A Mn that can independently change the halogen content 2+ Doped CsPbCl 3 Preparation method of nanocrystals
Injecting halogen precursors at high temperatures by halogen hot injection method solves the problem that Mn ions and halogen concentrations cannot be independently adjusted in the prior art, and the excellent optical performance and stability of Mn2+ doped CsPbCl3 nanocrystals are achieved, which is suitable for nanofluorescence Powder application.
Patent Information
- Application Number
- CN202210164869.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-02-23
AI Technical Summary
The prior art cannot independently adjust the Mn ion doping concentration and halogen vacancy concentration, which limits the optimization of the luminescence performance of Mn-doped perovskite nanocrystals.
Halogen precursors were injected at high temperature by using halogen hot injection method to individually change the halogen content and Mn ion concentration in the nanocrystals, regulate the density of halogen vacancy defect states, and realize the preparation of Mn2+ doped CsPbCl3 nanocrystals.
It realizes the individual adjustment of halogen density at fixed Mn2+ doping concentration, reduces defect states, improves the optical performance and stability of nanocrystals, and is potentially used in nanofluorescent powder.
Smart Images

Figure CN114591738B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a Mn2O3 catalyst capable of independently changing the halogen content. 2+ Doped CsPbCl 3 The invention discloses a method for preparing nanocrystals, belonging to the field of semiconductor luminescence. Background Art
[0002] All-inorganic CsPbX 3 (X=Cl, Br or I) Perovskite nanocrystals have attracted much attention due to their excellent optical properties, such as photoluminescence quantum yields (PLQYs) close to 100% and tunable emission wavelengths throughout the visible region, ultra-narrow emission half-width, and ultra-long carrier diffusion length, which make them have broad application prospects in optoelectronic devices such as solar cells, light-emitting diodes (LEDs), liquid crystal display backlights, photodetectors, etc. By doping Mn ions into semiconductor nanocrystals, their optical and magnetic properties can be regulated. In addition to the band edge emission from the matrix material, the luminescence of Mn-doped nanocrystals also has the orange-yellow characteristic emission of Mn ions. The luminescence efficiency of Mn ions is directly related to the doping concentration of Mn ions in the nanocrystals, which exceeds 50% under optimal conditions. At the same time, its luminescence band is very wide and has a large Stokes shift. More importantly, Mn-doped quantum dots have very long fluorescence lifetimes and good light / thermal stability, and reduce the toxicity problems caused by heavy lead metals in lead halide perovskite matrix materials. These excellent properties make Mn-doped perovskite nanocrystals very suitable for white light illumination.
[0003] For CsPbX 3 Nanocrystals, halogen X vacancy (V X ) defects form deep bound energy levels in the band gap, trapping electrons or holes to cause non-radiative recombination and reducing the radiative recombination of carriers, which is considered to be the main factor limiting the improvement of the luminescence efficiency of nanocrystals. It has been reported that the use of ligands or metal halides to passivate the surface V X It can effectively reduce deep energy level traps, thereby improving CsPbX 3 PLQYs of nanocrystals. 2+ Doped CsPbX 3 Nanocrystals, Mn 2+ Luminescence usually comes from the energy transfer of excitons in the matrix material, so its luminescence is closely related to the density of deep bound defect states in the matrix material. 2+ The mechanism of the effect of halogen content in doped perovskite nanocrystals on the optical quality of nanocrystals can provide a basis for optimizing Mn 2+ It provides some ideas for improving the luminescence efficiency of doped perovskite nanocrystals.
[0004] However, in conventional synthesis methods, MnX 2 and PbX2 Salts are used as precursors of manganese, lead and halogen to prepare Mn-doped perovskite nanocrystals. Therefore, the content of Mn ions or halogens in the precursor cannot be adjusted independently, making it impossible to achieve separate regulation of the two variables, the doping concentration of Mn ions or the halogen vacancy concentration, to study their influence mechanism on the luminescence properties of Mn ion-doped nanocrystals.
