An electromagnetic shielding film based on carbon nanotube composite waterborne polyurethane

By combining carbon nanotubes with water-based polyurethane and using electrospinning and vacuum impregnation technologies to prepare composite films, the problems of low utilization efficiency of nanoscale fillers and insufficient electromagnetic interference shielding performance in composite materials are solved, achieving high conductivity and excellent electromagnetic shielding. Effect.

CN114606763BActive Publication Date: 2024-10-11ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210373606.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-11
Publication Date
2024-10-11
Estimated Expiration
2042-04-11

AI Technical Summary

Technical Problem

It is difficult to effectively utilize nanoscale fillers in composite materials to improve mechanical and physical properties with existing technology, and there is also the problem of insufficient electromagnetic interference shielding performance.

Method used

Carbon nanotubes are combined with water-based polyurethane, a water-based polyurethane prepolymer is prepared through a prepolymer mixing method, and emulsified in water for chain growth. Nanofiber films are prepared using electrospinning, and the carbon nanotubes are combined with vacuum impregnation and ultrasound-assisted technology. Loaded on the fiber surface, it forms a composite film with high conductivity and excellent electromagnetic interference shielding performance.

Benefits of technology

The composite film achieves high electrical conductivity and good electromagnetic interference shielding effect, significantly improves the electromagnetic radiation shielding ability, and reduces the pollution of electromagnetic waves to the environment and human body.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of membrane materials, and discloses an electromagnetic shielding film based on carbon nanotube composite waterborne polyurethane. The present invention prepares a waterborne polyurethane prepolymer by a prepolymer mixing method, then directly emulsifies it in water and simultaneously performs chain growth to prepare a stable waterborne polyurethane, and uses a waterborne polyurethane emulsion (WPU) as a spinning solution to prepare a WPU nanofiber film by electrostatic spinning, which has high electrical conductivity, good mechanical properties and excellent electromagnetic interference shielding performance; then, vacuum impregnation and ultrasound are used to load CNTs on the surface of the WPU nanofiber film to form a conductive composite film that can be used for electromagnetic interference shielding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of film materials, and in particular to an electromagnetic shielding film based on carbon nanotube composite waterborne polyurethane. Background Art

[0002] Carbon nanotubes are tubular nanoscale graphite crystals, which are formed by one or more layers of graphene sheets bending around the central axis at a certain spiral angle. Carbon nanotubes can be divided into single-walled carbon nanotubes and multi-walled carbon nanotubes according to the number of graphene layers. The diameter of single-walled carbon nanotubes is generally 0.4-3nm, while multi-walled carbon nanotubes are coaxial tubes rolled up by multiple "graphene sheets". The interval between each sheet is 0.34nm, and the structure is kept stable by the van der Waals force. The total diameter can reach 100nm. Whether single-walled or multi-walled carbon nanotubes, they have a large aspect ratio, which can reach 1000~10000:1. They are truly one-dimensional materials. They can form a network structure in the matrix material, which can not only resist tensile loads and enhance the mechanical strength of the composite material, but also give the composite material special physical properties, such as changing the insulation and thermal insulation of the matrix material.

[0003] In the preparation method of composite materials, adding one material as a filler to another material system is the most common method. According to the size of the filler, it can be divided into macro fillers and nano fillers. Due to its large size, the macro filler will destroy the continuity of the matrix material and have a very adverse effect on the mechanical properties and processing properties of the composite material. In this case, it is very necessary to reduce the size of the filler. Once the diameter of the filler becomes nanoscale, the properties of the composite material will change significantly, and even when the amount of filler added is small (less than 5%), the mechanical and physical properties of the composite material can be greatly improved. Carbon nanotubes (CNTs), as a new type of one-dimensional carbon allotrope, have low density, large aspect ratio, good mechanical strength and high conductivity, and are excellent functional fillers for shielding materials.

