Cross-linked polyolefin separator, method for manufacturing the cross-linked polyolefin separator, and electrochemical device including the cross-linked polyolefin separator
By crosslinking polyolefin separators, the problem of insufficient elasticity and strength of lithium secondary battery separators at high temperatures is solved. Water-based or UV cross-linking technology is used to form high molecular weight polyolefin and Si-O-Si bond structure to ensure lithium Safety and insulation functions of secondary batteries.
Patent Information
- Application Number
- CN202080077462.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-08
- Filing Date
- 2020-11-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-06
AI Technical Summary
The existing lithium secondary battery separators are difficult to maintain elasticity and strength at high temperatures, resulting in safety problems. Especially in nickel-rich positive electrode active materials, there is a risk of increasing viscosity and loss of insulating function.
The crosslinked polyolefin separator is formed by aqueous cross-linking or UV cross-linking to increase the molecular weight and silicon content of the polyolefin to form Si-O-Si bonds and fibrillary entanglement structures, ensuring that it is in the range of 180°C to 220°C. The ratio of energy storage modulus to loss modulus is 2 or more to ensure mechanical and thermal safety of the partition.
The low viscosity and high elasticity of the separator at high temperature are achieved, the safety and insulation function of the electrochemical device are ensured, and the safety of lithium secondary batteries is improved, especially under conditions rich in nickel positive electrode active materials.
Smart Images

Figure CN114651366B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a cross-linked polyolefin separator, a method of manufacturing the cross-linked polyolefin separator, and an electrochemical device including the cross-linked polyolefin separator.
[0002] This application claims the priority of Korean Patent Application No. 10-2019-0142908 filed in Korea on November 8, 2019, the disclosure of which is incorporated herein by reference. Background Art
[0003] Energy storage technology has received increasing attention recently. As the application of energy storage technology has expanded to energy sources for mobile phones, cameras and laptops, and even electric vehicles, research and development work on electrochemical devices has been increasingly put into practice. In this context, electrochemical devices have received the most attention. Among these electrochemical devices, the development of rechargeable secondary batteries has become the focus. Recently, research and design of a new type of electrode and battery to improve the capacity density and specific energy of such batteries has been actively studied.
[0004] Among commercially available secondary batteries, lithium secondary batteries developed in the early 1990s have attracted much attention because they have a higher operating voltage and significantly higher energy density than conventional batteries such as nickel-hydrogen, nickel-cadmium, and lead sulfate batteries using liquid electrolytes.
[0005] Such a lithium secondary battery includes a positive electrode, a negative electrode, an electrolyte and a separator. Specifically, the separator needs to have an insulating property to separate and electrically insulate the positive electrode and the negative electrode from each other and a high ion conductivity to increase lithium ion permeability based on high porosity.
[0006] The separator has viscoelasticity, and therefore there is a problem that it is difficult to ensure safety due to an increase in viscosity when exposed to high temperatures.
[0007] In particular, when the positive electrode active material included in the positive electrode is a positive electrode active material rich in nickel, the above-mentioned problem becomes serious. Summary of the invention
[0008] Technical issues
[0009] The present disclosure is intended to solve the problems of the prior art, and thus the present disclosure is intended to provide a separator that can maintain elasticity even at high temperatures and an electrochemical device including the separator.
[0010] Specifically, the present disclosure aims to provide a separator and an electrochemical device including the same, the separator maintaining elasticity in a temperature range of 180° C. to 220° C. and maintaining its function of separating a positive electrode and a negative electrode from each other in a lithium secondary battery, thereby ensuring safety.
[0011] The present disclosure also aims to provide a separator which maintains strength at high temperatures to ensure resistance to external forces under high temperature exposure conditions, thereby ensuring the safety of an electrochemical device.
[0012] Technical Solution
[0013] In one aspect of the present disclosure, a cross-linked polyolefin separator according to any one of the following embodiments is provided.
[0014] According to the first embodiment,
[0015] Provided is a cross-linked polyolefin separator,
[0016] In a frequency-loss / storage modulus curve, the cross-linked polyolefin separator shows a ratio (A / B) of 2 or more of a storage modulus (G', storage modulus) (A) to a loss modulus (G", loss modulus) (B) within a frequency range of 1 rad / s or less of the cross-linked polyolefin separator,
[0017] The horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale.
[0018] According to the second embodiment,
[0019] Provided is a cross-linked polyolefin separator,
[0020] In the frequency-loss modulus curve, at 10 -1 In the frequency range of the cross-linked polyolefin separator of 1 rad / s to 1 rad / s, the cross-linked polyolefin separator shows a storage modulus (G') versus frequency curve with a gradient of 0.05-0.4,
[0021] The horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale.
[0022] According to a third embodiment, there is provided a cross-linked polyolefin separator as defined in the first embodiment or the second embodiment,
[0023] The storage modulus is 1.0×10 5 to 1.0×107 Pa.
[0024] According to a fourth embodiment, there is provided a cross-linked polyolefin separator as defined in any one of the first to third embodiments,
[0025] The loss modulus is 3.0×10 5 Pa or less.
[0026] According to a fifth embodiment, there is provided a cross-linked polyolefin separator as defined in any one of the first to fourth embodiments,
[0027] The cross-linked polyolefin separator is formed by aqueous cross-linking or UV cross-linking.
[0028] According to a sixth embodiment, there is provided a cross-linked polyolefin separator as defined in the fifth embodiment, the cross-linked polyolefin separator being formed by aqueous cross-linking,
[0029] The cross-linked polyolefin separator includes a Si—O—Si bond, and the cross-linked polyolefin separator has a silicon (Si) content of 0.01 to 20 parts by weight based on 100 parts by weight of the cross-linked polyolefin separator.
[0030] According to a seventh embodiment, there is provided a cross-linked polyolefin separator as defined in the fifth embodiment,
[0031] The cross-linked polyolefin separator is formed by UV cross-linking, and includes a plurality of fibrils and pores formed by entanglement of the fibrils with each other, wherein polyolefin chains forming the fibrils are directly cross-linked with each other.
[0032] In another aspect of the present disclosure, a lithium secondary battery according to the following embodiments is provided.
[0033] According to the eighth embodiment,
[0034] Provided is a lithium secondary battery comprising a positive electrode, a negative electrode and a separator interposed between the positive electrode and the negative electrode,
[0035] wherein the separator is a cross-linked polyolefin separator as defined in any one of the first to seventh embodiments,
[0036] The positive electrode comprises: a current collector; and a layer of positive electrode active material disposed on the current collector, wherein the positive electrode active material comprises Li[Ni a Co b Mn c M1 d M2 e]O2 (wherein M1 and M2 are each independently any one selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg and Mo, a, b, c, d and e each independently represent the atomic fraction of each element forming the oxide, a≥0.5, a+b+c+d+e=1, and b>d>e).