[0005] For example, a microwave-driven post-doping synthesis of CsPbCl is disclosed in a Chinese patent application document (publication number: CN111117614A). 3 :Mn 2+ Nanocrystal method, which uses MnCl 2 and PbCl 2 As a precursor of manganese, lead and halogen for the preparation of Mn-doped perovskite nanocrystals, it is not possible to independently regulate the two variables of Mn ion doping concentration or halogen vacancy concentration. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a Mn2O3 having excellent optical properties and independently changing the halogen content in order to solve the above problems existing in the prior art. 2+ Doped CsPbCl 3 Nanocrystal method.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] A Mn that can independently change the halogen content 2+ Doped CsPbCl 3 The method for preparing nanocrystals is characterized in that the method comprises the following steps: firstly heating and stirring lead acetate, manganese acetate, cesium oleate, oleic acid, oleylamine, and octadecene, and then hot-injecting a halogen precursor to obtain Mn 2+ Doped CsPbCl 3 Nanocrystals.
[0009] The present invention obtains a mixed solution containing cations such as lead, manganese, and cesium and surface ligands such as oleic acid and oleylamine in octadecene, and then injects a halogen precursor at a high temperature to rapidly realize the nucleation growth of perovskite nanocrystals to obtain Mn 2+ Doped CsPbCl 3 Nanocrystals. Compared with the conventional cation (cesium) ion injection method, this anion (halogen) injection method has unique advantages, that is, the halogen content in the nanocrystal can be changed independently without changing the ratio of cesium and lead cation precursors, thereby regulating the density of halogen vacancy defect states in the nanocrystal, and the content of Mn ions can be changed independently without changing the halogen content, so as to study the effect of Mn doping concentration on the luminescence properties of nanocrystals and further improve the luminescence properties of nanocrystals.
[0010] Preferably, the preparation method of cesium oleate comprises the following steps: 2 CO 3 The powder is placed in a flask, oleic acid and octadecene are added in a mass ratio of 1:(5-8), the flask is then heated to 100-140° C., stirred, vacuum treated, and then heated to 150-160° C. under nitrogen gas protection, and finally kept warm to obtain cesium oleate. The cesium oleate prepared by the present invention dissolves in an ODE solvent and exists in the form of ions. Compared with directly using cesium carbonate, it has higher chemical activity, can not only improve reaction efficiency, but also make nanocrystal nucleation faster, and the crystal field environment around Mn doping is more uniform.
[0011] Preferably, the heating and stirring temperature is 110-130° C. and the time is 0.5-1.5 h. Heating and stirring can ensure the dissolution of the perovskite precursor powder and ensure that water impurities in the solution can be completely removed.
[0012] Preferably, after heating and stirring, the temperature needs to be further increased under the protection of an inert gas.
[0013] Preferably, the inert gas is nitrogen.
[0014] Preferably, after hot injection of the halogen precursor, heat preservation, cooling and centrifugation treatments are sequentially performed.
[0015] Preferably, the holding time is 0.5-2 min.
[0016] Preferably, the cooling time is 0.5-1.5 min. The present invention controls the cooling time to 0.5-1.5 min, which is conducive to the Mn ions entering the lattice and becoming stable doping, and avoids the Mn ions adsorbed on the surface from becoming non-radiative luminescence centers, reducing the luminescence quantum efficiency and the stability of the nanocrystals.
[0017] Preferably, after centrifugation, the nanocrystals need to be dispersed in a non-polar solvent and a polar solvent is added for re-centrifugation.
[0018] Preferably, the non-polar solvent is n-hexane or toluene, and the polar solvent is ethyl acetate.
[0019] Preferably, the centrifugal speed is 8000-8800 rp / min, and the time is 1-10 min.
[0020] Preferably, the halogen precursor solution needs to be heated at 90-110° C. to be clarified before hot injection.
[0021] In the above-mentioned Mn 2+ Doped CsPbCl 3The preparation method of nanocrystals, the molar ratio of lead acetate, manganese acetate and cesium oleate is 1: (1-5): (0.5-0.8). The present invention needs to control the molar ratio of lead acetate, manganese acetate and cesium oleate to ensure the appropriate doping concentration of Mn ions, and can prevent the formation of low-dimensional perovskite structure and affect the optical properties. Compared with the conventional method of controlling the ratio of Cs:Pb at 1:1, the present invention controls the ratio of Cs:Pb at 3:5, so that the quantum dots grow faster and have smaller sizes, which is conducive to keeping the doping concentration of Mn unchanged.
