Two-dimensional or quasi-two-dimensional polymer film synthesis method, two-dimensional or quasi-two-dimensional polymer film and use thereof
By using surfactants and aromatic monomers to synthesize 2D or q2D polymer films in polar solvents, the problems of insufficient crystallinity and domain size of polymer films in the existing technology are solved, and efficient polymer film synthesis is achieved. , suitable for a variety of applications.
Patent Information
- Application Number
- CN202080057084.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-08-11
AI Technical Summary
Existing technologies are difficult to effectively synthesize two-dimensional or quasi-two-dimensional polymer films with high crystallinity and large areas, resulting in small crystal domain sizes and limiting the reliable functional development of emerging organic 2D materials.
By providing a monolayer of surfactant and aromatic monomer in a polar solvent, the monomer polymerization is initiated to form a 2D or q2D polymer film, and the hydrophilic group of the surfactant interacts with the functional group of the monomer to regulate the polymerization. growth direction to achieve high crystallinity and the formation of large-area films.
Successfully synthesized 2D or q2D polymer membranes have high crystallinity, defined pore sizes, and easily transferable crystal structures with average domain sizes in the range of 0.1 μm to 1 cm, making them suitable for the production of membranes, electronic devices, or catalysts.
Smart Images

Figure CN114651030B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for synthesizing a two-dimensional or quasi-two-dimensional polymer containing a surfactant, a two-dimensional or quasi-two-dimensional polymer film, and the use of the two-dimensional or quasi-two-dimensional polymer film in producing a film, an electronic device or a catalyst. Background Art
[0002] Both synthetic and natural polymers play important and ubiquitous roles in our everyday lives and, according to the definition proposed by Hermann Staudinger in the early 1920s (Staudinger 1920), they can generally be described by a sequence of repeating units linearly linked by covalent bonds.
[0003] There have been several attempts to go beyond Staudinger’s concept and synthesize sheet-like polymers with long-range order along two orthogonal directions, i.e., two-dimensional (2D) polymers, dating back to Gee’s interfacial polymerization experiments in 1935 (Gee 1935), Blumstein’s cross-linked polymers in the interlayer spaces of montmorillonite clay in 1958 (Blumstein et al. 1958), and Stupp’s bulk polymerization within self-assembled bilayers in 1993 (Stupp et al. 1993).
[0004] However, until the successful discovery of natural 2D polymers such as graphene layers separated from graphite, truly structurally defined 2D polymers had not yet been obtained (Novoselov et al., 2004, Chen et al., 2012). Xu et al. disclosed a method for preparing single-crystalline graphene on industrial copper foil. Xu et al. described a (5 x 50) cm 2 Graphene films with >99% ultra-highly oriented grains (Xu et al., 2017).
[0005] The discovery of graphene has also stimulated active research efforts devoted to the directed synthesis of 2D polymers. Bieri et al. described the surface-assisted synthesis of 2D poly(m-phenylene) networks (Bieri et al., 2009). Grill et al. disclosed the covalent assembly of porphyrin building blocks, and Cardenas et al. disclosed the covalent assembly of thiophenes by surface synthesis under ultrahigh vacuum (Grill et al., 2007, Cardenas et al., 2013). Unfortunately, the mobility of the monomers on the surface is limited, and only small domain sizes (typically tens of nanometers) can be obtained.
[0006] CN 109988325 A discloses a large-area ultra-thin high-crystallinity two-dimensional conjugated polymer film, wherein "high crystallinity" means different from a general amorphous film; a preparation method by chemical vapor deposition, which prepares a two-dimensional conjugated polymer film by interfacial copolymerization of a solid source of aromatic conjugated monomers on the surface of a substrate (preferably copper foil or gold foil); and its application.
[0007] Xiao et al. described single needle-like crystals of polythiophenes, particularly poly(3-hexylthiophene) (P3HT) and poly(3-octylthiophene) (P3OT), with different molecular conformations obtained by tetrahydrofuran vapor annealing and controlled solvent evaporation of commercial polythiophenes (Xiao et al., 2010).
[0008] Alternatively, 2D polymers can also be achieved by solution exfoliation of van der Waals (vdW) layered 2D covalent organic frameworks (Bunck and Dichtel 2013) or polymer crystals (Kissel et al. 2012) synthesized by solvothermal methods and / or solid-state polymerization. However, the exfoliation of defined lamellar structures and the precise control of their lateral size and thickness remain a challenge.
[0009] Furthermore, Sahabudeen et al. described the synthesis of free-standing, crystalline, monolayer or multilayer films of 2D polymers synthesized via air / water and liquid / water interfaces (Sahabudeen et al., 2016).
[0010] Yang et al. disclosed a method for preparing a surfactant Span80 and FeCl 3 A method for synthesizing polymer films by polymerization of pyrrole at a water / chloroform interface with the aid of pyrrole as an oxidant (Yang et al., 2016). Yang et al. described the formation of surfactant micelles and described different morphologies of polypyrrole, including disordered deposition of microspheres, vesicular aggregation, and a dense skeleton structure, depending on the surfactant concentration. In addition, Yang et al. disclosed that the prepared polypyrrole films had a vesicular structure that depended on the surfactant concentration, from disordered deposition of microspheres to the formation of vesicular aggregation, until a relatively dense skeleton structure was formed.
[0011] US 4872984 A discloses a water-permeable membrane synthesized by interfacial polymerization of monomers, aromatic polyamine reactants having at least two amine functional groups and monomers containing polyfunctional acyl halides or mixtures thereof, and aromatic amine reactants on a microporous support.
[0012] Sahabudeen et al. described the interfacial synthesis of structure-defined organic 2D materials synthesized via air / water and liquid / water interfaces (Sahabudeen et al., 2019), in particular the surfactant bilayer template approach, where the bilayer surface can be positively or negatively charged or modified with various functional groups, which offers the possibility of directing the growth of ultrathin nanosheets.
[0013] US 2011 / 281098 A1 discloses a method for preparing a polyaniline film on a support, the method being to prepare the polyaniline film by oxidative polymerization of aniline monomer in an aqueous acid medium, wherein the polymerization occurs in the presence of an oxidant, especially formic acid; and a salt MXx, especially a chloride. Preferably, the surface of the support is hydrophilic, the hydrophilicity being defined by a contact angle of 0 to less than 80°, using water as the liquid for measuring the angle.
[0014] Duan et al. described the preparation of semiconducting crystalline two-dimensional polyimide nanosheets by using hydrogen-bonding-induced pre-organization of pyromellitic acid (PMA) and melamine (MA), followed by imidization of the obtained planar hydrogen-bonded network (HBN) under a solvothermal process (Duan et al., 2019).
[0015] Unfortunately, the crystallinity of the resulting 2D polymers is still unsatisfactory, with small domain sizes (typically tens of nanometers), which poses a potential limitation to the development of reliable functions for this emerging class of organic 2D materials. Summary of the invention
[0016] The object of the present invention is to provide a method for the synthesis of two-dimensional (2D) or quasi-two-dimensional (q2D) polymer films which overcomes the disadvantages of the prior art.
[0017] This object is solved by providing a method for synthesizing a two-dimensional (2D) or quasi-two-dimensional (q2D) polymer film, the method comprising the following steps
[0018] a) providing a surfactant monolayer and at least one monomer in a polar solvent,
[0019] wherein the surfactant monolayer is aligned with the interface of the polar solvent and air,
[0020] wherein the monomer interacts with the surfactant monolayer,
[0021] wherein the monomer is an aromatic monomer,
[0022] b) initiating polymerization of said monomers, and
[0023] c) Polymerization and formation of 2D or q2D polymer films.
[0024] According to the invention, the method according to the invention is carried out in the order of steps a), b) and c).
[0025] As used herein, the term "polymer film" refers to a sheet-like organic macromolecule composed of connected organic monomers. According to the present invention, the polymer film is a non-metallic organic framework (MOF). Advantageously, the polymer film synthesized using the method according to the present invention is crystalline and has holes, preferably with a defined pore size. As used herein, the term "crystal" refers to a solid compound with a regular ordered structure. Crystallinity can be measured by X-ray diffraction or transmission electron microscopy. Further advantageously, the polymer film synthesized using the method according to the present invention is easy to transfer.
