is any one of the monovalent anions of iodine, bromine, chloride, and astatine.

[0014] The prepared perovskite ABX3 thin film has a thickness of 100 nm to 1000 nm. Both deposition and pause processes are performed in a vacuum environment with a vacuum level of 1 Pa to 50000 Pa. The evaporation temperature of the precursor AX material is 80 °C to 300 °C.

[0015] The present invention also discloses a perovskite thin film rhythmic deposition production equipment, which adopts the perovskite thin film rhythmic deposition production method as described above.

[0016] Please refer to Figure 2As shown, the perovskite thin film rhythmic deposition production equipment of the present invention includes a sample inlet chamber 1, a heating chamber 2, a deposition reaction chamber 3, and a sample outlet chamber 4, as well as a transport device for conveying the substrate 5 to be deposited. The transport device includes rollers 6 driven by a servo motor. The rollers 6 are evenly spaced, with the spacing not exceeding half the length of the long side of the substrate 5 to be deposited. The rollers 6 drive the support rollers, and the substrate 5 to be deposited is placed on the support rollers with the deposition surface facing down and moves on the support rollers.

[0017] The sample inlet chamber 1 and the heating chamber 2 are sequentially arranged at the front of the deposition reaction chamber 3, while the sample outlet chamber 4 is arranged at the rear of the deposition reaction chamber. The transmission device sequentially connects the sample inlet chamber 1, the heating chamber 2, the deposition reaction chamber 3, and the sample outlet chamber 4. After the deposition substrate 5 enters the sample inlet chamber 1, it passes through the heating chamber 2 and the deposition reaction chamber 3 sequentially via the transmission device, and finally exits from the sample outlet chamber 4.

[0018] The deposition reaction chamber 3 is equipped with two functional zones: a deposition zone and a reaction zone. The deposition zone includes one or more deposition sections, each containing at least one unit deposition station E. An evaporation source is located at each deposition station E, and the precursor AX material powder to be evaporated is placed in the evaporation source. The reaction zone includes one or more reaction sections, each containing at least one unit reaction station F. No evaporation source is located at each reaction station F. The deposition sections and reaction sections are spaced apart from each other. The deposition reaction chamber 3 is connected to a vacuum pump (not shown in the figure) via a pipeline. A heating device 7 is also provided in the deposition reaction chamber 3 to heat the substrate 5 to be deposited, on which a pre-prepared perovskite precursor BX2 thin film has been prepared.

[0019] A thin film detection device 8 is installed at some unit reaction stations F to track the thin film reaction process in real time. This device 8 includes one or a combination of several types, such as an imaging detection system, a UV-Vis spectrophotometer, a photoluminescence (PL) system, and an X-ray diffraction (XRD) system, to monitor the perovskite thin film reaction process in real time, thereby adjusting the opening and closing of the evaporation source in the remaining deposition stage. A double-opening baffle is installed at the evaporation source opening in the latter half of the deposition reaction chamber 3, allowing software control of the opening and closing of the evaporation source, thus regulating the perovskite thin film reaction process. The thin film detection device 8 can be installed at proportional intervals of 50%, 75%, and 100% within the deposition reaction chamber 3.

[0020] Please refer to the appendix. Figure 3As shown in the top view of the evaporation source, the evaporation source includes an evaporation crucible 9 with its opening facing upwards. The size of the evaporation crucible 9 matches the space of the evaporation source mounting slot. The evaporation crucible 9 includes an outer heat insulation layer 91, a middle heating layer 92, and an inner heat-conducting layer 93. A heating power cable 94 is provided on the heating layer 92 for connection to an external power interface. The inner heat-conducting layer 93 is preferably made of graphite. The middle heating layer 92 is typically a resistance heating layer. The power interface extends through the heat insulation layer 91 and can be connected to the power interface in the evaporation source mounting slot.

