Non-aqueous electrolyte secondary battery
By adjusting the tap density and CMC/SBR ratio of the negative electrode active material in the negative electrode composite layer of the nonaqueous electrolyte secondary battery, the problem of insufficient characteristics of the negative electrode composite material shedding and low temperature regeneration is solved, and the reliability and low temperature of the battery are improved performance.
Patent Information
- Application Number
- CN202080074885.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-31
- Filing Date
- 2020-10-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-10-19
AI Technical Summary
The composite material of existing nonaqueous electrolyte secondary batteries is prone to fall off during the negative electrode cutting process, resulting in internal short circuits and insufficient low-temperature regeneration characteristics, especially in applications such as electric vehicles.
By using negative electrode active substances with a tap density of 1.00 g/cm3 to 1.20 g/cm3 in the negative electrode composite layer, and reasonably adjusting carboxymethyl cellulose (CMC) and styrene butadiene rubber in the composite layer. The ratio of (SBR) ensures that the mass ratio of CMC to SBR is less than 2, totaling less than 1.5 mass %, to reduce the amount of cutting shedding and improve the low-temperature regeneration characteristics.
It effectively reduces the shedding of the negative electrode composite material during battery assembly, improves the low-temperature regeneration characteristics and reliability of the battery, and takes into account the high-speed charging and discharge performance of the battery and the long-term capacity maintenance rate.
Smart Images

Figure CN114616708B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a nonaqueous electrolyte secondary battery. Background Art
[0002] The negative electrode composite material layer constituting the negative electrode of the non-aqueous electrolyte secondary battery includes: a negative electrode active material, a thickening material and a binding material. As the negative electrode active material, carbon materials such as graphite are widely used. By adjusting the properties and contents of the negative electrode active material, the thickening material and the binding material, various properties of the secondary battery can be changed.
[0003] For example, Patent Document 1 discloses a secondary battery that improves cycle characteristics by containing in the negative electrode composite material layer natural graphite as a negative electrode active material having an amorphization degree of 0.3 to 0.5 based on Raman measurement, 1 mass % to 2 mass % of CMC as a thickening material, and 1 mass % to 2 mass % of SBR as a binding material.
[0004] In addition, Patent Document 2 discloses a secondary battery in which a negative electrode composite material layer contains a tap density of 0.7 g / cm 3 1 mass % or more of natural graphite, 1 mass % or more of CMC, and 1 mass % or more of SBR, thereby improving the cycle characteristics.
[0005] In addition, Patent Document 3 discloses a secondary battery in which a negative electrode composite material layer contains a specific surface area of 1 m 2 / g or more of graphite, 0.3% to 3% by mass of CMC, 0.3% to 5% by mass of SBR, and carbon fibers with a fiber diameter of 1nm to 1000nm as a conductive material to improve high-speed charge and discharge characteristics.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application No. 2014-528631
[0009] Patent Document 2: Japanese Patent Application Publication No. 2011-238622
[0010] Patent Document 3: Japanese Patent Application Publication No. 2005-222933 Summary of the invention
[0011] During the battery assembly process, when the negative electrode is cut into a certain size, the composite material of the negative electrode composite material layer may fall off. When the fallen composite material is wound into the battery, an internal short circuit may occur when the battery is charged or discharged. In addition, the part of the negative electrode composite material layer where the composite material falls off becomes brittle, so there is also the possibility that the composite material layer expands and contracts during battery charging and discharging, causing further falling of the composite material and causing an internal short circuit. Therefore, in order to improve the reliability of the battery, the falling of the negative electrode composite material must be suppressed. In addition, when using secondary batteries as power sources for electric vehicles (EVs), etc., excellent low-temperature regeneration characteristics are required. However, Patent Documents 1 to 3 do not consider the amount of negative electrode composite material that falls off and the low-temperature regeneration characteristics when the negative electrode is cut off.
[0012] A nonaqueous electrolyte secondary battery as one embodiment of the present invention comprises: an electrode body having a positive electrode and a negative electrode, and an outer shell for accommodating the electrode body. The negative electrode is characterized in that it comprises a negative electrode core body and a negative electrode composite material layer formed on the surface of the negative electrode core body, and the negative electrode composite material layer comprises a tap density of 1.00 g / cm 3 ~1.20g / cm 3 A negative electrode active material, a CMC content of 0.6 mass % to 0.8 mass % in the negative electrode composite material layer, and a SBR content of 0.4 mass % to 0.8 mass % in the negative electrode composite material layer, wherein the mass ratio of the CMC content to the SBR content in the negative electrode composite material layer is less than 2, and the total content of CMC and SBR in the negative electrode composite material layer is less than 1.5 mass %.