[0004] Polyurethane was first synthesized by German scientist Otto Bayer in the 1940s. After decades of development, polyurethane has been widely used in the fields of construction, aviation, leather, etc. due to its excellent flexibility, wear resistance, corrosion resistance, strong adhesion and other properties. Polyurethane is formed by repeated urethane bonds (-NHCOO-) formed by polyisocyanates and polymer polyols (including polyether polyols and polyester polyols) with the assistance of diffusants and other additives. Its reaction raw materials are not unique. As for isocyanates, there are dozens of varieties such as toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI). It is worth mentioning that the monomers of polyurethane can be simplified into polyisocyanates and polyols. Polyols generally have longer chain lengths, which promote the fluidity of polyurethane; polyisocyanates are usually very short, show higher crystallinity, and produce dense and stacked fragments. Therefore, the ratio of polyols and polyisocyanates can be controlled to form products as soft as rubber or as hard as metal. Therefore, polyurethane products are of various types and have a wide range of applications. Therefore, polyols and polyisocyanates are also vividly called the soft segment and hard segment of polyurethane. WPU emulsion is used as the polymer matrix because of its environmental protection and excellent elastic properties. WPU is selected as the polymer matrix, considering its environmental protection and easy processing advantages, and a certain thickness of film can be obtained. This fiber film can recover quickly after unloading the load, has the characteristics of high elongation at break, high elasticity, low modulus, and has high thermal conductivity / electrical conductivity, good mechanical properties and excellent electromagnetic interference shielding performance. The elastic properties of WPU give it excellent flexibility and stretchability, and it is expected to become a composite material for commercial electromagnetic interference shielding. Summary of the invention

[0005] The present invention provides an electromagnetic shielding film based on carbon nanotube composite waterborne polyurethane. The present invention prepares a waterborne polyurethane prepolymer by a prepolymer mixing method, then directly emulsifies it in water and simultaneously performs chain growth to prepare a stable waterborne polyurethane, uses a waterborne polyurethane emulsion (WPU) as a spinning solution, and the WPU nanofiber film prepared by electrostatic spinning has high electrical conductivity, good mechanical properties and excellent electromagnetic interference shielding performance; then, CNTs are loaded on the surface of the WPU nanofiber film by vacuum impregnation and ultrasound assistance to form a conductive composite film that can be used for electromagnetic interference shielding.

[0006] The specific technical solution of the present invention is: an electromagnetic shielding film based on carbon nanotube composite waterborne polyurethane, the preparation method of which comprises the following steps:

[0007] (1) Preparation of WPU solution: Place polyether 3050 in a container and perform vacuum dehydration at high temperature. After the water is completely removed, cool the system, add 2,2-dihydroxymethylpropionic acid (DMPA) and toluene diisocyanate (TDI) to the system while stirring, and stir vigorously under an inert atmosphere to carry out prepolymerization reaction to obtain a prepolymer; cool the system, add triethylamine to carry out neutralization reaction to neutralize the carboxylic acid groups in the prepolymer, and then add Na2SO3 and water and stir vigorously to emulsify to obtain a WPU solution.

[0008] The present invention selects toluene diisocyanate (TDI) and polyether as the starting synthetic raw materials. The synthesized polyurethane has good film-forming property and can be firmly combined with fiber molecules.

[0009] The advantages of TDI as an aromatic isocyanate are that it is not easy to oxidize and has a relatively high activity. Its reactivity is much greater than that of aliphatic isocyanates. The -NCO groups in aromatic diisocyanates have an inductive effect on each other, which increases the reactivity of diisocyanates.

[0010] Polyether contains three functional groups with a good spatial structure, and can be well combined with fiber molecules to form a film. Polyether polyurethane has good flexibility and excellent low-temperature performance because the ether group of the soft segment is easier to rotate, and there is no ester group that is relatively easy to hydrolyze in the polyether, so its hydrolysis resistance is better than that of polyester. Since polyols generally contain a small amount of water, the presence of water will cause TDI to react side by side, consume the -NCO group in the system, form urea compounds, increase the branching degree of the product, and may cause gelation reaction. Therefore, the polyols must be dehydrated before the prepolymerization reaction to reduce the occurrence of side reactions.

[0011] The reaction rate ratio of -NCO group with H2O and Na2SO3 is 1:500000, indicating that Na2SO3 has greater nucleophilicity than H2O. After being capped with Na2SO3, the polyurethane prepolymer becomes an anionic polymer and has good water solubility.