[0026] As used herein, the term "surfactant" (surface active agent) refers to a compound that reduces the surface tension between two liquids or between a gas and a liquid, wherein the surfactant comprises at least one hydrophilic group ("head") and at least one hydrophobic group ("tail"). Advantageously, surfactants direct organization, especially molecular orientation, and regulate polymerization.
[0027] In an embodiment, the surfactant is selected from the group consisting of a cationic surfactant, an anionic surfactant, and a neutral surfactant.
[0028] In an embodiment, the surfactant comprises a C14 to C20 alkyl or alkenyl group, preferably a C16 to C18 alkyl or alkenyl group.
[0029] In some embodiments, the surfactant is selected from bis(hexadecyl) phosphate, hexadecyltrimethylammonium bromide, wood wax alcohol, oleic acid, perfluorooctadecanoic acid, sodium dodecylbenzenesulfonate, (9Z)-octadecyl-9-en-1-yl sodium sulfate, sodium stearate, stearic acid, bis(hexadecyl) triethanolamine phosphate.
[0030] Most preferably, the surfactant is sodium (9Z)-octadecyl-9-en-1-yl sulfate (SOS) or octadecanoic acid (SA).
[0031] The conditions for forming a surfactant monolayer are known to those skilled in the art. The formation of a Langmuir monolayer is described by Kaganer et al. (Kaganer et al., 1999). For example, the minimum amount of SOS to form a monolayer of 6 cm in diameter is about 7 μl.
[0032] In an embodiment, the amount of surfactant used to provide a surfactant monolayer according to step a) is selected based on the surface area of the polar solvent. In an embodiment, for a surface area of 25 cm 2 of polar solvent or a surface area of 25 cm 2The surfactant monolayer was prepared with the amount of surfactant ranging from 1 μl to 20 μl for a surface area of 25 cm 2 of polar solvent or a surface area of 25 cm 2 In a further embodiment, the amount of surfactant is in the range of 0.04 μl / cm2 relative to the surface area of the polar solvent. 2 Up to 0.8 μl / cm 2 The surface area relative to the polar solvent is preferably 0.2 μl / cm 2 Up to 0.4 μl / cm 2 within the range.
[0033] In one embodiment, the surfactant monolayer is aligned with the interface of the polar solvent, wherein the hydrophilic groups of the surfactant face the polar solvent and the hydrophobic groups face the interface or extend out of the polar solvent. According to the present invention, the surfactant monolayer is aligned with the interface of the polar solvent and air.
[0034] Preferably, the surfactant monolayer is continuous. As used herein, the term "continuous" refers to an uninterrupted and uniform layer.
[0035] In an embodiment, the surfactant monolayer is formed by adding a surfactant solution in an organic solvent to a polar solvent and evaporating the organic solvent.
[0036] In an embodiment, the organic solvent is chloroform.
[0037] As used herein, the term "monomer" refers to a molecule that can undergo polymerization. Preferably, a surfactant monolayer and one monomer are provided in a polar solvent according to step a). In an alternative embodiment, two or three different monomers are provided in step a).
[0038] In an embodiment, the monomer is a natural or synthetic monomer, a polar or monopolar monomer, and / or a cyclic or linear monomer.
[0039] According to the invention, the monomer is an aromatic monomer. Advantageously, the aromatic monomer is rigid, planar or slightly curved, preferably forming a regular ordered film by polymerization. More advantageously, the aromatic monomer aligns the monomers, chains or layers of the 2D or q2D polymer, respectively, by π-π interactions. Thus, the crystallinity increases.
[0040] In a preferred embodiment, the monomer comprises an aromatic group, preferably selected from benzene, furan, naphthalene, perylene, porphyrin, pyrrole, thiophene, tetraphenylethylene, tetraphenylporphyrin, triphenylbenzene or triphenyltriazine.
[0041] Preferably, the monomer is a symmetrical monomer. As used herein, the term "symmetrical" refers to a molecule that is invariant after mirroring or rotation.
[0042] In an embodiment, the monomer is selected from alcohols, aldehydes, alkynes, amines, anhydrides, anilines, boric acid, carboxylic acids, diamines, diols, β-diketones, furans, halogenated hydrocarbons, hydrazines, hydroxyaldehydes, pyrroles, selenophenes and / or thiophenes. As used herein, the term "halogenated hydrocarbon" refers to a halogen-substituted hydrocarbon. In one embodiment, the halogenated hydrocarbon is an iodohydrocarbon or a bromohydrocarbon.
[0043] In a preferred embodiment, the monomers are selected from amines.
[0044] In certain cases, the monomer is selected from:
[0045]
[0046] In some embodiments, the concentration of the monomer is in the range of 0.1 mM to 5 mM, preferably in the range of 0.15 mM to 1.5 mM.
[0047] In an embodiment, the polar solvent in step a) is water and / or a water-miscible solvent. In another embodiment, the water-miscible solvent is selected from alcohol, preferably methanol or ethanol; dimethylformamide, acetonitrile. Preferably, the polar solvent is water.
[0048] In one embodiment, the hydrophilic group of the surfactant interacts with the monomer, preferably with at least one functional group of the monomer; through electrostatic interaction or covalent bonding. Advantageously, the monomer is pre-organized by interaction with the surfactant. Preferably, the monomer forms a monolayer by interaction with the surfactant.
[0049] In a preferred embodiment, the surfactant is selected according to the monomer. Advantageously, the growth direction of the polymerization in step c) is adjusted by the surfactant and monomer selection, in particular the horizontal or vertical growth direction.
[0050] As used herein, the term "horizontal growth direction" refers to the synthesis in the direction of an interface, preferably an interface of a polar solvent and air; and a layer stacking direction perpendicular to the interface.
[0051] As used herein, the term "vertical growth direction" refers to the direction of growth perpendicular to an interface, preferably perpendicular to the interface of a polar solvent and air; and the direction of layer stacking parallel to the interface.
[0052] Preferably, electrostatic interactions between the surfactant and the monomer result in a horizontal growth direction, and covalent bonds between the surfactant and the monomer result in a vertical growth direction.
[0053] For the horizontal growth direction, anionic surfactants are provided for monomers having cationic groups, in particular amino groups, boric acid or hydrazine; or positive partial charges, in particular sodium (9Z)-octadecyl-9-en-1-yl sulfate (SOS), sodium 4-dodecylbenzenesulfonate (SDBS) or dihexadecyl triethanolamine phosphate (DHP).
[0054] For the horizontal growth direction, monomers having anionic groups, especially carboxylic acids, or negative partial charges are provided with cationic surfactants, especially cetyltrimethylammonium bromide (CTAB).
[0055] For the vertical growth direction, the monomers having amino groups, boric acid or hydrazine are preferably provided with surfactants comprising carboxylic acid groups, in particular stearic acid (SA) or oleic acid (OA).
[0056] In other embodiments, a surfactant monolayer and at least one monomer are provided in a polar solvent according to step a), wherein the surfactant monolayer is aligned at the interface of the polar solvent, and the monomer interacts with the surfactant monolayer, in a range of 30 minutes to 24 hours, preferably in a range of 4 hours to 12 hours.
[0057] In one embodiment, the pH of the solution in steps a), b) and / or c) depends on the selected surfactant, monomer and polymerization reaction.
[0058] In another embodiment, the pH of the solution containing monomers with cationic groups, in particular amino groups, boronic acid or hydrazine or positive partial charges in step a) is in the range of pH 2 to pH 6, preferably in the range of pH 3 to pH 4.
[0059] In another embodiment, the pH of the solution containing monomers with cationic groups, in particular amino groups, boronic acids or hydrazines or positive partial charges in step b) and / or step c) is in the range of pH 6 to pH 8, preferably in the range of pH 6 to pH 7.
[0060] In another embodiment, the polymerization according to step c) is carried out at a temperature ranging from 0 to 100° C., preferably from 10 to 60° C., more preferably from 20 to 50° C. Advantageously, the process according to the invention can be carried out at low temperatures, preferably under ambient conditions.
[0061] In other embodiments, the polymerization according to step c) is carried out in the range of 10 hours to 7 days.
[0062] In one embodiment, the method according to the present invention further comprises removing the surfactant after steps a) to c).
[0063] Preferably, the surfactant is removed by rinsing or ultrasonic cleaning, preferably using chloroform.
[0064] In another embodiment, the method according to the invention, preferably step c), further comprises doping the polymer film. Advantageously, the polymerisation and doping of the 2D or q2D polymer film occur simultaneously.
