Purification of Scandium Concentrate
By using strong acid cationic resin to capture and elude metal pollutants in scandium concentrate, the problem of scandium oxide pollution is solved, and efficient purification and refining scandium oxide is achieved, which improves the transportation safety and market value of the product.
Patent Information
- Application Number
- CN202080075288.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-28
- Filing Date
- 2020-10-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-10-26
AI Technical Summary
Scandium oxide products may be contaminated by metal contaminants, especially radioactive metal contaminants, resulting in transportation restrictions and reduced commercial value. It is difficult for the prior art to effectively reduce the metal contaminant content in scandium concentrates.
Using a strongly acidic cationic resin, such as a sulfonate ion exchange resin, contacting the scandium concentrate, by capturing and eluting metal contaminants, to produce a purified scandium solution or raffinate, and subsequently preparing refined scandium oxidation by oxalic acid precipitation and calcination Products.
It effectively reduces the concentration of metal pollutants in scandium oxides to reach 500ppm or less, improves the purity and commercial value of the product, and ensures transportation safety and market competitiveness.
Smart Images

Figure CN114599439B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Provisional Patent Application No. 62 / 926,708, filed on October 28, 2019, and is incorporated herein in its entirety. Technical Field
[0003] The present disclosure relates to methods of reducing contamination in scandium concentrates using ion exchange resins. Background Art
[0004] Scandium (Sc) oxide products may be contaminated with metal contaminants, which in some embodiments may be radioactive. Contamination, especially contamination with radioactive metal contaminants, is problematic because it may limit the transportation of Sc oxide products and reduce their commercial value.
[0005] It would be highly desirable to provide a method for reducing the contamination of Sc concentrate with metal contaminants to produce a Sc oxide product having a metal contaminant content of 500 ppm (or less). Summary of the invention
[0006] The present disclosure relates to reducing contamination in scandium concentrates using strong acid cation resins, such as sulfonate ion exchange resins.
[0007] In a first aspect, the present disclosure provides a method for removing at least one metal contaminant from a scandium (Sc) concentrate. The method includes contacting the Sc concentrate with an acidic solution to produce an impure Sc solution. In one embodiment of the method, the method includes contacting the impure scandium solution with a first ion exchange resin that captures at least one metal contaminant to produce a first ion exchange resin complex and a purified Sc raffinate, wherein the first ion exchange resin has an affinity for at least one metal contaminant greater than the affinity for Sc, and optionally eluting Sc from the first ion exchange resin complex with a first elution solution to obtain a first Sc eluate and combining the first Sc eluate with the first Sc raffinate. In another embodiment of the method, the method also includes contacting the impure Sc solution with a second ion exchange resin that captures at least one metal contaminant and Sc to produce a second ion exchange resin complex; eluting Sc from the second ion exchange resin complex with a second elution solution to obtain a purified Sc eluate. In the method of the present disclosure, the concentration of at least one metal contaminant in the purified Sc eluate or the purified Sc raffinate is lower than the concentration of at least one metal contaminant in the impure Sc solution. Also in the method of the present disclosure, the first ion exchange resin and the second ion exchange resin are strongly acidic cationic resins with sulfonic acid functional groups in the form of potassium or sodium. In one embodiment, the Sc concentrate is in the form of a dry solid or an aqueous solid suspension or slurry. In another embodiment, the sulfonic acid functional group is in the form of sodium. In another embodiment, the oxidation state of the at least one metal contaminant is at least 3. In another embodiment, the at least one metal contaminant is thorium (Th) or zirconium (Zr). In a specific embodiment, the at least one metal contaminant is Th. In another embodiment, the pH of the impure Sc solution is about 1.5 to about 3.5, for example, the pH is about 3.0 to about 3.5. In another embodiment, the acidic solution is a HCl solution. In another embodiment, the method includes eluting Sc from the first ion exchange resin complex with a first elution solution to obtain a first Sc eluate and merging the first Sc eluate with the purified Sc raffinate. In yet another embodiment, the second elution solution or the second elution solution is an HCl solution. In yet another embodiment, the second ion exchange resin is a gel. In yet another embodiment, the first ion exchange resin is a macroporous resin. In one embodiment, the method further comprises eluting at least one metal contaminant from the first ion exchange resin complex or the second ion exchange resin complex. In another embodiment, the method further comprises regenerating the first ion exchange resin or the second ion exchange resin into a sodium or potassium form.