[0013] By means of the nonaqueous electrolyte secondary battery of the present disclosure, the reliability and low-temperature regeneration characteristics of the battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a perspective view of a secondary battery as an example of an embodiment, and shows the internal structure of a battery case in a state where the front side of an outer case is removed. DETAILED DESCRIPTION
[0015] By increasing the tap density of the negative active material contained in the negative composite material layer, the electrolyte liquid absorption path from the surface of the negative composite material layer to the negative core body becomes shorter, so the low temperature regeneration characteristics are improved. However, the circularity of the negative active material with a high tap density is high, so if the negative composite material layer contains a negative active material with a high tap density, compared with the case of containing a negative active material with a low tap density, the gap between the active materials becomes larger, and the free CMC not adsorbed on the surface of the negative active material exists in large quantities, and the negative electrode becomes hard. If the negative electrode becomes hard, the negative composite material containing the negative active material becomes easy to fall off when the negative electrode is cut into a certain size in the battery assembly process, so the CMC content is preferably less, but if the CMC content is too little, the dispersibility of the negative composite material slurry deteriorates and the negative composite material layer cannot be formed. In addition, SBR has flexibility, so if the content in the negative composite material layer is increased, the negative electrode can be made soft. If the total content of CMC and SBR in the negative electrode composite material layer increases, the negative electrode will be soft and the negative electrode composite material containing the negative electrode active material can be suppressed from falling off, but the resistance of the battery will increase and the low temperature regeneration characteristics will deteriorate. The inventors of the present invention have conducted in-depth research and found that: for a tap density as high as 1.00 g / cm 3 ~1.20g / cm 3 Mixing CMC and SBR in a specified ratio as the negative electrode active material can reduce the amount of negative electrode composite material falling off when the negative electrode is cut in the battery assembly process (hereinafter referred to as cutting falling off amount) and improve the low temperature regeneration characteristics of the battery.
[0016] Hereinafter, an example of an embodiment of the present disclosure is described in detail. In this embodiment, a secondary battery 100 having a square metal outer shell 1 is exemplified, but the outer shell is not limited to the square shape, for example, it may also be cylindrical, etc. In addition, a wound electrode body 3 in which a positive electrode and a negative electrode are wound with a separator interposed therebetween is exemplified, but it may also be a stacked electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with a separator interposed therebetween. The electrode body 3 is preferably a wound type. In addition, in both the positive electrode and the negative electrode, the case where each composite material layer is formed on both sides of each core body is exemplified, but it is not limited to the case where each composite material layer is formed on both sides of each core body, as long as it is formed on at least one surface.
[0017] like Figure 1 For example, the secondary battery 100 comprises: a wound electrode body 3 formed into a flat shape with a flat portion and a pair of curved portions, in which a positive electrode and a negative electrode are wound with a separator interposed therebetween; an electrolyte; and an outer case 1 for accommodating the electrode body 3 and the electrolyte. The outer case 1 and the sealing plate 2 are both made of metal, preferably aluminum or an aluminum alloy.
[0018] The outer shell 1 has a bottom that is substantially rectangular in bottom view, and a side wall portion that is vertically arranged at the periphery of the bottom. The side wall portion is formed perpendicular to the bottom. The size of the outer shell 1 is not particularly limited, and as an example, the horizontal length is 60 to 160 mm, the height is 60 to 100 mm, and the thickness is 10 to 40 mm.
[0019] The positive electrode is a strip having a positive electrode core body made of metal and positive electrode composite material layers formed on both sides of the core body, and a strip-shaped positive electrode core body exposed portion 4 is formed at one end in the width direction, where the positive electrode core body is exposed in the length direction. Similarly, the negative electrode is a strip-shaped negative electrode core body exposed portion 5 is formed at one end in the width direction, where the negative electrode core body is exposed in the length direction. The electrode body 3 has a structure in which the positive electrode and the negative electrode are wound with a separator interposed therebetween, with the positive electrode core body exposed portion 4 being arranged at one end side in the axial direction and the negative electrode core body exposed portion 5 being arranged at the other end side in the axial direction.