[0037] In yet another aspect of the present disclosure, a method of manufacturing a cross-linked polyolefin separator according to any one of the following embodiments is provided.
[0038] According to a ninth embodiment, there is provided a method for manufacturing a cross-linked polyolefin separator, comprising the following steps:
[0039] (S1) introducing a polyolefin, a diluent, an initiator, a crosslinking catalyst and an alkoxysilane containing a carbon-carbon double bond group into an extruder, followed by mixing, to perform reactive extrusion of a silane-grafted polyolefin composition;
[0040] (S2) forming and orienting the reactively extruded silane-grafted polyolefin composition into a sheet form;
[0041] (S3) extracting the diluent from the oriented sheet to obtain a porous membrane;
[0042] (S4) heat-fixing the porous film while orienting the porous film at 100-150% based on the width of the porous film initially introduced into the heat-fixing bath; and
[0043] (S5) performing aqueous crosslinking of the thermally fixed porous membrane,
[0044] Wherein in the frequency-loss / storage modulus curve, within the frequency range of the cross-linked polyolefin separator of 1 rad / s or less, the cross-linked polyolefin separator shows a ratio (A / B) of storage modulus (G', storage modulus) (A) to loss modulus (G", loss modulus) (B) of 2 or greater, the horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted to a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted to a logarithmic scale.
[0045] According to a tenth embodiment, there is provided a method for producing a cross-linked polyolefin separator as defined in the ninth embodiment,
[0046] Wherein step (S4) is a step of heat fixing the porous membrane, wherein the porous membrane is subjected to a first orientation at 100-180% based on the width of the porous membrane initially introduced into the heat fixing bath, and then the porous membrane is subjected to a second orientation at a reduced orientation ratio of 100-150% based on the width of the porous membrane initially introduced into the heat fixing bath.
[0047] According to an eleventh embodiment, there is provided a method for manufacturing a cross-linked polyolefin separator as defined in the tenth embodiment,
[0048] wherein the ratio (t2 / t1) of the time (t1) at which the first orientation starts after the porous film is initially introduced into the heat fixing bath based on the time (t2) at which the second orientation starts after the porous film is initially introduced into the heat fixing bath is 0.5-1.5.
[0049] According to a twelfth embodiment, there is provided a method of manufacturing a cross-linked polyolefin separator as defined in any one of the ninth to eleventh embodiments,
[0050] The heat setting temperature is 100-140° C., and the heat setting time is 10-120 seconds.
[0051] In yet another aspect of the present disclosure, a method of manufacturing a cross-linked polyolefin separator according to any one of the following embodiments is provided.
[0052] According to the thirteenth embodiment,
[0053] Provided is a method for manufacturing a cross-linked polyolefin separator, the cross-linked polyolefin separator comprising a cross-linked polyolefin porous substrate, the cross-linked polyolefin porous substrate comprising a plurality of fibrils and pores formed by entanglement of the fibrils, wherein polyolefin chains forming the fibrils are directly cross-linked with each other, the method comprising the following steps:
[0054] applying a Type 2 photoinitiator composition including a Type 2 photoinitiator to an uncrosslinked polyolefin porous substrate; and
[0055] The ultraviolet rays are irradiated onto the polyolefin porous substrate coated with the type 2 photoinitiator composition, wherein the ultraviolet rays are irradiated at 10-2500 mJ / cm 2 The irradiation light dose is irradiated with ultraviolet light, and
[0056] In a frequency-loss / storage modulus curve, the cross-linked polyolefin separator shows a ratio (A / B) of 2 or more of a storage modulus (G', storage modulus) (A) to a loss modulus (G", loss modulus) (B) within a frequency range of 1 rad / s or less of the cross-linked polyolefin separator,
[0057] The horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale.
[0058] According to a fourteenth embodiment, there is provided a method for manufacturing a cross-linked polyolefin separator as defined in the thirteenth embodiment,
[0059] The type 2 photoinitiator includes thioxanthone (TX), thioxanthone derivatives, benzophenone (BPO), benzophenone derivatives, or a mixture of two or more thereof.
[0060] According to a fifteenth embodiment, there is provided a method for manufacturing a cross-linked polyolefin separator as defined in the thirteenth embodiment or the fourteenth embodiment,
[0061] The concentration of the type 2 photoinitiator in the type 2 photoinitiator composition is 0.01-0.3 wt %.
[0062] Beneficial Effects
[0063] According to an embodiment of the present disclosure, a separator having improved mechanical or thermal safety depending on silane cross-linking in the separator may be provided.
[0064] According to an embodiment of the present disclosure, a separator having improved mechanical or thermal safety by using an ultra high molecular weight polyolefin may be provided.
[0065] According to an embodiment of the present disclosure, a lithium secondary battery having improved safety by using a separator according to an embodiment of the present disclosure can be provided, especially for a lithium secondary battery provided with a positive electrode including a nickel-rich positive electrode active material, which has relatively low safety due to its low self-heating temperature.
[0066] According to an embodiment of the present disclosure, a separator having low viscosity and high elasticity at high temperatures can be provided. Therefore, the separator maintains its strength at high temperatures and fully ensures resistance to external forces under high temperature exposure conditions, thereby being able to provide an electrochemical device with improved safety.
[0067] According to an embodiment of the present disclosure, a cross-linked polyolefin separator may be obtained through a simplified method compared to a conventional method. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] The accompanying drawings illustrate preferred embodiments of the present disclosure and, together with the foregoing disclosure, are used to provide a further understanding of the technical features of the present disclosure. Therefore, the present disclosure should not be construed as being limited to the accompanying drawings.
[0069] Figure 1 is a graph illustrating the loss / storage modulus of each separator according to Examples and Comparative Examples. DETAILED DESCRIPTION
[0070] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms used in the specification and the appended claims should not be interpreted as being limited to the common meaning and dictionary meaning, but rather interpreted based on the meaning and concept of the technical aspects of the present disclosure on the basis of the principle that the inventor is allowed to appropriately define the terms for the best interpretation.
[0071] As used herein, the expression “one part is connected to another part” covers not only “one part is directly connected to another part” but also “one part is electrically connected to another part” by means of other elements interposed therebetween.
[0072] Throughout the specification, the expression "a portion comprises an element" does not exclude the presence of any additional elements but means that the portion may further include other elements.
[0073] Furthermore, it will be understood that the terms “comprises” and / or “comprising”, or “includes” and / or “including”, when used in this specification, refer to the presence of any specified shapes, quantities, steps, operations, components, elements and / or groups thereof, but do not preclude the addition of one or more other shapes, quantities, steps, operations, components, elements and / or groups thereof.