[0021] Please continue to refer to the appendix. Figure 2 As shown, after the perovskite precursor BX2 material is deposited to form a precursor BX2 film, the precursor BX2 film needs to enter a certain vacuum environment. The vacuum degree in the deposition reaction chamber 3 is 1 Pa to 50000 Pa. Then, the precursor AX material is heated (heating temperature range: 80℃ to 300℃) to form its vapor, which is deposited onto the precursor BX2 film and reacts to form a perovskite ABX3 film. The precursor AX material is placed in the evaporation crucible 9. This deposition and reaction process needs to be alternated, i.e., deposition for a while - reaction for a while - deposition for a while - reaction for a while. During deposition, the area under the substrate 5 is where the precursor AX material is placed in the evaporation crucible 9, while during the reaction, the area under the substrate 5 is where the evaporation crucible 9 is not. Therefore, in the direction of linear movement of the substrate 5, the evaporation crucibles 9 are arranged alternately, with some stations having evaporation crucibles 9 and others not. In the traditional perovskite coating process, the coating process is continuous.

[0022] The evaporation source used in this invention is a detachable evaporation source, which can be installed in the corresponding evaporation source mounting tank according to the needs of rhythmic production, serving as the material deposition section. The workstations without evaporation sources are used as material reaction sections. The most basic rhythmic production method is to alternately set up the deposition section and the reaction section at equal intervals. The entire deposition reaction chamber 3 is controlled by a vacuum regulation system consisting of a vacuum gauge, a vacuum pump, and a gas supply pipeline to control the required gas pressure. An upper heating device 7 is installed on the top of each evaporation source mounting tank to maintain the temperature during the perovskite crystallization reaction.

[0023] The length of the unit deposition station E is L. di =v*t d / n, the length L of the unit reaction station F ri =v*t r / m, where v is the moving speed (cm / s) of the substrate to be deposited. t d The deposition time (s) required to form a good perovskite film, t rThe reaction time (s) required to form a good perovskite thin film, t d :t r =1:0.5~1:100, n is the number of unit deposition sites. m represents the number of unit reaction stations.

[0024] Specifically, the lengths of the deposition section and the reaction section of the deposition reaction chamber 3 decrease sequentially along the front and rear directions of the deposition reaction chamber 3, or it can be described as the number of unit workstations included in the deposition section and the reaction section decreasing sequentially along the front and rear directions, that is, the lengths of the deposition section and the reaction section located in the front section of the deposition reaction chamber 3 are greater than the lengths of the deposition section and the reaction section located in the rear section of the deposition reaction chamber 3.

[0025] The above setup is based on the following principle: In the actual production of perovskite thin films, if deposition and reaction are only exchanged once, severe over-deposition and incomplete reaction may occur, affecting the yield and repeatability of the process. Therefore, a better solution is to use a repeated, uniformly alternating arrangement. This design breaks down the excessively long deposition and reaction functional areas into several small, spaced deposition and reaction sections. This arrangement allows a small amount of reactant to be deposited on the substrate 5 each time, enabling rapid reaction. This significantly reduces the amount of reactant deposited on the substrate 5 each time it passes through a deposition section (the deposition amount in each section is 1 / n of the previous amount). According to the principles of reaction kinetics, this promotes faster reaction of the reactants as they pass through the reaction section, reducing over-deposition or incomplete reaction and improving the yield and repeatability of the process. Furthermore, since each reaction and deposition section has its own independent heating device, this arrangement allows for independent temperature control of each section, or even shutting off heating in certain areas, based on the actual reaction conditions, making the reaction more consistent with reality.

[0026] On the other hand, according to the principles of reaction kinetics, the reaction rate slows down as reactants are generated, such as... Figure 1 As shown. In this case, the arrangement design can be adjusted accordingly, so that the length of the station located at the front of the deposition reaction chamber 3 is greater than the length of the station located at the rear of the deposition reaction chamber 3.

[0027] Specifically, in the perovskite thin film rhythmic deposition production equipment of the present invention, the gas pressure of the deposition reaction chamber 3 is controlled between 1 Pa and 50000 Pa, the temperature of the heating chamber 2 is set between 100°C and 400°C, the temperature of the evaporation source is controlled between 80°C and 300°C, the temperature of the heating device 7 is controlled between 50°C and 250°C, and the speed of the roller 6 is adjustable in the range of 1 mm / s to 400 mm / s.

