Preparation method and application of carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film
By introducing carboxylated multi-walled carbon nanotube intermediate layer into the nanofiltration membrane, the contradiction between the permeability and retention rate of the existing nanofiltration membrane in lithium resource recovery is solved, and high lithium ion enrichment and water flux are achieved The improvement is suitable for lithium battery wastewater treatment, with excellent permeability and selectivity.
Patent Information
- Application Number
- CN202210227818.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-03-08
AI Technical Summary
The existing nanofiltration membranes are difficult to improve permeability while increasing the interception rate, and there are problems such as poor hydrophilicity, poor permeability, poor thermal stability and easy pollution, making it difficult to meet the needs of lithium resource recycling and environmental protection.
Carboxylated multi-walled carbon nanotubes are used as intermediate layer material, and nanocomposite membranes are prepared by ultrasonic stirring, vacuum suction filtration, interfacial polymerization and other steps to form a carboxylated multi-walled carbon nanotube intermediate layer with high permeability and high selectivity. Thin film nanocomposite film.
The high lithium ion enrichment rate and water flux have been achieved, breaking the trade-off effect between permeability and retention rate in traditional polymer films, improving the mechanical strength and selectivity of the film, and suitable for retirement three Treatment of acid-soaked wastewater in the lithium battery.
Smart Images

Figure CN114609067B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a nano composite film and application thereof. Background Art
[0002] With the increasing shortage of global fossil resources and the increasing emphasis on environmental protection, it is a common understanding that the development and application of some high-tech technologies such as electric vehicles can reduce environmental pollution, which will also lead to the continuous expansion of lithium resource consumption. However, the problem of recycling and processing of waste lithium batteries comes with it. Lithium-ion batteries contain a large amount of valuable metals and organic matter. If they are not recycled, they will cause environmental pollution and waste of resources. Moreover, the supply of lithium resources is difficult to meet the strong demand for lithium consumption. Therefore, it is urgent to recycle lithium metal in wastewater, which can not only alleviate the consumption of lithium resources, but also solve the environmental problems caused by the discharge of waste lithium batteries.
[0003] In continuous operation, membrane separation technology is easy to operate, has low energy consumption, and can be controlled at any time, so it has shown broad application prospects in lithium resource recovery. The size of nanofiltration membrane is between that of ultrafiltration membrane and reverse osmosis membrane, with high permeability and selectivity, and is widely used in seawater desalination, sewage treatment and other fields. At present, the most widely used nanofiltration membrane is thin film composite (TFC) nanofiltration membrane, and the interfacial polymerization method has the advantages of self-inhibition, mild reaction conditions, fast membrane formation speed, and the formed polyamide selective layer is extremely thin, thus becoming the most commonly used and most effective method for preparing nanofiltration membrane. However, the prepared TFC membrane still faces the problems of poor hydrophilicity, poor permeability, low interception performance, poor thermal stability, and easy pollution of traditional polyamide membranes. Therefore, how to prepare a nanofiltration membrane with high permeability, high selectivity, and high mechanical strength has become a hot spot and difficulty for scientific researchers to pay attention to and solve. Summary of the invention
[0004] The present invention aims to solve the technical problem that the existing polymer films are subject to the trade-off effect between permeability and retention rate, and it is difficult to increase the permeation flux while increasing the retention rate of the membrane, and to provide a method for preparing a carboxylated multi-walled carbon nanotube intermediate layer film nanocomposite membrane and its application.