[0074] As used herein, the terms "approximately," "substantially," or the like are used as a continuous meaning from or to a stated numerical value when an acceptable manufacturing error or material error unique to the stated meaning is proposed, and are used for the purpose of preventing unscrupulous infringers from improperly using the disclosed content, including precise numerical values or absolute numerical values provided to facilitate understanding of the disclosed content.
[0075] As used herein, the expression "A and / or B" means "A, B, or both."
[0076] In one aspect, a cross-linked polyolefin separator and an electrochemical device including the cross-linked polyolefin separator are provided.
[0077] The separator for lithium secondary batteries shows excellent safety when the interval between the shutdown temperature and the melting temperature is large. In order to expand the interval between the shutdown temperature and the melting temperature, it is necessary to control the shutdown temperature to decrease and control the melting temperature to increase.
[0078] Therefore, according to the present disclosure, cross-linking is used to obtain a separator with a higher melting temperature. Here, cross-linking can be water-based cross-linking or UV cross-linking. As another method to increase the melting temperature, there is a method of increasing the molecular weight of polyolefin to improve elasticity. When a polyolefin resin with a large molecular weight is used, the fluidity at high and low temperatures is reduced, thereby increasing elasticity. Here, the polyolefin resin with a large molecular weight can be an ultra-high molecular weight polyolefin.
[0079] Meanwhile, such a cross-linked separator has viscoelasticity, and there is a problem in that when the separator is exposed to high temperature, the viscosity of the viscoelastic property increases, thereby making it difficult to ensure safety.
[0080] The present inventors focused on the above-mentioned problems and conducted extensive studies to provide a separator that can ensure safety even at high temperatures and an electrochemical device including the separator.
[0081] Meanwhile, as used herein, "high temperature" refers to a temperature of 180 to 220°C and may refer to a temperature at which the separator is melted or higher.
[0082] The cross-linked polyolefin separator according to an embodiment of the present disclosure,
[0083] In a frequency-loss / storage modulus curve, the cross-linked polyolefin separator shows a ratio (A / B) of 2 or more of a storage modulus (G', storage modulus) (A) to a loss modulus (G", loss modulus) (B) within a frequency range of 1 rad / s or less of the cross-linked polyolefin separator,
[0084] The horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale.
[0085] The present inventors have conducted intensive research to provide a cross-linked polyolefin separator that can ensure safety even at high temperatures. As a means of solving this technical problem, it is intended to reduce the viscosity of the separator at high temperatures and increase its elasticity at high temperatures, so that the separator can have improved high temperature safety.
[0086] In particular, when the viscosity of the separator decreases and the elasticity increases at high temperatures, the separator maintains its strength at high temperatures, and the separator itself has no fluidity, which can prevent the short circuit between the positive and negative electrodes, thereby improving the safety of the separator.
[0087] According to an embodiment of the present disclosure, in a frequency-loss / storage modulus curve, when G' is greater than G", especially when G' / G" is 2 or greater, a separator with improved safety can be provided, wherein the horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted to a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted to a logarithmic scale.
[0088] When G" is greater than G', the separator exhibits higher viscosity than elasticity, and thus there is a problem that the pores of the separator may be rapidly clogged at high temperatures.
[0089] Meanwhile, when G' / G" is less than 2, there is a problem that the separator shows fluidity and undesirably loses its function as an insulator.
[0090] As used herein, storage modulus (G') refers to the ability of a material to store energy and can be represented by the following formula 1:
[0091] [Formula 1]
[0092] G'=(stress / strain)cosδ
[0093] Here, the storage modulus can be determined by dynamic mechanical analysis.
[0094] According to the present disclosure, the storage modulus is determined using Dynamic Mechanical Analysis via a Temperature sweep test in the temperature range of 180° C. to 220° C. and a frequency of 1 rad / s.
[0095] According to an embodiment of the present disclosure, at a temperature of 190° C. and a frequency of 1 rad / s, the storage modulus may be 1.0×10 5 to 1.0×10 7 Pa, 1.2×10 5 Up to 5.0×10 6 Pa, 1.5×10 5 Up to 2.0×10 6Pa, 1.7×10 5 to 1.0×10 6 Pa, or 1.9×10 5 to 3.8×10 5 When the storage modulus is within the above range, there is an advantage that the separator maintains its strength at high temperatures.
[0096] As used herein, loss modulus (G") refers to the ability of a material to lose energy when deformed and can be represented by the following formula 2:
[0097] [Formula 2]
[0098] G”=(stress / strain)sinδ
[0099] Here, the loss modulus can be determined by dynamic mechanical analysis.
[0100] According to the present disclosure, the loss modulus is determined using Dynamic Mechanical Analysis via a Temperature sweep test in the temperature range of 180° C. to 220° C. and a frequency of 1 rad / s.
[0101] According to an embodiment of the present disclosure, at a temperature of 190° C. and a frequency of 1 rad / s, the loss modulus may be 3.0×10 5 Pa or less, 1.0×10 4 Up to 3.0×10 5 Pa, 2.0×10 4 to 1.5×10 5 Pa, 5.0×10 4 to 1.2×10 5 Pa, or 7.0×10 4 to 1.1×10 5 When the loss modulus is within the above range, there is an advantage that the separator does not show fluidity.
[0102] The ratio (A / B) of the storage modulus (G') (A) to the loss modulus (G") (B) of a separator is a relative measure of the elastic contribution compared to the viscosity contribution.
[0103] Specifically, when the ratio is 1 or more, the separator exhibits properties similar to a solid. On the other hand, when the ratio is 1 or less, the separator exhibits properties similar to a liquid.
[0104] At the same time, the ratio A / B is used as a relative measure to determine the uniformity and flowability of the extruded sheet during casting and orientation.
[0105] Therefore, in order to make the manufacturing process of the separator easy, the value of A / B is preferably low. In the finished separator, the value of A / B is preferably high, and specifically, according to an embodiment of the present disclosure, A / B is preferably 2 or more.
[0106] According to an embodiment of the present disclosure, within the frequency range of the partition of 1 rad / s or less, the partition may exhibit a ratio (A / B) of storage modulus (G') (A) to loss modulus (G") (B) of 2 or greater, 2-7, 2-5, 2.1-4.7, or 2.18-4.68. When the ratio of A / B is within the above range, the advantage is that the partition can maintain the function as an insulator while maintaining strength at high temperatures.
[0107] In another aspect of the present disclosure, a cross-linked polyolefin separator is provided, wherein in a frequency-loss modulus curve, -1 Within the frequency range of the cross-linked polyolefin separator from 0.1 rad / s to 1 rad / s, the cross-linked polyolefin separator shows a storage modulus (G') versus frequency curve with a gradient of 0.05-0.4, the horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted to a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted to a logarithmic scale.
[0108] Reference will be made to the above description regarding the storage modulus and the loss modulus.