[0028] This invention also discloses a method for depositing perovskite thin films on substrates using the perovskite thin film rhythmic deposition production equipment as described above, comprising the following steps: Step 1: Add precursor AX powder material to the evaporation source of each deposition station E in the deposition reaction chamber 3, adjust the vacuum degree of the deposition reaction chamber 3, and start the heating device 7.

[0029] Step 2: The substrate 5, pre-prepared with a perovskite precursor BX2 thin film, is placed in the sample loading chamber and transferred into the deposition reaction chamber 3. The substrate 5 passes sequentially through the unit deposition station E and the unit reaction station F, finally yielding a fully reacted perovskite ABX3 thin film on the substrate 5. During the deposition reaction in the deposition reaction chamber 3, a thin film detection device 8 installed at the top of some reaction stations will track the reaction progress of the perovskite thin film in real time.

[0030] The following specific embodiments further illustrate the rhythmic deposition method and equipment for perovskite thin films of the present invention.

[0031] Example 1 Please continue to refer to the appendix. Figure 2 As shown, the first type of rhythmic deposition equipment for perovskite thin films disclosed in this invention consists of several parts: a sample inlet chamber 1, a heating chamber 2, a deposition reaction chamber 3, and a sample outlet chamber 4. The sample inlet chamber 1 functions similarly to a transition chamber, allowing the substrate 5 to be deposited to enter the low-pressure chamber from atmospheric pressure outside. The heating chamber 2 is connected to the deposition reaction chamber 3, and its temperature is higher than that of the deposition reaction chamber 3, allowing the substrate 5 to be deposited to rapidly heat to the reaction temperature before entering the deposition reaction chamber 3 for reaction. The substrate 5 is conveyed by rollers 6 driven by a servo motor. The substrate 5 is placed face down on the rollers 6, which support the substrate 5 and prevent the deposition surface from contacting the rollers 6. The rollers 6 are evenly spaced, with the interval not exceeding half the length of the long side of the substrate 5. In the deposition reaction chamber 3, an evaporation source mounting slot and a power interface for installing the evaporation source are designed between every two rollers 6. This evaporation source mounting slot can be used to install an evaporation source to form a deposition section, or it can be left empty and used as a reaction section. The installation will be based on the needs of rhythmic production. Figure 2 This diagram illustrates a basic rhythmic production method—alternating deposition and reaction sections at equal intervals. Only five evaporation sources are shown in this diagram; in actual production, more may be installed.

[0032] In the deposition reaction chamber 3, a heating device 7 is installed at the top of each evaporation source mounting slot. This device is located below the chamber cover, close to the substrate 5 to be deposited, and is used to maintain the temperature of the perovskite deposition reaction on the substrate 5. The reaction pressure of the entire deposition reaction chamber 3 is maintained by a vacuum regulation system consisting of a vacuum gauge, a vacuum pump, and a gas supply pipeline (not shown in the attached diagram). Furthermore, a thin film detection device 8 is installed at the top of some reaction sections to monitor the reaction status of the thin film formed on the substrate 5 in real time and transmits the detected information to the control system of the entire production line. The control system determines the opening and closing of subsequent evaporation sources based on the deviation between the current state information of the substrate 5 and the state information of a standard substrate. A double-leaf baffle is installed at the evaporation source opening in the rear half of the deposition reaction chamber, allowing software control of the opening and closing of the evaporation sources, thereby regulating the reaction process of the perovskite thin film. The aforementioned thin film detection equipment includes one or a combination of several types such as imaging detection systems, ultraviolet-visible spectrophotometers (UV-vis), photoluminescence detectors (PL), and X-ray diffraction systems (XRD). The entire production line is connected to the control system via PID controllers, various sensors, etc., and all operations are controlled through the human-machine interface on the control system.

