A two-junction solar cell and a method for preparing the same
By introducing a two-junction structure into crystalline silicon solar cells and combining thin-film solar cell units with crystalline silicon solar cell units, the problem of crystalline silicon solar cells being insensitive to light in specific wavelength bands is solved, thus improving the conversion efficiency.
Patent Information
- Application Number
- CN202011372280.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-30
AI Technical Summary
Crystalline silicon solar cells are insensitive to light in wavelengths below 300 nm or above 1100 nm, resulting in low conversion efficiency for solar cells with single-junction tunneling oxide passivated metal structures.
It adopts a two-junction solar cell structure, including an N-type crystalline silicon substrate, with the front and back sides consisting of multiple thin films and electrodes, respectively. The thin film solar cell units are combined with the crystalline silicon solar cell units in series to utilize sunlight that is not absorbed by the crystalline silicon solar cells.
It improves the overall solar energy conversion efficiency and solves the problem of low conversion efficiency in single-junction tunneling oxide passivated metal structure solar cells.
Smart Images

Figure CN114639742B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photovoltaic technology, and in particular to a two-junction solar cell and a preparation method thereof. Background Art
[0002] Crystalline silicon solar cells are the most mature and widely used solar cells, accounting for more than 90% of the photovoltaic market and will dominate for a long time in the future. At the same time, because crystalline silicon solar cells are only sensitive to light in the visible 300-1100nm band, they can generate photocurrent and output it to the external circuit. This means that crystalline silicon solar cells cannot use light with a wavelength less than 300nm or greater than 1100nm, resulting in low conversion efficiency of solar cells currently using a single-junction tunnel oxide passivation metal structure. Summary of the invention
[0003] In view of this, the present invention provides a two-junction solar cell and a preparation method thereof to solve the problem of low conversion efficiency of solar cells using a single-junction tunneling oxide layer passivation metal structure.
[0004] In order to solve the above problems, the present invention discloses a two-junction solar cell, comprising an N-type crystalline silicon substrate, wherein the crystalline silicon substrate comprises a front side and a back side, wherein:
[0005] A diffused P-type layer, a first tunneling thin film layer, a first P-type semiconductor layer, a first passivation layer, a first transparent conductive film layer, a first N-type semiconductor layer, a second tunneling thin film layer, a second P-type semiconductor layer, a second transparent conductive film layer and a first anti-reflection layer are sequentially prepared on the front surface from inside to outside;
[0006] A first metal electrode is formed between the first P-type semiconductor layer and the first transparent conductive film layer, and a second metal electrode is formed on the second transparent conductive film layer, wherein the second metal electrode penetrates the first anti-reflection layer outwardly;
[0007] The back surface is provided with a third tunneling thin film layer, a second N-type semiconductor layer, a second passivation layer and a second anti-reflection layer in sequence from inside to outside;
[0008] A third metal electrode connected to the second N-type semiconductor layer is prepared on the second N-type semiconductor layer, and the third metal electrode penetrates the second passivation layer and the second anti-reflection layer outwardly.
[0009] Optionally, the dopant of the diffused P-type layer is boron, and the maximum doping concentration of the dopant is 10 18 ~10 20 cm -3 , the boron concentration is 10 17 cm -3The diffusion junction depth is 0.2~0.8μm.
[0010] Optionally, the first tunneling film layer is a mixture film of group IVA elements, an oxide film, a nitride film or a nitride oxide film, or a metal oxide film;
[0011] The thickness of the first tunneling thin film layer is 1-5 nm.
[0012] Optionally, the first P-type semiconductor layer and the second P-type semiconductor layer are polycrystalline boron-doped films or amorphous boron-doped films of group IVA elements, or are highly conductive polarity P-type semiconductor films of compounds of group IIA elements or group VIA elements;
[0013] The thickness of the first P-type semiconductor layer or the second P-type semiconductor layer is 15-150 nm.
[0014] Optionally, the first passivation layer comprises a stack of one or more film layers selected from the group consisting of an aluminum oxide film, a silicon oxide film, an intrinsic film, and a P-type heavily doped amorphous IVA group element mixture film;
[0015] The thickness of the first passivation layer is 3-5 nm.