[0109] According to an embodiment of the present disclosure, within the frequency range of the partition of 1 rad / s or less, the partition can show a storage modulus (G') versus frequency curve with a gradient of 0.05-0.4, 0.07-0.35, 0.1-0.3, 0.12-0.28, or 0.133-0.267. When the gradient is within the above range, the partition can maintain its function as an insulator at high temperatures.
[0110] According to an embodiment of the present disclosure, the separator may be formed by aqueous cross-linking or UV cross-linking.
[0111] According to an embodiment of the present disclosure, the separator may include 50 parts by weight or more of the ultra high molecular weight polyolefin based on 100 parts by weight of the total polyolefin.
[0112] According to the present disclosure, the separator is not particularly limited as long as it is a cross-linked separator. However, aqueous cross-linking is particularly advantageous because the separator can have maximized elasticity at high temperatures.
[0113] In particular, when the separator is formed by aqueous cross-linking, it includes Si-O-Si bonds, and the content of silicon (Si) in the separator may be 0.01-20 parts by weight based on 100 parts by weight of the separator.
[0114] When the separator maintains the above-defined silane content, the crosslinking degree of the separator is maintained at 30 to 80% to provide a separator having a high melting temperature.
[0115] According to an embodiment of the present disclosure, the cross-linked polyolefin is formed by UV cross-linking and includes a plurality of fibrils and pores formed by entanglement of the fibrils with each other, wherein polyolefin chains forming the fibrils are directly cross-linked with each other.
[0116] Here, "fibrils" refer to those formed by longitudinal stretching and orientation of polymer chains forming a polyolefin porous substrate during the manufacturing process of the porous substrate, so that the binding force between adjacent molecular chains can be increased and the chains can be assembled in the longitudinal direction. As a result, the cross-linked polyolefin porous substrate according to the present disclosure has a layered structure including a plurality of fibrils arranged in parallel with the substrate surface.
[0117] Here, the expression "directly crosslinked (direct crosslinking)" refers to a state of direct crosslinking between polyolefin chains that form fibrils substantially comprising polyolefin (preferably, fibrils consisting only of polyolefin) after providing reactivity to the fibrils by adding a type 2 photoinitiator. Therefore, crosslinking occurring between an additionally introduced crosslinking agent and the polyolefin chain does not correspond to "direct crosslinking".
[0118] The term "direct crosslinking" refers to crosslinking accomplished by a Type 2 photoinitiator.
[0119] As is known to all, photoinitiators are divided into Type 1 photoinitiators and Type 2 photoinitiators.
[0120] Type 1 photoinitiators undergo unimolecular bond cleavage upon absorption of light and are then converted into reactive species. The function of Type 1 photoinitiators does not require any other chemical substances. It is known that when a Type 1 photoinitiator and a curing agent are used to crosslink polyolefin (e.g., polyethylene) chains, the initiator or curing agent combines with free radicals generated by the polyethylene chains to cause crosslinking.
[0121] In contrast, Type 2 photoinitiators are known to undergo a bimolecular reaction upon absorption of light and react with another molecule (eg, a co-initiator or synergist) to form a reactive compound.
[0122] However, even if a type 2 photoinitiator is used according to the present disclosure, it will form free radicals and be converted into reactive compounds, while hydrogen atoms are removed only by hydrogen abstraction by light absorption, without the help of other co-initiators or synergists, and allow the polyolefin itself to be converted into a reactive polyolefin. Therefore, according to an embodiment of the present disclosure, a cross-linked polyolefin porous substrate can be provided, which includes directly cross-linked polyolefin chains of fibrils formed by polyolefin compounds. In this case, the polyolefin porous substrate can maintain its pore structure as it was before direct cross-linking, even after direct cross-linking. Therefore, thermal safety can be provided.
[0123] The cross-linked polyolefin separator according to the present disclosure may be obtained by the following method, but is not limited thereto.
[0124] In yet another aspect of the present disclosure, there is provided a method for manufacturing a cross-linked polyolefin separator, comprising the following steps:
[0125] (S1) introducing a polyolefin, a diluent, an initiator, a crosslinking catalyst and an alkoxysilane containing a carbon-carbon double bond group into an extruder, followed by mixing, to perform reactive extrusion of a silane-grafted polyolefin composition;
[0126] (S2) forming and orienting the reactively extruded silane-grafted polyolefin composition into a sheet form;
[0127] (S3) extracting the diluent from the oriented sheet to obtain a porous membrane;
[0128] (S4) heat-fixing the porous film while orienting the porous film at 100-150% based on the width of the porous film initially introduced into the heat-fixing bath; and
[0129] (S5) performing aqueous crosslinking of the thermally fixed porous membrane,
[0130] wherein in a frequency-loss / storage modulus curve, within a frequency range of the cross-linked polyolefin separator of 1 rad / s or less, the cross-linked polyolefin separator exhibits a ratio (A / B) of 2 or greater of a storage modulus (G', storage modulus) (A) to a loss modulus (G", loss modulus) (B),
[0131] The horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale.
[0132] Step (S1) is a step of introducing ungrafted polyolefin, diluent, initiator, crosslinking catalyst and alkoxysilane containing carbon-carbon double bond group into an extruder, and mixing and reacting to perform reactive extrusion.
[0133] According to an embodiment of the present disclosure, the polyolefin may be: polyethylene; polypropylene; polybutene; polypentene; polyhexene; polyoctene; a copolymer of at least two of ethylene, propylene, butene, pentene, 4-methylpentene, hexane, heptane and octene; or a mixture thereof.
[0134] Specifically, polyethylene includes low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), high-density polyethylene (HDPE), etc. Among them, the most preferred is high-density polyethylene having high crystallinity and high resin melting point.
[0135] According to an embodiment of the present disclosure, the polyolefin may have a weight average molecular weight of 200,000-1,000,000, 220,000-700,000, or 250,000-600,000. According to the present disclosure, by using a high molecular weight polyolefin having a weight average molecular weight of 200000-1000000 as a starting material, a separator having excellent strength and heat resistance can be obtained while ensuring the film uniformity and film processability of the separator.
[0136] According to an embodiment of the present disclosure, the diluent may include liquid or solid paraffin oil, mineral oil, wax, soybean oil, etc., which are currently used to manufacture separators through a wet process.
[0137] According to an embodiment of the present disclosure, the diluent may be a diluent capable of liquid-liquid phase separation for the polyolefin. For example, the diluent may be: a phthalic acid ester, such as dibutyl phthalate, dihexyl phthalate, dioctyl phthalate or the like; an aromatic ether, such as diphenyl ether; ether), benzyl ether or the like; C10-C20 fatty acid, such as palmitic acid, stearic acid, oleic acid, linoleic acid or the like; C10-C20 fatty acid alcohol, such as palmitic acid alcohol, stearic acid alcohol, oleic acid alcohol or the like; or a fatty acid ester formed by combining one or at least two fatty acids of a saturated or unsaturated fatty acid in which the fatty acid group has 4 to 26 carbon atoms, or an unsaturated fatty acid in which the double bond is substituted by epoxy, with a C1-C10 alcohol having 1 to 8 hydroxyl groups, such as palmitic acid monoester, diester or triester, stearic acid monoester, diester or triester, oleic acid monoester, diester or triester, linoleic acid monoester, diester or triester, or the like.