[0065] As used herein, the term "doping" refers to the introduction of impurities into a material to adjust the electrical properties. Preferably, the polymer film is doped with hydrogen chloride. Advantageously, the doped polymer film synthesized using the method according to the present invention is an electrical conductor.
[0066] In some embodiments, the method according to the invention is copolymerization. The term "copolymerization" refers to the polymerization of at least two monomers. Advantageously, the 2D polymer film is formed by copolymerization. In one embodiment, the polymerization according to step c), in particular the copolymerization, is a condensation reaction.
[0067] In the case of a specific copolymerization, the monomer comprises at least three functional groups, wherein the at least three functional groups of the monomer are the same or different. Preferably, the at least three functional groups are the same.
[0068] Preferably, the monomer comprises three to five functional groups, more preferably four functional groups.
[0069] In a preferred embodiment, the monomer is selected from alcohols, aldehydes, amines, anhydrides, anilines, boric acid, carboxylic acids, diamines, diols, β-diketones, hydrazines and / or hydroxyaldehydes.
[0070] Preferably, the monomer is a benzene derivative, a porphyrin derivative, a tetraphenylethylene derivative, a triphenylbenzene derivative or a triphenyltriazine derivative, most preferably 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin, tetraphenylethylene, triphenylbenzaldehyde or triphenyltriazine.
[0071] In a preferred embodiment, the initiation of the polymerization according to step b) is achieved by adding a further monomer having at least two functional groups.
[0072] In an embodiment, the another monomer comprises two to four functional groups, preferably two functional groups.
[0073] Preferably, the other monomer is a perylene derivative, a naphthalene derivative or a benzene derivative, most preferably isochromeno[4′,5′,6′:6,5,10]anthraquinone[2,1,9-def]isochromene-1,3,8,10-tetraone or 1H,3H-furo[3,4-f][2]benzofuran-1,3,5,7-tetraone.
[0074] In certain cases, the other monomer is selected from:
[0075]
[0076] In an embodiment, the ratio of the monomer to the other monomer is in the range of 1:1 to 1:5, preferably 1:1 to 1:2.
[0077] In one embodiment, the polymerization initiation according to step b) is achieved by a catalyst, preferably a steam catalyst; and / or a base. Advantageously, the steam catalyst does not significantly change the pH value. Preferably, the steam catalyst is trifluoromethanesulfonic acid (TfOH). Advantageously, the base increases the solubility of the monomers, in particular the solubility of monomers containing carboxyl or anhydride groups. Preferably, the base is selected from alkali metal hydroxides, in particular LiOH, NaOH and KOH.
[0078] In other cases, the monomer comprises at least two functional groups and the other monomer comprises at least three functional groups. In an alternative preferred embodiment, the monomer comprises two functional groups and the other monomer comprises four functional groups.
[0079] In another case of copolymerization, a monomer and a further monomer are provided in step a) and polymerization is initiated in step b) using a catalyst and / or a base.
[0080] In some embodiments, the monomer and the other monomer are selected from a boronic acid and a diol, an amine and an aldehyde, a hydrazine and an aldehyde, a carbohydrazide and an aldehyde, an amine and a beta-diketone, an amine and an anhydride, or an amine and a carboxylic acid.
[0081] In another embodiment of the method according to the invention, the polymerization is a homopolymerization. The term "homopolymerization" refers to the polymerization of one monomer. In other embodiments, the polymerization according to step c) is in particular a homopolymerization reaction selected from oxidation reactions, glasser reactions or Ullmann couplings.
[0082] In one embodiment, the monomer comprises one or two functional groups.
[0083] In other embodiments, the monomer is selected from alkynes, anilines, furans, halogenated hydrocarbons, pyrroles, selenophenes, and / or thiophenes.
[0084] In another embodiment, the initiation of polymerization according to step b) is achieved by adding at least one polymerization initiator, such as ammonium persulfate (APS) or ferric chloride, preferably APS.
[0085] Another object of the present invention is a two-dimensional (2D) or quasi-two-dimensional (q2D) polymer film composed of aromatic monomers, wherein the ratio of the crystal area to the total surface area is between 50% and 100%, wherein the average crystal domain size is between 0.1 μm 2 Up to 1cm 2 and wherein the film thickness is in the range of 0.1 nm to 80 nm.
[0086] Advantageously, the 2D or q2D polymer film is crystalline. Preferably, the ratio of crystalline area to total surface area is between 65% and 100%.
[0087] In some embodiments, the 2D or q2D polymer film is a polyamide, polyaniline, polyazine, polyborate, polyfuran, polyhydrazone, polyimide, polyimine, poly-β-ketoenamine, polypyrrole, polyselenophene, or polythiophene.
[0088] In an embodiment, the 2D or q2D polymer film according to the invention comprises one layer (monolayer) or several layers (multilayer). Advantageously, the layers are chemically and structurally identical.
[0089] According to the present invention, the thickness of the polymer film is in the range of 0.1 nm to 80 nm, preferably in the range of a monolayer to a few layers, in particular 1 nm to 40 nm, most preferably in the range of 1 nm to 10 nm. Advantageously, the film thickness of the polymer film synthesized by the method according to the present invention can be adjusted by the temperature and reaction time according to step c).
[0090] The thickness can be determined by atomic force microscopy (AFM) or transmission electron microscopy (TEM).
[0091] According to the present invention, the average crystal domain size of the polymer film is 0.1 μm 2 Up to 1cm 2 In the range of 0.1 μm 2 Up to 100 μm 2 More preferably, within the range of 1 μm 2 Up to 150μm 2 within the range.
[0092] The average domain size can be determined by phase contrast scanning electron microscopy and analyzed using ImageJ following the standard "Particle Analysis" protocol.
[0093] In an embodiment, the structure of the polymer membrane according to the invention is a square lattice or a double pore lattice structure. Advantageously, the structure of the polymer membrane according to the invention can be adjusted by the amount and geometry of the monomer functional groups.
[0094] In an embodiment, the 2D or q2D polymer film according to the present invention is a homopolymer or a copolymer.
[0095] As used herein, the term "2D" polymer film refers to a sheet-like monomolecular macromolecule composed of ordered monomers laterally connected by covalent bonds.
[0096] In an embodiment, the 2D polymer film according to the present invention is a polyamide, a polyazine, a polyborate, a polyhydrazone, a polyimide, a polyimine or a poly-β-ketoenamine.
[0097] As used herein, the term "q2D" polymer film refers to a regularly ordered supramolecular polymer in which the interactions of the polymer chains are carried out through weak intermolecular interactions. Advantageously, the weak intermolecular interactions between the polymer chains lead to excellent long-range order, particularly in a fully unfolded coil conformation of the polymer chains without chain folding.
[0098] In an embodiment, the q2D polymer film according to the present invention is polyaniline, polyfuran, polypyrrole, polyselenophene or polythiophene.
[0099] In one embodiment, the q2D polymer film according to the present invention, preferably the doped q2D polymer film according to the present invention, has a S cm -1 Up to 200S cm -1 , preferably 100S cm -1 Up to 160S cm -1 Transverse conductivity in the range.
[0100] Another aspect of the invention is the use of a 2D or q2D polymer film according to the invention and / or a method for synthesizing a 2D or q2D polymer according to the invention for producing a membrane, an electronic device or a catalyst.
[0101] As used herein, the term "membrane" refers to a device that acts as a selective barrier, meaning that it allows some molecules or particles to pass through, but prevents other molecules or particles from passing through, more preferably by size exclusion. Advantageously, the 2D or q2D polymer membrane according to the present invention is suitable as a membrane material due to the defined pore size.
[0102] As used herein, the term "electronic device" refers to a device that can affect electrons or their associated fields. Advantageously, the individual polymer chains of q2D polymer films provide multiple pathways for interchain charge transport and bypassing of possible defects.
[0103] In some embodiments, the electronic device is an electrode, preferably a transparent electrode for a display; a supercapacitor, preferably a flexible supercapacitor for a wearable electrical storage device; or a sensor, preferably for detecting ammonia or a volatile organic compound, such as acetic acid, heptaldehyde, heptane, heptanoic acid, 3-heptanone, hexanal, hexane, hexanoic acid, 2-hexanone, nonanal, nonane. Advantageously, the polymer film according to the present invention, preferably the q2D polymer film according to the present invention is a chemiresistor. As used herein, the term "chemiresistor" refers to a material that changes its resistance in response to changes in the chemical environment.