[0020] A positive electrode collector 6 is connected to the laminated portion of the exposed portion 4 of the positive electrode core of the positive electrode, and a negative electrode collector 8 is connected to the laminated portion of the exposed portion 5 of the negative electrode core of the negative electrode. Suitable positive electrode collectors 6 are made of aluminum or aluminum alloy. Suitable negative electrode collectors 8 are made of copper or copper alloy. The positive terminal 7 has: a positive electrode external conductive portion 13 arranged on the battery external side of the sealing plate 2, a positive electrode bolt portion 14 connected to the positive electrode external conductive portion 13, and a positive electrode embedded portion 15 embedded in a through hole provided in the sealing plate 2, and electrically connected to the positive electrode collector 6. In addition, the negative terminal 9 has: a negative electrode external conductive portion 16 arranged on the battery external side of the sealing plate 2, a negative electrode bolt portion 17 connected to the negative electrode external conductive portion 16, and a negative electrode embedded portion 18 embedded in a through hole provided in the sealing plate 2, and electrically connected to the negative electrode collector 8.
[0021] The positive terminal 7 and the positive electrode collector 6 are fixed to the sealing plate 2 via an inner insulating member and an outer insulating member, respectively. The inner insulating member is disposed between the sealing plate 2 and the positive electrode collector 6, and the outer insulating member is disposed between the sealing plate 2 and the positive terminal 7. Similarly, the negative terminal 9 and the negative electrode collector 8 are fixed to the sealing plate 2 via an inner insulating member and an outer insulating member, respectively. The inner insulating member is disposed between the sealing plate 2 and the negative electrode collector 8, and the outer insulating member is disposed between the sealing plate 2 and the negative terminal 9.
[0022] The electrode body 3 is accommodated in the outer shell 1. The sealing plate 2 is connected to the opening edge of the outer shell 1 by laser welding or the like. The sealing plate 2 has an electrolyte injection hole 10, and after the electrolyte is injected into the outer shell 1, the electrolyte injection hole 10 is sealed by a sealing plug. The sealing plate 2 is formed with a gas discharge valve 11 for discharging gas when the pressure inside the battery reaches a predetermined value or more.
[0023] The electrolyte is a non-aqueous electrolyte comprising a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. For example, carbonates, lactones, ethers, ketones, esters, etc. can be used as the non-aqueous solvent, and these solvents can be mixed and used in two or more kinds. When two or more solvents are mixed and used, it is preferred to use a mixed solvent comprising cyclic carbonates and chain carbonates. For example, as cyclic carbonates, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used, and as chain carbonates, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) can be used. The non-aqueous solvent may also contain a halogen substituted body obtained by replacing at least a part of the hydrogen of the above-mentioned solvent with a halogen atom such as fluorine. As the electrolyte salt, LiPF6, LiBF4, LiCF3SO3, etc. and mixtures thereof can be used. The amount of electrolyte salt dissolved in the non-aqueous solvent can be set to 0.5 to 2.0 mol / L, for example. In addition, additives such as vinylene carbonate (VC) can also be appropriately added. It should be noted that the electrolyte is not limited to a liquid electrolyte, and a solid electrolyte using a gel polymer or the like may be used.
[0024] Hereinafter, the positive electrode, the negative electrode, and the separator constituting the electrode body 3 , in particular, the negative electrode composite material layer constituting the negative electrode will be described in detail.
[0025] [positive electrode]
[0026] The positive electrode includes: a positive electrode core, and a positive electrode composite material layer formed on the surface of the positive electrode core. The positive electrode core can be made of, for example, a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, a thin film of the metal disposed on the surface, etc. The positive electrode composite material layer includes, for example, a positive electrode active material, a binding material, a conductive material, etc. The positive electrode can be made, for example, as follows: a positive electrode composite material slurry including a positive electrode active material, a binding material, a conductive material, etc. is applied to the positive electrode core and dried to form a positive electrode composite material layer, and then the positive electrode composite material layer is rolled, so that it can be made.
[0027] Examples of positive electrode active materials include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. Examples of lithium transition metal oxides include Li x CoO2、Li x NiO2、Li x MnO2、Li xCo y Ni 1-y O2、Li x Co y M 1-y O z , Li x Ni 1- y M y O z , Li x Mn2O4、Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3). They can be used alone or in combination. In terms of achieving a high capacity of the secondary battery 100, the positive electrode active material preferably contains Li x NiO2、Li x Co y Ni 1-y O2、Li x Ni 1-y M y O z Lithium nickel composite oxides such as (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3).