[0016] Optionally, the first N-type semiconductor layer and the second N-type semiconductor layer are polycrystalline doped films or amorphous phosphorus-doped films based on a mixture of group IVA elements, or are highly conductive polarity N-type semiconductor films of compounds of group IIA elements or group VIA elements;
[0017] The thickness of the first N-type semiconductor layer and the second N-type semiconductor layer is 15-150 nm.
[0018] Optionally, the second passivation layer includes a single layer of film material or a stack of multiple layers of film materials selected from the group consisting of a silicon nitride film layer, a silicon oxide film, an intrinsic film, and an N-type heavily doped amorphous IVA group element film;
[0019] The thickness of the second passivation layer is 3-15 nm.
[0020] Optionally, the thickness of the first transparent conductive film layer and the second transparent conductive film layer is 60-100 nm.
[0021] A preparation method is also provided for preparing the above-mentioned two-junction solar cell, the index method comprising the steps of:
[0022] Cleaning and texturing both sides of the N-type crystalline silicon substrate;
[0023] Performing boron diffusion treatment on the front surface of the N-type crystalline silicon substrate to form the diffused P-type layer;
[0024] Performing backside wrapping and expansion processing on the borosilicate glass on the front and back sides of the N-type crystalline silicon substrate;
[0025] Performing tunneling layer growth operations on the front side and the back side of the N-type crystalline silicon substrate respectively to obtain the first tunneling thin film layer and the third tunneling thin film layer;
[0026] Forming the first P-type semiconductor layer on the first tunneling thin film layer, and forming the second N-type semiconductor layer on the third tunneling thin film layer;
[0027] Performing deposition and annealing treatment on the N-type crystalline silicon substrate to obtain the first passivation layer and the second passivation layer;
[0028] preparing a second anti-reflection layer on the second passivation layer;
[0029] preparing the first transparent conductive film layer on the first passivation layer;
[0030] The first metal electrode and the second metal electrode are prepared on the first transparent conductive polishing layer by screen printing, and the third metal electrode is prepared on the second anti-reflection layer, wherein the first metal electrode penetrates the first passivation layer and has deep contact with the first P-type semiconductor layer;
[0031] The first N-type semiconductor layer, the second tunneling thin film layer, the second P-type semiconductor layer, the second transparent conductive film layer and the first anti-reflection layer are sequentially prepared on the first transparent conductive film layer.
[0032] It can be seen from the above technical scheme that the present invention provides a two-junction solar cell and a preparation method thereof, the cell is prepared based on an N-type crystalline silicon substrate, and a crystalline silicon solar cell unit including a diffused P-type layer, a first tunneling thin film layer, a first P-type semiconductor layer, a first passivation layer, and a first transparent conductive film layer is prepared on the front side in sequence from the inside to the outside, and also includes a thin film solar cell unit composed of a first N-type semiconductor layer, a second tunneling thin film layer, a second P-type semiconductor layer, and a second transparent conductive film layer. The two solar cell units are connected in series through a first metal electrode, and the entire solar cell is connected to an external circuit through a second metal electrode and a third metal electrode. Since the thin film solar cell unit can utilize sunlight that cannot be absorbed by the crystalline silicon solar cell, the combination of the two can effectively improve the overall solar energy conversion efficiency, thereby solving the problem of low conversion efficiency of solar cells using a single-junction tunneling oxide layer passivated metal structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 A cross-sectional view of a two-junction solar cell according to an embodiment of the present application;
[0035] Figure 2 A flow chart of a preparation method according to an embodiment of the present application;
[0036] Figure 2a A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0037] Figure 2b A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0038] Figure 2c A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0039] Figure 2d A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0040] Figure 2e A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0041] Figure 2f A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0042] Figure 2g A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0043] Figure 2h A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0044] Figure 2i A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0045] Figure 2j A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0046] Figure 2k A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0047] Figure 2lA cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0048] Figure 2m A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0049] Figure 2n A cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application;
[0050] Figure 2o This is a cross-sectional view of a two-junction solar cell during the preparation process according to an embodiment of the present application. DETAILED DESCRIPTION
[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] Embodiment 1
[0053] Figure 1 This is a cross-sectional view of a two-junction solar cell according to an embodiment of the present application.
