Transfer method of two-dimensional semiconductor materials
By using PMMA for dry transfer in a high-humidity environment, the problems of damage, wrinkles and contamination during the transfer of two-dimensional semiconductor materials are solved, efficient and lossless transfer is achieved, and the electrical properties of the material are significantly improved.
Patent Information
- Application Number
- CN202210274087.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-20
AI Technical Summary
Existing two-dimensional semiconductor material transfer methods can easily cause material damage, wrinkles or contamination, affecting its electrical properties.
PMMA is used to replace PDMS, and dry transfer is performed in a high-humidity environment. Through steps such as spin coating PMMA, heating and curing, segmentation and attachment, and removal of PMMA adhesive layer, efficient and lossless transfer of two-dimensional semiconductor materials is achieved.
It improves the transfer efficiency of two-dimensional materials, avoids wrinkles and contamination, and significantly improves the electrical properties of the transferred semiconductor film.
Smart Images

Figure CN114649200B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor material technology, in particular to the transfer of two-dimensional semiconductor materials, and specifically to an efficient and lossless method for transferring two-dimensional semiconductor materials. Background Art
[0002] Two-dimensional materials refer to materials in which electrons can move freely (in-plane motion) only in two dimensions at the nanoscale (1-100nm). Since the discovery of graphene, the world's first two-dimensional material, two-dimensional materials have attracted considerable attention and research due to their extraordinary physical, electronic and optoelectronic properties (including sensitivity, transparency and semiconductor properties). To date, two-dimensional materials have formed a large family, including graphene, transition metal chalcogenides, black phosphorus and other major categories. Currently, the most widely studied are two-dimensional semiconductor materials in transition metal chalcogenides. Taking molybdenum disulfide as an example, a single layer of molybdenum disulfide has good electrical properties, and the electron mobility at room temperature is as high as 200cm 2 v -1 s -1 , electronic switching ratio up to 10 8 , has great application potential in high-performance logic circuits and is expected to shine in the post-Moore era.
[0003] In the prior art, chemical vapor deposition is generally used to prepare two-dimensional semiconductor materials on a growth substrate, and then the two-dimensional semiconductor materials are transferred from the growth substrate to a target substrate to prepare semiconductor transistors.
[0004] Since the electrical properties of two-dimensional semiconductor materials are easily affected by material morphology, how to quickly and non-destructively transfer two-dimensional semiconductor materials from the growth substrate to the target substrate has become a key issue in the preparation process of two-dimensional semiconductor materials.
[0005] The existing two-dimensional material transfer methods mainly include PMMA water-assisted transfer method and PDMS dry transfer method. In the PMMA water-assisted transfer method, the molybdenum disulfide material needs to be in direct contact with pure water. After the molybdenum disulfide is transferred to the target substrate and air-dried, the two-dimensional material is prone to wrinkles, and impurities in the pure water are also prone to contaminating the material. In the PDMS dry transfer method, PDMS is directly attached to the growth substrate, and the two-dimensional material is transferred out by heating to increase the adsorption force, and then attached to the target substrate. However, PDMS cannot be completely and tightly attached to the growth substrate, resulting in many materials cannot be transferred, and even damage, and low transfer efficiency.
[0006] Therefore, existing two-dimensional material transfer methods may cause damage, wrinkles or contamination to the original two-dimensional semiconductor film during the transfer process, affecting the electrical properties of the transferred material. Summary of the invention
[0007] The purpose of the present invention is to propose an efficient and lossless two-dimensional semiconductor material transfer method to address the damage or impact caused to the two-dimensional semiconductor film by the PMMA water-assisted transfer method and the PDMS dry transfer method in the prior art. PMMA is used to replace PDMS, and a single-layer two-dimensional material is dry-transferred in a high humidity environment. This not only ensures the transfer efficiency of the two-dimensional material, but also avoids the introduction of wrinkles and contamination caused by the traditional water-assisted transfer method, thereby effectively improving the electrical properties of the single-layer two-dimensional material semiconductor film after transfer.