[0008] According to a second aspect, the present disclosure provides a purified scandium (Sc) eluate obtained or obtainable by a method described herein.
[0009] According to a third aspect, the present disclosure provides a purified scandium (Sc) raffinate obtained or obtainable by the process described herein.
[0010] According to a fourth aspect, the present disclosure provides a method for preparing a refined scandium (Sc) oxide product. The method comprises precipitating the purified Sc eluate described herein or the purified Sc raffinate described herein with oxalic acid to obtain a precipitation slurry having a solid portion and a liquid portion. The method further comprises separating the solid portion of the precipitation slurry from the liquid portion of the precipitation slurry to obtain a separated solid portion. The method further comprises calcining the separated solid portion to obtain a refined Sc oxide product. The refined Sc oxide product obtained has a concentration of less than 500 ppm of at least one metal contaminant.
[0011] According to a fifth aspect, the present disclosure provides a refined scandium (Sc) oxide product obtained or obtainable by a process as described herein. The refined scandium oxide product has a concentration of less than 500 ppm of at least one metal contaminant. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Having generally described the nature of the invention, reference will now be made to the accompanying drawings which show, by way of illustration, preferred embodiments of the invention, and in which:
[0013] Figure 1 is a process flow diagram of a first ion exchange method according to one embodiment of the method for removing metal contaminants from a scandium (Sc) concentrate described herein.
[0014] Figure 2 is a process flow diagram of a second ion exchange method according to another embodiment of the method for removing metal contaminants from a scandium (Sc) concentrate described herein.
[0015] Figure 3 The percent retention of scandium (left column for each condition) and thorium (right column for each condition) on the gel-type resin is provided as a function of the number of processing cycles. The percent retention is provided numerically at the top of each column. DETAILED DESCRIPTION
[0016] The present disclosure relates to a method for reducing the presence of contaminating metal elements in a scandium concentrate. As used in the context of the present disclosure, the expression "scandium concentrate" refers to an amorphous (e.g., aqueous solid suspension or slurry) or crystalline (e.g., dry solid form) carbonate-bicarbonate-hydroxide precipitate of scandium. The precipitate can be obtained by processing a raw material containing scandium, such as liquid effluents and solid residues from: titanium dioxide (TiO2) raw material upgrading equipment (UGS process, etc.), TiO2 pigment production (sulfate or chloride process), aluminum oxide (Al2O3) production (Bayer process), nickel ore processing, zirconium raw material processing, uranium ore processing, tungsten ore processing, etc. The expression "scandium concentrate" also refers to scandium oxide or any other scandium-containing solid compound containing a large amount of impurities such as thorium, zirconium, etc.
[0017] In some embodiments, a scandium concentrate can be obtained by neutralizing a scandium carbonate solution from an initial pH of about 11.0 to a final pH of 6.5 by adding a strong acid (e.g., HCl). The scandium concentrate can be re-slurried and washed with deionized water and optionally recovered by filtration. An embodiment of a method for obtaining a scandium concentrate is provided in WO2019 / 213753, which is incorporated herein in its entirety.
[0018] In the first step of the process, the Sc concentrate is treated with a strong acid (e.g., HCl) to obtain a solution having a pH of about 1.5 to 3.5 (in some embodiments, about 3.0 to 3.5, or about 3.0) (referred to herein as an impure Sc solution). In one embodiment, the pH of the impure Sc solution is at least about 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, or 3.4, and in another embodiment, the pH of the impure Sc solution does not exceed about 3.5, 3.4, 3.3, 3.2, 3.1, 3.0, 2.9, 2.8, 2.7, 2.6, 2.5, 2.4, 2.3, 2.2, 2.1, 2.0, 1.9, 1.8, 1.7, or 1.6. In another embodiment, the pH of the impure Sc solution is about 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3 or 3.4 to about 3.5, 3.4, 3.3, 3.2, 3.1, 3.0, 2.9, 2.8, 2.7, 2.6, 2.5, 2.4, 2.3, 2.2, 2.1, 2.0, 1.9, 1.8, 1.7 or 1.6. In one embodiment, the pH of the impure Sc solution is at least about 3.0, 3.1, 3.2, 3.3 or 3.4. In another embodiment, the pH of the impure Sc solution does not exceed about 3.5, 3.4, 3.3, 3.2 or 3.1. In another embodiment, the pH of the impure Sc solution is about 3.0, 3.1, 3.2, 3.3 or 3.4 to about 3.5, 3.4, 3.3, 3.2 or 3.1. In yet another embodiment, the pH of the impure Sc solution is about 3.0. In one embodiment, the Sc concentration of the impure Sc solution is about 1 to 20 g / L, and in some embodiments, the Sc concentration is about 1 to 10 g / L, 2 to 6 g / L or 4 to 5 g / L.