[0054] Reference Figure 1 As shown, the two-junction solar cell provided in this embodiment is a power generation element of a solar module. The cell is prepared based on an N-type crystalline silicon substrate 1. The crystalline silicon substrate includes a front side and a back side. The so-called front side and back side are relative concepts, that is, the side facing the sunlight is used as the front side of the crystalline silicon substrate, and the other side is used as the back side.
[0055] On the front side of the N-type crystalline silicon substrate, there are sequentially prepared, from the inside to the outside, a diffused P-type layer 1', a first tunneling thin film layer 2, a first P-type semiconductor layer 3, a first passivation layer 5, a first transparent conductive film layer 9, a first N-type semiconductor layer 10, a second tunneling thin film layer 11, a second P-type semiconductor layer 12, a second transparent conductive film layer 13 and a first anti-reflection layer 14.
[0056] A first metal electrode 7 is formed between the first P-type semiconductor layer 3 and the first transparent conductive film layer 9 , and a second metal electrode 14 is formed on the second transparent conductive film layer. The second metal electrode penetrates the first anti-reflection layer outward.
[0057] On the back side of the N-type crystalline silicon substrate, a third tunneling thin film layer 2', a second N-type semiconductor layer 4, a second passivation layer 6, and a second anti-reflection layer 15 are sequentially prepared from the inside to the outside. A third metal electrode 8 connected to the second N-type semiconductor layer is prepared on the second N-type semiconductor layer, and the third metal electrode penetrates the second passivation layer and the second anti-reflection layer outward.
[0058] The second metal electrode and the third metal electrode constitute the external electrodes of the battery, which are used to connect to an external circuit so as to output the circuit generated by the solar cell to the external circuit. In other words, the solar cells are connected in series and parallel through the second metal electrode and the third metal electrode.
[0059] The dopant of the diffused P-type layer is boron, the maximum doping concentration of the dopant is 1018~1020cm-3, and the diffusion junction depth at a boron concentration of 1017cm-3 is 0.2~0.8μm.
[0060] The first tunneling film layer is a film of group IVA elements, an oxide film, a nitride film or a nitride oxide film, or a mixture film of multiple group IVA elements, or a metal oxide film; the thickness of the first tunneling film layer is 1-5 nm.
[0061] The first P-type semiconductor layer and the second P-type semiconductor layer are polycrystalline boron-doped thin films or amorphous boron-doped thin films of group IVA elements, or highly conductive polarity P-type semiconductor films of compounds of group IIA elements or group VIA elements; the thickness of the first P-type semiconductor layer or the second P-type semiconductor layer is 15 to 150 nm. The thickness of the first P-type semiconductor layer and the second P-type semiconductor layer can be the same or different.
[0062] The first passivation layer is an aluminum oxide film, a silicon oxide film, an intrinsic film, a P-type heavily doped amorphous IVA group element mixture film, or a laminated film made of one or more of the above film layers. The thickness of the first passivation layer is 3-5 nm.
[0063] The first N-type semiconductor layer and the second N-type semiconductor layer are polycrystalline doped thin films or amorphous phosphorus-doped thin films based on a mixture of group IVA elements, or are strong conductive polarity N-type semiconductor films of compounds of group IIA elements or group VIA elements; the thickness of the first N-type semiconductor layer and the second N-type semiconductor layer is 15-150nm. The thickness of the two N-type semiconductor layers can be the same or different.
[0064] The second passivation layer is a silicon nitride film layer, a silicon oxide film, an intrinsic film or an N-type heavily doped amorphous IVA group element film, or a laminated film including the above-mentioned multiple films. The thickness of the second passivation layer is 3 to 15 nm. The thickness of the first transparent conductive film layer and the second transparent conductive film layer is 60 to 100 nm.
[0065] It can be seen from the above technical scheme that this embodiment provides a two-junction solar cell, which is prepared based on an N-type crystalline silicon substrate, and a crystalline silicon solar cell unit including a diffused P-type layer, a first tunneling thin film layer, a first P-type semiconductor layer, a first passivation layer, and a first transparent conductive film layer is prepared on the front side in sequence from the inside to the outside, and also includes a thin-film solar cell unit composed of a first N-type semiconductor layer, a second tunneling thin film layer, a second P-type semiconductor layer, and a second transparent conductive film layer. The two solar cell units are connected in series through a first metal electrode, and the entire solar cell is connected to an external circuit through a second metal electrode and a third metal electrode. Since the thin-film solar cell unit can utilize sunlight that cannot be absorbed by the crystalline silicon solar cell, the combination of the two can effectively improve the overall solar energy conversion efficiency, thereby solving the problem of low conversion efficiency of solar cells using a single-junction tunneling oxide layer passivated metal structure.