[0022] In the above-mentioned Mn 2+ Doped CsPbCl 3 The method for preparing nanocrystals comprises a volume ratio of oleic acid, oleylamine and octadecene of 1: (0.5-1.5): (8-12). The method controls the ratio of oleic acid, oleylamine and octadecene to ensure that the perovskite precursor can be completely dissolved in the solution in the form of ions, and ensures that the solution has a low viscosity and sufficient reaction space, effectively passivates the surface of the perovskite nanocrystals and prevents the agglomeration of the perovskite nanocrystals. The addition of oleylamine can not only promote the full dissolution of lead acetate and manganese acetate in the solution, but also keep the ion concentration ratio and relative activity unchanged when the precursor ratio remains unchanged, thereby facilitating the stability of the Mn doping concentration during the nucleation process.
[0023] In the above-mentioned Mn 2+ Doped CsPbCl 3 The method for preparing nanocrystals is as follows: the ratio of the amount of the added halogen precursor to the amount of cesium oleate is 1: (0.08-0.16).
[0024] In a Mn 2+ Doped CsPbCl 3 The method for preparing nanocrystals comprises the following steps: the hot injection temperature of the halogen precursor is 240-260°C.
[0025] In the above-mentioned Mn 2+ Doped CsPbCl 3 The method for preparing nanocrystals is that the halogen precursor is prepared by oleylamine and hydrochloric acid.
[0026] Preferably, the specific preparation process of the halogen precursor is: heat oleylamine and hydrochloric acid to 100-130°C and stir, perform vacuum treatment, and finally heat to 130-180°C under nitrogen gas protection and keep warm for 25-40 minutes.
[0027] Preferably, the mass ratio of hydrochloric acid to oleylamine is 1:(8-12).
[0028] Preferably, Mn 2+Doped CsPbCl 3 Mn in nanocrystals 2+ The PL intensity ratio of the excitons is 0.005-3.615.
[0029] Preferably, Mn 2+ Doped CsPbCl 3 Nanocrystalline Mn 2+ The half-width of the emission peak is 70-85nm, and the half-width of the exciton emission peak is 8-15nm.
[0030] Compared with the prior art, the present invention has the advantages that: the present invention synthesizes Mn by halogen hot injection method 2+ Doped CsPbCl 3 Perovskite nanocrystals have achieved the first 2+ Under the condition of fixed doping concentration, the halogen density is changed alone. By adjusting the halogen content, the defect (trap) state is reduced, the electron-phonon coupling effect and the thermal degradation effect at high temperature are reduced, so that the optical performance and stability are better. The perovskite nanocrystal of the present invention realizes the regulation of excitons and Mn by changing the halogen content. 2+ Optical properties, with potential application in nano-phosphors. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of the equipment prepared in Example 1;
[0032] Figure 2 The Mn prepared in Example 1 2+ Doped CsPbCl 3 Transmission electron microscope (TEM) images of nanocrystals at different magnifications;
[0033] Figure 3 The Mn prepared in Example 1 2+ Doped CsPbCl 3 Photoluminescence spectrum (PL) of nanocrystals;
[0034] Figure 4 The Mn prepared in Example 2 2+ Doped CsPbCl 3 Transmission electron microscopy (TEM) image of nanocrystals;
[0035] Figure 5 The Mn prepared in Example 2 2+ Doped CsPbCl 3 Photoluminescence spectrum (PL) of nanocrystals;
[0036] Figure 6 The Mn prepared in Example 3 2+ Doped CsPbCl 3 Transmission electron microscopy (TEM) image of nanocrystals;
[0037] Figure 7 The Mn prepared in Example 3 2+ Doped CsPbCl 3 Photoluminescence spectrum (PL) of nanocrystals;
[0038] Figure 8 The Mn prepared in Example 4 2+ Doped CsPbCl 3 Transmission electron microscopy (TEM) image of nanocrystals;
[0039] Fig. 9 The Mn prepared in Example 4 2+ Doped CsPbCl 3 Photoluminescence spectrum (PL) of nanocrystals;
[0040] Fig.10 The Mn prepared in Example 5 2+ Doped CsPbCl 3 Transmission electron microscopy (TEM) image of nanocrystals;
[0041] Fig.11 The Mn prepared in Example 5 2+ Doped CsPbCl 3 Photoluminescence spectrum (PL) of nanocrystals;