[0104] As used herein, the term "catalyst" refers to a material that increases the rate of a chemical reaction. In an embodiment, a 2D or q2D polymer according to the present invention catalyzes water splitting, decomposition of organic compounds in solution, or oxidation reactions.
[0105] In other embodiments, the previously described embodiments can be combined, in particular the features of the method according to the invention that can be applied to 2D polymer films and the use of 2D polymer films according to the invention and / or the method according to the invention. In addition, the features of the method according to the invention, in particular homopolymerization, can be applied to quasi-2D polymer films. By reading the specification and other parts of the present invention, those skilled in the art will easily understand various changes and modifications within the spirit and scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0106] The invention will now be further explained by means of the following non-limiting figures and examples.
[0107] Figure 1 shows A) a scheme of a method according to the invention: (i) and (ii) providing a surfactant (3) and a monomer (1), (i) wherein a surfactant (3) monolayer is aligned with the interface of a polar solvent and air, (ii) wherein the monomer (1) interacts with the surfactant (3) monolayer, (iii) initiating polymerization of the monomer (1), and (iv) polymerization and formation of a 2D or q2D polymer film. B) a scheme for polymerizing a monomer, in particular aniline, using electrostatic interactions with the surfactant (9Z)-sodium octadecyl-9-en-1-yl sulfate (SOS). C) a mechanism for oxidative polymerization of aniline to polyaniline.
[0108] Figure 2 A reaction scheme for the synthesis of 2D polymers according to the present invention is shown: the monomer 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin (1) is reacted with isochromeno[4',5',6':6,5,10]anthraquinone[2,1,9-def]isochromene-1,3,8,10-tetraone (2a) using a surfactant SOS (3a), or is reacted with 1H,3H-furano[3,4-f][2]benzofuran-1,3,5,7-tetraone (2b) using a surfactant SOS (7d) or stearic acid (SA) (overnight) (3b) to generate a polyimide (2DPI, 4a) or a polyamide (2DPA, 4b) through a condensation reaction.
[0109] Figure 3 shows the isotherms of surface pressure versus average molecular area (π-A) for A) sodium oleyl sulfate (SOS) and B) stearic acid (SA).
[0110] Figure 4 shows the spectroscopic characterization of 2D polymers and monomers: A) FTIR spectra of monomer 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin (1), another monomer isochromeno[4',5',6':6,5,10]anthraquinone[2,1,9-def]isochromene-1,3,8,10-tetraone (2a), another monomer 1H,3H-furano[3,4-f][2]benzofuran-1,3,5,7-tetraone (2b), 2DPI and 2DPA. B) UV-visible spectra of 2DPI, monomer 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin (1) and another monomer isochromeno[4',5',6':6,5,10]anthraquinone[2,1,9-def]isochromene-1,3,8,10-tetraone (2a) used for 2DPI synthesis. C) UV-visible spectra of 2DPA, monomer 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin (1) and another monomer 1H,3H-furo[3,4-f][2]benzofuran-1,3,5,7-tetraone (2b) used for the synthesis of 2DPA.
[0111] Figure 5 Structural characterization of 2DPI is shown: A) 2DPI film measured by bright field transmission electron microscopy (TEM). Dark areas are crystals. B) Selected area electron diffraction (SAED) pattern of the crystalline domains in (A). Arrows indicate 0.33 nm -1 100 and 010 reflections at (i.e. 3 nm). C) Aberration-corrected high-resolution transmission electron microscopy (AC-HRTEM) image of 2DPI (Inset: simulated image of 2DPI projected along
[001] , overlaid with structural model: dots represent carbon, oxygen, nitrogen and hydrogen atoms, respectively). D) SAED pattern of amorphous 2DPI film synthesized at air-water interface without surfactant.
[0112] Figure 6 Structural characterization of 2DPA is shown: A) 2DPA film measured by bright field TEM. The dark areas are crystals. B) SAED pattern of the crystal domains in (A). The reflections of 100 and 010 are at 0.65 nm, respectively. -1 and 0.52nm -1 C) AC-HRTEM image of 2DPA (inset: simulated image of 2DPA projected along
[001] , with the structural model overlaid: the dots represent carbon, oxygen, nitrogen and hydrogen atoms, respectively).
[0113] Figure 7 Structural characterization of v2DPA is shown: A) SAED pattern of v2DPA. The 120 and 001 reflections were measured at 1.29 nm. -1 and 1.05nm -1B) AC-HRTEM image of v2DPA showing 001 lattice fringes.
[0114] Figure 8 Matrix-assisted laser desorption ionization (MALDI)-time of flight (TOF)-mass spectrometry (MS) of a film containing a vertical precursor formed by SA and monomeric 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin (1) is shown. A) Chemical structure and molecular weight. B) MALDI TOF spectrum of a film formed by monomeric 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin (1) under a SA monolayer. Zoom in range from 880 m / z to 950 m / z.
[0115] Fig. 9 Optical microscopy images of PANI films prepared using different surfactants are shown: A) dihexadecyl phosphate, B) sodium oleyl sulfate, C) sodium dodecylbenzene sulfonate and D) no surfactant. All films were prepared in 48 hours reaction and 0.02M HCl.
[0116] Fig.10 Structural characterization of q2D PANI single crystals: A) SAED pattern. B) AC-HRTEM image of q2D PANI along the
[001] axis. The 200 and 020 reflections are at 2.96 nm, respectively. -1 and 2.70nm -1 (Inset: corresponding FFT).
[0117] Fig.11 Spectral and conductivity characterization of q2D PANIs are shown: A) Thickness of q2D PANIs versus reaction time. B) 430 nm absorbance and corresponding transmittance plot of q2D PANIs from A). C) UV-Vis-NIR absorption of q2D PANIs prepared at different HCl acid concentrations from 0.02 M to 1 M. D) Current (I)-voltage (V) characteristics of q2D PANIs from C) and compared with graphene CVD.
[0118] Fig.12 The sensing responses of q2D PANI as a chemiresistor for ammonia and volatile organic compounds (VOCs) are shown: A) Sensing responses (ΔR / R) of q2D PANI (1 M HCl) to different ammonia concentrations (30, 60, 90, and 120 ppb) 0 B) Sensing response ΔR / R of q2DPANI (0.02M HCl) chemiresistor to different heptaldehyde concentrations (10, 20, 30, 40 and 50 ppm) 0C) Bar graph of heptaldehyde sensor array based on q2D PANI and various dopants (thickness; bar): 0.02 M HCl (~5 nm; first); 0.02 M HCl (~9.3 nm; second); 0.005 M HCl (~9.3 nm; third); 0.02 M sulfuric acid (~9.3 nm; fourth); 0.02 M phytic acid (~9.3 nm; fifth); 0.02 M trifluoromethylsulfonic acid (~9.3 nm; sixth).
[0119] Fig.13 A reaction scheme for the synthesis of boronate-linked 2D polymer films using the method according to the present invention is shown.
[0120] Fig.14 Shown are (A) HR-TEM images of 2D borate polymer films. (B) Zoomed-in HR-TEM image from region A (squares) of image. Inset is the lattice averaged image calculated from DFT. (C) Experimental and D) simulated electron diffraction patterns, with circles representing (100) and (010) planes, respectively.
[0121] Figure 15 shows the morphology and diffraction data of the polythiophene film. (A) Transmission electron microscope image. (B) Selected area electron diffraction (SAED) pattern of the film, showing Diffraction features and hexagonal lattice. DETAILED DESCRIPTION
[0122] Surfactant monolayer formation
[0123] Add 20 μL of sodium oleyl sulfate (SOS) (1 mg ml in chloroform) -1 ) is distributed on the surface of 100 ml of Milli-Q water in a 200 ml beaker. The mean molecular area (mma) is It can be calculated by the following formula:
[0124]
[0125] Where Ae = 25.12 cm 2 , is the effective area; M w =M w,sos =370.5 g mol -1 , is the molecular weight of SOS; Na=6.02×10 23 mol -1 is Avogadro's constant; m = m sos =20μg, which is the mass of the surfactant. The mma allows SOS molecules to form a monolayer, such as Figure 3A This is confirmed by the π-A isotherm in the experiment.