[0005] The method for preparing the carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film of the present invention is carried out according to the following steps:
[0006] 1. dispersing carboxylated multi-walled carbon nanotubes in deionized water and stirring with ultrasound at room temperature to obtain a carboxylated multi-walled carbon nanotube aqueous solution;
[0007] The mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution is 0.001wt% to 0.008wt%;
[0008] 2. Coat the carboxylated multi-walled carbon nanotube aqueous solution in step 1 on the polyethersulfone membrane washed with anhydrous ethanol by vacuum filtration, dry in a drying oven at a temperature of 50° C. to 70° C. for 25 min to 35 min, and cool to room temperature;
[0009] The present invention has no special limitation on the vacuum filtration device, and any vacuum filtration device well known to those skilled in the art can be used;
[0010] 3. Soak the film cooled in step 2 in deionized water for 25 to 30 minutes, take it out and dry it naturally in the air, then soak it in a PIP (piperazine) aqueous solution for 1 to 5 minutes, pour out the liquid, and dry the film naturally in the air to obtain a PIP saturated film;
[0011] The concentration of the PIP aqueous solution is 10 g / L to 20 g / L;
[0012] 4. Immerse the PIP saturated film prepared in step 3 in a hexane solution of TMC (trimesoyl chloride) for 30s to 90s to cause an interfacial polymerization reaction, pour out the liquid, and then place the film in a drying oven for heat treatment for 10min to 20min at a temperature of 50°C to 70°C;
[0013] The concentration of the TMC n-hexane solution is 0.1 g / L to 2 g / L;
[0014] 5. Rinse with deionized water to remove unreacted monomers and solvents on the membrane surface, and dry at room temperature to obtain a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane.
[0015] The carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane prepared by the present invention is applied to the treatment of acid leaching wastewater of retired ternary lithium batteries. The treatment method is: adjusting the pH of the wastewater to 1-2, and enriching the lithium element through filtering through the composite membrane.
[0016] The carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane prepared by the present invention breaks the trade-off effect between the permeability and interception rate of traditional polymer films and achieves a higher lithium enrichment rate.
[0017] Previously, retention rate and water flux were two important parameters for evaluating nanofiltration membranes. However, in order to better reflect the selectivity of the present invention for metal ions and the enrichment of lithium elements in acid leaching wastewater of retired ternary lithium batteries, the concept of enrichment rate was proposed, and the enrichment rate and water flux were used to evaluate the performance of the present invention.
[0018] The enrichment rate E (%) is defined as: under certain operating conditions, the concentration of solute in the permeate (Cp) and the concentration of solute in the feed solution (C f) and multiply by 100:
[0019]
[0020] Water flux is defined as the volume of water that passes through a unit membrane area per unit time under certain operating conditions. The unit in this invention is L / (m 2 h).
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention embeds a nanomaterial intermediate layer during the preparation of a traditional thin film composite membrane (TFC), utilizes the nanomaterial's nanochannels and negative charges to modify the TFC membrane, and further adjusts the permeation path of pure water and the filtration rate of metal ions, thereby affecting the membrane's permeation of water in wastewater or the retention of metal ions.
[0023] The present invention uses carboxylated multi-walled carbon nanotubes as the middle layer, and the optimized low monomer concentration PIP and TMC used form a thinner polyamide selection layer on the surface of the middle layer to obtain a good nano-technology thickness. The carboxylated multi-walled carbon nanotubes provide a large number of nanochannels, which greatly improve the water flux and enrichment rate of the membrane, and at the same time improve the mechanical strength of the membrane. The prepared new thin film nanocomposite membrane (TFNi) has better permeability and interception than traditional TFC membranes, and has the hydrophilicity, antibacterial and thermal stability of nanomaterials, and can be widely used in the separation of various salts. At the same time, the membrane was used for the first time to treat acid leaching wastewater from retired ternary lithium batteries. The maximum enrichment rates of monovalent lithium ions, divalent nickel ions, divalent manganese ions and divalent cobalt ions were 85.86%, 1.38%, 4.73% and 0 respectively. It has high selectivity, achieves the maximum enrichment of lithium elements, and can fully intercept Ni in the wastewater. 2+ , Mn 2+ 、Co 2+ , improve Li + The enrichment rate can also increase the pure water permeation flux of the membrane. The maximum water flux is 31.83L / (m 2 h). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The synthetic process flow chart of the carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film of the present invention;