[0066] Embodiment 2
[0067] Figure 2 The present invention is a flow chart of a preparation method according to an embodiment of the present application.
[0068] Reference Figure 1 As shown, this embodiment provides a preparation method for preparing the two-junction solar cell provided in the above embodiment, which specifically includes the following steps:
[0069] S1. Clean and texturize both sides of the N-type crystalline silicon substrate.
[0070] The selected N-type crystalline silicon substrate 1 has a resistivity of 0.5-3Ω.cm and a size of 158.78*158.75mm. 2 The single crystal silicon wafer is cleaned, the damaged layer is removed, and the texture is made on both sides to form a random pyramid structure on the front and back of the crystal silicon wafer, such as Figure 2a shown.
[0071] S2. Perform boron diffusion treatment on the front side of the N-type crystalline silicon substrate to form a diffused P-type layer.
[0072] Boron is diffused on the front side of the N-type crystalline silicon substrate after texturing by using a boron diffusion furnace to form a P-type layer 1', thereby obtaining a pn junction. Figure 2b As shown, the maximum doping concentration of the P-type layer is 10 20 cm -3 , the boron concentration is 10 17 cm -3 The diffusion junction depth is 0.5μm.
[0073] S3. Perform backside wrapping and expansion processing on the borosilicate glass on the front and back sides of the N-type crystalline silicon substrate.
[0074] The borosilicate glass on both sides of the N-type crystalline silicon substrate is removed by a cleaning machine, and the back side is expanded. The effect is as follows: Figure 2c shown.
[0075] S4. Prepare a first tunneling thin film layer and a third tunneling thin film layer.
[0076] In the unloading section of the cleaning machine, the flip mechanism is used to realize the UV ozone treatment of the front and back surfaces of the silicon wafer to realize the growth of the ultra-thin tunneling oxide layer, obtain the first tunneling film layer 2 on the front side, and obtain the third tunneling film layer 2' on the back side, such as Figure 2d As shown, the thickness of the two tunneling thin film layers is 1-3 nm. In fact, the two tunneling thin film layers are continuous at the edge of the crystalline silicon substrate.
[0077] S5, preparing a first P-type semiconductor layer and a second N-type semiconductor layer.
[0078] When preparing the first tunneling film layer and the third tunneling film layer, boron-doped amorphous silicon is deposited on the front side and phosphorus-doped amorphous silicon is deposited on the back side using an anti-winding plating carrier type reactive magnetron sputtering device, with thicknesses of 70nm and 120nm, respectively, and doping concentrations of 6 10 20 / cm 3 and 10 21 / cm 3 ; Then, the cell is subjected to a high temperature annealing treatment at about 890°C for 20 minutes in a tubular annealing furnace, so that a first P-type semiconductor layer 3 is formed on the first tunneling film layer doped on the front side, and a second N-type semiconductor layer 4 is formed on the third tunneling film layer on the back side. The structure is as follows Figure 2e shown.
[0079] S6. Perform deposition and annealing to obtain a first passivation layer and a second passivation layer.
[0080] After the preparation of the first P-type semiconductor layer and the second N-type semiconductor layer is completed, a 3nm aluminum oxide film is deposited on the front side by an atomic layer deposition device to form a first passivation layer 5, and a 3nm silicon oxide film is deposited on the back side to form a second passivation layer 6. The structure is as follows Figure 2f shown.
[0081] S7. Prepare a second anti-reflection layer on the second passivation layer.
[0082] After the preparation of the two passivation layers is completed, a silicon nitride and silicon oxide laminated film is deposited on the back of the material through a tubular PECVC to form a second anti-reflection layer 15. The thickness of the second anti-reflection layer can be actually adjusted according to the characteristics of the single-sided or double-sided battery. Its structure is as follows: Figure 2g shown.
[0083] S8. Prepare a first transparent conductive film layer on the first passivation layer.