[0126] Similar to SOS, 15 μl of stearic acid (SA, 1 mg ml in chloroform) was added. -1 ) is distributed at the interface between air and 100 ml Milli-Q water. mma is Allow SA molecules to form a monolayer, such as Figure 3B This is confirmed by the π-A isotherm in the experiment.
[0127] Horizontal synthesis of 2D polyimide (2DPI) on water surface
[0128] To synthesize 2DPI, a SOS monolayer was prepared on water (Figure 1a(i)), and then a monomer (5,10,15,20-tetrakis(4-aminophenyl)porphyrin, 1) (1.5×10 -7 mol)(Figure 1a(ii)). Electrostatic interactions and hydrogen bonding promoted the adsorption of the monomers under the surfactant monolayer and the subsequent pre-organization (Figure 1a(iii)). Next, another monomer (isochromeno[4′,5′,6′:6,5,10]anthraquinone[2,1,9-def]isochromene-1,3,8,10-tetraone, 2a) (3.0×10 -7 mol) was injected into the aqueous phase and then diffused into the pre-organized monomers, where 2D polymerization was triggered on the water surface. The polycondensation reaction was left at 20 °C for 7 days under ambient conditions to obtain several layers of 2DPI crystals ( Figure 2 Fourier transform infrared spectroscopy (FTIR) confirmed the formation of imide bonds in 2DPI, and the C=O characteristic peak (1695 cm -1 ), eliminating the NH stretching of the monomer (V 伯 Amino, 3350cm -1 ) and the C=O vibration of another monomer (V 羧酸二酐 , 1755cm -1 )( Figure 3A The UV-visible absorption spectrum of 2DPI shows a characteristic Soret (S) band at 437 nm and a Q band at 748 nm, which corresponds to the porphyrin structure in 2DPI ( Figure 3B ).
[0129] Structural characterization
[0130] For structural characterization, the polymer films were horizontally transferred onto 300 nm SiO2 / Si substrates for optical microscopy and atomic force microscopy (AFM), onto quartz glass for UV-visible absorption spectroscopy, onto copper foil for infrared spectroscopy (IR), and onto holey copper grids for TEM characterization.
[0131] Mass spectrometry was performed on a Bruker Autoflex Speed MALDI TOF MS (BrukerDaltonics, Bremen, Germany) using dihydroxyanthraquinone as matrix. Optical images were acquired using a Zeiss AxioScope A1 in differential interference mode. AFM was performed in air using a custom-made Ntegra Aura / Spectra, SMENA head from NT-MDT (Moscow, Russia) operating in contact mode. AC-HRTEM imaging and SAED were performed on the image side of a Cs-corrected FEITitan 80-300 microscope operating at 300 kV. To reduce electron irradiation damage on the polymer film, the total electron dose used to acquire the SAED patterns and HRTEM images was limited to 400 kV, respectively. (Dose rate: )and (Dose rate: UV-visible absorption spectra were obtained at room temperature on a UV-visible-near infrared spectrophotometer Cary 5000. Fourier transform infrared spectroscopy (FTIR) was performed on a TensorII (Bruker) equipped with an attenuated total reflectance (ATR) unit.
[0132] After removing the surfactant with chloroform, the film remained stable and uniform. 2 AFM measurements on a 100nm / Si wafer showed a film thickness of ~2nm, corresponding to ~5 layers. When transferred onto a holey copper grid, the film was freely suspended on a hexagonal grid with a side length of ~25μm.
[0133] Bright field TEM shows polymer crystals (dark) bridged by amorphous regions (bright) in the film. Figure 4A ). The area ratio between the crystalline and amorphous regions was ~2.2, indicating that 69% of the tested area was crystalline. In addition, the 2DPI film was deposited on a silicon substrate and chemically exfoliated by ultrasound in dichloromethane. After exfoliation, the 2DPI film showed a step-like structure at the edges of the crystalline domains. AFM measurements showed that the step heights in different regions were 0.4±0.10nm and 0.7±0.1nm, which can correspond to the thickness of a monolayer and a bilayer, respectively.
[0134] Selected area electron diffraction on free-standing 2DPI films revealed a The square unit is consistent with the 2DPI sliding AA stack atomic model obtained by density functional tight binding (DFTB) calculations ( Figure 4C ).
[0135] Visualization of the molecular structure of 2DPI by AC-HRTEM ( Figure 4C ), showing a square lattice with a spacing of 30.0 Å. Based on the AC-HRTEM image simulation (inset, Figure 4C ), the darkest part corresponds to the pores between the porphyrin units. To determine the crystallinity of 2DPI, selected area electron diffraction (SAED) was performed at different locations on a 3mm x 3mm grid. All diffraction patterns in each selected grain are identical, indicating that each domain is a single crystal. The average domain size is ~3.5μm 2 , corresponding to a molecular weight (MW) of 5.4×10 8 g mol -1 The structure of the 2D polymer is defined.
[0136] AC-HRTEM images were used to characterize the edge structure of 2DPI domains. Figure 2 A shows two crystalline domains bridged by an amorphous segment. By comparing the AC-HRTEM image and its fast Fourier transform (FFT) pattern, it is found that the domain edges are parallel to the (100) and (010) planes of 2DPI.
[0137] Horizontal synthesis of 2DPI on a water surface without surfactant (reference example)
[0138] As described above, the synthesis of 2DPI was performed without the use of surfactants. Only amorphous films were obtained ( FIG. 4D ).
[0139] Synthesis of 2DPI horizontally on the water surface using other surfactants
[0140] As mentioned above, 2DPI was synthesized using the surfactant sodium dodecylbenzene sulfonate (SDBS). SDBS functions similarly to SOS in that it can guide the self-assembly of monomers (1) through electrostatic interactions to form 2DPI crystals.
[0141] Horizontal synthesis of 2D polyamide (2DPA) on water surface
[0142] 2DPA crystals were synthesized by polymerization of a monomer (5,10,15,20-(tetrakis(4-aminophenyl))porphyrin, 1) and another monomer (1H,3H-furo[3,4-f][2]benzofuran-1,3,5,7-tetraone, 2b) at the SOS-water interface under the same synthetic conditions as those for the synthesis of 2DPI.
[0143] A double-pore structure ( Figure 2 ) and crystalline 2D polymers with a thickness of ~10 nm. FTIR results confirmed the formation of polyamides, with the C=O stretch of the amide at 1660 cm -1 , NH stretching is 1335cm -1 ( Figure 3A). The UV-visible absorption spectrum of 2DPA also showed the characteristic Soret (S) and Q bands of the porphyrin unit at 485 nm and 847 nm, respectively (Figure 3C). The average crystalline domain of 2DPA was 0.1 μm-0.2 μm wide and up to 2 μm long. The area ratio between the crystalline and amorphous regions was ∼1.9, indicating that 66% of the polyamide film was crystalline.
[0144] The edge of the crystal region of 2DPA shows a layer-by-layer stacking morphology. The SAED pattern shows that 0.52nm -1 and 0.65nm -1 The first-order reflection at Figure 5 B), corresponding to the lattice constants and This is consistent with the DFTB calculation results. AC-HRTEM further confirmed the crystal structure, where the darkest part represents the larger pores of 2DPA ( Figure 5 C). Similar to 2DPI, the monomers in 2DPA crystals have a face-011 orientation and extend horizontally on the water surface. The crystallites are elongated along the
[100] direction. The higher growth rate along the
[100] axis is attributed to 2DPA and precursor-H There is a slight mismatch between the lattice parameters, which favors the growth of the crystal in the
[010] direction.
[0145] Vertical synthesis of 2DPA in water
[0146] For the vertical synthesis of 2DPA in water, the synthesis was carried out under the same synthetic conditions as for the horizontal synthesis of 2DPA. However, stearic acid (SA) was used as a surfactant, whose carboxyl group could react with one of the amine groups of the monomer 5,10,15,20-(tetrakis(4-aminophenyl))porphyrin (1) to form a covalent amide bond at the air-water interface, which was experimentally verified by MALDI-TOF-MS ( Figure 7 ).
[0147] Figure 7 The target molecule at 940 m / z is shown, which corresponds to a monomer (chemical formula: C 62 H 68 N 8 O). The peaks at 925 m / z, 912 m / z, and 898 m / z correspond to the loss of one, two, and three -NH 2 Amide molecule fragment after the group.