[0138] The diluent may include any one of the above-mentioned components or a mixture of at least two of them.
[0139] According to an embodiment of the present disclosure, based on 100 parts by weight of the ungrafted polyolefin, the content of the diluent can be 100-350 parts by weight, 125-300 parts by weight, or 150-250 parts by weight. When the total content of the diluent meets the above range, the problems caused by the increase in the content of the ungrafted polyolefin can be reduced, such as reduced porosity and pore size, reduced interconnection between holes and significantly reduced permeability, increased viscosity and extrusion load of the polyolefin composition, and processing difficulties. The problems caused by the reduction in the content of the ungrafted polyolefin can also be reduced, such as reduced compatibility of the ungrafted polyolefin with the diluent, and problems such as orientation fracture and uneven thickness caused by extruding the ungrafted polyolefin in gel form without thermodynamically mixing the ungrafted polyolefin with the diluent.
[0140] According to an embodiment of the present disclosure, the alkoxysilane containing a carbon-carbon double bond group is a crosslinking agent that initiates silane crosslinking, is grafted onto polyolefin through vinyl groups, and performs the function of crosslinking polyolefin through aqueous crosslinking caused by alkoxy groups.
[0141] According to an embodiment of the present disclosure, the alkoxysilane containing a carbon-carbon double bond group may include a compound represented by the following Chemical Formula 1:
[0142] [Chemical formula 1]
[0143]
[0144] wherein R1, R2 and R3 each independently represent a C1-C10 alkoxy group or a C1-C10 alkyl group, provided that at least one of R1, R2 and R3 represents an alkoxy group; and
[0145] R represents a vinyl group, an acryloyloxy group, a methacryloyloxy group or a C1-C20 alkyl group, wherein at least one hydrogen atom of the alkyl group is substituted with a vinyl group, an acryloyl group, an acryloyloxy group, a methacryloyloxy group or a methacryloyl group.
[0146] Meanwhile, R may further include an amino group, an epoxy group or an isocyanate group.
[0147] According to an embodiment of the present disclosure, the alkoxysilane containing a carbon-carbon double bond group may include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, (3-methacryloxypropyl)trimethoxysilane, (3-methacryloxypropyl)triethoxysilane, vinylmethyldimethoxysilane, vinyl-tri(2-methoxyethoxy)silane, vinylmethyldiethoxysilane, or a mixture of at least two thereof.
[0148] According to an embodiment of the present disclosure, based on 100 parts by weight of the total weight of the polyolefin and the diluent, the content of the alkoxysilane containing the carbon-carbon double bond group can be 0.1-3.0 parts by weight, 0.2-2.0 parts by weight, or 0.5-1.5 parts by weight. When the content of the alkoxysilane containing the carbon-carbon double bond group satisfies the above range, the problem of decreased crosslinking degree caused by low silane content and reduced grafting rate and deterioration of the appearance of the extruded sheet caused by high silane content and unreacted silane residue can be prevented.
[0149] According to an embodiment of the present disclosure, the initiator can be any initiator as long as it can generate free radicals. Non-limiting examples of initiators include 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP), benzoyl peroxide, acetyl peroxide, dilauroyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, cumyl peroxide, hydrogen peroxide, potassium persulfate or the like.
[0150] According to an embodiment of the present disclosure, based on 100 parts by weight of the alkoxysilane containing a carbon-carbon double bond group, the content of the initiator can be 0.1-20 parts by weight, specifically 1-10 parts by weight, and more specifically 2-5 parts by weight. When the content of the initiator satisfies the above range, the problem of a decrease in the silane grafting rate caused by a low initiator content and cross-linking between polyethylene molecules in an extruder due to a high initiator content can be prevented.
[0151] According to an embodiment of the present disclosure, a cross-linking catalyst is added to accelerate silane cross-linking.
[0152] According to an embodiment of the present disclosure, the cross-linking catalyst may be a carboxylate, an organic base, an inorganic acid or an organic acid of a metal such as tin, zinc, iron, zinc or cobalt. Non-limiting examples of cross-linking catalysts include: metal carboxylates such as dibutyltin dilaurate, dibutyltin diacetate, stannous acetate, stannous octoate, zinc naphthenate, zinc octoate and cobalt naphthenate; organic bases such as ethylamine, dibutylamine, hexylamine and pyridine; inorganic acids such as sulfuric acid and hydrochloric acid; organic acids such as toluenesulfonic acid, acetic acid, stearic acid and maleic acid. These cross-linking agents may be used alone or in combination.
[0153] According to an embodiment of the present disclosure, based on 100 parts by weight of the alkoxysilane containing carbon-carbon double bond groups, the content of the crosslinking catalyst can be 0.1-20 parts by weight, 1-10 parts by weight or 2-5 parts by weight. When the content of the crosslinking catalyst meets the above range, the silane can be crosslinked to a desired level and prevent undesirable side reactions in the lithium secondary battery. In addition, there is no problem associated with cost, such as the waste of catalyst.
[0154] According to the embodiment of the present disclosure, based on the polyolefin of 100 weight parts, the content of diluent can be 100-350 weight parts, 125-300 weight parts or 150-250 weight parts.When the total content of diluent meets the above range, the problem caused by the content increase of polyolefin can be reduced, such as porosity and pore size reduction, interconnection reduction between holes and permeability reduction significantly reduce, viscosity and extrusion load increase of polyolefin composition and processing difficulty and the like.The problem caused by the content reduction of polyolefin can also be reduced, such as the compatibility reduction of polyolefin and diluent and the problem of orientation fracture and uneven thickness caused by extruding polyolefin in gel form without thermodynamic mixing of polyolefin and diluent.
[0155] According to an embodiment of the present disclosure, the silane-grafted polyolefin composition may further include conventional additives for improving specific functions, such as an antioxidant, a UV stabilizer, an antistatic agent, a nucleating agent, or the like, if necessary.
[0156] According to an embodiment of the present disclosure, the reactive extrusion step may be performed by using a single-screw extruder or a twin-screw extruder.
[0157] Next, the reactively extruded silane-grafted polyolefin composition is formed and oriented in the form of a sheet (S2).
[0158] For example, the reactively extruded silane grafted polyolefin composition is extruded by using an extruder equipped with a T-die or the like, and then a cooled extrudate may be formed by a general casting or calendaring process using a water cooling or air cooling mode.