[0084] By using an anti-winding plate type reactive magnetron sputtering device, an 80 nm indium tin titanium oxide (ITO) transparent conductive film is deposited on the first passivation layer as the first transparent conductive film layer 9, and its structure is as follows: Figure 2h As shown, the square resistance of the first transparent conductive film layer is 20Ω / square.
[0085] S9. Prepare a first metal electrode and a third metal electrode.
[0086] The first metal electrode 7 and the third metal electrode 8 are prepared on the first transparent conductive polishing layer by screen printing. Figure 2i As shown; the first metal electrode must be able to burn through the ITO film layer 9 and the aluminum oxide film layer 5, and contact the surface of the boron-doped polysilicon 3 to a certain depth, and the gate line height exposed outside the ITO 9 is less than 5nm, and the exposed part of the electrode is a silver electrode.
[0087] S10, sequentially preparing a first N-type semiconductor layer, the second tunneling thin film layer, a second P-type semiconductor layer, the second transparent conductive film layer and the first anti-reflection layer.
[0088] The anti-winding plate type plasma enhanced chemical vapor deposition equipment is used to deposit a phosphorus-doped amorphous silicon film on the front side of the cell to form a first N-type semiconductor layer 10, such as Figure 2j As shown, the thickness of the first N-type semiconductor layer is 20 nm, and the phosphorus doping concentration is 3 10 21 / cm 3 , the deposition temperature is 200-220℃.
[0089] The intrinsic hydrogenated amorphous silicon film is deposited on the front of the cell by using an anti-winding plating carrier type plasma enhanced chemical vapor deposition device to form a second tunneling film layer 11, such as Figure 2k As shown, the thickness of the second tunneling thin film layer is 5 nm, and the deposition temperature is 200-220° C.;
[0090] The anti-winding plating carrier type plasma enhanced chemical vapor deposition equipment is used to deposit a boron hydride-doped amorphous silicon film on the front side of the cell to form a second P-type semiconductor layer 12, such as Figure 2 l As shown, the thickness of the second P-type semiconductor layer is 20 nm, and the boron doping concentration is 8 10 20 / cm 3 , deposition temperature is 200-220°C;
[0091] An ITO film, namely the second transparent conductive film layer 13, is deposited on the front of the cell using an anti-winding plating carrier type reactive magnetron sputtering device. Figure 2mAs shown, the thickness of the second transparent conductive film layer is 100 nm, the square resistance is 40Ω / square, and the deposition temperature is room temperature.
[0092] Finally, a low-temperature silver paste is printed on the front of the cell by screen printing to obtain a second metal electrode 14, such as Figure 2 o As shown, its curing temperature is lower than 180°C.
[0093] You can also use laser scanning to trim the back edge of the cell (such as Figure 2n ) to expose the bare silicon wafer. This process can be an optional process depending on the actual situation.
[0094] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0095] It will be appreciated by those skilled in the art that the embodiments of the present invention may be provided as methods, devices, or computer program products. Therefore, the embodiments of the present invention may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware. Moreover, the embodiments of the present invention may take the form of a computer program product implemented on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program codes.
[0096] The embodiments of the present invention are described with reference to the flowcharts and / or block diagrams of the methods, terminal devices (systems), and computer program products according to the embodiments of the present invention. It should be understood that each process and / or block in the flowchart and / or block diagram, as well as the combination of the processes and / or blocks in the flowchart and / or block diagram, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor, or other programmable data processing terminal device to generate a machine, so that the instructions executed by the processor of the computer or other programmable data processing terminal device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.
[0097] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing terminal device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce a manufactured product including an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.
[0098] These computer program instructions can also be loaded onto a computer or other programmable data processing terminal device so that a series of operating steps are executed on the computer or other programmable terminal device to produce a computer-implemented process, thereby providing instructions for executing on the computer or other programmable terminal device to implement the process. Figure 1 A process or multiple processes and / or boxes Figure 1 A step that specifies a function in one or more boxes.
[0099] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.
[0100] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.