[0148] Therefore, the monomers can be anchored vertically under the SA monolayer as precursors (i.e., precursor-V). Compared with precursor-H, grazing-incidence wide-angle X-ray scattering (GIWAXS) measurements of precursor-V showed dense π-π stacking peaks along the in-plane direction (data not shown), indicating edge-to-edge alignment of the monomers, allowing 2D polymerization along the vertical direction.
[0149] As expected, the GIWAXS pattern confirmed that the growth direction of the 2DPA layer has been adjusted from horizontal to vertical (v2DPA). SAED pattern ( Figure 6 A) has 001 reflection, AC-HRTEM image ( Figure 6 B) The presence of 001 lattice fringes further confirms the edge conformation of the 2DPA layer. AFM shows that v2DPA has a lamellar morphology with a layer step height of ~1.8nm. The crystallinity of v2DPA is significantly higher than that of 2DPA. On a 3mm x 3mm grid, no amorphous fragments can be identified within v2DPA, and the domain size of v2DPA is as high as ~121μm 2 , and there is no significant change in the crystallographic orientation within the plane.
[0150] Synthesis of Quasi-Two-Dimensional (q2D) Polyaniline (PANI)
[0151] The q2D PANI membrane was synthesized by oxidative polymerization of aniline monomer at the air-water interface with the assistance of a surfactant monolayer. Figure 1A To prepare the surfactant monolayer, 10 μl of the surfactant was dissolved in chloroform (1 mg ml -1 ) and an oil-based sodium sulfate solution filtered through a PFTE syringe filter (0.2 μm, 1-15 ml, ThermoFisher) was distributed on the water surface (50 ml) in a glass well with a diameter of 6 cm, where the chloroform was allowed to evaporate for 30 minutes. Subsequently, aniline monomer (1.5 μM in 1 ml of water) was added to the aqueous subphase using a pipette. The glass well was then covered with a Petri dish and kept for ~24 hours to allow the aniline monomer to diffuse and adsorb under the surfactant monolayer. Subsequently, 1 mL of 1 M hydrochloric acid and ammonium persulfate (APS, 10 mg / 1 mL in water) were added to the subphase in sequence to trigger the oxidative polymerization of aniline at 1°C ( Figure 1B and C). After a few hours, the solution eventually turned dark green, indicating that the aniline monomers were successfully polymerized into PANI. q2D PANI then appeared on the water surface.
[0152] Low concentrations of monomers and catalysts (APS) slowed down the polymerization reaction and favored the formation of ultrathin PANI films with high crystallinity. After 48 h of polymerization, a uniform and continuous q2D PANI film was obtained on the water surface.
[0153] Prior to characterization, the q2D PANI film on the substrate was rinsed with chloroform (20 ml) and ethanol (20 ml) for about 1 hour, respectively.
[0154] Synthesis of q2D with other surfactants PANI
[0155] Various surfactants were investigated in the q2D PANI synthesis. All membranes were prepared in 48 h reaction and 0.02 M HCl. The anionic surfactant dihexadecyl phosphate ( Figure 8 A) Sodium oleyl sulfate ( Figure 8 B) and sodium dodecylbenzenesulfonate ( Figure 8 C) produces large-area continuous and uniform PANI films. In addition, q2D PANI films with good morphological uniformity, free of cracks and pinholes were obtained using surfactants headed by sulfate ions (sodium oleyl sulfate and sodium dodecylbenzene sulfonate). This can be attributed to the highest negative charge density of sulfate groups, which facilitates electrostatic interaction with aniline monomers.
[0156] Synthesis of surfactant-free q2D PANI (reference example)
[0157] As described above, the synthesis of q2D PANI was performed without the use of surfactant. Only fibrous PANI ( Figure 8 D).
[0158] Structural characterization of q2D PANI films
[0159] To transfer the q2D PANI film, a solid substrate was placed under the floating film and the aqueous subphase was gently removed until the film fell onto the substrate surface. The ~8 cm diameter Q2D PANI film was transferred to a 300 nm thick SiO 2 / Si wafer (diameter ). Under an optical microscope, q2D PANI was uniform and the edge of the film was clearly visible. q2D PANI could span large holes with an edge of ~20 μm on a copper TEM grid, indicating its high mechanical stability. AFM measurements at the edge of the film by random sampling showed an average thickness of ~9.3 nm after 48 h of polymerization. The thickness at different locations was almost the same, and the selected area (5×5 μm 2 ) has a root mean square (RMS) roughness of 0.3 nm, indicating that the q2D PANI film has good morphological uniformity.
[0160] The single crystal domain size statistics obtained by SAED are 1.1μm-1.5μm (i.e. 1.2-2.3μm 2 ), the maximum domain size exceeds 2.3 μm (i.e. ~5.2 μm 2 ).like Fig. 9As shown, the linear polymer chains are arranged parallel to each other and stacked into quasi-2D molecular sheets. Unlike polymers obtained by solution synthesis, the PANI chains in the molecular sheets show excellent long-range order without chain folding or any entanglement. Since the average single crystal size of q2D PANI is 1.1μm-1.5μm, we estimate that the length of the PANI chains in each crystal reaches the same scale, corresponding to ∼10 6 monomer units and ~10 8 g mol -1 Molecular weight.
[0161] Thickness control and spectral characterization of q2D PANI films
[0162] The formation of q2D PANI is confined to the surfactant-water interface, where monomers in the aqueous subphase are continuously transported to the interface for oxidative polymerization. Therefore, extending the reaction time increases the monomer conversion rate and correspondingly increases the film thickness. Fig.10 As shown in A, the thickness of q2DPANI increases at a constant rate of 5 nm per day (in 0.02 M HCl) during the first five days and then stabilizes at around 30 nm after seven days when all monomers are consumed.
[0163] The film crystallinity significantly increases with the increase of thickness, while the crystal structure remains unchanged. The thickness of the thinnest q2D PANI film is 2.6 ± 0.4 nm (after 12 h of reaction), corresponding to two molecular layers (one layer is ∼1.3 nm according to SAED and GIWAXS results).
[0164] According to UV-Vis-NIR spectroscopy, q2D PANI exhibited a characteristic absorbance (polaron-π*) at 430 nm, which was linearly correlated with the reaction time within the first five days ( Fig.10 B), and follows the Beer-Lambert law. The transmittance of q2D PANI decreases with the reaction time ( Fig.10 B). Nevertheless, after 7 days of reaction (~30 nm thick), a transmittance of ~90% can still be observed on q2D PANI, which can be attributed to the good chain ordering that reduces light scattering.
[0165] To increase the doping level of q2D PANI, the acid concentration (hydrochloric acid) was increased to 1 M ( Fig.10 C). Using 1 M HCl, a longer induction period (about 12 h) was observed, with the polymerization rate decreasing to 4.2 nm per day. By increasing the HCl concentration of the aqueous subphase from 0.02 M to 1 M, we could identify a monotonic increase in absorbance at 360 nm (π-π* transition of the benzene ring) and above 600 nm (free carrier absorption) ( Fig.10C), which is a characteristic of PANI (emeraldine) doping form and is conducive to achieving high conductivity.
[0166] Measurement of electrical conductivity of q2D PANI membrane
[0167] The electrical conductivity of the q2D PANI film was measured using a dual-probe (lateral conductivity) and current-sensing AFM (vertical conductivity). The corresponding IV curves along the two directions showed that there was an ohmic contact between -0.5 V and +0.5 V, indicating that the lateral conductivity in the 9.3 nm thick q2D PANI film doped with 0.02 M HCl was 8.7 × 10 -3 S cm -1 , the vertical conductivity is 5.0×10 - 5 Scm -1 The superior lateral conductivity is attributed to the long-range ordering and extended coil conformation of the PANI chains along the in-plane direction, which enhances the hopping transport between adjacent PANI chains.
[0168] When the doping acid concentration of the subphase increases from 0.02 M to 1 M, the corresponding lateral conductivity of q2D PANI increases to 23 S cm -1 ( Fig.10 D). The IV current of q2D PANI doped with 1 M HCl (0.69 mA at 50 mV) is even better than that of commercial graphene synthesized by chemical vapor deposition (0.61 mA at 50 mV). By additional doping with HCl vapor, the conductivity of q2D PANI increases to 160 S cm -1 The electrical conductivity of q2D PANI greatly exceeds that of low-crystallinity PANI films.