[0042] Fig.12 The Mn prepared in Example 6 2+ Doped CsPbCl 3 Transmission electron microscopy (TEM) image of nanocrystals;
[0043] Fig.13 The Mn prepared in Example 6 2+ Doped CsPbCl 3 Photoluminescence spectrum (PL) of nanocrystals;
[0044] Fig.14 The Mn prepared in Example 7 2+ Doped CsPbCl 3 Photoluminescence spectrum (PL) of nanocrystals;
[0045] Fig.15 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 X-ray diffraction (XRD) pattern of nanocrystals;
[0046] Fig.16 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 UV-visible absorption pattern of nanocrystals;
[0047] Fig.17 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 Quantum efficiency diagram of nanocrystals;
[0048] Fig.18 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 Nanocrystalline Mn 2+ / Exciton PL intensity ratio diagram;
[0049] Fig.19 Mn prepared in Examples 1-4 2+ Doped CsPbCl 3 Normalized exciton temperature-dependent spectral intensity diagram of nanocrystals;
[0050] Fig. 20 Mn prepared in Examples 1-4 2+ Doped CsPbCl 3 Normalized Mn of nanocrystals 2+ Temperature spectrum intensity diagram;
[0051] Fig.21 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 Exciton lifetime curve of nanocrystals;
[0052] Fig. 22 Mn prepared in Example 1-6 2+ Doped CsPbCl 3 Nanocrystalline Mn 2+ Life span graph.
[0053] Fig.23 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 The actual Mn content of nanocrystals 2+ Doping concentration.
[0054] Fig.24 Mn prepared in Examples 1, 8-9 2+ Doped CsPbCl 3 The actual Mn content of nanocrystals 2+ Doping concentration. DETAILED DESCRIPTION
[0055] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the accompanying drawings, but the present invention is not limited to these embodiments.
[0056] Embodiment 1:
[0057] S1, 520mg Cs 2 CO 3 The powder was placed in a 50 mL three-necked flask, and 2 mL of oleic acid and 14 mL of octadecene were added. The three-necked flask was then placed on a heating mantle and heated to 120°C with stirring. The vacuum pump was turned on for 1 hour until no bubbles were generated in the three-necked flask and the flask was clear. The temperature was raised to 150°C under nitrogen gas protection and kept warm for 30 minutes to obtain cesium oleate, which was then placed in a headspace bottle for use. It needed to be heated at 100°C until clear before use.
[0058] S2. Place 20 mL of oleylamine and 2 mL of hydrochloric acid in a 50 mL three-necked flask, then place the three-necked flask in a heating mantle, heat to 120 °C and stir, turn on the vacuum pump for 2 hours until no bubbles are generated in the three-necked flask, raise the temperature to 150 °C under nitrogen gas protection, keep warm for 30 minutes to obtain a halogen precursor, and then put it into a headspace bottle for use. It needs to be heated at 100 °C until clear before use.
[0059] S3. Add 65mg of lead acetate, 52mg of manganese acetate, 0.6mL of cesium oleate, 1mL of oleic acid, 1mL of oleylamine and 10mL of octadecene to a 50mL three-necked flask, then place the three-necked flask on a heating mantle and heat it to 120°C with stirring, turn on the vacuum pump for 1h until no bubbles are generated in the three-necked flask and it is clear, heat it to 250°C under nitrogen protection, immediately hot-inject 1.0mL of halogen precursor, keep it warm for 1min, quickly immerse the three-necked flask in an ice bath, and cool it to room temperature to obtain the stock solution. The stock solution is quickly centrifuged in a centrifuge at a speed of 8500rpm / min for 5min to obtain a crude product, the crude product is dispersed in toluene and ethyl acetate is added, and centrifuged again, and this step is repeated twice to obtain Mn 2+ Doped CsPbCl 3 Nanocrystals.
[0060] Embodiment 2:
[0061] The only difference from Example 1 is that the hot injection amount of the halogen precursor in step S3 is 0.8 mL.
[0062] Embodiment 3:
[0063] The only difference from Example 1 is that the hot injection amount of the halogen precursor in step S3 is 0.6 mL.