[0101] The technical solution provided by the present invention is introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A two-junction solar cell, characterized in that: The invention comprises an N-type crystalline silicon substrate, wherein the crystalline silicon substrate comprises a front side and a back side, wherein: A diffused P-type layer, a first tunneling thin film layer, a first P-type semiconductor layer, a first passivation layer, a first transparent conductive film layer, a first N-type semiconductor layer, a second tunneling thin film layer, a second P-type semiconductor layer, a second transparent conductive film layer and a first anti-reflection layer are sequentially prepared on the front surface from inside to outside; A first metal electrode is formed between the first P-type semiconductor layer and the first transparent conductive film layer, and a second metal electrode is formed on the second transparent conductive film layer, wherein the second metal electrode penetrates the first anti-reflection layer outwardly; The reverse surface is provided with a third tunneling thin film layer, a second N-type semiconductor layer, a second passivation layer and a second anti-reflection layer in sequence from inside to outside; A third metal electrode connected to the second N-type semiconductor layer is formed on the second N-type semiconductor layer, and the third metal electrode penetrates the second passivation layer and the second anti-reflection layer outwardly; The first tunneling film layer is a mixture film of group IVA elements, an oxide film, a nitride film or a nitride oxide film, or a metal oxide film; The thickness of the first tunneling thin film layer is 1-5 nm; The first P-type semiconductor layer and the second P-type semiconductor layer are polycrystalline boron-doped films or amorphous boron-doped films of group IVA elements, or are highly conductive polarity P-type semiconductor films of compounds of group IIA elements or group VIA elements; The thickness of the first P-type semiconductor layer or the second P-type semiconductor layer is 15-150 nm.
2. The two-junction solar cell according to claim 1, characterized in that: The dopant of the diffused P-type layer is boron, the maximum doping concentration of the dopant is 1018-1020 cm-3, and the diffusion junction depth at a boron concentration of 1017 cm-3 is 0.2-0.8 μm.
3. The two-junction solar cell according to claim 1, characterized in that: The first passivation layer comprises a stack of one or more film layers selected from the group consisting of an aluminum oxide film, a silicon oxide film, an intrinsic film, and a P-type heavily doped amorphous IVA group element mixture film; The thickness of the first passivation layer is 3-5 nm.
4. The two-junction solar cell according to claim 1, characterized in that: The first N-type semiconductor layer and the second N-type semiconductor layer are polycrystalline doped films or amorphous phosphorus-doped films based on a mixture of group IVA elements, or are highly conductive polarity N-type semiconductor films of compounds of group IIA elements or group VIA elements; The thickness of the first N-type semiconductor layer and the second N-type semiconductor layer is 15-150 nm.
5. The two-junction solar cell according to claim 1, characterized in that: The second passivation layer comprises a single layer of film material or a stack of multiple layers of film materials selected from the group consisting of a silicon nitride film layer, a silicon oxide film, an intrinsic film, and an N-type heavily doped amorphous IVA group element film; The thickness of the second passivation layer is 3-15 nm.
6. The two-junction solar cell according to claim 1, characterized in that: The thickness of the first transparent conductive film layer and the second transparent conductive film layer is 60-100 nm.
7. A preparation method for preparing a two-junction solar cell according to any one of claims 1 to 6, characterized in that: The preparation method comprises the steps of: Cleaning and texturing both sides of the N-type crystalline silicon substrate; Performing boron diffusion treatment on the front surface of the N-type crystalline silicon substrate to form the diffused P-type layer; Performing backside wrapping and expansion processing on the borosilicate glass on the front and back sides of the N-type crystalline silicon substrate; Performing tunneling layer growth operations on the front side and the back side of the N-type crystalline silicon substrate respectively to obtain the first tunneling thin film layer and the third tunneling thin film layer; Forming the first P-type semiconductor layer on the first tunneling thin film layer, and forming the second N-type semiconductor layer on the third tunneling thin film layer; Performing deposition and annealing treatment on the N-type crystalline silicon substrate to obtain the first passivation layer and the second passivation layer; preparing a second anti-reflection layer on the second passivation layer; preparing the first transparent conductive film layer on the first passivation layer; The first metal electrode and the second metal electrode are prepared on the first transparent conductive polishing layer by screen printing, and the third metal electrode is prepared on the second anti-reflection layer, wherein the first metal electrode penetrates the first passivation layer and has deep contact with the first P-type semiconductor layer; The first N-type semiconductor layer, the second tunneling thin film layer, the second P-type semiconductor layer, the second transparent conductive film layer and the first anti-reflection layer are sequentially prepared on the first transparent conductive film layer.