[0169] Chemical sensing using q2D PANI films
[0170] Due to the ultrathinness of q2D PANI and the wide tunability of its conductivity (e.g., upon exposure to acids, bases, and polar compounds), q2D PANI is a promising electrode material for chemical sensing. 3 The sensor was fabricated by transferring 9.3 nm thick q2D PANI onto a SiO2 coated with an Au electrode. 2 Made on a substrate. Fig.11 A shows continuous exposure to NH at concentrations ranging from 15 ppb to 120 ppb at room temperature. 3 The normalized sensing response ΔR / R0 at NH 3 After exposure, the current decreases (resistance increases), which is due to the NH 3Deprotonation of q2D PANI. The lowest detection limit (defined as the concentration that provides a signal-to-noise ratio of at least 3) was 30 ppb, which is lower than most reported PANI sensors. This sensitivity is even higher than that of nitrogen- and boron-doped carbon nanotubes (100 ppb) under the same test conditions (Wang et al., 2012) and is relevant to the diagnosis of certain diseases, such as liver cirrhosis, renal failure, and diseases caused by Helicobacter pylori. 3 The high performance in sensing can be attributed to its ultrathinness, fully exposed active sites, and NH 3 molecular Diffusion provides an efficient pathway for long-range ordered chain structures.
[0171] Next, the q2D PANI membrane was evaluated for use in clinically relevant chemiresistor applications by exposure to volatile organic compounds (VOCs). Heptanal, a representative VOC, has been detected in blood, breath, and urine samples and can therefore be used as a biomarker for disease diagnosis and health monitoring. Fig.11 B shows the sensing properties of a 5 nm thick q2DPANI-based chemiresistor that exhibits extremely fast response upon exposure to heptanal vapor and excellent reversibility upon flushing with dry nitrogen. The resistance of the chemiresistor increases with increasing heptanal concentration (from 10 to 50 ppm), which is likely caused by the swelling of q2D PANI due to heptanal adsorption. The weak binding between VOC and q2DPANI ensures a reversible (peak-like) resistance response in sensing. Furthermore, the sensitivity can be tuned by various doping acids as well as film thickness ( Fig.11 C). Overall, the ~2% ΔR / R0 (at 10 ppm) of q2DPANI exceeds that of existing PANI-based devices (~1.7% at 25 ppm) (Deng et al., 2018), which is sufficient to detect VOCs released from patients (~205.5 ppm) and healthy controls (~22.8 ppm).
[0172] Table 1. Synthesis of 2D and q2D polymer films according to the present invention in water by synthesizing 2DPI, 2DPA or v2DPA using surfactants (9Z)-octadecyl-9-en-1-yl sulfate (SOS), sodium 4-dodecylbenzenesulfonate (SDBS), dihexadecyl triethanolamine phosphate (DHP), oleic acid (OA), cetyltrimethylammonium bromide (CTAB) or octadecanoic acid (SA).
[0173]
[0174]
[0175] Table 2. Synthesis of 2D and q2D polymer films according to the present invention in water by homopolymerization of q2D PANI using the surfactant dihexadecyl triethanolamine phosphate (DHP).
[0176]
[0177] Horizontal synthesis of 2D boronates on water
[0178] Fig.13 The interfacial synthesis process of 2D borate esters according to the present invention is shown. Specifically, a chloroform solution of SOS surfactant is dropped onto a water surface, and RSO facing the water phase after chloroform evaporation is formed. 4 - The polar head groups form a SOS monolayer. Subsequently, 1 ml of an acidic aqueous solution containing 5,10,15,20-(tetrakis-4-dihydroxyborylphenyl)porphyrin (TDBP) (1 μmol) and HCl (1 mmol) was injected into 40 ml of the aqueous phase. Due to the protonated porphyrin of TDBP and the head group RSO of SOS 4 - Due to the electrostatic interaction between the two, TDBP was easily adsorbed underneath the SOS monolayer. Next, 1 ml of an acidic aqueous solution containing 1,2,4,5-tetrahydroxybenzene (TTHB) (4 μmol) and HCl (1 mmol) was added to the aqueous phase and then diffused to the pre-adsorbed TDBP. The mixed solution (pH 1.3) was treated at 50 °C to trigger the polycondensation reaction at the interface. After 7 days, a free-standing COF film with glossy reflection was observed on the water surface. The synthesized 2D borate polymer film was robust enough on water and could be fully transferred to different substrates for morphological and structural characterization, such as on Si / SiO 2 substrate and TEM grid.
[0179] The molecular structure of 2D borate polymer films, especially the single-crystalline domains, was investigated by HR-TEM ( Fig.14 A) Visualization showing the long-range ordered square lattice ( Fig.14 A and B). Based on HR-TEM image simulation, the darkest parts correspond to the pores between the porphyrin units, while the bright areas show the square arrangement of the 2D boronate polymer backbone. Selected area electron diffraction (SAED) pattern ( Fig.14 C) shows a square diffraction pattern with the nearest reflection corresponding to 0.406 nm -1 (i.e., a = b = 2.46 nm, γ = 90°), which is consistent with the density functional theory (DFT) calculated atomic model of the AA-eclipsed stack of 2D borate polymer films (calculated reflections at (100) and (010): 0.402 nm -1 Fig.14D). The results show that the 2D polymer film has a high degree of crystallinity.
[0180] Horizontal synthesis of 2D polythiophene on water surface
[0181] As shown in Figure 15, as a first step, a CTAB monolayer was constructed on the water surface in a 200 ml beaker (containing 150 ml water); then a thiophene suspension (in 0.5 ml MiliQ water) containing 0.05 ml thiophene and 0.5 mg SDS surfactant was injected into the aqueous subphase. The SDS surfactant helped thiophene to form a stable suspension. Subsequently, the polymerization was triggered by adding 10 mg ammonium persulfate (APS) and 0.5 ml HCl (37%). After 12 h of reaction, a gray film floated on the water surface. The film was transferred to different substrates for various characterizations.
[0182] like Fig.15A As shown, the film is a large-area sheet, which can be characterized by selected area electron diffraction (SAED), showing The crystallinity was further analyzed by grazing-incidence wide-angle X-ray scattering (GIWAXS).
[0183] Cited Non-Patent Literature
[0184] Bieri,M.,Treier,M.,Cai,J.,Ait-Mansour,K.,Ruffieux,P., O., P., Kastler, M., Rieger, M., Feng, X., Müllen, K., Fasel, R. (2009) Porous graphenes: two-dimensional polymer synthesis with atomic precision. Chem. Commun. 45, 6919-6921.
[0185] Blumstein, A., Herz, J., Sinn, V., Sadron, C. (1958) Sur un procede depolymerisation en couche adsorbee. Comptes Rendus Acad. Sci. 246,1856-1858.
[0186] Bunck, DN, Dichtel, WR (2013) Bulk synthesis of exfoliated two-dimensional polymers using hydrazine-linked covalent organic frameworks. J Am. Chem. Soc. 135, 14952-14955.
[0187] Cardenas, L., Gutzler, R., Lipton-Duffin, J., Fu, C., Brusso, JL, Dinca, L. E., Vondracek, M., Fagot-Revurat, Y., Malterre D., Rosei, F., Perepichka, D. F. (2013) Synthesis and electronic structure of a twodimensional-conjugated polythiophene. Chem. Sci. 4, 3263-3268.
[0188] Chen, L., Hernandez, Y., Feng, X., Mullen, K. (2012) From nanographene and graphene nanoribbons to graphene sheets: chemical synthesis. Angew. Chem. Int. Ed. 51, 7640-7654.
[0189] Deng, YF, Sun, JX, Jin, H., Khatib, M., Li, XH, Wei, ZS, Wang, F., Horev, YD, Wu, W., Haick, H. (2018) Chemically modified polyaniline for the detection of volatile biomarkers of minimal sensitivity to humidity and bending. Adv. Healthc. Mater. 7(15), 1800232.
[0190] Duan H, Lyu P, Liu J, Zhao Y, Xu Y (2019) Semiconducting Crystalline Two-Dimensional Polyimide Nanosheets with Superior Sodium Storage Properties. ACS Nano 132473-2480.
[0191] Gee, G. (1935) Reactions in monolayers of drying oils. Ii. Polymerization of the oxidized forms of the maleic anhydride compound of beta elaeostearin. Proc. Royal Soc. A. 153, 129-141.
[0192] Grill, L., Dyer, M., Lafferentz, L., Persson, M., Peters, MV, Hecht, S. (2007) Nano-architectures by covalent assembly of molecular building blocks. Nat. Nanotechnol. 2, 687-691.