[0033] The basic process for preparing perovskite thin films using the rhythmic deposition equipment of this embodiment includes the following steps: Step 11: Open the top cover of the deposition reaction chamber 3, install evaporation sources at equal intervals in the evaporation source installation slot, with the opening of the evaporation source facing upwards, and connect the power interface on it to the power interface in the evaporation source installation slot. Then add precursor AX material powder to each evaporation source. The amount of material added accounts for 1 / 3 to 2 / 3 of the volume of the evaporation source groove, and it is usually an organic halide powder material.

[0034] Step 12: Close the top cover of the deposition reaction chamber 3, then turn on the vacuum pump to evacuate the chamber. At the same time, set various process parameters in the operating software of the control system, including setting the temperature of the heating chamber 2 to 100℃~400℃, the heating temperature of the evaporation source to 80℃~300℃, the temperature of the heating device 7 to 50℃~250℃, the evaporation pressure of the chamber to 1Pa~50000Pa, and the transmission speed of the roller 6 to 1mm / s~400mm / s, etc.

[0035] Step 13: A metal halide film is pre-prepared on the substrate 5 to be deposited, and then the film is placed face down on the roller in front of the sample inlet chamber 1. The automatic operation mode is started in the control software. At this time, the door of the sample inlet chamber 1 is opened, and the substrate 5 to be deposited will enter the sample inlet chamber 1 under the drive of the roller 6. Then the door of the sample inlet chamber 1 is closed, the vacuum pump is turned on to reduce the pressure inside the chamber. When it drops to the reaction pressure, the door between the sample inlet chamber 1 and the heating chamber 2 is opened, and the substrate 5 to be deposited enters the heating chamber 2. Then it is rapidly heated to the reaction temperature and enters the deposition reaction chamber 3.

[0036] Step 14: After entering the deposition reaction chamber 3, the substrate 5 to be deposited first passes through the first unit deposition station. The gaseous organic halide molecules generated by the evaporation source will first deposit onto the metal halide surface of the substrate 5 and react to form perovskite crystals. Simultaneously, the organic halide molecules on the surface will also diffuse into the film layer. When the substrate 5 continues to the first unit reaction station, the surface material deposition pauses, but the molecular diffusion reaction within the film layer continues, allowing the previously deposited organic halides to fully react. Continuing forward, it will reach the second unit deposition station, where new organic halide surface deposition begins and further diffuses into the film for reaction. This process alternates as the substrate 5 moves through the deposition reaction chamber 3 until the reaction is completed and the substrate is sent to the sample outlet chamber 4. During the deposition reaction in the deposition reaction chamber 3, the thin film detection device 8 installed at some of the unit reaction stations will track the reaction progress of the perovskite thin film in real time.

[0037] Step 15: The sample outlet chamber 4 will be replenished with gas, preferably nitrogen or dry air, to raise the pressure to atmospheric pressure. Then, the outlet door will be opened to transfer the substrate 5 with the prepared perovskite thin film out, completing the preparation of a perovskite thin film for one component.

[0038] The above appendix Figure 2 The alternating, equally spaced deposition and reaction sections shown represent the most basic form of the rhythmic deposition equipment for perovskite thin films in this invention. However, in the actual perovskite thin film production process, at the beginning of the reaction, the organic halides deposited on the surface react rapidly with the metal halides, growing into fine perovskite seed crystals. At this stage, the chemical reaction rate ν is relatively high. As the reaction proceeds, the perovskite crystals within the film continuously grow, causing the chemical reaction rate ν of subsequently deposited organic halides to gradually decrease when reacting with the metal halides. Depending on the type of reactant and whether doping has been performed, the decrease in the chemical reaction rate may be initially rapid followed by a slower rate, or vice versa, but the overall trend is always downward, ultimately resulting in the formation shown in the attached figure. Figure 1The diagram shows an empirical region for perovskite crystallization, where the horizontal axis uses a measurable mesoscopic physical quantity—the thickness T of the perovskite formed by the reaction. Based on this empirical process, the time required for the same amount of organic halide deposition to fully react with the metal halide varies at different reaction stages, with the time required increasing towards the later stages of the reaction. Therefore, the perovskite thin film rhythmic deposition production equipment of this invention will be derived from the basic alternating arrangement of deposition and reaction sections into two forms that better reflect the actual perovskite crystallization process: the first is a constant reaction section length with decreasing deposition section length; the second is a constant deposition section length with increasing reaction section length. Both of these configurations can be achieved using the detachable evaporation source designed in this invention. For example, in the first configuration, the reaction section remains constant, and multiple evaporation sources can be continuously installed in the first deposition section to form a longer deposition section. Subsequently, the number of evaporation sources in the spaced-out deposition sections decreases, thus achieving a decreasing deposition section length. In the second embodiment, the deposition section length remains constant. As the evaporation source is installed to form the deposition section, the number of spaced evaporation source mounting slots gradually increases. These mounting slots without evaporation sources combine to form reaction sections of progressively longer lengths, allowing more time for the subsequently deposited organic halides to fully react with the remaining metal halides. This flexible and rhythmic setup is a key feature of this invention, enabling the vapor-phase preparation of perovskite thin films under different conditions through flexible combinations of evaporation sources. It should be noted that all the above-mentioned combinations fall under the concept of rhythmic production and are within the scope of protection of this invention.