[0019] The method of the present disclosure is designed to at least partially remove some metal contaminants from the Sc concentrate by treating an impure Sc solution. The oxidation state of the metal contaminants that can be removed from the impure Sc solution by the method of the present disclosure (in the impure Sc solution) is at least 3. For example, they can include, but are not limited to, thorium (Th), iron (Fe), chromium (Cr) and zirconium (Zr). In a specific embodiment, the metal contaminants that can be removed from the impure Sc solution by the method of the present disclosure can include (and in some embodiments are limited to) thorium (Th) and zirconium (Zr). In a specific embodiment, the metal contaminants that can be removed from the impure Sc solution by the method of the present disclosure can include (and in some embodiments are limited to) thorium (Th). In some embodiments, the concentration of each metal contaminant in the Sc impure solution is about 10 to 500 mg / L. In one embodiment, the concentration of each metal contaminant in the Sc impure solution is at least about 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 150, 200, 250, 300, 350, 400, 450 mg / mL or more. In another embodiment, the concentration of each metal contaminant in the Sc impure solution is no more than 500, 450, 400, 350, 300, 250, 200, 150, 100, 90, 80, 70, 60, 50, 40, 30, 20 mg / mL or less. In another embodiment, the concentration of each metal contaminant in the Sc impure solution is about 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 150, 200, 250, 300, 350, 400, 450 mg / mL and about 500, 450, 400, 350, 300, 250, 200, 150, 100, 90, 80, 70, 60, 50, 40, 30, 20 mg / L.
[0020] Once the impure Sc solution is obtained, it is contacted with an ion exchange resin. "Ion exchange resin" is understood to be a resin that has an affinity for the metal ion of interest. The ion exchange resins that can be used in the methods of the present disclosure can be prepared with particles of so-called "chromatographic size" (e.g., an average diameter of about 200-400 μm) or "standard size" (e.g., an average diameter of about 300–1200 μm). The particles of the ion exchange resin can be cross-linked before being presented to the process.
[0021] The ion exchange resin used in the method for the present disclosure is a strongly acidic cationic resin, for example a sulfonate cationic resin. In the context of the present disclosure, the ion exchange resin comprises the sulfonic acid moiety that can capture metal ion pollutants and can also capture Sc in some embodiments. As known in the art, the ion exchange capacity (for example electric charge) that the strong cationic resin demonstrates does not change or changes very little with pH. In some embodiments, the strong cationic exchange resin does not or almost does not demonstrate change in the pH range of 1 to 14 (for example 2 to 14). This contrasts with the weak cation exchange resin that is only ionized in a limited pH range (for example 2 to 9).
[0022] The ion exchange resin used in the method of the present disclosure is in potassium or sodium form. As is known in the art, the "form" of an ion exchange resin refers to the counter cation adsorbed on the sulfonic acid functional group before treatment. In the present disclosure, it is preferred that the ion exchange resin includes potassium or sodium counter cations. In a specific embodiment, the ion exchange resin of the present disclosure includes sodium counter cations (e.g., in the resin in sodium form).
[0023] In some embodiments of the present disclosure, ion exchange resins in gel form may be used. Gel resins typically have small pores (e.g., about 1 to 2 nm when hydrated). Embodiments of gel ion exchange resins that can be used in the present disclosure include, but are not limited to, Purolite PCR642 TM or SSTC60 TM 、Diaion UBK(8) TM .