[0012] The stability of the synthesized anionic waterborne polyurethane is closely related to the degree of neutralization. When the degree of neutralization increases to 100%, the -COOH in 2,2-dihydroxymethylpropionic acid (DMPA) is completely neutralized to form a salt to form an ion center, which plays a role in stabilizing the latex. When the degree of neutralization exceeds, the thickness of the adsorption layer increases, the hydrodynamic volume of the particles increases, and the particle size and viscosity increase. Triethylamine is also a flocculant. Free triethylamine molecules can agglomerate with polyurethane molecules to increase the particle size of polyurethane macromolecules.

[0013] (2) Preparation of WPU nanofiber film: The WPU solution was loaded into a syringe as a spinning solution, and the WPU nanofiber film was prepared by electrospinning technology.

[0014] Electrospinning technology has many advantages such as simple equipment, controllable process and low cost. It can prepare nanofiber films with large specific surface area and high porosity.

[0015] (3) Preparation of CNTs dispersion: CNTs and sodium dodecylbenzene sulfonate are added to water and subjected to ultrasonic treatment to obtain a uniformly dispersed CNTs dispersion.

[0016] Sodium dodecylbenzene sulfonate is a commonly used anionic surfactant, which is easily soluble in water and forms a translucent solution. It is chemically stable to alkali, dilute acid and hard water. Carbon nanotubes (CNTs), as a new type of one-dimensional carbon allotrope, have low density, large aspect ratio, good mechanical strength and high conductivity, and are excellent functional fillers for shielding materials. Ultrasonic dispersion equipment is suitable for laboratory-scale, low-viscosity medium dispersion of carbon nanotubes, so it can be used to prepare CNTs dispersions with good dispersion.

[0017] (4) Preparation of electromagnetic shielding film: Place the WPU nanofiber film in a container, evacuate the container, inject the CNTs dispersion into the container, immerse the WPU nanofiber film in a vacuum environment, take it out, dry and solidify it, then take it out and place it in another container filled with water, use ultrasound to strengthen the bonding strength of CNTs on the fiber surface, finally wash it with water and dry it to obtain an electromagnetic shielding film.

[0018] The present invention adopts the impregnation method. On the one hand, when the pores of the WPU film come into contact with the CNTs dispersion, capillary pressure is generated due to the effect of surface tension, which allows the liquid to penetrate into the capillary; on the other hand, the active components of the CNTs dispersion can be effectively adsorbed on the surface of the WPU film. The air in the carrier is evacuated in advance, which can increase the impregnation amount or the impregnation depth. In summary, the impregnation method has high utilization rate, small dosage and low cost.

[0019] Preferably, in step (1):

[0020] The temperature of the high temperature vacuum dehydration is 110-130°C and the time is 2-3h; the temperature of the prepolymerization reaction is 75-85°C and the time is 2-8h; the temperature of the neutralization reaction is 1-10°C and the time is 5-15min.

[0021] In terms of g, the amount of polyether 3050 used is 30-50 g, the amount of 2,2-dihydroxymethylpropionic acid (DMPA) used is 30-40 g, the amount of toluene diisocyanate (TDI) used is 3-8 g, the amount of triethylamine used is 1-5 g, and the amount of Na2SO3 used is 2-5 g.

[0022] The prepolymerization conditions determine that the R value is 1.5, the amount of chain extender is 6%, and polyether 3050 and toluene diisocyanate (TDI) are prepolymerized at 75-85℃ for 2-8h. Under these conditions, the prepolymer fully synthesized by the reaction has a low viscosity and a moderate molecular weight. The temperature of the end-capping reaction is selected at about 1-10℃, and the end-capping agent is Na2SO3, which has the highest end-capping rate. As the temperature rises, the side reactions increase; the main reaction cannot be protected for too long, which has little effect on the final end-capping rate.

[0023] Preferably, in step (1), the solid content of the WPU solution is 35-45wt%.