[0028] Examples of the conductive material include carbon black (CB), acetylene black (AB), Ketjen black, graphite and other carbon particles, etc. These may be used alone or in combination of two or more.
[0029] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide-based resins, acrylic resins, and polyolefin-based resins, etc. These may be used alone or in combination of two or more.
[0030] [negative electrode]
[0031] The negative electrode includes: a negative electrode core and a negative electrode composite material layer formed on the surface of the negative electrode core. The negative electrode core can be made of, for example, a foil of a metal such as copper that is stable within the potential range of the negative electrode, or a thin film of the metal disposed on the surface. The negative electrode composite material layer includes: a tap density of 1.00 g / cm 3 ~1.20g / cm 3The negative electrode active material, the content of CMC in the negative electrode composite material layer is 0.6 mass % to 0.8 mass %, and the content of SBR in the negative electrode composite material layer is 0.4 mass % to 0.8 mass %. In addition, in the negative electrode composite material layer, the mass ratio of the content of CMC to the content of SBR is less than 2, and the total content of CMC and SBR in the negative electrode composite material layer is less than 1.5 mass %. Thus, the amount of cutting and shedding can be reduced, and the low temperature regeneration characteristics of the battery can be improved. The negative electrode can be made as follows: After a negative electrode composite material slurry containing at least a negative electrode active material, CMC and SBR is applied to the negative electrode core and dried to form a negative electrode composite material layer, the negative electrode composite material layer is rolled, so that it can be made.
[0032] As the negative electrode active material, there is no particular limitation as long as it can reversibly absorb and release lithium ions. For example, carbon materials such as natural graphite and artificial graphite, metals such as silicon (Si) and tin (Sn) that can alloy with lithium, or alloys containing metal elements such as Si and Sn, composite oxides, etc. can be used. As the negative electrode active material, carbon materials are preferred, and natural graphite is more preferred. The negative electrode active material can be used alone or in combination of two or more.
[0033] The negative electrode active material may also be a roughly spherical shape with an average circularity of 0.8 or more. As a result, the electrolyte absorption path from the surface of the negative electrode composite material layer to the negative electrode core becomes shorter, thereby improving the low-temperature regeneration characteristics. It should be noted that in the present application specification, the average circularity refers to the projection area of the negative electrode active material as S and the circumference as L, expressed as 4πS / L 2 Definition. The circularity of a circle is 1, and the more elongated the shape becomes, the less circularity it becomes. The average circularity is the average circularity calculated by observing 100 negative electrode active materials with a scanning electron microscope and measuring the area S and perimeter L of the active material using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health).
[0034] The average particle size of the negative electrode active material can be 8 μm to 13 μm. The average particle size and average circularity of the negative electrode active material are within the specified range, so that the tap density of the negative electrode active material can be 1.00 g / cm 3 ~1.20g / cm 3 In the present application, the average particle size of the negative electrode active material refers to the median particle size (D50) based on volume. D50 refers to the particle size at which the cumulative frequency of the particle size distribution based on volume becomes 50% from the smaller particle size, and is also called the median diameter. The particle size distribution of the negative electrode active material can be measured using a laser diffraction particle size distribution measuring device (e.g., SALD-2200 manufactured by Shimadzu Corporation) using an aqueous solution of a surfactant as a dispersion medium.
[0035] The tap density of the negative electrode active material is 1.00 g / cm 3 ~1.20g / cm 3 , preferably 1.03 g / cm 3 ~1.18g / cm 3 , more preferably 1.05 g / cm 3 ~1.15g / cm 3 . The higher the tap density of the negative electrode active material, the more improved the low-temperature regeneration characteristics, but the amount of cutting and shedding will increase. By making the tap density of the negative electrode active material within the above range, it is possible to achieve both improved low-temperature regeneration characteristics and reduced cutting and shedding. The tap density can be calculated as follows: stack a connecting filling frame (about 50 mL) on a measuring cylinder of a constant volume (for example, 50 mL) and introduce 60 g of negative electrode active material. After tapping 300 times, remove the filling frame and calculate based on the mass of the negative electrode active material in the measuring cylinder volume. The tap density of the negative electrode active material can be measured, for example, using TVP-1A (constant volume type) manufactured by TSUTSUISCIENTIFIC INSTRUMENTS CO., LED.