[0064] Embodiment 4:
[0065] The only difference from Example 1 is that the hot injection amount of the halogen precursor in step S3 is 0.4 mL.
[0066] Embodiment 5:
[0067] The only difference from Example 1 is that the hot injection amount of the halogen precursor in step S3 is 1.2 mL.
[0068] Embodiment 6:
[0069] The only difference from Example 1 is that the hot injection amount of the halogen precursor in step S3 is 1.5 mL.
[0070] Embodiment 7:
[0071] The only difference from Example 1 is that the hot injection amount of the halogen precursor in step S3 is 0.2 mL.
[0072] Embodiment 8:
[0073] The only difference from Example 1 is that the amount of manganese acetate added in step S3 is 69.2 mg.
[0074] Embodiment 9:
[0075] The only difference from Example 1 is that the amount of manganese acetate added in step S3 is 173 mg.
[0076] Figure 1 This is a schematic diagram of the equipment prepared in Example 1. The nanocrystals of the present invention achieve the regulation of excitons and Mn by changing the halogen content. 2+ Optical properties, with potential application in nano-phosphors.
[0077] Figure 2-3 The Mn prepared in Example 1 2+ Doped CsPbCl 3 Transmission electron microscope (TEM) images and emission spectra (PL) images of nanocrystals at different magnifications show that the size of the nanocrystals is 11.8 nm. Tetragonal CsPbCl 3 (101) interplanar spacing, the exciton emission peak is 409nm, and the half-peak width is 10nm. Its particularly narrow half-peak width of luminescence indicates that the size distribution of the nanocrystals is relatively uniform and there are fewer defects inside the crystal. In addition, the emission peak is 586nm, and the half-peak width is 76nm. The luminescence band comes from the typical Mn ion d electron 4 T 1 - 6 A 1 The energy level transition indicates that Mn ions have been incorporated into the perovskite lattice, replacing the Pb ion lattice. The ratio of the luminescence intensity of Mn ions to excitons is the highest, indicating an effective energy transfer process from excitons to Mn ions.
[0078] Figure 4-5 The Mn prepared in Example 2 2+ Doped CsPbCl 3The transmission electron microscope (TEM) and spectrum (PL) images of the nanocrystals show that the size of the nanocrystals is 11.8nm, the exciton emission peak is 409nm, and the extremely narrow half-peak width of the emission indicates that the size distribution of the nanocrystals is relatively uniform and there are fewer defects inside the crystal. In addition, the emission peak is 586nm, and the half-peak width is 76nm. The luminescence band comes from the typical Mn ion d electron 4 T 1 - 6 A 1 The energy level transition indicates that Mn ions have been incorporated into the perovskite lattice, replacing the Pb ion lattice. The ratio of the luminescence intensity of Mn ions to excitons is lower than that of Example 1, indicating that the energy transfer efficiency from excitons to Mn ions is reduced, which is related to the large number of surface defects in the nanocrystals.
[0079] Figure 6-7 The Mn prepared in Example 3 2+ Doped CsPbCl 3 The transmission electron microscope (TEM) and emission spectrum (PL) images of the nanocrystals show that the size of the nanocrystals is 12.4 nm, the exciton emission peak is 410 nm, the half-peak width is 10 nm, and the Mn 2+ The emission peak is 586nm and the half-peak width is 76nm. The ratio of the luminescence intensity of Mn ions to excitons is further reduced compared with Example 2, indicating that the energy transfer efficiency from excitons to Mn ions is further reduced, indicating that the further reduction of halogens leads to more surface defects of nanocrystals.
[0080] Figure 8-9 The Mn prepared in Example 4 2+ Doped CsPbCl 3 The transmission electron microscope (TEM) and emission spectrum (PL) images of the nanocrystals show that the size of the nanocrystals is 11.8 nm, the exciton emission peak is 409 nm, the half-peak width is 10 nm, and the Mn 2+ The emission peak is 586nm and the half-peak width is 76nm. Similar to the above trend, the further reduction of halogen content leads to more surface defects of nanocrystals and lower energy transfer efficiency from excitons to Mn ions.