[0008] To achieve the above object, a first aspect of the present invention provides a method for transferring a two-dimensional semiconductor material, comprising:
[0009] Step 1: preparing a two-dimensional semiconductor material on a growth substrate using a chemical vapor deposition method to obtain a two-dimensional semiconductor material / growth substrate structure;
[0010] Step 2, spin-coating PMMA on the surface of the two-dimensional semiconductor material / growth substrate, and placing the growth substrate with the PMMA spin-coated on a hot plate for heating and curing, wherein the cured PMMA condenses on the surface of the growth substrate into a thin film, i.e., a PMMA cured adhesive layer, thereby obtaining a three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / growth substrate;
[0011] Step 3, maintaining the transfer environment humidity above 50% RH, observing the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / growth substrate under a microscope, determining the target area to be transferred, separating the PMMA cured adhesive layer in the area from other areas with a small carving knife, and then using tweezers to clamp the two-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material in the target area from the growth substrate and directly attach it to the target substrate, to obtain a three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate;
[0012] Step 4, leaving the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate to stand at room temperature for a certain period of time, and then soaking the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate in a room temperature acetone solution to remove the PMMA cured adhesive layer on the surface; finally, soaking the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate in isopropanol for 5 minutes to remove the residual acetone solution; finally, blow drying with a nitrogen gun to obtain a double-layer structure of two-dimensional semiconductor material / target substrate, and completing the transfer of the two-dimensional semiconductor material.
[0013] As an optional embodiment, in the step 2, PMMA is spin-coated on the surface of the two-dimensional semiconductor material / growth substrate, wherein the PMMA specification is 200k, the rotation speed is set to 1000-1200 r / min, and the rotation time is 1-5 min.
[0014] As an optional embodiment, in step 2, the growth substrate on which PMMA is spin-coated is placed on a hot plate for heating and curing, wherein the heating temperature is 80±10° C. and the heating time is 3-5 min.
[0015] As an optional embodiment, in the step 2, the thickness of the PMMA cured adhesive layer is 500-900 nm.
[0016] As an optional embodiment, the two-dimensional semiconductor material includes MoS 2 , WS 2 、MoSe 2 One of the above, wherein the growth substrate comprises SiO 2 / Si、HfO 2 / Si, one of soda-lime glass.
[0017] As an optional embodiment, in step 3, the transfer environment is a clean room of Class 100, and the number of dust particles of 0.5 μm per cubic meter in the air is less than 1 million.
[0018] As an optional embodiment, in step 3, the tweezers used in the transfer process are pointed anti-static tweezers.
[0019] As an optional embodiment, in step 4, the standing time at room temperature is 8-16 hours.
[0020] As an optional embodiment, in step 4, the soaking time in the room temperature acetone solution is 1-5 hours; the soaking time in the isopropanol is 1-30 minutes.
[0021] According to the above embodiments of the present invention, the significant advantages compared with the existing ones are:
[0022] The method for transferring two-dimensional semiconductor materials of the present invention uses PDMS instead of PMMA, and performs dry transfer of the two-dimensional semiconductor material in a high humidity environment, thereby solving the shortcomings of wet transfer and dry transfer in the prior art, ensuring the transfer efficiency of the two-dimensional material, and avoiding the introduction of wrinkles and contamination caused by the traditional water-assisted transfer method, thereby achieving efficient and lossless transfer of the two-dimensional semiconductor material, and effectively improving the electrical properties of the single-layer two-dimensional material semiconductor film after transfer, thereby solving the problem that the existing transfer method may cause damage, wrinkles or contamination to the original two-dimensional semiconductor film during the transfer process, thereby affecting the electrical properties of the transferred material.
[0023] It should be understood that all combinations of the aforementioned concepts and the additional concepts described in more detail below can be considered as part of the inventive subject matter of the present disclosure as long as such concepts are not mutually inconsistent. In addition, all combinations of the claimed subject matter are considered as part of the inventive subject matter of the present disclosure.