[0036] The oil absorption of the negative electrode active material can be 43ml / 100g to 52ml / 100g. The oil absorption can be calculated according to the DBP (dibutyl phthalate) absorption method A (mechanical method) specified in JIS K-6217-4 "Basic properties of carbon black for rubber Part 4: Method for calculating DBP absorption". Here, DBP is changed to linseed oil. Specifically, in 30g of negative electrode active material particles stirred with two blades, 4cm 3 Linseed oil is added at a rate of 1 / min. The change in viscosity characteristics at this time is detected by a torque detector, and its output is converted into torque by a microcomputer. The amount of linseed oil corresponding to the torque at the moment of 100% of the maximum torque generated is converted into particles per 100g of negative electrode active material, so that the oil absorption can be calculated. The oil absorption of the negative electrode active material can be measured, for example, using an absorption tester (manufactured by ASAHISOUKEN CORPORATION, model name "S-500").
[0037] The BET specific surface area of the negative electrode active material can be 3.5 m 2 / g~4.8m 2 By making the BET specific surface area of the negative electrode active material within the above range, the initial discharge capacity of the battery can be improved, and a high capacity retention rate can be obtained even after high-temperature storage. The BET specific surface area can be measured using nitrogen gas using a commercially available measuring device such as HM model-1201 of Macsorb.
[0038] The content of CMC in the negative electrode composite material layer (hereinafter referred to as C CMC ) is 0.6 mass % to 0.8 mass %. In the present application specification, CMC refers to carboxymethyl cellulose or a salt thereof. As salts of carboxymethyl cellulose, for example, sodium carboxymethyl cellulose and ammonium carboxymethyl cellulose can be cited. As suitable examples of CMC, carboxymethyl cellulose, sodium carboxymethyl cellulose (CMC-Na) and the like can be cited. CMC can function as a binding material, and can also function as a thickening material to adjust the viscosity of the negative electrode composite material slurry.
[0039] The mass average molecular weight of CMC can be 3.7×10 5 ~4.3×10 5 By setting the mass average molecular weight of CMC to this range, the thixotropic properties of the negative electrode slurry become better, and the coating properties of the composite material slurry on the core body can be improved. In addition, the hardness of the composite material layer of the electrode plate becomes more appropriate, and the amount of cutting and shedding can be suppressed.
[0040] The content of SBR in the negative electrode composite material layer (hereinafter referred to as C SBR ) is 0.4 mass % to 0.8 mass %. In the present specification, SBR refers to styrene butadiene rubber or a modified form thereof. The average primary particle size of SBR is preferably 120 to 250 nm, more preferably 150 to 230 nm.
[0041] The Tg of SBR may be 5° C. or lower. This makes SBR soft, and thus the flexibility of the negative electrode can be improved.
[0042] The mass ratio of the content of CMC to the content of SBR in the negative electrode composite material layer (hereinafter referred to as C CMC / C SBR ) is less than 2, the total content of CMC and SBR (hereinafter referred to as C CMC +C SBR ) is less than 1.5% by mass. Thus, the amount of cutting and shedding can be reduced, and the low-temperature regeneration characteristics of the battery can be improved.
[0043] The negative electrode composite material layer may include, in addition to CMC and SBR, fluorine-containing resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin and other binding materials, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc., within the range that does not hinder the effect of the present embodiment.
[0044] The packing density of the negative electrode composite material layer can be 1.05 g / cm 3 ~1.25g / cm 3The thickness can be 65 μm to 75 μm. The packing density and thickness of the negative electrode composite material layer can be determined by the following method.
[0045] (1) Cut the negative electrode into 10 cm 2 The size of the cut negative electrode was measured by measuring the mass A (g) and thickness C (cm).
[0046] (2) The negative electrode composite material layer was peeled off from the cut negative electrode, and the mass B (g) of the negative electrode core and the thickness D (cm) of the core were measured.
[0047] (3) Thickness (μm) = (CD) × 10 4 The thickness of the negative electrode composite material layer was calculated using the formula
[0048] (4) By filling density (g / cm 3 The packing density of the negative electrode composite material layer was calculated using the formula: )=(AB) / [(CD)×10].
[0049] [Separator]
[0050] For example, a porous sheet having ion permeability and insulation can be used as the separator. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the separator, olefin resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator can be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, a multilayer separator including a polyethylene layer and a polypropylene layer can also be used, and a separator coated with materials such as aramid resins and ceramics on the surface can also be used.