[0159] According to an embodiment of the present disclosure, a separator having improved mechanical strength and puncture strength may be provided through the orientation step as described above.
[0160] According to an embodiment of the present disclosure, orientation can be performed by sequential or simultaneous orientation using a roller or a tenter. In the longitudinal and transverse directions, the orientation ratio can be 3 times or more, or 4-10 times, and the total orientation ratio can be 14-100 times. When the orientation ratio satisfies the above ratio, the problems of insufficient orientation in one direction, destruction of the physical property balance between the longitudinal and transverse directions, and reduction of tensile strength and puncture strength can be prevented. When the total orientation ratio satisfies the above range, the problem of non-orientation or failure of pore formation can be prevented.
[0161] According to embodiments of the present disclosure, the orientation temperature may vary with the melting point of the polyolefin and the concentration and type of the diluent.
[0162] According to an embodiment of the present disclosure, when the polyolefin is polyethylene and the diluent is liquid paraffin, in the case of longitudinal (MD) orientation, the orientation temperature may be 70-160°C, 90-140°C, or 100-130°C. In the case of transverse (TD) orientation, the orientation temperature may be 90-180°C, 110-160°C, or 120-150°C, and when bidirectional orientation is performed simultaneously, the orientation temperature may be 90-180°C, 110-160°C, or 120-150°C. When the orientation temperature satisfies the above range, the problem of fracture or non-orientation caused by lack of softness due to low orientation temperature can be prevented. In addition, partial over-orientation or physical property differences caused by high orientation temperature can be prevented.
[0163] Then, the diluent is extracted from the formed and oriented sheet, thereby obtaining a silane-grafted polyolefin porous membrane (S3).
[0164] According to an embodiment of the present disclosure, the diluent may be extracted from the porous membrane by using an organic solvent, and then the porous membrane may be dried.
[0165] According to an embodiment of the present disclosure, the organic solvent is not particularly limited as long as it can extract the diluent. However, methyl ethyl ketone, dichloromethane or hexane, which has high extraction efficiency and shows a high drying rate, is suitably used.
[0166] According to an embodiment of the present disclosure, the extraction can be any conventional solvent extraction process, such as an immersion process, a solvent spray process or an ultrasonic process, and these processes can be used alone or in combination. After the extraction is performed, the content of the residual diluent should preferably be 1 wt % or less. When the content of the residual diluent is greater than 1 wt %, the physical properties decrease, and the permeability of the porous membrane decreases. The content of the residual diluent may be affected by the extraction temperature and the extraction time. In order to increase the solubility of the diluent in the organic solvent, a higher extraction temperature is preferred. However, considering the safety issues caused by the boiling of the organic solvent, the extraction temperature is preferably 40°C or below. When the extraction temperature is equal to or lower than the solidification point of the diluent, the extraction efficiency will be significantly reduced. Therefore, the extraction temperature should be higher than the solidification point of the diluent.
[0167] In addition, the extraction time may vary with the thickness of the porous membrane. In the case where the separator thickness is 5-15 μm, the extraction time may be appropriately 1-3 minutes.
[0168] Then, the porous film is heat-fixed (S4). Heat-fixing is a process of fixing and heating the porous film so as to forcibly fix the porous film to be shrunk to remove residual stress.
[0169] Here, in the heat fixing step, the porous film is oriented at 100-150% based on the width of the porous film initially introduced into the heat fixing bath. According to an embodiment of the present disclosure, the orientation can be performed at 100%, 105%, or 110% or more, and 150%, 150%, or 130% or less within the above range. When the orientation ratio satisfies the above range, the residual stress of the separator can be effectively removed while ensuring the desired thickness and porosity.
[0170] Here, step (S4) is a step of thermally fixing the porous membrane.
[0171] The porous film is subjected to a first orientation at 100-180% based on the width of the porous film initially introduced into the heat fixing bath, and then the porous film is subjected to a second orientation at a reduced orientation ratio of 100-150% based on the width of the porous film initially introduced into the heat fixing bath. In other words, the porous film subjected to the second orientation has a smaller width than the porous film subjected to the first orientation.
[0172] When the width of the porous film in the second orientation is reduced compared to the first orientation, thermal shrinkage of the resulting separator can be reduced.
[0173] When the orientation is excessively performed and exceeds the above range, the crosslinking points where crosslinking occurs may be spaced apart from each other, making it difficult to perform effective crosslinking. As a result, the expected effect of sufficiently increasing the storage modulus cannot be obtained, and thus the resulting separator exhibits rheological properties similar to those of a conventional non-crosslinked separator.
[0174] Here, the ratio (t2 / t1) of the time (t1) when the first orientation starts after the porous film is initially introduced into the heat fixing bath based on the time (t2) when the second orientation starts after the porous film is initially introduced into the heat fixing bath is 0.5-1.5, 0.7-1.3 or 0.8-1.2.
[0175] Higher heat fixation temperatures are beneficial for reducing shrinkage. However, when the heat fixation temperature is too high, the porous film may partially melt, resulting in clogging of the micropores formed in the porous film, thereby reducing permeability. When the polyolefin is polyethylene, the heat fixation temperature may be 100-140°C, 105-135°C, or 110-130°C. When the polyolefin is polyethylene and the heat fixation temperature meets the above range, the polyolefin molecules can be rearranged to remove the residual stress of the porous film, and the pore clogging problem of the porous film caused by partial melting can be reduced. As the heat fixation temperature increases, the thermal shrinkage of the separator can be improved. At the same time, as the heat fixation temperature decreases, the resistance of the separator will decrease.
[0176] When the temperature of heat fixation is high, the time of heat fixation is set to a relatively short time. When the temperature of heat fixation is low, the time of heat fixation is set to a relatively long time. According to an embodiment of the present disclosure, the time of heat fixation can be 10-120 seconds, 20-90 seconds or 30-60 seconds. When heat fixation is performed within the above time range, the polyolefin molecules can be rearranged to remove the residual stress of the porous film, and the pore clogging problem of the porous film caused by partial melting can be reduced.
[0177] Afterwards, the heat-fixed porous film is crosslinked in the presence of water (S5). According to an embodiment of the present disclosure, crosslinking can be carried out at 60-100° C., 65-95° C., or 70-90° C. According to an embodiment of the present disclosure, crosslinking can be carried out at a humidity of 60-95% for 6-50 hours. In order to accelerate crosslinking, a crosslinking catalyst can be used. In general, as a crosslinking catalyst, a carboxylate, an organic base, an inorganic acid or an organic acid of a metal such as tin, zinc, iron, zinc or cobalt can be used. Specific examples of crosslinking catalysts include: dibutyltin dilaurate, dibutyltin diacetate, stannous acetate, stannous octoate, zinc naphthenate, zinc octoate, cobalt naphthenate, ethylamine, dibutylamine, hexylamine, pyridine, inorganic acids such as sulfuric acid and hydrochloric acid, organic acids such as toluenesulfonic acid, acetic acid, stearic acid and maleic acid, or the like. The cross-linking catalyst may be used by adding the cross-linking catalyst during the preparation of the silane-grafted polyolefin solution, by applying a solution or dispersion of the cross-linking catalyst to the porous membrane, or the like.