[0081] Figure 10-11 The Mn prepared in Example 5 2+ Doped CsPbCl 3 The transmission electron microscope (TEM) and emission spectrum (PL) images of the nanocrystals show that the size of the nanocrystals is 11.9 nm, the exciton emission peak is 409 nm, the half-peak width is 10 nm, and the Mn 2+ The emission peak is 586 nm and the half-peak width is 76 nm. As the halogen content increases, the ratio of the Mn ion to the exciton luminescence intensity remains essentially unchanged relative to Example 1, indicating that 1 mL of OAm-Cl is sufficient to passivate the halogen vacancies on the perovskite surface.
[0082] Figure 12-13 The Mn prepared in Example 6 2+ Doped CsPbCl 3 The transmission electron microscope (TEM) and emission spectrum (PL) images of the nanocrystals show that the size of the nanocrystals is 12.0 nm, the exciton emission peak is 409 nm, the half-peak width is 10 nm, and the Mn 2+ The emission peak is 586 nm and the half-peak width is 76 nm. As the halogen content increases, the ratio of the Mn ion to the exciton luminescence intensity remains essentially unchanged relative to Example 1, indicating that 1 mL of OAm-Cl is sufficient to passivate the halogen vacancies on the perovskite surface.
[0083] Fig.14 The Mn prepared in Example 7 2+ Doped CsPbCl 3 The emission spectrum (PL) of the nanocrystal shows that the exciton emission peak is 409nm, the half-peak width is 10nm, and the Mn 2+ The emission peak is 586nm and the half-peak width is 76nm. In this sample, the Mn ion luminescence is very weak, indicating that when the halogen content is far from enough, there are many halogen hole defects in the nanocrystals, which leads to the serious inhibition of the energy transfer process from excitons to Mn ions.
[0084] Fig.15 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 The X-ray diffraction (XRD) pattern of nanocrystals shows that samples of Examples 1-7 all conform to the tetragonal phase CsPbCl 3 (PDF#18-0366) structure, the diffraction angle does not move substantially.
[0085] Fig.16 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 The UV-visible absorption diagram of the nanocrystals shows that the UV absorption peaks of the samples of Examples 1-7 overlap and are basically unchanged.
[0086] Fig.17 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 The quantum efficiency diagram of nanocrystals shows that the PLQYs of samples in Examples 1-7 are 55.98%, 51.67%, 23.1%, 18.8%, 14.54%, 52.82%, and 49.61%, respectively. This shows that with the increase of the amount of halogen precursor, the luminous efficiency of nanocrystals first increases and then remains basically unchanged, indicating that the halogen content is the factor that affects the Mn-doped CsPbCl3 The main factors affecting the luminescence properties of nanocrystals.
[0087] Fig.18 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 Nanocrystalline Mn 2+ / exciton PL intensity ratio diagram, it can be seen from the figure that the intensity ratios of examples 1-7 samples are 3.61, 3.02, 2.56, 0.89, 0.005, 3.57, and 3.59, respectively, indicating that the change of halogen content affects the energy transfer efficiency from excitons to Mn ions and the defect state density on the surface of nanocrystals.
[0088] Fig.19 Mn prepared in Examples 1-4 2+ Doped CsPbCl 3 The normalized exciton temperature-dependent spectral intensity diagram of the nanocrystals shows that the exciton intensity of the sample in Example 1 decreases faster.
[0089] Fig. 20 Mn prepared in Examples 1-4 2+ Doped CsPbCl 3 Normalized Mn of nanocrystals 2+ The temperature spectrum intensity diagram shows that the Mn content of the sample in Example 1 is 2+ It increases faster and then decreases, while the strength of the sample in Example 4 does not increase but only decreases.
[0090] Fig.21 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 The exciton lifetime curve of nanocrystals shows that the exciton lifetime curves of samples of Examples 1-7 can be fitted with three exponentials, and the lifetimes are 2.27ns, 1.89ns, 1.61ns, 1.49ns, 2.05ns, 2.07ns, and 2.02ns, respectively. The non-monotonic change of the exciton lifetime indicates that the defect state density of the nanocrystals and the energy transfer efficiency from excitons to Mn ions change with the change of the halogen content.