[0024] In other embodiments of the present disclosure, macroporous forms of ion exchange resins may be used. Macroporous resins typically have large pores (e.g., about 20 to 100 nm when hydrated). Embodiments of macroporous ion exchange resins that can be used in the present disclosure include, but are not limited to, Purolite C150. TM or PCR145K TM .
[0025] In the method of the present disclosure, two different types of ion exchange resins can be used. In a first embodiment, the method uses a first ion exchange resin that preferentially captures metal contaminants rather than Sc (at least not in a large amount). In this first embodiment, one or more metal contaminants form a complex with the first ion exchange resin (e.g., a loaded resin or a second ion exchange resin complex). In addition, when using the first ion exchange resin, a Sc raffinate is obtained. In this first aspect, since some Sc can be captured by resin, Sc can be eluted from the first ion exchange resin complex (e.g., a loaded resin) to obtain the first Sc eluent, which can optionally be merged with the Sc raffinate. In the first aspect of the method using the first ion exchange resin, a macroporous resin can be used.
[0026] In a second embodiment, the method uses a second ion exchange resin that can capture both the metal contaminants and Sc present in the impure Sc solution and form a complex therewith. When using the second ion exchange resin, the captured Sc needs to be eluted from the resin to obtain a second Sc eluent. The elution step can be carried out by contacting, for example, a second ion exchange resin complex (e.g., loaded resin) with a second eluent solution. Those skilled in the art will know how to select an eluent solution suitable for obtaining the second Sc eluent. In one embodiment, the eluent solution is a strong acid eluent solution, such as HCl solution (e.g., 1N HCl solution, 2N HCl solution, or 3N HCl solution). In a second embodiment of the method using the first ion exchange resin, macroporous or gel resins can be used.
[0027] In the method for the present disclosure, once Sc eluent and / or raffinate are obtained, resin can be regenerated to carry out new ion exchange circulation. In such an embodiment, the first and / or second ion exchange resin can be carried out elution step with other elution solution to remove the metal contaminants that may have been captured by resin. Those skilled in the art will know how to select the elution solution that is suitable for at least partially removing the metal contaminants captured or removing the metal contaminants captured by most of. In one embodiment, the elution solution is a strong acid elution solution, such as HCl solution (such as 4N HCl solution, 5N HCl solution, 6N HCl solution or 8N HCl solution). The metal contaminants of wash-out can be further processed or discarded.
[0028] The method of the present disclosure may further include a step for producing a refined scandium oxide product. In some embodiments, the content of each metal ion contaminant (e.g., metal contaminant) of the scandium oxide obtained using the purified Sc eluate and / or Sc raffinate described herein may be less than about 500, 450, 400, 350, 300, 250, 200, 150, 100, 90, 80, 70, 60, 50, 40, 30 or 10 ppm. In embodiments where the scandium concentrate includes Th as a metal ion contaminant, the scandium oxide obtained using the purified Sc eluate and / or raffinate described herein may have a Th content of less than about 500, 450, 400, 350, 300, 250, 200, 150, 100, 90, 80, 70, 60, 50, 40, 30 or 10 ppm in some embodiments.
[0029] exist Figure 1 An embodiment of a first embodiment of the method using a first ion exchange resin capable of preferentially capturing metal contaminants and Sc is shown in step 130. In a preliminary step, the crude Sc concentrate 105 can be dissolved in step 110 at a pH of 1.5 to 3.5 (for example at a pH of 3.0) and heated to a temperature of 20 to 100°C (for example, approximately 90°C). The dissolution step 110 can be accomplished using a concentrated acid (for example, HCl). The dissolution step produces a slurry 115, which is presented to a solid / liquid separation step 120. The solid residue obtained after step 120 (which may include, for example, Fe, Ti, Zr, Th, etc.) can be discarded as waste. The separated liquid obtained in step 120 is considered to be an impure Sc solution 125. In Figure 1 In FIG. 1 , an impure Sc solution containing Th as a metal ion contaminant is shown. In step 130, the impure Sc solution is loaded on a first ion exchange resin to produce a Sc solution containing metal ion contaminants ( Figure 1 Because the first ion exchange resin does not substantially capture Sc, step 130 produces a purified Sc raffinate 135-B. The loaded resin 133-A can be submitted to an elution step to collect Sc that may have been captured by the first ion exchange resin ( Figure 1Sc metal ions captured by the oxalate solution (not shown). The purified Sc raffinate 135-B (optionally combined with the obtained Sc eluate) can be presented to a precipitation step 140 with the addition of oxalic acid 143. The precipitation step 140 can be carried out at a temperature of 20 to 100° C. (e.g., at about 60° C.). The precipitation step can produce a slurry 145, which can be presented to a solid / liquid separation step 150. The solid 155 obtained from the separation step 150 can be presented to a calcination step 160, and the spent oxalate solution can be treated or reused. The calcination step 160 can include a step of subjecting the solid 155 to a temperature of 600 to 1000° C. (e.g., at about 900° C.) until a refined scandium oxide product 165 is obtained.