[0051] <Example>
[0052] Hereinafter, the present disclosure will be further described by way of examples, but the present disclosure is not limited to these examples.
[0053] [Negative electrode active material]
[0054] Natural graphite was used as the negative electrode active material. The five types of natural graphite used were natural graphites A to E. Table 1 shows the tap density, average circularity, average particle size (D50), oil absorption, and BET specific surface area of each type.
[0055] [Table 1]
[0056]
[0057] <Example 1>
[0058] [Production of positive electrode]
[0059] Using LiNi 0.35 Co0.35 Mn 0.30 The composite oxide shown in O2 is used as the positive electrode active material. The positive electrode active material, PVdF and carbon black are mixed in a mass ratio of 90:3:7, and N-methyl-2-pyrrolidone is added while kneading to prepare a positive electrode composite material slurry. Next, the positive electrode composite material slurry is applied to both sides of a long strip of positive electrode core formed by aluminum foil with a thickness of 13μm, and the coating is dried. The dried coating is compressed so that the filling density becomes 2.5g / cm 3 After that, it is cut into a specified electrode size to make a positive electrode having positive electrode composite material layers formed on both sides of the positive electrode core. It should be noted that in the positive electrode, a positive electrode core exposed portion for connecting a positive electrode current collector is provided at one end in the width direction along the length direction of the positive electrode.
[0060] [Production of negative electrode]
[0061] Natural graphite A was used as the negative electrode active material. The negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.8:0.6:0.6, and an appropriate amount of water was further added to prepare a negative electrode composite material slurry. C calculated from the above mixing ratio CMC / C SBR 1. C CMC +C SBR The mass average molecular weight of CMC is 4.0×10 5 , the Tg of SBR is 1.0℃.
[0062] The negative electrode composite material slurry is coated on both sides of the negative electrode core formed by copper foil by die coating, and after the coating film is dried, a negative electrode with a negative electrode composite material layer formed on both sides of the negative electrode core is produced. The negative electrode composite material layer of the negative electrode is rolled by a roller to a packing density of 1.2 g / cm 3 After the thickness reaches 67 μm, it is cut into a predetermined electrode size. It should be noted that in the negative electrode, a negative electrode core exposed portion for connecting a negative electrode current collector is provided at one end in the width direction along the length direction of the negative electrode.
[0063] [Production of electrode body]
[0064] After the positive electrode and the negative electrode are wound with a strip-shaped separator having a width of 120 mm, the wound body is pressurized in the radial direction to be formed into a flat shape to produce a wound electrode body. The wound body is formed by winding a separator / positive electrode / separator / negative electrode stacked in sequence on a cylindrical winding core (two separators are the same). In addition, the positive electrode and the negative electrode are wound in such a way that the exposed parts of their respective cores are located on opposite sides of the winding body in the axial direction. The pressurization conditions of the winding body are set to a pressurization temperature of 75°C, a pressurization pressure of 100 kN, and a pressurization time of 3 minutes.
[0065] [Preparation of electrolyte]
[0066] LiPF6 was added to a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) in a volume ratio of 3:3:4 (25°C, 1 atm) to give a concentration of 1 mol / L, and vinylene carbonate was further added to give a concentration of 0.3% by mass to prepare an electrolyte solution.
[0067] [Manufacturing of Secondary Batteries]
[0068] A secondary battery (square battery) is made using the electrode body, the electrolyte and the square battery case. A positive terminal is installed on the sealing plate constituting the battery case, and a positive electrode collector is connected to the positive terminal. In addition, a negative terminal is installed on the sealing plate, and a negative electrode collector is connected to the negative terminal. Then, the positive electrode collector is welded on the exposed part of the core of the positive electrode, and the negative electrode collector is welded on the exposed part of the core of the negative electrode. In a state where it is arranged in an insulating sheet formed into a box shape, the electrode body integrated with the sealing plate is accommodated in a square bottomed cylindrical outer shell (lateral length 148.0mm (internal dimension 146.8mm), thickness 17.5mm (internal dimension 16.5mm), height 65.0mm (internal dimension 64.0mm)) constituting the battery case, and the opening of the outer shell is blocked with a sealing plate. After 65 g of electrolyte was injected from the electrolyte injection hole of the sealing plate to allow the electrolyte to fully impregnate the electrode body, dummy charging was performed and a sealing plug was attached to the injection hole to obtain a secondary battery (battery capacity: 8 Ah).