[0024] The foregoing and other aspects, embodiments and features of the present invention can be more fully understood from the following description in conjunction with the accompanying drawings. Other additional aspects of the present invention, such as the features and / or beneficial effects of the exemplary embodiments, will be apparent from the following description or learned from the practice of the specific embodiments according to the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings are not intended to be drawn to scale. In the drawings, each identical or nearly identical component shown in various figures may be represented by the same reference numeral. For clarity, not every component is labeled in every figure. Embodiments of various aspects of the present invention will now be described by way of example and with reference to the accompanying drawings, in which:
[0026] Figure 1a-1h is a schematic diagram of a method for transferring a two-dimensional semiconductor material according to an exemplary embodiment of the present invention, that is, a process of dry-transferring a two-dimensional semiconductor material using PMMA in a high humidity environment;
[0027] Figure 2a Taking molybdenum disulfide two-dimensional material as an example, Figure 1a-1h Optical microscope image of molybdenum disulfide obtained after transferring it to the target substrate using the transfer method shown, Figure 2b is an optical microscope image of molybdenum disulfide obtained after transferring molybdenum disulfide to a target substrate using the transfer method of Example 2;
[0028] Figure 3a yes Figure 2a AFM characterization of the transferred MoS2 sample. Figure 3b is an AFM characterization of molybdenum disulfide obtained after transferring molybdenum disulfide to a target substrate using the transfer method of Example 3;
[0029] Figure 4 This is a schematic diagram of the structure of a molybdenum disulfide transistor based on molybdenum disulfide;
[0030] Figure 5 It is a schematic diagram comparing transfer characteristic curves of a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method of the present invention and a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method of Example 3;
[0031] Figure 6a-6bSchematic diagrams of output characteristic curves of a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method according to the example of the present invention and a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method according to Example 3, respectively.
[0032] The meanings of the various symbols in the accompanying drawings are as follows:
[0033] 10. Growth substrate; 20. Two-dimensional semiconductor material; 30. PMMA curing adhesive layer; 50. Target substrate.
[0034] 100, PMMA; 200, heating plate; 300, constant humidity chamber (ambient humidity is controlled at 50% RH); 400, small carving knife; 500; tweezers (preferably anti-static tweezers); 600, acetone solution; 700, IPA solution; 800, nitrogen gun. DETAILED DESCRIPTION
[0035] In order to better understand the technical content of the present invention, specific embodiments are given and described as follows in conjunction with the accompanying drawings.
[0036] Various aspects of the present invention are described in this disclosure with reference to the accompanying drawings, in which many illustrative embodiments are shown. The embodiments of the present disclosure are not necessarily intended to include all aspects of the present invention. It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways, because the concepts and embodiments disclosed by the present invention are not limited to any implementation. In addition, some aspects disclosed by the present invention can be used alone or in any appropriate combination with other aspects disclosed by the present invention.
[0037] Combination Figure 1a-1h The transfer method of two-dimensional semiconductor materials shown in the example aims to propose a dry transfer of two-dimensional semiconductor materials using PMMA in a high humidity environment, which not only ensures the transfer efficiency of molybdenum disulfide, but also avoids the introduction of wrinkles and contamination, and makes up for the shortcomings of the two transfer methods (dry and wet transfer) in the prior art, and effectively improves the electrical performance of the single-layer molybdenum disulfide semiconductor transistor after transfer.