[0024] Preferably, in step (2), the conditions for electrospinning are: temperature of 20-30°C, relative humidity of 20-30%, voltage of 15-20kv; the specification of the metal needle tip used for electrospinning is 25-18G, the inner diameter is 0.3-0.4mm, and the outer diameter is 0.70-0.75mm; the spinning solution flux is 2-4ml / h.

[0025] Preferably, in step (3), in terms of mg and ml, the amount of CNTs used is 20-30 mg, the amount of sodium dialkylbenzene sulfonate used is 100-150 mg, and the amount of water used is 10-15 ml.

[0026] Preferably, in step (3), the ultrasonic power is 20-30%, and the ultrasonic time is 20-30 min.

[0027] Preferably, in step (4), the injection amount of the CNTs dispersion is 20-30 mg, and the immersion time is 5-15 min.

[0028] Preferably, in step (4), the drying conditions are: 60-75°C, 10-13h; and the ultrasonic time is 10-15min.

[0029] Compared with the prior art, the beneficial effects of the present invention are:

[0030] The present invention prepares waterborne polyurethane prepolymer by prepolymer mixing method, then directly emulsifies it in water and simultaneously performs chain growth to prepare stable waterborne polyurethane, uses waterborne polyurethane emulsion (WPU) as spinning solution, and the WPU nanofiber film prepared by electrostatic spinning has high conductivity, good mechanical properties and excellent electromagnetic interference shielding performance; then CNTs are loaded on the surface of the WPU nanofiber film by vacuum impregnation and ultrasound assistance to form a conductive composite film that can be used for electromagnetic interference shielding. The composite film not only has good conductive properties, but also can effectively shield electromagnetic interference, can largely solve the problem of electromagnetic radiation, and reduce electromagnetic pollution caused by electromagnetic waves to the surrounding environment and human body. DETAILED DESCRIPTION

[0031] The present invention will be further described below in conjunction with the embodiments.

[0032] Example 1

[0033] 1) Preparation of WPU solution: Weigh 30g of polyether 3050 and place it in a four-necked flask. Dehydrate it under high temperature vacuum at 110℃ for 2h. After the water is completely removed, install a thermometer, a stirrer and a reflux condenser on the flask. After the system temperature cools to 75℃, add 30g of 2,2-dihydroxymethylpropionic acid (DMPA) and 5g of toluene diisocyanate (TDI) to the system while stirring. Stir the reaction vigorously for 4h under N2 atmosphere with a magnetic stirring device to obtain a prepolymer. The change of NCO value during the reaction is determined by standard dibutylamine titration. According to the NCO value determined by this method, the stoichiometric amount of BD is added dropwise and dissolved in 30ml of acetone C3H6O until the theoretical NCO content is reached. The temperature was lowered by using a vacuum circulation cooling system, and 3 g of triethylamine was added to react for 5 minutes to neutralize the carboxylic acid groups in the prepolymer. The neutralization reaction temperature was 3°C and the time was 5 minutes. Then 2 g of Na2SO3 and pure distilled water were added and stirred vigorously to perform an emulsification reaction to obtain a WPU solution with a solid content of 35 wt%.

[0034] 2) Preparation of WPU nanofiber film: The electrospinning of nanofibers was carried out on a magnetic field-assisted electrospinning device, called magneto-electrospinning (MES). A medical syringe was used to contain the WPU spinning solution, and the temperature was set to 25 °C and the relative humidity was 25% at an electrospinning voltage of 15 kv, and the metal needle tip connected to the positive pole of the power supply was used as the spinning tip. The specification of the metal needle tip for electrospinning was 25G, with an inner diameter of 0.3 mm and an outer diameter of 0.70 mm. A piece of flat aluminum foil connected to the negative pole of the power supply was used as a collector for the electrospun fibers and was glued to the surface of the permanent magnet. The rotation distance was controlled by fixing the permanent magnet and the grounded aluminum foil on the distance regulator. In order to avoid the droplets hanging vertically from the needle and the covering of the spun nanofibers, the needle and the collector were placed on the same horizontal line so that the droplets could move horizontally and parabolically under the action of gravity, and they were separated from the electrospun nanofibers. The spinning solution reached the needle tip through the syringe, maintaining a spinning solution flux of 2 ml / h. When the high-voltage DC power supply is turned on, the droplet suspended on the needle tip is stretched by a combination of electric and magnetic forces. In the space between the tip and the aluminum foil, the droplet is stretched and refined, the solution evaporates, and the fiber is solidified. Finally, a nanofiber WPU film of a certain thickness is deposited on the aluminum foil.