[0030] Figure 1 The step of regenerating the resin once the purified Sc raffinate 135-B and optional Sc eluate are obtained is also included. To this end, the resin 133-A can be treated with a strong acid solution (e.g., Figure 1 6N HCl solution as shown) to perform elution step 134. The eluate from step 134 can be further processed. The resin 133-B obtained after step 134 can be washed with an aqueous solution (e.g., Figure 1 The washed resin 133-C obtained from step 136 can be regenerated in step 138 using an alkaline solution (e.g., a 5-10% NaOH solution). The alkaline solution added in step 138 includes sodium or potassium ions. The regenerated resin 139 can be used in step 130 to perform an ion exchange step.
[0031] exist Figure 2 An embodiment of a second embodiment of the method using a second ion exchange resin capable of capturing both metal contaminants and Sc is shown in steps 130 and 132. Prior to steps 130 and 132, the crude Sc concentrate can be dissolved in step 110 at a pH of 1.5 to 3.5 (e.g., at a pH of 3.0) and heated to a temperature of 20 to 100°C (e.g., approximately 90°C). The dissolution step 110 can be accomplished using a concentrated acid (e.g., HCl). The dissolution step produces a slurry 115, which can be presented to a solid / liquid separation step 120. The solid residue obtained after step 120 (which may include, for example, Fe, Ti, Zr, Th, etc.) can be discarded as waste. The separated liquid obtained in step 120 is considered to be an impure Sc solution 125. In Figure 2 In FIG. 1 , an impure Sc solution containing Th as a metal ion contaminant is shown. In step 130, the impure Sc solution is loaded onto a first ion exchange resin to produce a loaded resin 131-A (also referred to as a second ion exchange resin complex) containing both Sc and Th. Figure 2Sc is separated from Th in the resin and the resin is presented to the elution step 132. In the elution step 132, a strong acid (e.g. Figure 2 3N HCl solution as shown) is applied to the loaded resin 131-A to obtain a purified Sc eluent 135-A. The acid used to elute Sc must be strong enough to remove Sc from the resin and leave behind most of the metal ion contaminants (e.g., Figure 2 Th) and most other contaminants in the Sc eluate. The purified Sc eluate 135-A can be presented to a precipitation step 140 where oxalic acid 143 is added. The precipitation step 140 can be performed at a temperature of 20 to 100° C., for example at about 60° C. The precipitation step 140 produces a slurry 145 which can be presented to a solid / liquid separation step 150. The solid 155 obtained from the separation step 150 can be presented to a calcination step 160, and the spent oxalate solution can be treated or reused. The calcination step 160 may include a step of subjecting the solid 155 to a temperature of 600 to 1000° C., for example a temperature of about 900° C., until a refined scandium oxide product 165 is obtained.
[0032] Figure 2 The step of regenerating the resin once the purified Sc eluent 135-A is obtained is also included. To this end, the resin 133-A can be treated with a strong acid solution (e.g., Figure 2 6N HCl solution as shown) for elution step 134. Because the second ion exchange resin has a greater affinity for metal contaminants than for Sc, the acidic solution for eluting metal ion contaminants from resin 133-A has a higher normality than the acidic solution for eluting Sc from resin 131-A. The eluate from step 134 can be further processed. Resin 133-B obtained after step 134 can be treated with an aqueous solution (e.g., Figure 2 The washed resin 133-C obtained from step 136 can be regenerated in step 138 using an alkaline solution (e.g., a 5-10% NaOH solution). The alkaline solution in step 138 includes sodium ions or potassium ions ( Figure 2 Regenerated resin 139 may be used in step 130 to perform an ion exchange step.