[0038] As an example, a dry transfer method of a two-dimensional semiconductor material using PMMA in a high humidity environment includes:
[0039] Step 1: preparing a two-dimensional semiconductor material on a growth substrate using a chemical vapor deposition method to obtain a two-dimensional semiconductor material / growth substrate structure;
[0040] Step 2, spin-coating PMMA on the surface of the two-dimensional semiconductor material / growth substrate, and placing the growth substrate with the PMMA spin-coated on a hot plate for heating and curing, wherein the cured PMMA condenses on the surface of the growth substrate into a thin film, i.e., a PMMA cured adhesive layer, thereby obtaining a three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / growth substrate;
[0041] Step 3, maintaining the transfer environment humidity above 50% RH, observing the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / growth substrate under a microscope, determining the target area to be transferred, separating the PMMA cured adhesive layer in the area from other areas with a small carving knife, and then using tweezers to clamp the two-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material in the target area from the growth substrate and directly attach it to the target substrate, to obtain a three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate;
[0042] Step 4. Leave the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate at room temperature for a certain period of time, in order to allow the two-dimensional semiconductor material and the target substrate to adsorb more closely; then soak the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate in a room temperature acetone solution to remove the PMMA cured adhesive layer on the surface; finally, soak the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate in isopropanol for 5 minutes to remove the residual acetone solution; finally, blow dry with a nitrogen gun to obtain a double-layer structure of two-dimensional semiconductor material / target substrate, completing the transfer of the two-dimensional semiconductor material.
[0043] In step 3 of the aforementioned embodiment, the reason for maintaining high humidity in the transfer environment is that high humidity will infiltrate into the PMMA cured adhesive layer, making it more viscous, which is conducive to lifting the two-dimensional semiconductor material from the growth substrate.
[0044] As an optional embodiment, in the step 2, PMMA is spin-coated on the surface of the two-dimensional semiconductor material / growth substrate, wherein the PMMA specification is 200k, the rotation speed is set to 1000-1200 r / min, and the rotation time is 1-5 min.
[0045] As an optional embodiment, in step 2, the growth substrate on which PMMA is spin-coated is placed on a hot plate for heating and curing, wherein the heating temperature is 80±10° C. and the heating time is 3-5 min.
[0046] As an optional embodiment, in the step 2, the thickness of the PMMA cured adhesive layer is 500-900 nm.
[0047] As an optional embodiment, the two-dimensional semiconductor material includes MoS 2 , WS2 、MoSe 2 One of the above, wherein the growth substrate comprises SiO 2 / Si、HfO 2 / Si, one of soda-lime glass.
[0048] As an optional embodiment, in step 3, the transfer environment is at least a clean room class 100 area, and the number of dust particles of 0.5 μm per cubic meter in the air is less than 1 million.
[0049] As an optional embodiment, in step 3, the tweezers used in the transfer process are pointed anti-static tweezers.
[0050] As an optional embodiment, in step 4, the standing time at room temperature is 8-16 hours.
[0051] As an optional embodiment, in step 4, the soaking time in the room temperature acetone solution is 1-5 hours; the soaking time in the isopropanol is 1-30 minutes.
[0052] Below we take molybdenum disulfide two-dimensional material as an example and combine specific examples to explain the implementation of the transfer method of the present invention in more detail.
[0053] Example 1
[0054] Step 1: Use chemical vapor deposition to deposit HfO 2 MoS deposited on Si growth substrate 2 Two-dimensional semiconductor material, a two-layer structure of two-dimensional semiconductor material / growth substrate is obtained, such as Figure 1a As shown;
[0055] Step 2, spin-coating PMMA on the surface of the two-dimensional semiconductor material / growth substrate; wherein the PMMA specification is 200k, the rotation speed is set to 1000r / min, and the rotation time is 1min;
[0056] Then, the growth substrate with the PMMA spin-coated is placed on a hot plate for heating and curing. Figure 1b As shown, the heating temperature is 80°C and the heating time is 5 minutes; the cured PMMA will condense into a thin film with a thickness of about 700 nm on the surface of the growth substrate, obtaining a three-layer structure of PMMA cured glue layer / two-dimensional semiconductor material / growth substrate;
[0057] Step 3: Use a constant humidity chamber or air humidifier to keep the transfer environment humidity above 50% RH, so that the PMMA cured adhesive layer has higher viscosity and can easily lift the two-dimensional semiconductor material from the growth substrate; observe the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / growth substrate under a microscope, find the target area to be transferred, and use a small carving knife to separate the PMMA cured adhesive layer in this area from other areas, such as Figure 1c ; Then use tweezers to clamp the two-layer structure of PMMA cured glue layer / two-dimensional semiconductor material in the target area and directly attach it to the target substrate to obtain a three-layer structure of PMMA cured glue layer / two-dimensional semiconductor material / target substrate, such as Figure 1d and 1e As shown;
[0058] Step 4: Leave the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate at room temperature for about 12 hours, in order to allow the two-dimensional semiconductor material to adsorb more closely to the target substrate; then soak the structure in a room temperature acetone solution for 4 hours to remove the PMMA cured adhesive layer on the surface. Figure 1f ;
[0059] Finally, the structure was immersed in isopropanol for 5 min to remove the residual acetone solution. Figure 1g ; Then blow dry with a nitrogen gun to obtain a double-layer structure of two-dimensional semiconductor material / target substrate, and the transfer is completed. Figure 1h shown.