[0035] 3) Preparation of CNTs dispersion: Take 20 mg of CNTs, weigh 100 mg of sodium dodecylbenzene sulfonate, and add them to 10 ml of deionized water. Use a cell crusher to ultrasonically treat the CNTs, set the power to 20%, and ultrasonicate for 20 minutes to obtain a uniformly dispersed CNTs dispersion.

[0036] 4) Preparation of CNTs / WPU film: The WPU film was placed in a vacuum bottle, and the air was removed by a vacuum pump. The CNTs dispersion obtained in step 3) was then injected into the vacuum bottle by a syringe. The WPU film was immersed in a vacuum environment for 5 minutes and then taken out. It was then placed in a blast oven and dried and cured at 70°C for 10 hours. It was then taken out and placed in a container filled with deionized water. Ultrasonic assistance was applied for 10 minutes to strengthen the firmness of the conductive material on the fiber surface. Finally, it was washed with deionized water several times and dried to obtain a conductive CNTs / WPU film with a conductivity of 367.4 Sm −1 , electromagnetic interference (EMI) shielding efficiency (SE) is 23.2dB, and the elongation at break is 60%.

[0037] Example 2

[0038] 1) Preparation of WPU solution: Weigh 40g of polyether 3050 and place it in a four-necked flask, dehydrate it under high temperature vacuum at 120℃ for 2.5h, and wait for the water to be completely removed. Install a thermometer, a stirrer and a reflux condenser on the flask, wait for the system temperature to cool to 80℃, and add 35g of 2,2-dihydroxymethylpropionic acid (DMPA) and 6g of toluene diisocyanate (TDI) to the system while stirring. Use a magnetic stirring device to vigorously stir the reaction for 6h under N2 atmosphere to obtain a prepolymer. The change of NCO value during the reaction is determined by the standard dibutylamine titration method. According to the NCO value determined by this method, the stoichiometric amount of BD is added dropwise and dissolved in 35ml of acetone C3H6O until the theoretical NCO content is reached. The temperature was lowered by a vacuum circulation cooling system, and 4 g of triethylamine was added to react for 10 minutes to neutralize the carboxylic acid groups in the prepolymer. The neutralization reaction temperature was 6°C and the time was 10 minutes. Then 3 g of Na2SO3 and pure distilled water were added and stirred vigorously to perform an emulsification reaction to obtain a WPU solution with a solid content of 40 wt%.

[0039] 2) Preparation of WPU nanofiber film: The electrospinning of nanofibers was carried out on a magnetic field-assisted electrospinning device, called magneto-electrospinning (MES). A medical syringe was used to contain the WPU spinning solution, and the temperature was set to 20 °C and the relative humidity was 20% at an electrospinning voltage of 17 kv, and the metal needle tip connected to the positive pole of the power supply was used as the spinning tip. The specification of the metal needle tip for electrospinning was 22G, with an inner diameter of 0.35 mm and an outer diameter of 0.725 mm. A piece of flat aluminum foil connected to the negative pole of the power supply was used as a collector for the electrospun fibers and was glued to the surface of the permanent magnet. The rotation distance was controlled by fixing the permanent magnet and the grounded aluminum foil on the distance regulator. In order to avoid the droplets hanging vertically from the needle and the covering of the spun nanofibers, the needle and the collector were placed on the same horizontal line so that the droplets could move horizontally and parabolically under the action of gravity, and they were separated from the electrospun nanofibers. The spinning solution reaches the needle tip through a syringe, maintaining a spinning solution flux of 3 ml / h. When the high-voltage DC power supply is turned on, the droplet suspended on the needle tip is stretched by a combination of electric and magnetic forces. In the space between the tip and the aluminum foil, the droplet is stretched and refined, the solution evaporates, and the fiber is solidified. Finally, a nanofiber WPU film of a certain thickness is deposited on the aluminum foil.