[0178] In yet another aspect of the present disclosure, a method for manufacturing a cross-linked polyolefin separator is provided.
[0179] Specifically, a method for manufacturing a cross-linked polyolefin separator is provided, the cross-linked polyolefin separator comprising a cross-linked polyolefin porous substrate, the cross-linked polyolefin porous substrate comprising a plurality of fibrils and pores formed by entanglement of the fibrils with each other, wherein polyolefin chains forming the fibrils are directly cross-linked with each other, the method comprising the following steps:
[0180] applying a Type 2 photoinitiator composition including a Type 2 photoinitiator to an uncrosslinked polyolefin porous substrate; and
[0181] The ultraviolet rays are irradiated onto the polyolefin porous substrate coated with the type 2 photoinitiator composition, wherein the ultraviolet rays are irradiated at 10-2500 mJ / cm 2 The irradiation light dose is irradiated with ultraviolet light, and
[0182] In a frequency-loss / storage modulus curve, the cross-linked polyolefin separator shows a ratio (A / B) of 2 or more of a storage modulus (G', storage modulus) (A) to a loss modulus (G", loss modulus) (B) within a frequency range of 1 rad / s or less of the cross-linked polyolefin separator,
[0183] The horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale.
[0184] In other words, according to the present disclosure, a cross-linked polyolefin separator having a specific G' to G" relationship and a specific G' gradient is provided. The separator having such a relationship can function as an insulator while maintaining its strength at high temperatures. In other words, when the temperature of the lithium secondary battery rises rapidly due to abnormal external conditions, the storage modulus representing the solid properties of the separator is maintained at a higher value than the loss modulus representing the liquid properties of the separator, so that the separator can maintain its shape without losing its function as an insulator.
[0185] As described above, a cross-linked polyolefin separator can be obtained by using an alkoxysilane containing a carbon-carbon double bond group while controlling the orientation ratio during thermal fixation. In addition, a cross-linked polyolefin separator can be obtained by using a type 2 photoinitiator as described below.
[0186] first,
[0187] A Type 2 photoinitiator composition is applied to a polyolefin porous substrate.
[0188] According to an embodiment of the present disclosure, the type 2 photoinitiator may include thioxanthone (TX), thioxanthone derivatives, benzophenone (BPO), benzophenone derivatives, or a mixture of two or more thereof.
[0189] Specific examples of thioxanthone derivatives may include, but are not limited to, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2-dodecylthioxanthone, 2,4-diethylthioxanthone, 2,4-dimethylthioxanthone, 1-methoxycarbonylthioxanthone, 2-ethoxycarbonylthioxanthone, 3-(2-methoxyethoxycarbonyl)-thioxanthone, 4-butoxycarbonyl-thioxanthone, 3-butoxycarbonyl-7-methylthioxanthone, 1-cyano-3-chlorothioxanthone, 1-ethoxycarbonyl-3-chlorothioxanthone, 1-ethoxycarbonyl-3-ethoxythioxanthone, 1-ethoxycarbonyl-3-aminothioxanthone, 1-ethoxycarbonyl-3-phenylsulfonylthioxanthone, 3,4-bis[2-(2-methoxyethoxy)ethoxycarbonyl]thioxanthone, 1-ethoxycarbonyl-3-(1-methyl- 1-Morpholinoethyl)-thioxanthone, 2-methyl-6-dimethoxymethyl-thioxanthone, 2-methyl-6-(1,1-dimethoxy-benzyl)-thioxanthone, 2-morpholinomethylthioxanthone, 2-methyl-6-morpholinomethyl-thioxanthone, N-allylthioxanthone-3,4-dicarboximide, N-octylthioxanthone-3,4-dicarboximide, N-(1,1,3,3-tetrakis)-thioxanthone, methylbutyl)-thioxanthone-3,4-dicarboximide, 1-phenoxythioxanthone, 6-ethoxycarbonyl-2-methoxythioxanthone, 6-ethoxycarbonyl-2-methylthioxanthone, thioxanthone-2-polyethylene glycol ester, 2-hydroxy-3-(3,4-dimethyl-9-oxo-9H-thioxanthone-2-oxy)-N,N,N-trimethyl-1-propylamine chloride, or the like.
[0190] According to the present disclosure, specific examples of benzophenone derivatives may include, but are not limited to, 4-phenylbenzophenone, 4-methoxybenzophenone, 4,4'-dimethoxy-benzophenone, 4,4'-dimethylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-dimethylaminobenzophenone, 4,4'-diethylaminobenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-(4-methylphenylthio)-benzophenone, 3,3'-dimethyl-4-methoxy-benzophenone, 4-(2-methylphenylthio) ... -(2-hydroxyethylthio)-benzophenone, 4-(4-tolylthio)benzophenone, 4-benzoyl-N,N,N-trimethylbenzylamine chloride, 2-hydroxy-3-(4-benzoylphenoxy)-N,N,N-trimethyl-propylamine chloride monohydrate, 4-hydroxybenzophenone, 4-(13-acryloyl-1,4,7,10,13-pentaoxotridecanyl)-benzophenone, 4-benzoyl-N,N-dimethyl-N-[2-(1-oxo-2-propenyl)oxy]ethyl-benzylamine chloride, or the like.
[0191] According to the present disclosure, when a Type 2 photoinitiator is used, there is an advantage that crosslinking can be accomplished at a lower light dose compared to crosslinking using a Type 1 photoinitiator and / or crosslinking agent.
[0192] According to an embodiment of the present disclosure, the type 2 photoinitiator may be 2-isopropylthioxanthone, thioxanthone, or a mixture thereof. When the type 2 photoinitiator is 2-isopropylthioxanthone, thioxanthone, or a mixture thereof, the crosslinking reaction may be carried out at a lower dose (such as 500 mJ / cm ) than when any other photoinitiator (such as benzophenone) is used for crosslinking. 2 ) for cross-linking.
[0193] According to an embodiment of the present disclosure, a composition including a type 2 photoinitiator can be prepared by dissolving the type 2 photoinitiator in a solvent. The solvent can be acetone, isopropyl alcohol (IPA), N-methyl pyrrolidone (NMP), methanol, or a mixture of two or more thereof. The type 2 photoinitiator can be present in the composition at a concentration of 0.01-0.4 wt %, 0.01-0.3 wt %, 0.03-0.3 wt % or 0.05-0.2 wt %. When the concentration is higher than the above range, rapid crosslinking occurs during UV irradiation, resulting in shrinkage of the partition, and a polyethylene main chain scission occurs, resulting in reduced mechanical strength. Within the above content range of the type 2 photoinitiator, suitable crosslinking can be performed without shrinking during the crosslinking process.