[0025] Figure 2 This is a diagram showing the structural formula of carboxylated multi-walled carbon nanotubes in step 1 of experiment 1. DETAILED DESCRIPTION
[0026] Specific implementation method 1: This implementation method is a method for preparing a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film, which is specifically carried out according to the following steps:
[0027] 1. dispersing carboxylated multi-walled carbon nanotubes in deionized water and stirring with ultrasound at room temperature to obtain a carboxylated multi-walled carbon nanotube aqueous solution;
[0028] The mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution is 0.001wt% to 0.008wt%;
[0029] 2. Coat the carboxylated multi-walled carbon nanotube aqueous solution in step 1 on the polyethersulfone membrane washed with anhydrous ethanol by vacuum filtration, dry in a drying oven at a temperature of 50° C. to 70° C. for 25 min to 35 min, and cool to room temperature;
[0030] 3. Soak the film cooled in step 2 in deionized water for 25 to 30 minutes, take it out and dry it naturally in the air, then soak it in the PIP aqueous solution for 1 to 3 minutes, pour out the liquid, and dry the film naturally in the air to obtain a PIP saturated film;
[0031] The concentration of the PIP aqueous solution is 12 g / L to 18 g / L;
[0032] 4. Immerse the PIP saturated film prepared in step 3 in a n-hexane solution of TMC for 45s to 75s to cause an interfacial polymerization reaction, pour out the liquid, and then place the film in a drying oven for heat treatment for 12min to 18min at a heat treatment temperature of 50°C to 70°C;
[0033] The concentration of the TMC n-hexane solution is 0.2 g / L to 1 g / L;
[0034] 5. Rinse with deionized water to remove unreacted monomers and solvents on the membrane surface, and dry at room temperature to obtain a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane.
[0035] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the carboxylated multi-walled carbon nanotubes described in step 1 are powders with a purity of 98%, an outer diameter of 10 nm to 20 nm, and a length of 10 μm to 30 μm. Other aspects are the same as those of specific embodiment 1.
[0036] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the ultrasonic stirring time in step 1 is 12 min to 18 min, and the ultrasonic stirring frequency is 30 kHz to 40 kHz. Other aspects are the same as specific implementation method 1 or 2.
[0037] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that: the preparation method of the polyethersulfone membrane after washing with anhydrous ethanol described in step 2 is: soaking the polyethersulfone membrane in anhydrous ethanol for 1.5h to 2.5h can remove impurities on the surface of the polyethersulfone membrane and improve the hydrophilicity of the surface of the polyethersulfone membrane. Others are the same as specific embodiments 1 to 3.
[0038] Specific embodiment 5: This embodiment differs from specific embodiment 4 in that: the vacuum filtration pressure in step 2 is -0.1MPa to -0.085MPa; vacuum filtration can make the carboxylated multi-walled carbon nanotubes evenly coated on the surface of the polyethersulfone membrane, thereby improving the bonding force between the carboxylated multi-walled carbon nanotube intermediate layer and the polyethersulfone-based membrane. The rest is the same as specific embodiment 4.
[0039] Specific embodiment six: This embodiment is the application of the carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane prepared in specific embodiment one, which is applied to the treatment of acid leaching wastewater from retired ternary lithium batteries. The treatment method is: adjusting the pH of the wastewater to 1-2, and enriching the lithium element through filtering through the composite membrane.
[0040] Specific embodiment 7: This embodiment differs from specific embodiment 6 in that the metal ions in the acid leaching wastewater of retired ternary lithium batteries are one or more of monovalent lithium ions, divalent nickel ions, divalent manganese ions and divalent cobalt ions. The rest is the same as specific embodiment 6.
[0041] Specific implementation eight: This implementation differs from specific implementation seven in that: the Li + The concentration of Ni is 50mg / L~100mg / L; 2+ The concentration of Mn is 100mg / L~600mg / L; 2+ The concentration of Co is 50mg / L~200mg / L; 2+ The concentration is 50 mg / L to 200 mg / L. Other aspects are the same as those of the seventh embodiment.