[0039] Example 2 Please refer to the appendix. Figure 4 As shown, this embodiment is a rhythmic production method derived from the most basic perovskite thin film rhythmic deposition production equipment of Example 1, where the reaction section length remains constant and the deposition section length decreases. Taking the first deposition section as an example of a combination of three evaporation sources (in actual production, there will be more), the basic process of preparing perovskite thin films using the perovskite thin film rhythmic deposition production equipment of this embodiment includes the following steps: Step 21: Fill the deposition reaction chamber 3 with nitrogen to bring the internal pressure to atmospheric pressure. Then, open the chamber cover and install evaporation sources in the first to third evaporation source mounting slots to form the first deposition section. The fourth evaporation source mounting slot is left empty as the first reaction section. Next, install evaporation sources in the fifth and sixth evaporation source mounting slots to form the second deposition section. The seventh evaporation source mounting slot is left empty as the second reaction section. An evaporation source is installed in the eighth evaporation source mounting slot as the third deposition section. The ninth evaporation source mounting slot is left empty as the third reaction section. A spare evaporation source is installed in the tenth evaporation source mounting slot, with a double-opening baffle installed at its opening. Simultaneously, thin film detection equipment is installed in the first to third reaction sections to track the reaction status of the perovskite thin film in real time and transmit the status information to the control system. The control system controls the opening and closing of the spare evaporation source baffle, allowing the perovskite thin film with insufficient reaction to continue depositing a small amount of evaporation material for further reaction, ensuring sufficient film reaction.

[0040] Step 22: After installing the evaporation sources, add organic halide powder material to each evaporation source, the amount of which is 1 / 2 of the volume of the evaporation source groove. Then close the top cover of the deposition reaction chamber 3, turn on the vacuum pump to evacuate the chamber, and evacuate the air pressure to 10. 3 Pa, and at the same time, set various process parameters on the operating software in the control system, including setting the temperature of the heating chamber 2 to 200℃, the heating temperature of the evaporation source to 150℃, the temperature of the heating device 7 to 100℃, and the transmission speed of the roller 6 to 10mm / s, etc.

[0041] Step 23: After the above process parameters stabilize, place the substrate 5, on which the metal halide film has been pre-prepared, face down on the roller in front of the sample inlet chamber 1. Start the automatic operation mode in the control software. At this time, the outer door of the sample inlet chamber 1 opens, and the substrate 5, driven by the roller 6, enters the sample inlet chamber 1 at a speed of 100 mm / s and stops inside. Then, the outer door of the sample inlet chamber 1 closes, and the vacuum pump is turned on to reduce the internal pressure. When the pressure drops to 10... 3 At a certain speed (Pa), the door between the sample introduction chamber 1 and the heating chamber 2 is opened, and the deposition substrate 5 enters the heating chamber 2 at a speed of 100 mm / s and stops. Then, the temperature is rapidly increased to the reaction temperature of 100℃. After waiting for 60 seconds, the deposition substrate 5 enters the deposition reaction chamber 3 at a speed of 10 mm / s.