[0193] Kaganer, VM, Mohwald, H., Dutta, P. (1999) Structure and phase transitions in Langmuir monolayers. Rev. Mod. Phys. 71, 779-819.
[0194] Kissel,P.,Erni,R.,Schweizer,WB,Rossell,MD,King,BT,Bauer,T., S., Schlüter, AD, Sakamoto, J. (2012) A two-dimensional polymer prepared by organic synthesis. Nat. Chem. 4, 287-291.
[0195] Novoselov, KS, Geim, AK, Morozov, SV, Jiang, D., Zhang, Y., Dubonos, SV, Grigorieva, IV, Firsov, AA (2004) Electric field effect in atomically thin carbon films. Science 306, 666-669.
[0196] Sahabudeen, H., Qi, H., Glatz, B. A., Tranca, D., Dong, R., Hou, Y., Zhang, T., Kuttner, C., Lehnert, T., Seifert, G., Kaiser, U., Fery, A., Zheng, Z., Feng, X. (2016) Wafer-sized multifunctional polyimine-based two-dimensional conjugated polymers with high mechanical stiffness. Nat. Commun. 7, 13461.
[0197] Sahabudeen H, Dong R, Feng X (2019) Interfacial Synthesis of Structurally Defined Organic Two-dimensional Materials: Progress and Perspectives, Chinese Journal of International Chemistry, 73(6): 480-486.
[0198] Staudinger, H. (1920) Polymerisation.Ber.Dtsch.Chem.Ges.53,1073-1085.
[0199] Stupp, S., Son, S., Lin, H., Li, L. (1993) Synthesis of two-dimensional polymers. Science 259, 59-63.
[0200] Wang, Y., Liu, JL, Tran, HD, Mecklenburg, M., Guan, XN, Stieg, AZ, Regan, BC, Martin, DC, Kraner, RB (2012) Morphological and dimensional control via hierarchical assembly of doped oligoaniline single crystals. J. Am. Chem. Soc. 134(22), 9251-9262.
[0201] Xiao X, Wang Z, Hu Z, He T (2010) Single Crystals of Polythiophene with Different Molecular Con-formations Obtained by Tetrahydrofuran Vapor Annealing and Controlling Solvent Evaporation. Journal of Physical Chemistry Part B 114(22), 7452-7460.
[0202] Xu X, Zhang Z, Dong J, Yi D, Niu J, Wu M, Lin L, Yin R, Li M, Zhou J, Wang S, Sun J, Duan X, Gao P, Jiang Y, Wu X, Peng H, Ruoff RS, Liu Z, Yu D, Wang E, Ding F, Liu K (2017) Ultrafast epitaxial growth of metre-sized single-crystal graphene on industrial Cu foil. Science Bulletin 62(15), 1074-1080.
[0203] Yang QH,Tu ZY,Zhao NY(2016)Research on interfacial polymerization of pyrrole assist with Span80 system.IOP Conference Series:Materials Science and Engineering 137,012070.
[0204] Reference numerals
[0205] 1 Monomer
[0206] 2 Another monomer
[0207] 3 Surfactants
[0208] 4 Polymer
Claims
1. A method for synthesizing a two-dimensional (2D) or quasi-two-dimensional (q2D) polymer film, the method comprising the following steps: a) providing a surfactant monolayer and at least one monomer in a polar solvent, wherein the monomer is an aromatic monomer, wherein the at least one monomer is selected from alcohols, aldehydes, alkynes, amines, anhydrides, boric acid, carboxylic acids, β-diketones, furans, halogenated hydrocarbons, hydrazines, pyrroles, selenophenes and / or thiophenes, The polar solvent is water and / or a water-miscible solvent. wherein the surfactant monolayer is aligned with the interface of the polar solvent and air, wherein the hydrophilic groups of the surfactant are oriented toward the polar solvent and the hydrophobic groups of the surfactant are oriented toward the interface or out of the polar solvent, wherein the monomer interacts with the surfactant monolayer, The hydrophilic group of the surfactant interacts with at least one functional group of the monomer through electrostatic interaction or covalent bond interaction. b) initiating polymerization of said monomers, and c) Polymerization and formation of two-dimensional (2D) or quasi-two-dimensional (q2D) polymer films.
2. The method according to claim 1, wherein the surfactant is selected from the group consisting of bis(hexadecyl) phosphate, hexadecyltrimethylammonium bromide, wood wax alcohol, oleic acid, perfluorooctadecanoic acid, sodium dodecylbenzenesulfonate, (9Z)-octadecyl-9-en-1-yl sodium sulfate, sodium stearate, stearic acid, and bis(hexadecyl) triethanolamine phosphate.
3. The method of claim 1, wherein the at least one monomer comprises an aromatic group selected from the group consisting of benzene, furan, naphthalene, perylene, porphyrin, pyrrole, thiophene, tetraphenylethylene, tetraphenylporphyrin, triphenylbenzene, and triphenyltriazine.
4. The method according to claim 1 or 2, wherein the water-miscible solvent is selected from alcohol, dimethylformamide or acetonitrile.
5. The method according to claim 4, wherein the alcohol is selected from methanol or ethanol.
6. The method of claim 1 or 2, wherein the at least one monomer comprises at least three functional groups, wherein the at least three functional groups of the monomer are the same or different.
7. The method according to claim 1 or 2, wherein for the horizontal growth direction, an anionic surfactant is provided for the first monomer having a cationic group or a positive partial charge, and a cationic surfactant is provided for the first monomer having an anionic group or a negative partial charge.
8. The method according to claim 6, wherein the initiation of the polymerization in step b) is achieved by adding another monomer having at least two functional groups.
9. The method of claim 8, wherein the at least one monomer and the another monomer are selected from the group consisting of: a boronic acid and a diol, an amine and an aldehyde, a hydrazine and an aldehyde, a carbohydrazide and an aldehyde, an amine and a β-diketone, an amine and an anhydride, or an amine and a carboxylic acid.
10. The method according to claim 1 or 2, wherein the at least one monomer comprises one or two functional groups and the initiation of the polymerization of step b) is achieved by adding at least one polymerization initiator.
11. A two-dimensional 2D or quasi-two-dimensional q2D polymer film composed of aromatic monomers prepared by the method according to any one of claims 1 to 10, wherein the ratio of the crystal area to the total surface area is 50% to 100%, wherein the crystallinity is determined by X-ray diffraction or transmission electron microscopy, The average crystal domain size is 0.1 μm 2 Up to 1cm 2 The average domain size was determined by phase contrast scanning electron microscopy and analyzed using ImageJ following the standard “Particle Analysis” protocol. The film thickness is in the range of 0.1 nm to 80 nm, wherein the thickness is determined by atomic force microscopy or transmission electron microscopy.
12. The two-dimensional 2D or quasi-two-dimensional q2D polymer film according to claim 11, which is composed of polyamide, polyaniline, polyazine, polyborate, polyfuran, polyhydrazone, polyimide, polyimine, poly-β-ketoenamine, polypyrrole, polyselenophene or polythiophene.
13. The two-dimensional (2D) or quasi-two-dimensional (q2D) polymer film according to claim 11 or 12, wherein the film thickness is in the range of 1 nm to 10 nm.
14. The two-dimensional 2D or quasi-two-dimensional q2D polymer film according to claim 11 or 12, wherein the average crystal domain size is within 0.1 μm. 2 Up to 100 μm 2 within the range.
15. Use of the two-dimensional 2D or quasi-two-dimensional q2D polymer film according to any one of claims 11 to 14 and / or the method for synthesizing a two-dimensional 2D or quasi-two-dimensional q2D polymer film according to any one of claims 1 to 10 for producing membranes, electronic devices or catalysts.
Citation Information
Patent Citations
Large-area ultrathin high-crystalline-state two-dimensional conjugated polymer film as well as preparation method and application thereof
CN109988325A
Method of preparing polyaniline films and highly self-oriented films obtained
US20110281098A1
Interfacially synthesized reverse osmosis membrane containing an amine salt and processes for preparing the same
US4872984A
Two-dimensional colloid crystal thin film and preparation method thereof
CN102617874A
Self-supporting two-dimensional single-layered supramolecular polymer and application of two-dimensional single-layered supramolecular polymer in nano separation membrane
CN104804198A