[0060] Example 2
[0061] The operation is similar to that of Example 1, except that the transfer process in step 3 is not performed in a high humidity environment, but in an environment below 50% RH. In Example 2, the humidity of the transfer environment is 30%.
[0062] Combination Figure 2b As shown, the molybdenum disulfide two-dimensional material obtained by the transfer method of Example 2 had damage defects.
[0063] Example 3
[0064] The operation is similar to that of Example 1, except that the transfer process in step 3 is not carried out in a humidity environment greater than 50% RH, but in pure water.
[0065] Combination Figure 3b As shown, the molybdenum disulfide two-dimensional material obtained by the transfer method of Example 3 had wrinkle defects.
[0066] Optical microscopic characterization
[0067] Combination Figure 2a and 2bIt can be seen from the comparison that based on the present invention Figures 1a-1f The transfer method of the exemplary embodiment (Example 1) is intact for the molybdenum disulfide transferred to the target substrate. In Example 2, which is used as the control example 1, the molybdenum disulfide transferred to the target substrate by the transfer method of Example 2 is damaged in many places. The difference between the embodiment and the control example 1 is the environmental humidity during the transfer, indicating that the environmental humidity has a significant effect on the material transfer. In the present invention, a high humidity RH50% or more transfer environment is used to achieve efficient and lossless transfer of two-dimensional materials, and the transfer effect is excellent.
[0068] The example of PMMA transferring molybdenum disulfide under low humidity is similar to the PDMS dry transfer process. Both of them are not adsorbed tightly enough to the growth substrate, resulting in damage to the two-dimensional material after transfer. Therefore, the time delay of this control group verifies the superiority of PMMA dry transfer under high humidity over traditional dry transfer.
[0069] AFM characterization
[0070] Combination Figure 3a and 3b It can be seen from the comparison that based on the present invention Figures 1a-1f In the transfer method of the exemplary embodiment (Example 1), the morphology of the molybdenum disulfide transferred to the target substrate is very flat. In Example 3, which is used as the control example 2, the molybdenum disulfide transferred to the target substrate using the transfer method of Example 3 has many wrinkles. Since the transfer process in Control Example 2 is carried out in pure water, which is consistent with the traditional PMMA wet transfer, this shows that the direct contact between molybdenum disulfide and water during the transfer process will cause wrinkles in the molybdenum disulfide and reduce the quality of the film. This is because the capillary force of water acts on the molybdenum disulfide. Therefore, this control group experiment further verifies the superiority of dry transfer of PMMA under high humidity compared with traditional wet transfer.
[0071] Comparison of MoS2 transistor characteristics
[0072] by Figure 4 Take the molybdenum disulfide transistor shown as an example. Figure 5 The transfer characteristic curve comparison of a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method of the present invention (Example 1) and a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method of Example 3 is exemplarily shown.
[0073] One of the main parameters for evaluating transistor performance is usually the field effect mobility g m , and its calculation formula is as follows:
[0074]
[0075] Where L and W are the channel length and width of the transistor respectively, and Cox is the back gate dielectric HfO2 The unit capacitance.