[0069] <Example 2>
[0070] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that natural graphite B was used as the negative electrode active material. The obtained negative electrode and secondary battery are referred to as Example 2.
[0071] <Example 3>
[0072] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that natural graphite C was used as the negative electrode active material. The obtained negative electrode and secondary battery are referred to as Example 3.
[0073] <Example 4>
[0074] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 99.0:0.6:0.4 to prepare a negative electrode composite material slurry.
[0075] <Example 5>
[0076] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.6:0.6:0.8 to prepare a negative electrode composite material slurry.
[0077] <Example 6>
[0078] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.6:0.8:0.6 to prepare a negative electrode composite material slurry.
[0079] <Comparative Example 1>
[0080] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that natural graphite D was used as the negative electrode active material. The obtained negative electrode and secondary battery were designated as Comparative Example 1.
[0081] <Comparative Example 2>
[0082] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that natural graphite E was used as the negative electrode active material. The obtained negative electrode and secondary battery were designated as Comparative Example 2.
[0083] <Comparative Example 3>
[0084] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 99.2:0.6:0.2 to prepare a negative electrode composite material slurry.
[0085] <Comparative Example 4>
[0086] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.4:0.6:1.0 to prepare a negative electrode composite material slurry.
[0087] <Comparative Example 5>
[0088] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 99.0:0.8:0.2 to prepare a negative electrode composite material slurry.
[0089] <Comparative Example 6>
[0090] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.8:0.8:0.4 to prepare a negative electrode composite material slurry.
[0091] <Comparative Example 7>
[0092] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.4:0.8:0.8 to prepare a negative electrode composite material slurry.
[0093] <Comparative Example 8>
[0094] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.6:1.0:0.4 to prepare a negative electrode composite material slurry.
[0095] <Comparative Example 9>
[0096] A negative electrode and a secondary battery were obtained in the same manner as in Example 1 except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.4:1.0:0.6 to prepare a negative electrode composite material slurry.
[0097] <Comparative Example 10>
[0098] The negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed in a mass ratio of 98.9:0.5:0.6 to prepare a negative electrode composite material slurry. In addition, the negative electrode was obtained in the same manner as in Example 1, but the dispersibility of the negative electrode composite material slurry deteriorated, and a negative electrode composite material layer could not be formed, and a negative electrode and a secondary battery could not be obtained. This result is referred to as Comparative Example 10.
[0099] [Determination of liquid absorption time]
[0100] Each negative electrode of the embodiment and the comparative example was dried in a thermostatic bath heated to 200°C under a nitrogen atmosphere for 10 hours, and each negative electrode was cut into a size of 5 cm × 5 cm to prepare a sample. 3.0 μL of polypropylene carbonate (PC) was dripped onto the surface of each sample from a vertical direction, and the time until PC was absorbed into the interior of the sample was visually determined. For each sample, the measurement was performed 6 times, and the average value was taken as the liquid absorption time. The shorter the liquid absorption time, the smoother the replacement of the electrolyte from the surface of the negative electrode composite material layer to the core material side can be carried out, so the electrolyte discharged from the negative electrode composite material layer during discharge is quickly absorbed by the negative electrode composite material layer during charging. As a result, the shorter the liquid absorption time, the better the low-temperature regeneration characteristics, and the more the reduction in rapid charge and discharge cycle characteristics is suppressed.
[0101] [Determination of cutting shedding amount]
[0102] Each negative electrode of the example and the comparative example was cut under the following conditions, and the amount of cutting and falling was determined from the area of the powder of the negative electrode composite material falling during the cutting.
[0103] (1) The negative electrode was cut into 100 mm × 100 mm pieces to prepare sample pieces.
[0104] (2) The sample piece was placed on white paper and cut into 100 mm pieces from the end of the sample piece using a cutter so that the negative electrode composite material fell off the white paper.
[0105] (3) Using a stereoscopic microscope, an image of the negative electrode composite material after removal was taken. The magnification of the stereoscopic microscope was 10 times.
[0106] (4) The image obtained above is read on a computer and binarized using image analysis software (e.g. ImageJ, manufactured by the National Institutes of Health, USA) to convert the negative electrode composite material after detachment into black and the white paper into white, thereby obtaining a binary processed image.
[0107] (5) The area of the negative electrode composite material after shedding is calculated from the binary processed image.
[0108] (6) The above steps (1) to (5) were repeated 10 times, and the average value of the area of the negative electrode composite material after removal was taken as the amount of cutting removal.