[0033] It will be appreciated by those skilled in the art that the final purity of the scandium oxide product 165 is directly affected by the initial purity of the scandium eluate or raffinate obtained after the ion exchange step 130 (and optionally 132). The methods described herein increase the final purity of the scandium oxide product by increasing the purity of the scandium eluate.
[0034] Example I - Resin Conditions (H + Form or Na + Effect of the form of ferrite on the selectivity of scandium and thorium
[0035] Using two H + form (i.e., having protons occupying active sites on the resin) or Na + Selectivity tests were performed on a strong cationic (sulfonate) gel-type resin in the 1% form (i.e., with sodium cations occupying the active sites of the resin). In each test, 15 mL of the resin and 100 mL of an impure scandium solution containing 4-5 g / L Sc at pH 3.0 were mixed in a beaker at ambient temperature for 12 hours to reach equilibrium. + For the use of Na + The resins were tested in the form of 200 μL of 100 μL ... + The resin in the form of 100% is more selective for scandium than for thorium. About 98% of the thorium is adsorbed on H + The thorium adsorbs on the Na + In the form of resin.
[0036] Table 1 Use H + Form and Na + Results of selectivity testing of two strong cationic (sulfonate) gel-type resins in the form of .
[0037]
[0038] Example II - Effect of pH of impure scandium solution on the selectivity of the resin for scandium and thorium
[0039] In order to evaluate the effect of the pH of the impure scandium solution on the selectivity of scandium and thorium of the strong cationic (sulfonate) resin, the gel-type chromatography resin Purolite PCR642 and the impure scandium solutions with different pH values containing 4-5g / L Sc and acidified with HCl were tested. All tests were carried out in a beaker, where 15mL of resin and 100mL of impure scandium solution were mixed together at ambient temperature for 12 hours to reach equilibrium. Prior to the test, the resin was adjusted to Na by contacting the resin with sodium hydroxide solution (5% w / w NaOH) solution for several hours. + form. After each test, the solutions were recovered by filtration and analyzed for their scandium and thorium content. As shown in Table 2, the selectivity of the resin for scandium is higher at relatively high pH values. The optimum pH for best selectivity is between 3.0 and 3.5. At these pH values, 75% of scandium is adsorbed, compared to less than 25% of thorium. At pH>3.5, scandium losses are significant because scandium begins to precipitate in solid form.
[0040] Table 2 Results of tests using (impure) scandium solution feeds at different pH values and the gel-type chromatography resin Purolite PCR642.
[0041]
[0042] Example III - Effect of Resin Type (Gel, or Macroporous) and Particle Size (Standard, or Chromatographic) on Its Scandium and Thorium Selectivity
[0043] To evaluate the effect of resin type (gel or macroporous) and resin particle size (300-1200 μm for standard, or 200-400 μm for chromatography) on the selectivity of scandium and thorium, different strong cationic (sulfonate) resins were used along with an impure scandium solution at pH 3.0 containing 4–5 g / L Sc and acidified with HCl. All tests were performed in a beaker where 15 mL of resin and 100 mL of the impure scandium solution were mixed together at ambient temperature for 12 hours to reach equilibrium. Prior to testing, the resin had been conditioned to Na by contact with a sodium chloride (5% w / w NaOH) solution for several hours. + form. After each test, the solutions were recovered by filtration and analyzed for their scandium and thorium contents. As shown in Table 3, the macroporous resin adsorbed almost 100% of the thorium in the solution. In addition, the results of Table 3 show that the resin of the chromatographic particle size is more selective for thorium than for scandium.
[0044] Table 3 Results of tests with different types and sizes of strong cationic (sulfonate) resins
[0045]
[0046] Example IV - Column purification of impure scandium solution using gel-type resin
[0047] UBK(8) resin from Diaion (a strong cationic resin made of polystyrene gel crosslinked with divinylbenzene (Na + A continuous column test was performed using a sulfonate in the form of a sulfonate. The adsorption was carried out in a column with a diameter of 1.5 cm and a resin volume of 12 mL, wherein the flow rate of the impure scandium solution was about 5 mL / min. The resin was washed with 100 mL of water at a flow rate of 10 mL / min. The scandium was eluted with 100 mL of a 3N HCl solution at a flow rate of 5 mL / min. The total recovery of scandium from the impure scandium solution to the scandium eluate was 73%, while the total recovery of thorium was only 2.7%, indicating that scandium has a higher selectivity relative to thorium. Finally, 300 mL of a 6N HCl solution was used to elute thorium from the resin at a flow rate of 5 mL / min.