[0042] Step 24: After entering the deposition reaction chamber 3, the substrate 5 to be deposited first passes through the first deposition section. The first deposition section consists of three evaporation sources. As the substrate 5 passes over these sources, gaseous organic halide molecules are continuously deposited on its deposition surface. These molecules react rapidly upon deposition onto the metal halide surface, forming perovskite crystals. Simultaneously, the surface organic halide molecules diffuse into the film layer, reacting with the metal halides within the film. When the substrate 5 continues into the first reaction section, surface material deposition pauses, while molecular diffusion within the film layer continues, allowing the organic halides deposited in the first deposition section to fully react. For the same component, the front part enters the reaction section first, while the rear part remains in the deposition section. This does not affect the uniformity of the final perovskite film, as the reaction process is consistent for any point on the film. The substrate 5 then continues forward to the second deposition section. This deposition section consists of two evaporation sources. Compared to the first deposition section, the amount of organic halides deposited on the substrate 5 in the second deposition section is reduced. New organic halides are deposited on the surface and further diffuse into the film to react. This process alternates as the substrate 5 is moved in the deposition reaction chamber 3 until the reaction is just completed and the substrate is sent to the sample outlet chamber 4, thus completing the process of preparing a perovskite thin film on the substrate 5.

[0043] Example 3 Please refer to the appendix. Figure 5 As shown, this embodiment is a rhythmic production method derived from the most basic rhythmic deposition equipment of Example 1, where the deposition section length remains constant while the reaction section length increases. The basic process for preparing perovskite thin films using the rhythmic deposition equipment of this embodiment includes the following steps: Step 31: Fill the deposition reaction chamber 3 with nitrogen to bring the internal pressure to atmospheric pressure. Then, open the chamber cover and install an evaporator in the first evaporator installation slot as the first deposition section. The second evaporator installation slot is left empty as the first reaction section. Next, install an evaporator in the third evaporator installation slot as the second deposition section. Then, combine the fourth and fifth evaporator installation slots, leaving them empty, to form the second reaction section. Following a rhythmic arrangement with a constant deposition section length and an increasing reaction section length, install one evaporator in the sixth evaporator installation slot as the third deposition section. The seventh to ninth evaporator installation slots are left empty and combined to form the third reaction section. Install one evaporator in the tenth evaporator installation slot as the fourth deposition section. The eleventh and twelfth evaporator installation slots are left empty and combined to form the fourth reaction section (discontinuous sections in the diagram are omitted). Install a spare evaporator in the fifteenth evaporator installation slot, with a double-opening baffle installed at its opening. Meanwhile, a thin film detection device 8 is installed in the last evaporation source mounting tank of the second to fourth reaction stages. This device is used to track the reaction status of the perovskite thin film in real time and transmit the status information to the control system. The control system then controls the opening and closing of the backup evaporation source baffle, allowing the perovskite thin film with insufficient reaction to continue to deposit a small amount of evaporation material for reaction, thus ensuring the full reaction of the thin film.

[0044] Step 32: After installing the evaporation sources, add organic halide powder material to each evaporation source, the amount of which is 1 / 2 of the volume of the evaporation source groove. Then close the top cover of the deposition reaction chamber 3, turn on the vacuum pump to evacuate the chamber, and evacuate the air pressure to 10. 3 Pa, and at the same time, set various process parameters on the operating software in the control system, including setting the temperature of the heating chamber 2 to 200℃, the heating temperature of the evaporation source to 150℃, the temperature of the heating device 7 to 100℃, and the transmission speed of the roller 6 to 10mm / s, etc.