[0109] [Evaluation of low temperature regeneration characteristics]
[0110] Each battery of the example and the comparative example was charged under the following conditions to determine the low-temperature regeneration value.
[0111] (1) Charging was performed at 25° C. until the SOC reached 50%.
[0112] (2) For batteries with SOC 50%, charge at -10°C for 5 seconds at currents of 3.7It, 12.5It, 17.5It, 22.5It, 31.2It and 37.5It respectively (It is It (A) = rated capacity (Ah) / 1 (h)).
[0113] (3) Measure the battery voltage immediately after charging for 5 seconds, plot the battery voltage against each current value, and find the current value IP (A) that corresponds to the battery voltage (V) at SOC 100%. Multiply the current value IP by the battery voltage (V) at SOC 100% to calculate the low temperature regeneration value (W).
[0114] Table 2 summarizes the results of the liquid absorption time, cutting shedding amount, and low-temperature regeneration characteristics of the examples and comparative examples. In addition, Table 2 also records the relationship between the amount of the negative electrode active material used and the amount of CMC and SBR in the negative electrode composite material layer (C CMC , C SBR , C CMC / C SBR , C CMC +C SBR ).
[0115] [Table 2]
[0116]
[0117] As can be seen from Table 2, Examples 1 to 5, as compared with Comparative Examples 1 to 9, all suppressed the amount of cutting and falling to a certain level or less, and all maintained a high low-temperature regeneration characteristic.
[0118] Description of Reference Numerals
[0119] 1 Outer shell
[0120] 2 Sealing plate
[0121] 3 Electrode body
[0122] 4. Positive electrode core exposed part
[0123] 5 Negative electrode core exposed part
[0124] 6. Positive electrode collector
[0125] 7 Positive terminal
[0126] 8 Negative electrode collector
[0127] 9 Negative terminal
[0128] 10 Electrolyte injection hole
[0129] 11 Gas exhaust valve
[0130] 13 Positive electrode external conductive part
[0131] 14 Positive electrode bolt
[0132] 15 Positive electrode embedding part
[0133] 16 Negative electrode external conductive part
[0134] 17 Negative electrode bolt
[0135] 18 Negative electrode embedding part
[0136] 100 Secondary batteries
Claims
1. A non-aqueous electrolyte secondary battery comprising: an electrode body having a positive electrode and a negative electrode, and an outer shell accommodating the electrode body, The negative electrode comprises: a negative electrode core body and a negative electrode composite material layer formed on a surface of the negative electrode core body. The negative electrode composite material layer comprises: a tap density of 1.00 g / cm 3 ~1.20g / cm 3 a negative electrode active material, 0.6 mass % to 0.8 mass % of CMC in the negative electrode composite material layer, and 0.4 mass % to 0.6 mass % of SBR in the negative electrode composite material layer, In the negative electrode composite material layer, the mass ratio of the content of CMC to the content of SBR is less than 2, The total content of CMC and SBR in the negative electrode composite material layer is 1.2 mass % or less.
2. The nonaqueous electrolyte secondary battery according to claim 1, in, The oil absorption of the negative electrode active material is 43 ml / 100 g to 52 ml / 100 g.
3. The nonaqueous electrolyte secondary battery according to claim 1 or 2, in, The BET specific surface area of the negative electrode active material is 3.5 m 2 / g~4.8m 2 / g.
4. The nonaqueous electrolyte secondary battery according to claim 1 or 2, in, The negative electrode active material has a substantially spherical shape with an average circularity of 0.8 or more.
5. The nonaqueous electrolyte secondary battery according to claim 1 or 2, in, The average particle size of the negative electrode active material is 8 μm to 13 μm.
6. The nonaqueous electrolyte secondary battery according to claim 1 or 2, in, The negative electrode active material is natural graphite.
7. The nonaqueous electrolyte secondary battery according to claim 1 or 2, in, The Tg of SBR is 5°C or less.
8. The nonaqueous electrolyte secondary battery according to claim 1 or 2, in, The mass average molecular weight of CMC is 3.7×10 5 ~4.3×10 5 .
9. The nonaqueous electrolyte secondary battery according to claim 1 or 2, in, The electrode body is a wound type in which the positive electrode and the negative electrode are wound with a separator interposed therebetween. The packing density of the negative electrode composite material layer is 1.05 g / cm 3 ~1.25g / cm 3 , thickness is 65μm~75μm.