[0042] The present invention is verified by the following tests:
[0043] Experiment 1: This experiment is a method for preparing a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film, which is specifically carried out in the following steps:
[0044] 1. dispersing carboxylated multi-walled carbon nanotubes in deionized water and stirring with ultrasound at room temperature to obtain a carboxylated multi-walled carbon nanotube aqueous solution;
[0045] The ultrasonic stirring time was 15 min, and the ultrasonic stirring frequency was 35 kHz;
[0046] The mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution is 0.001wt%;
[0047] The carboxylated multi-walled carbon nanotubes are powders with a purity of 98%, an outer diameter of 10nm to 20nm, and a length of 10μm to 30μm;
[0048] 2. Coat the carboxylated multi-walled carbon nanotube aqueous solution in step 1 on the polyethersulfone membrane washed with anhydrous ethanol by vacuum filtration, fix the obtained double-layer membrane in a culture dish, seal it with plastic wrap, pierce holes and put it into an oven at a drying temperature of 60° C. for 30 min, and cool it to room temperature;
[0049] The preparation method of the polyethersulfone membrane after being washed with anhydrous ethanol is as follows: soaking the polyethersulfone membrane in anhydrous ethanol for 2 hours to remove impurities on the surface of the polyethersulfone membrane, improve the hydrophilicity of the surface of the polyethersulfone membrane, and finally drying;
[0050] The vacuum filtration pressure is -0.1MPa to -0.085MPa; vacuum filtration can make the carboxylated multi-walled carbon nanotubes evenly coated on the surface of the polyethersulfone membrane, thereby improving the bonding force between the middle layer of the carboxylated multi-walled carbon nanotubes and the polyethersulfone-based membrane;
[0051] The vacuum filtration device comprises a circulating water multi-purpose vacuum pump and a filter cup-sand core-filter bottle connection type membrane making device, wherein the polyethersulfone membrane cleaned with anhydrous ethanol is placed on the upper part of the sand core, the filter cup is fixed on the upper part of the sand core, the lower part of the sand core is connected to the filter bottle, and the circulating water multi-purpose vacuum pump is connected, and then the carboxylated multi-walled carbon nanotube aqueous solution is poured into the filter cup from above, and the carboxylated multi-walled carbon nanotube solution is vacuum filtered onto the polyethersulfone membrane to form an intermediate layer;
[0052] 3. Soak the film cooled in step 2 in deionized water for 30 minutes, take it out and dry it naturally in the air, then immerse it in the PIP aqueous solution for 2 minutes, pour out the liquid, and dry the film naturally in the air to obtain a PIP saturated film;
[0053] The concentration of the PIP aqueous solution is 15 g / L;
[0054] 4. Immerse the PIP saturated film prepared in step 3 in a n-hexane solution of TMC for 60 seconds to cause an interfacial polymerization reaction, pour out the liquid, and then place the film in a drying oven for heat treatment for 15 minutes at a temperature of 60°C.
[0055] The concentration of the TMC n-hexane solution is 0.4 g / L;
[0056] 5. Rinse with deionized water to remove unreacted monomers and solvents on the membrane surface, and dry at room temperature to obtain a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane, which is recorded as M-1.
[0057] Experiment 2: This experiment differs from Experiment 1 in that the mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution in step 1 is 0.002 wt %, and the rest is the same as Experiment 1. The resulting thin film nanocomposite membrane is denoted as M-2.
[0058] Experiment 3: This experiment is different from Experiment 1 in that the mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution in step 1 is 0.003 wt %, and the rest is the same as Experiment 1. The resulting thin film nanocomposite membrane is denoted as M-3.
[0059] Experiment 4: This experiment is different from Experiment 1 in that the mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution in step 1 is 0.004 wt %, and the rest is the same as Experiment 1. The resulting thin film nanocomposite membrane is denoted as M-4.
[0060] Experiment 5: This experiment is different from Experiment 1 in that the mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution in step 1 is 0.005 wt %, and the rest is the same as Experiment 1. The resulting thin film nanocomposite membrane is denoted as M-5.
[0061] Experiment 6: This experiment is different from Experiment 1 in that the mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution in step 1 is 0.006 wt %, and the rest is the same as Experiment 1. The resulting thin film nanocomposite membrane is denoted as M-6.
[0062] Experiment 7: This experiment is different from Experiment 1 in that the mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution in step 1 is 0.007 wt %, and the rest is the same as Experiment 1. The resulting thin film nanocomposite membrane is denoted as M-7.