[0040] 3) Preparation of CNTs dispersion: Take 25 mg of CNTs and weigh 125 mg of sodium dodecylbenzene sulfonate, add them to 12 ml of deionized water. Use a cell crusher to ultrasonically treat the CNTs, set the power to 25%, and ultrasonicate for 25 minutes to obtain a uniformly dispersed CNTs dispersion.

[0041] 4) Preparation of CNTs / WPU film: The WPU film was placed in a vacuum bottle, and the air was removed by a vacuum pump. The CNTs dispersion obtained in step 3) was then injected into the vacuum bottle by a syringe. The WPU film was immersed in a vacuum environment for 10 minutes and then taken out. It was then placed in a blast oven, dried and cured at 60°C for 10 hours, and then taken out and placed in a container filled with deionized water. Ultrasonic assistance was applied for 11 minutes to strengthen the firmness of the conductive material on the fiber surface. Finally, it was washed with deionized water several times and dried to obtain a conductive CNTs / WPU film with a conductivity of 374.8 Sm −1 , the electromagnetic interference (EMI) shielding efficiency (SE) is 23.9dB, and the elongation at break is 61%.

[0042] Example 3

[0043] 1) Preparation of WPU solution: Weigh 50g of polyether 3050 and place it in a four-necked flask. Dehydrate it under high temperature vacuum at 130℃ for 3h. After the water is completely removed, install a thermometer, a stirrer and a reflux condenser on the flask. After the system temperature is cooled to 85℃, add 40g of 2,2-dimethylolpropionic acid (DMPA) and 7g of toluene diisocyanate (TDI) to the system while stirring. Stir the reaction vigorously for 8h under N2 atmosphere with a magnetic stirring device to obtain a prepolymer. The change of NCO value during the reaction is determined by standard dibutylamine titration. According to the NCO value determined by this method, the stoichiometric amount of BD is added dropwise and dissolved in 40ml of acetone C3H6O until the theoretical NCO content is reached. The temperature was lowered by using a vacuum circulation cooling system, and 5 g of triethylamine was added to react for 15 minutes to neutralize the carboxylic acid groups in the prepolymer. The neutralization reaction temperature was 9°C and the time was 15 minutes. Then 4 g of Na2SO3 and pure distilled water were added and stirred vigorously to perform an emulsification reaction to obtain a WPU solution with a solid content of 45 wt%.

[0044] 2) Preparation of WPU nanofiber film: The electrospinning of nanofibers was carried out on a magnetic field-assisted electrospinning device, called magneto-electrospinning (MES). A medical syringe was used to contain the WPU spinning solution, and the temperature was set to 30 °C and the relative humidity was 30% at an electrospinning voltage of 19 kv, and the metal needle tip connected to the positive pole of the power supply was used as the spinning tip. The specification of the metal needle tip for electrospinning was 19G, with an inner diameter of 0.4 mm and an outer diameter of 0.75 mm. A piece of flat aluminum foil connected to the negative pole of the power supply was used as a collector for the electrospun fibers and was glued to the surface of the permanent magnet. The rotation distance was controlled by fixing the permanent magnet and the grounded aluminum foil on the distance regulator. In order to avoid the droplets hanging vertically from the needle and the covering of the spun nanofibers, the needle and the collector were placed on the same horizontal line so that the droplets could move horizontally and parabolically under the action of gravity, and they were separated from the electrospun nanofibers. The spinning solution reached the needle tip through the syringe, maintaining a spinning solution flux of 4 ml / h. When the high-voltage DC power supply is turned on, the droplet suspended on the needle tip is stretched by a combination of electric and magnetic forces. In the space between the tip and the aluminum foil, the droplet is stretched and refined, the solution evaporates, and the fiber is solidified. Finally, a nanofiber WPU film of a certain thickness is deposited on the aluminum foil.