[0076] Combination Figure 5 The transfer characteristic curves of the molybdenum disulfide transistor shown in the figure are compared. Substituting the data corresponding to the two embodiments in the figure into the mobility formula, it can be obtained that the field effect mobility of embodiment 1 and embodiment 3 is 35cm 2 v -1 s -1 and 18cm 2 v - 1 s -1 It can be seen that the former is nearly twice that of the latter, which means that compared with the traditional wet transfer, the PMMA dry transfer under high humidity proposed in the present invention can protect the quality of the two-dimensional material to a great extent and improve its electrical properties.
[0077] Figure 6a-6b The output characteristic curves of a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method of the present invention (Example 1) and a molybdenum disulfide transistor prepared from molybdenum disulfide obtained by the transfer method of Example 3 are exemplarily shown.
[0078] It can be seen from the figure that under the same voltage, the saturation current of the molybdenum disulfide transistors of Example 1 and Example 3 are 100A / m and 20A / m respectively, and the former is nearly 5 times that of the latter, indicating that the electrical performance of the former is far superior to that of the latter. This further proves the advantages of PMMA dry transfer under high humidity for two-dimensional semiconductor materials in logic device applications.
[0079] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.
Claims
1. A method for transferring a two-dimensional semiconductor material, characterized in that: The following steps are involved: Step 1: depositing a two-dimensional semiconductor material on a growth substrate to obtain a two-dimensional semiconductor material / growth substrate structure; Step 2, spin-coating PMMA on the surface of the two-dimensional semiconductor material / growth substrate, and placing the growth substrate with the PMMA spin-coated on a hot plate for heating and curing, wherein the cured PMMA condenses on the surface of the growth substrate into a thin film, i.e., a PMMA cured adhesive layer, thereby obtaining a three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / growth substrate; Step 3, maintaining the transfer environment humidity above 50% RH, observing the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / growth substrate under a microscope, determining the target area to be transferred, separating the PMMA cured adhesive layer in the area from other areas, and then using tweezers to clamp the two-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material in the target area from the growth substrate and directly attach it to the target substrate to obtain a three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate; Step 4. Leave the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate at room temperature for a certain period of time, then soak it in a room temperature acetone solution to remove the PMMA cured adhesive layer on the surface, and finally soak the three-layer structure of PMMA cured adhesive layer / two-dimensional semiconductor material / target substrate in isopropanol for 5 minutes to remove the residual acetone solution; finally, blow dry it with a nitrogen gun to obtain a two-layer structure of two-dimensional semiconductor material / target substrate, and complete the transfer of the two-dimensional semiconductor material.
2. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: In the step 2, PMMA is spin-coated on the surface of the two-dimensional semiconductor material / growth substrate, wherein the PMMA specification is 200k, the rotation speed is set to 1000-1200r / min, and the rotation time is 1-5min.
3. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: The growth substrate on which the PMMA is spin-coated is placed on a hot plate for heating and curing, wherein the heating temperature is 80±10° C. and the heating time is 3-5 minutes.
4. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: The thickness of the PMMA cured adhesive layer is 500-900 nm.
5. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: The two-dimensional semiconductor material includes one of MoS2, WS2, and MoSe2, and the growth substrate includes one of SiO2 / Si, HfO2 / Si, and soda-lime glass.
6. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: In step 3, the transfer environment is a clean room of Class 100, and the number of dust particles of 0.5 μm per cubic meter in the air is less than 1 million.
7. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: In step 3, the tweezers used in the transfer process are pointed anti-static tweezers.
8. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: In step 4, the standing time at room temperature is 8-16 hours.
9. The method for transferring a two-dimensional semiconductor material according to claim 1, characterized in that: In step 4, the soaking time in the room temperature acetone solution is 1-5 hours; the soaking time in the isopropanol is 1-30 minutes.
Citation Information
Patent Citations
Heat-release adhesive tape-based two-dimensional transition metal chalcogenide transfer method
CN106298466A
Method for preparing two-dimensional transition metal sulfide through directional transfer CVD method
CN110676218A
Two-dimensional Van der Waals bipolar transistor based on tellurium nanosheets and construction method thereof
CN113130637A
Large-area graphene transfer method
US20160137507A1
Dry graphene transfer from metal foils