[0045] Step 33: After the above process parameters stabilize, place the substrate 5, on which the metal halide film has been pre-prepared, face down on the roller in front of the sample inlet chamber 1. Start the automatic operation mode in the control software. At this time, the outer door of the sample inlet chamber 1 opens, and the substrate 5, driven by the roller 6, enters the sample inlet chamber 1 at a speed of 100 mm / s and stops inside. Subsequently, the outer door of the sample inlet chamber 1 closes, and the vacuum pump is turned on to reduce the internal pressure. When the pressure drops to 10... 3 At a certain temperature (Pa), the door between the sample introduction chamber 1 and the heating chamber 2 is opened, and the deposition substrate 5 enters the heating chamber 2 at a speed of 100 mm / s and stops. Then, the temperature is rapidly increased to the reaction temperature of 100℃, and after waiting for 60 seconds, the deposition substrate 5 enters the deposition reaction chamber 3 at a speed of 10 mm / s.

[0046] Step 34: After entering the deposition reaction chamber 3, the substrate 5 to be deposited first passes through the first deposition section. In the first deposition section, the gaseous organic halide molecules generated by the evaporation source will first deposit onto the metal halide surface of the substrate 5 and react rapidly to form perovskite crystals. Simultaneously, the organic halide molecules on the surface will also diffuse into the film layer, reacting with the metal halides within the film. When the substrate 5 continues to move into the first reaction section, the surface material deposition pauses, while the molecular diffusion reaction within the film layer continues, allowing the organic halides deposited in the first deposition section to fully react. Then, the substrate 5 continues forward to the second deposition section, where new organic halide surface deposition begins and further diffuses into the film for reaction. Since a small amount of perovskite seed crystals have already formed in the first deposition stage, the chemical reaction rate of the organic halides deposited in the second deposition stage when reacting with the metal halides is relatively lower. This results in a longer distance for the substrate 5 to enter the second reaction stage, which is the rhythmic production method demonstrated in this embodiment, where the deposition stage length remains constant while the reaction stage length increases. Similarly, after the third deposition stage, the substrate 5 will enter the even longer third reaction stage, allowing more time for a complete reaction until it is sent to the sample outlet 4, thus completing the process of preparing a perovskite thin film on the substrate 5.

[0047] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for producing perovskite thin films by rhythmic deposition, characterized in that, The process includes the following: A substrate containing a pre-prepared perovskite precursor BX2 film is placed in a deposition reaction chamber to evaporate and deposit the precursor AX material. The deposition is paused after a certain period of time, allowing sufficient time for the precursor AX material deposited on the surface of the precursor BX2 film to diffuse into the precursor BX2 film and form perovskite ABX3 crystals. After a pause, the deposition is repeated. This process of deposition and pause is repeated rhythmically multiple times, allowing the AX material to enter the interior of the BX2 film and react fully with the BX2 material, thereby obtaining ABX3 perovskite crystals with no BX2 material residue or with excess AX material. The deposition duration and pause time are preset until a perovskite ABX3 film of the set thickness is obtained, at which point the rhythmic deposition process ends. Among them, precursor BX2 is a metal halide material, precursor AX is an organohalide powder material, and A is a methylamino group CH3NH3. + , Ethylamino group CH3CH2NH3 + , Methamidinyl CH(NH2)2 + Ethylamidinyl CH3C(NH2)2 + Na + K + 、Rb + and Cs + B is any one of the monovalent cations, B is any one of the divalent metal cations of lead, tin, tungsten, copper, zinc, gallium, germanium, arsenic, selenium, rhodium, palladium, silver, cadmium, indium, antimony, osmium, iridium, platinum, gold, mercury, thallium, bismuth, and polonium, and X is any one of the monovalent anions of iodine, bromine, chloride, and astatine. The ratio of deposition duration to pause time is 1:0.5 to 1:

100.

2. The method for rhythmic deposition of perovskite thin films as described in claim 1, characterized in that, The thickness of the prepared perovskite ABX3 thin film is 100 nm to 1000 nm.

3. The method for rhythmic deposition of perovskite thin films as described in claim 1, characterized in that, Both deposition and pause processes were carried out in a vacuum environment with a vacuum level of 1 Pa to 50,000 Pa.

4. The method for rhythmic deposition of perovskite thin films as described in claim 1, characterized in that, The evaporation temperature of the precursor AX material is 80℃~300℃.