[0048] Four cycles of adsorption (80 mL of acidified impure scandium solution at a flow rate of 5 mL / min), washing (30 mL of water at a flow rate of 5 mL / min), scandium elution (100 mL of 3N HCl solution at a flow rate of 5 mL / min), thorium elution (300 mL of 6N HCl solution at a flow rate of 5 mL / min), washing (100 mL of water at a flow rate of 5 mL / min), and conditioning (50 mL of a 5 wt% NaOH solution at a flow rate of 5 mL / min) were performed on the same column. The scandium eluates were combined and 50 mL of a 240 g / L hot oxalic acid solution was added to precipitate scandium as scandium oxalate. The precipitate was filtered, washed with deionized water, and calcined at 850°C overnight. The thorium content of the final product (scandium oxide) was determined by inductively coupled plasma mass spectrometry (ICP-MS) and found to be 410 ± 25 ppm (mg / kg). The chemical analyses of the initial solution (acidified impure scandium solution), the solution treated with the resin (raffinate), the scandium eluate and the resulting precipitated product are shown in Table 4.
[0049] Table 4 Chemical analysis of the initial solution, the raffinate, the scandium eluate and the filtrate of the scandium oxalate precipitation
[0050]
[0051]
[0052] The stability of the resin after four cycles of treatment as described above was determined. Figure 3 As shown in Figure 2, the adsorption of scandium remained stable, with 81 ± 3% of Sc adsorbed each time, corresponding to an average resin capacity of about 21 g / L Sc. Figure 3 As shown, the adsorption of thorium was low, 14 ± 3% per pass. Example V - Selectivity Testing and Column Purification of Impure Scandium Solutions Using Macroporous Resins
[0053] PCR145K resin from Purolite (a strong cationic resin made of macroporous polystyrene beads cross-linked with divinylbenzene (Na + The sulfonate form) was tested for selectivity.
[0054] For the selectivity test, 5-15 mL of resin was mixed with 100-200 mL of impure scandium solution (~5 g / L Sc, pH 3.0) at ambient temperature for 12-16 hours. After each test, the solution was analyzed again for scandium and thorium content. It was thus observed that the resin adsorbed 97% of thorium and only 7% of scandium (see Table 5 below, Test 4).
[0055] Table 5 Effect of test variables on the adsorption of scandium and thorium
[0056]
[0057] The selectivity of the PCR 145K resin for thorium is superior to that of corresponding gel-type resins (such as those described in Example IV, see Table 6).
[0058] Table 6 Comparison of gel-type and macroporous resins
[0059]
[0060]
[0061] * For gel-type resin, the adsorbed Sc is PCR145K resin is unadsorbed Sc.
[0062] A continuous column test was also performed using the resin PCR145K. Adsorption was performed in a column with a diameter of 1.5 cm and containing 12 mL of resin with a flow rate of 1 mL / min of 200 mL of an impure scandium solution. The resin was washed with 30 mL of water at a flow rate of 10 mL / min. Thorium was eluted with 300 mL of a 6N HCl solution at a flow rate of 5 mL / min. The resin was treated with 100 mL of a 5% w / w NaOH solution at a flow rate of 5 mL / min.
[0063] Oxalic acid is added to the raffinate (the solution after Th is adsorbed on the PCR145K resin) to precipitate scandium oxalate, and the purity of the final scandium oxide product is determined. The precipitation of scandium oxalate is completed by adding 50 mL of a 240 g / L hot oxalic acid solution to approximately 200 mL of a scandium-containing raffinate. The scandium oxalate precipitate is filtered, washed with water, and calcined overnight at 850°C to convert it into scandium oxide. The initial solution feed solution (impure scandium solution with a pH of 3.0), the raffinate, and the filtrate after the precipitation of scandium oxalate are analyzed by ICP-MS. The mass balance (based on chemical analysis) is shown in Table 7.