[0063] Comparative Example 1: The difference from Experiment 1 is that no carboxylated multi-walled carbon nanotubes are added, step 1 is cancelled, and in step 2, the polyethersulfone membrane is only soaked in anhydrous ethanol for 2 hours to remove impurities on the surface of the polyethersulfone membrane and improve the hydrophilicity of the polyethersulfone membrane surface, and finally dried. The rest is the same as Experiment 1. The final thin film nanocomposite membrane is recorded as M-0.
[0064] Application Example 1:
[0065] The composite membranes prepared in Experiment 1 to Comparative Example 1 were respectively placed in ultrafiltration cups and fixed. 50 mL of deionized water was added to the ultrafiltration cups, which were sealed and connected to an air compressor and the ultrafiltration cups. The membranes were pre-pressed for the first time at a pressure of 2 bar. After the membranes were pre-pressed, a stopwatch and a measuring cylinder were used to measure the volume of liquid passing through the membrane per unit time. The water flux was calculated according to the following formula:
[0066]
[0067] Where: J is the flux L / (m 2·h), t is the test time (h), V is the volume of aqueous solution that permeates the membrane within time t (L), and A is the effective membrane area (m 2 ).
[0068] According to the above formula, the pure water flux of the carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane under a pressure of 2 bar can be calculated. The specific results are shown in Table 1.
[0069] Application Example 2:
[0070] Prepare Ni with an initial concentration of 5 g / L 2+ , Mn 2+ 、Co 2+ and Li + aqueous solution, Ni 2+ Take 40mL of solution, Mn 2+ and Co 2+ Take 10mL of each solution, Li + Take 7.5mL of the solution, mix 4 solutions in a 500mL volumetric flask, make up to volume with deionized water, and adjust the pH to 1.65 with hydrochloric acid; add 20mL of the mixed solution to the ultrafiltration cup, seal it and connect the air compressor and the ultrafiltration cup, and filter the mixed solution through the composite membrane prepared in Test 1 to Comparative Example 1 at a pressure of 2bar. Take the feed liquid and the permeate, filter them with a 0.22μm filter head, divide the filtered feed liquid and the permeate into 2 parts, add 1% concentrated nitric acid to one part, and then dilute it 50 times with ultrapure water, and use a flame atomic absorption spectrophotometer to detect the Co in the solution. 2+ concentration; add 1% acid to the other part, dilute it 100 times with ultrapure water, and use flame atomic absorption spectrophotometer to detect Ni in the solution 2+ , Mn 2+ , Li + Concentration. Previously, the retention rate and water flux were two important parameters for evaluating nanofiltration membranes. However, in order to better reflect the selectivity of the present invention for metal ions and the enrichment of lithium elements in the acid leaching wastewater of retired ternary lithium batteries, the concept of enrichment rate is proposed, and the enrichment rate is calculated with reference to the following formula:
[0071]
[0072] Where: E is the enrichment rate (%), Cp is the concentration of ions in the permeate (mg / L), C f is the concentration of ions in the feed solution (mg / L).
[0073] According to the above formula, it can be calculated that + The solution concentration is 75 mg / L, Ni 2+ The solution concentration is 400 mg / L, Mn 2+ The solution concentration is 100 mg / L, Co 2+When the solution concentration is 100 mg / L, the carboxylated multi-walled carbon nanotube interlayer nanocomposite film has a strong affinity for Ni at a pressure of 2 bar. 2+ , Mn 2+ 、Co 2+ and Li + The specific results are shown in Table 2.
[0074] Table 1 Pure water flux of composite membrane
[0075]
[0076] As can be seen from Table 1, the addition of the carboxylated multi-walled carbon nanotube intermediate layer promotes the pure water flux of the composite membrane. The pure water flux of the composite membrane with the highest pure water flux can reach 31.83 L / (m 2 h).
[0077] Table 2 Thin film nanocomposite film for Ni 2+ , Mn 2+ 、Co 2+ and Li + The enrichment rate
[0078]
[0079] It can be seen from Table 1 that the addition of the carboxylated multi-walled carbon nanotube intermediate layer promotes the enrichment performance of the composite membrane. The composite membrane with the highest enrichment performance is + 、Ni 2+ , Mn 2+ and Co 2+ The maximum enrichment rates are 85.86%, 1.38%, 4.73% and 0 respectively.