[0045] 3) Preparation of CNTs dispersion: Take 30 mg CNTs, weigh 150 mg sodium dodecylbenzene sulfonate, and add them to 14 ml deionized water. Use a cell crusher to ultrasonically treat the CNTs, set the power to 30%, and ultrasonicate for 30 minutes to obtain a uniformly dispersed CNTs dispersion.

[0046] 4) Preparation of CNTs / WPU film: Place the WPU film in a vacuum bottle, use a vacuum pump to remove the air, and then inject the CNTs dispersion obtained in step 3) into the vacuum bottle through a syringe. After the WPU film is immersed in a vacuum environment for 15 minutes, it is taken out and placed in a blast oven. Dry and cure at 75°C for 12 hours, then take it out and place it in a container filled with deionized water. Ultrasonic assistance is used for 10 minutes to strengthen the firmness of the conductive material on the fiber surface. Finally, it is washed with deionized water several times and dried to obtain a conductive CNTs / WPU film with a conductivity of 372.6 Sm −1 , the electromagnetic interference (EMI) shielding efficiency (SE) is 24.7dB and the elongation at break is 62%.

[0047] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0048] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. An electromagnetic shielding film based on carbon nanotube composite waterborne polyurethane, characterized in that: The preparation method comprises the following steps: (1) Preparation of WPU solution: Place polyether 3050 in a container, dehydrate under high temperature and vacuum, cool after the water is completely removed, add 2,2-dihydroxymethyl propionic acid and toluene diisocyanate to the system while stirring, and stir vigorously under an inert atmosphere to carry out prepolymerization reaction to obtain a prepolymer; cool down, add triethylamine to carry out neutralization reaction to neutralize the carboxylic acid groups in the prepolymer, and then add Na2SO3 and water and stir vigorously to emulsify to obtain a WPU solution; The temperature of the high temperature vacuum dehydration is 110-130°C, and the time is 2-3h; the temperature of the prepolymerization reaction is 75-85°C, and the time is 2-8h; the temperature of the neutralization reaction is 1-10°C, and the time is 5-15min; The dosage of polyether 3050 is 30-50g, the dosage of 2,2-dimethylol propionic acid is 30-40g, the dosage of toluene diisocyanate is 3-8g, the dosage of triethylamine is 1-5g, and the dosage of Na2SO3 is 2-5g; The solid content of the WPU solution is 35-45wt%; (2) Preparation of WPU nanofiber film: The WPU solution was loaded into a syringe as a spinning solution, and the WPU nanofiber film was prepared by electrospinning technology; (3) Preparation of CNTs dispersion: CNTs and sodium dodecylbenzene sulfonate are added to water and subjected to ultrasonic treatment to obtain a uniformly dispersed CNTs dispersion; in terms of mg and ml, the amount of CNTs used is 20-30 mg, the amount of sodium dodecylbenzene sulfonate used is 100-150 mg, and the amount of water used is 10-15 ml; Preparation of electromagnetic shielding film: put the WPU nanofiber film into a container, evacuate it, inject the CNTs dispersion into the container, immerse the WPU nanofiber film in a vacuum environment, take it out, dry and solidify it, then take it out and put it in another container filled with water, use ultrasound to strengthen the bonding firmness of CNTs on the fiber surface, finally wash it with water and dry it to obtain the electromagnetic shielding film; The injection amount of CNTs dispersion is 20-30 mg, and the immersion time is 5-15 min.

2. The electromagnetic shielding film according to claim 1, characterized in that: In step (2), the conditions for electrospinning are: temperature of 20-30°C, relative humidity of 20-30%, voltage of 15-20kv; the specification of the metal needle tip used for electrospinning is 25-18G, the inner diameter is 0.3-0.4mm, and the outer diameter is 0.70-0.75mm; the spinning solution flux is 2-4ml / h.

3. The electromagnetic shielding film according to claim 1, characterized in that: In step (3), the ultrasonic power is 20-30%, and the ultrasonic time is 20-30 minutes.

4. The electromagnetic shielding film according to claim 1, characterized in that: In step (4), the drying conditions are: 60-75°C, 10-13h; and the ultrasonic time is 10-15min.