[0064] Table 7 Mass balance of initial solution, raffinate (solution treated with PCR145K) and solution after scandium oxalate precipitation
[0065]
[0066] The thorium content of the final scandium oxide product was analyzed and found to be only 56±13 ppm (mg / kg), which is far below the specification for commercial applications (usually less than 150 ppm Th).
[0067] Although the present invention has been described in conjunction with specific embodiments, it should be understood that the scope of the claims should not be limited by the preferred embodiments described in the examples, but should be given the broadest interpretation consistent with the entire specification.
Claims
1. A method for removing at least one metal contaminant from a scandium (Sc) concentrate, the method comprising: (a) contacting the Sc concentrate with an acidic solution to produce an impure Sc solution; and (b) contacting the impure scandium solution with a first ion exchange resin that captures at least one metal contaminant to produce a first ion exchange resin complex and a purified Sc raffinate, wherein the first ion exchange resin has a greater affinity for the at least one metal contaminant than for Sc; or contacting the impure Sc solution with a second ion exchange resin that captures at least one metal contaminant and Sc to produce a second ion exchange resin complex, wherein the second ion exchange resin has a greater affinity for the at least one metal contaminant than for Sc; eluting Sc from the second ion exchange resin complex with a second elution solution to obtain a purified Sc eluate; wherein the concentration of at least one metal contaminant in the purified Sc eluate or the purified Sc raffinate is lower than the concentration of at least one metal contaminant in the impure Sc solution; and Wherein the first ion exchange resin and the second ion exchange resin are strong acid cation resins having sulfonic acid functional groups in potassium or sodium form, the ion exchange capacity of the strong acid cation exchange resins does not show a change in the pH range of 1 to 14.
2. The method according to claim 1, wherein the Sc concentrate is in the form of a dry solid or an aqueous solid suspension.
3. The method of claim 1, wherein the sulfonic acid functional group is in the sodium form.
4. The method according to any one of claims 1 to 3, wherein the oxidation state of the at least one metal contaminant is at least 3. The method according to claim 4 , wherein the at least one metal contaminant is thorium (Th) or zirconium (Zr). The method according to claim 5 , wherein the at least one metal contaminant is Th.
7. The method according to any one of claims 1 to 3, wherein the pH of the impure Sc solution is from 1.5 to 3.
5.
8. The method according to claim 7, wherein the pH of the impure Sc solution is 3.0 to 3.
5.
9. The method according to any one of claims 1 to 3, wherein the acidic solution is an HCl solution.
10. The method according to any one of claims 1 to 3, comprising eluting Sc from the first ion exchange resin complex with a first elution solution to obtain a first Sc eluate and combining the first Sc eluate with the purified Sc raffinate.
11. The method according to any one of claims 1 to 3, wherein the second elution solution is a HCl solution.
12. The method of any one of claims 1 to 3, wherein the second ion exchange resin is a gel.
13. The method of any one of claims 1 to 3, wherein the first ion exchange resin is a macroporous resin.
14. The method of any one of claims 1 to 3, further comprising eluting at least one metal contaminant from the first ion exchange resin complex or the second ion exchange resin complex.
15. The method of claim 14, further comprising regenerating the first ion exchange resin or the second ion exchange resin to a sodium or potassium form.
16. A purified scandium (Sc) eluate obtained by the method of any one of claims 1 to 9, 11, 12, 14 and 15.
17. A purified scandium (Sc) raffinate obtained by the method of any one of claims 1 to 10 and 13 to 15.
18. A method for preparing a refined scandium (Sc) oxide product, the method comprising: (i) precipitating the purified Sc eluate according to claim 16 or the purified Sc raffinate according to claim 17 with oxalic acid to obtain a precipitate slurry having a solid portion and a liquid portion; (ii) separating the solid portion of the precipitation slurry from the liquid portion of the precipitation slurry to obtain a separated solid portion; and (iii) calcining the separated solid portion to obtain a refined Sc oxide product, wherein the refined Sc oxide product has a concentration of less than 500 ppm of at least one metal contaminant.
19. The refined scandium (Sc) oxide product obtained by the method according to claim 18.