5. A perovskite thin film rhythmic deposition production equipment, characterized in that, The system includes a deposition reaction chamber, which contains two functional zones: a deposition zone and a reaction zone. The deposition zone comprises one or more deposition sections, each containing at least one unit deposition station. An evaporation source is located at each unit deposition station, and the precursor AX material powder to be evaporated is placed in the evaporation source. The reaction zone comprises one or more reaction sections, each containing at least one unit reaction station. No evaporation source is located at each unit reaction station. The deposition sections and reaction sections are spaced apart. The deposition reaction chamber is connected to a vacuum pump via piping. A heating device is also installed within the deposition reaction chamber to heat the substrate to be deposited, on which a pre-prepared perovskite precursor BX2 thin film has been prepared. The precursor BX2 material is a metal halide material, and the precursor AX material powder is an organic halide powder material, where A is methylamino group CH3NH3. + , Ethylamino group CH3CH2NH3 + , Methamidinyl CH(NH2)2 + Ethylamidinyl CH3C(NH2)2 + Na + K + 、Rb + and Cs + B is any one of the monovalent cations, B is any one of the divalent metal cations of lead, tin, tungsten, copper, zinc, gallium, germanium, arsenic, selenium, rhodium, palladium, silver, cadmium, indium, antimony, osmium, iridium, platinum, gold, mercury, thallium, bismuth, and polonium, and X is any one of the monovalent anions of iodine, bromine, chloride, and astatine. The perovskite thin film rhythmic deposition production equipment also includes a transport device for conveying the substrate to be deposited, as well as a sample inlet chamber, a heating chamber, and a sample outlet chamber. The sample inlet chamber and the heating chamber are sequentially located at the front of the deposition reaction chamber, while the sample outlet chamber is located at the rear of the deposition reaction chamber. The transport device sequentially connects the sample inlet chamber, the heating chamber, the deposition reaction chamber, and the sample outlet chamber. A thin film detection device is set at some unit reaction stations. The thin film detection device includes one or more of the following types: imaging detection system, ultraviolet-visible light spectrophotometer, photoluminescence detection system, and X-ray diffraction system, which are used to monitor the reaction process of the perovskite thin film in real time, thereby adjusting the opening and closing of the evaporation source in the remaining deposition section. The length of the unit deposition station is L. di =v*t d / n, the length L of the unit reaction station ri =v*t r / m, where v is the moving speed of the substrate to be deposited (cm / s), t d The deposition time (s) required to form a good perovskite film, t r The reaction time (s) required to form a good perovskite thin film, t d :t r =1:0.5~1:100, where n is the number of unit deposition sites and m is the number of unit reaction sites; The lengths of the deposition section and the reaction section of the deposition reaction chamber decrease sequentially from front to back in the direction of the front and rear sections of the deposition reaction chamber, respectively. That is, the lengths of the deposition section and the reaction section located at the front of the deposition reaction chamber are greater than the lengths of the deposition section and the reaction section located at the rear of the deposition reaction chamber.

6. The perovskite thin film rhythmic deposition production equipment as described in claim 5, characterized in that, The evaporation source includes an evaporation crucible with its opening facing upwards. The evaporation crucible includes an outer heat insulation layer, a middle heating layer, and an inner heat-conducting layer. A heating power line is provided on the heating layer to connect to an external power interface.

7. A method for depositing perovskite thin films on substrates using the perovskite thin film rhythmic deposition production equipment as described in claim 5 or 6, characterized in that, Includes the following steps: Step 1: Add precursor AX powder material to the evaporation source of each deposition station in the deposition reaction chamber, adjust the vacuum level of the deposition reaction chamber, and start the heating device. Step 2: Place the substrate to be deposited, which has been pre-prepared with a perovskite precursor BX2 thin film, into the deposition reaction chamber. The substrate passes through the deposition section and the reaction section in sequence, and finally the perovskite ABX3 thin film generated by the reaction is obtained on the substrate.

Citation Information

Patent Citations

  • A preparation method of perovskite thin film and a preparation method of solar cell thereof

    CN109216547A

  • Chemical adsorption self-limiting auxiliary method for promoting controllable crystal growth of perovskite film

    CN109970353A