Claims
1. A method for preparing a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film, characterized in that The preparation method of the carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film is carried out according to the following steps:
1. dispersing carboxylated multi-walled carbon nanotubes in deionized water and stirring with ultrasound at room temperature to obtain a carboxylated multi-walled carbon nanotube aqueous solution; The mass concentration of the carboxylated multi-walled carbon nanotube aqueous solution is 0.001wt% to 0.008wt%; 2. Coat the carboxylated multi-walled carbon nanotube aqueous solution in step 1 on the polyethersulfone membrane washed with anhydrous ethanol by vacuum filtration, dry in a drying oven at a temperature of 50° C. to 70° C. for 25 min to 35 min, and cool to room temperature; 3. Soak the film cooled in step 2 in deionized water for 25 to 30 minutes, take it out and dry it naturally in the air, then soak it in the PIP aqueous solution for 1 to 3 minutes, pour out the liquid, and dry the film naturally in the air to obtain a PIP saturated film; The concentration of the PIP aqueous solution is 12 g / L to 18 g / L; 4. Immerse the PIP saturated film prepared in step 3 in a n-hexane solution of TMC for 45s to 75s to cause an interfacial polymerization reaction, pour out the liquid, and then place the film in a drying oven for heat treatment for 12min to 18min at a heat treatment temperature of 50°C to 70°C; The concentration of the TMC n-hexane solution is 0.2 g / L to 1 g / L; 5. Rinse with deionized water to remove unreacted monomers and solvents on the membrane surface, and dry at room temperature to obtain a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane.
2. The method for preparing a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film according to claim 1, characterized in that The carboxylated multi-walled carbon nanotubes described in step 1 are powders with a purity of 98%, an outer diameter of 10 nm to 20 nm, and a length of 10 μm to 30 μm.
3. The method for preparing a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film according to claim 1, characterized in that The ultrasonic stirring time in step 1 is 12 min to 18 min, and the ultrasonic stirring frequency is 30 kHz to 40 kHz.
4. The method for preparing a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film according to claim 1, characterized in that The preparation method of the polyethersulfone membrane after washing with anhydrous ethanol in step 2 is: soaking the polyethersulfone membrane in anhydrous ethanol for 1.5 hours to 2.5 hours can remove impurities on the surface of the polyethersulfone membrane and improve the hydrophilicity of the surface of the polyethersulfone membrane.
5. The method for preparing a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film according to claim 1, characterized in that The vacuum filtration pressure in step 2 is -0.1MPa to -0.085MPa; vacuum filtration can make the carboxylated multi-walled carbon nanotubes evenly coated on the surface of the polyethersulfone membrane, thereby improving the bonding force between the carboxylated multi-walled carbon nanotube middle layer and the polyethersulfone-based membrane.
6. The use of a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite film as claimed in claim 1, characterized in that The carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane is applied to the treatment of acid leaching wastewater from retired ternary lithium batteries. The treatment method is: adjusting the pH of the wastewater to 1-2, and enriching the lithium element through filtering through the composite membrane.
7. The use of a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane according to claim 6, characterized in that The metal ions in the acid leaching wastewater of retired ternary lithium batteries are Li + 、Ni 2+ , Mn 2+ and Co 2+ One or more of the .
8. The use of a carboxylated multi-walled carbon nanotube intermediate layer thin film nanocomposite membrane according to claim 7, characterized in that The Li + The concentration of Ni is 50mg / L~100mg / L; 2+ The concentration of Mn is 100mg / L~600mg / L; 2+ The concentration of Co is 50mg / L~200mg / L; 2+ The concentration is 50mg / L~200mg / L.
Citation Information
Patent Citations
Preparation method for chitosan-modified ferrite-filled multi-wall carbon nano tube / polythiophene composite wave-absorbing material
CN104086953A
Preparation method of ZnO nanowire / multi-wall carbon nanotube modified polypropylene composite film
CN110746628A
Cited By
Polyamide composite membrane with carbon nano tube as middle layer as well as preparation method and application of polyamide composite membrane
CN121927466A