[0091] Fig. 22 Mn prepared in Example 1-6 2+ Doped CsPbCl 3 Nanocrystalline Mn 2+ Life curve diagram, from which it can be seen that the Mn of samples in Examples 1-6 2+The lifetime curve can be fitted with a single exponential, and the lifetimes are 1.78ms, 1.78ms, 1.78ms, 1.77ms, 1.78ms, and 1.78ms, respectively. The luminescence of Mn ions conforms to the single exponential fitting, indicating that after the exciton transfers energy to the Mn ion, the 5d electrons of the Mn ion 4 T 1 - 6 A 1 The energy level transition luminescence efficiency is close to 100%, indicating that the crystal field environment around the Mn ions is uniform and has relatively few defect states.
[0092] Fig.23 Mn prepared in Example 1-7 2+ Doped CsPbCl 3 The actual Mn content of nanocrystals 2+ Doping content. As can be seen from the figure, changing the halogen content will not change the actual Mn 2+ Doping concentration.
[0093] Fig.24 Mn prepared in Examples 1, 8-9 2+ Doped CsPbCl 3 The actual Mn content of nanocrystals 2+ As can be seen from the figure, with the increase of Mn precursor content, the actual Mn 2+ The doping levels are also increasing.
[0094] From the above results, it can be seen that the present invention synthesized a series of Mn 2+ Doped CsPbCl 3 Nanocrystals can be used to fix Mn 2+ The density of halogen is changed independently under the condition of doping concentration. 2+ The emission shows a single exponential decay, which means that Mn 2+ The emission efficiency is close to unity. Excitons and Mn 2+ The PL of the MnO4+M ... 2+ Since there are many deep energy defect states in the OAm-Cl deficient samples, the Mn 2+ The PL of Mn shows different trends, and the additional OAm-Cl can passivate these defect states well, transforming the deep defect states into shallow defect states. The results and analysis here will help to clarify the effect of halogen vacancies on Mn 2+ The potential mechanisms that influence the PL properties of doped perovskite nanocrystals will be helpful in further developing the potential applications of these materials.
[0095] The parts of the technical scope of the present invention that are not exhausted by the midpoint value of the embodiment and the new technical solutions formed by the equivalent replacement of single or multiple technical features in the technical solutions of the embodiments are also within the scope of protection claimed by the present invention, and unless otherwise specified, there is no unique and irreplaceable combination between all the parameters involved in the solutions of the present invention.
[0096] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
[0097] Although the present invention has been described in detail and some specific embodiments have been cited, it is obvious to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.
Claims
1. A Mn that can independently change the halogen content 2+ The method for preparing doped CsPbCl3 nanocrystals is characterized in that: The method comprises the following steps: S1. Place 520 mg of Cs2CO3 powder in a 50 mL three-necked flask, add 2 mL of oleic acid and 14 mL of octadecene, then place the three-necked flask on a heating mantle and heat it to 120 °C with stirring, turn on the vacuum pump for 1 hour until no bubbles are generated in the three-necked flask and it is clear, heat it to 150 °C under nitrogen protection, keep it warm for 30 minutes to obtain cesium oleate, and then put it into a headspace bottle for use. It needs to be heated at 100 °C until it is clear before use; S2. Place 20 mL of oleylamine and 2 mL of hydrochloric acid in a 50 mL three-necked flask, then place the three-necked flask in a heating jacket and heat to 120°C with stirring, turn on the vacuum pump for 2 hours until no bubbles are generated in the three-necked flask, heat to 150°C under nitrogen protection, keep warm for 30 minutes to obtain a halogen precursor, and then put it into a headspace bottle for use. It needs to be heated at 100°C until clear before use; S3, add 65mg of lead acetate, 52mg of manganese acetate, 0.6mL of cesium oleate, 1mL of oleic acid, 1mL of oleylamine and 10mL of octadecene into a 50mL three-necked flask, then put the three-necked flask into a heating jacket and heat it to 120°C with stirring, turn on the vacuum pump for 1h until there are no bubbles in the three-necked flask and it is clear, heat it to 250°C under nitrogen protection, immediately hot-inject 1.0mL of halogen precursor, keep it warm for 1min, quickly immerse the three-necked flask in an ice bath, and cool it to room temperature to obtain a stock solution; The stock solution was centrifuged quickly at 8500 rpm / min for 5 min to obtain a crude product, which was dispersed in toluene and added with ethyl acetate and centrifuged again. This step was repeated twice to obtain Mn 2+ Doped CsPbCl3 nanocrystals.