[0194] Reference will be made to the above description regarding the polyolefin porous substrate that can be used in the present disclosure.
[0195] According to an embodiment of the present disclosure, the composition (type 2 photoinitiator composition) including type 2 photoinitiator can be applied to the polyolefin porous substrate by immersing the polyolefin porous substrate in the type 2 photoinitiator composition, or by spraying the type 2 photoinitiator composition on at least one surface of the polyolefin porous substrate, or in a similar manner. However, the scope of the present disclosure is not limited thereto. For example, the type 2 photoinitiator composition can be applied to the polyolefin porous substrate for 0.1 seconds to 5 minutes, but the scope of the present disclosure is not limited thereto. Then, the polyolefin porous substrate coated with the type 2 photoinitiator composition can be dried. For example, drying can be carried out at room temperature for 30 seconds to 10 minutes.
[0196] Then, the polyolefin porous substrate coated with the composition is subjected to UV irradiation, wherein the ultraviolet irradiation dose is 10-2500 mJ / cm 2 .
[0197] UV irradiation is performed by using a UV curing system, while taking into account other conditions, such as the weight ratio of the photoinitiator, and appropriately controlling the UV irradiation time and the irradiation dose. For example, the UV irradiation time and the irradiation dose can be set in such a manner that the polyolefin fibrils can be sufficiently cross-linked to provide a polyolefin porous substrate having a melting temperature of about 160° C. or higher, or 170° C. or higher, and the polyolefin porous substrate is not damaged by the heat generated by the UV lamp. In addition, the UV lamp used in the UV curing system can be appropriately selected from a high-pressure mercury lamp, a metal lamp, a gallium lamp, or the like, depending on the photoinitiator used for cross-linking, and the light emission wavelength and the dose can be appropriately selected according to the overall process.
[0198] According to an embodiment of the present disclosure, ultraviolet light is irradiated onto the polyolefin porous substrate coated with the type 2 photoinitiator composition, wherein the UV light dose is 10-2500 mJ / cm 2 , 50-1000mJ / cm 2 , or 150-500mJ / cm 2 .
[0199] According to an embodiment of the present disclosure, the "UV light dose" can be determined by using a portable light dose meter called an H type UV bulb and a UV power puck available from Miltec. When the light dose is determined using an H type UV bulb available from Miltec, three types of wavelength values, UVA, UVB, and UVC, are provided according to the wavelength, and the ultraviolet light used herein corresponds to UVA.
[0200] According to the present disclosure, a method for determining “UV light dose” includes passing a UV power puck through a conveyor belt in the presence of a light source under the same conditions as the sample, and defining the UV light dose value displayed in the UV power puck as the “UV light dose”.
[0201] The use of a photoinitiator causes crosslinking of the fibrils, allowing the separator to maintain the storage modulus even at high temperatures, with very slight changes in the loss modulus. In addition, it is known that in the case of conventional polymers that conform to the Maxwell model, the storage modulus theoretically has a gradient of about 2 depending on the frequency change before the use of a photoinitiator. However, when elasticity increases rapidly while crosslinking occurs, this change in the gradient becomes gentle.
[0202] In yet another aspect of the present disclosure, a lithium secondary battery including the separator is provided.
[0203] Specifically, a lithium secondary battery is provided, which includes: a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is the above-mentioned cross-linked polyolefin separator, and the positive electrode includes: a current collector; and a layer of positive electrode active material disposed on the current collector, wherein the positive electrode active material includes Li[Ni a Co b Mn c M1 d M2 e ]O2 (wherein M1 and M2 are each independently any one selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg and Mo, a, b, c, d and e each independently represent the atomic fraction of each element forming the oxide, a≥0.5, a+b+c+d+e=1, and b>d>e).
[0204] The positive electrode active material is a Ni-rich positive electrode active material having a layered structure, and has the advantage of being able to achieve a high capacity of 200 mAh / g or more. On the other hand, the positive electrode including such a positive electrode active material shows a low self-heating temperature, so the safety is relatively low.
[0205] The present inventors have conducted intensive research to solve the problems related to safety. We have found that when the above separator is used in combination with a positive electrode, safety can be significantly improved.
[0206] Embodiments will be described more fully below so that the present disclosure can be easily understood. However, the following embodiments can be embodied in a variety of different forms and should not be construed as being limited to the exemplary embodiments set forth herein. On the contrary, these exemplary embodiments are provided to make the present disclosure thorough and complete and to fully convey the scope of the present disclosure to those skilled in the art.
[0207] Example 1
[0208] First, polyethylene (Hanwha Total, VO601) with a weight average molecular weight of 600,000 as polyolefin was introduced into the extruder hopper and conveyed at a flow rate of 3 kg / hr. Next, liquid paraffin oil (Kukdong Oil & Chem. LP350) as a diluent was introduced into the first injection port at a flow rate of 5 kg / hr and mixed with the polyethylene conveyed to the extruder. Then, liquid paraffin oil (Kukdong Oil & Chem. LP350) as a diluent is mixed with 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane as an initiator and vinyltrimethoxysilane as an alkoxysilane containing a carbon-carbon double bond group, wherein the proportions of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and vinyltrimethoxysilane are 0.05 parts by weight and 2.5 parts by weight, respectively, based on 100 parts by weight of the combined weight of the polyolefin and the diluent, and the resulting mixture is supplied to the second injection port at a flow rate of 2 kg / hr.
[0209] Then, reactive extrusion was performed at a temperature of 200° C. to obtain a silane-grafted polyethylene composition.
[0210] The resulting silane-grafted polyethylene composition was molded into a sheet shape by a T-die and a cold casting roll operating at 40°C. Then, MD orientation was performed at a ratio of 6 times the length by using a transmission ratio of a roller maintained at 110°C, and TD orientation was performed at a ratio of 7 times the width by using a tenter in an oven maintained at 120°C. After that, the oriented sheet was immersed in a dilution bath containing dichloromethane to remove the diluent remaining in the oriented sheet, thereby providing a porous film having pores formed therein. Then, in a heat fixing bath maintained at 128°C, orientation was further performed in the width direction at a ratio of 20% based on the width of the porous film initially introduced, and relaxation was performed in the later stage of the heat fixing bath. In this way, a porous film with a width increased by 10% compared to the width of the initial porous film was wound.
[0211] The wound porous film was placed in an oven at a temperature of 60° C. and a relative humidity of 85% for 2 days to obtain a cross-linked polyolefin separator.
[0212] The obtained separator had a thickness of 9 μm and an air permeation time of 77 seconds / 100 cc.
[0213] Example 2
[0214] A crosslinked polyolefin separator was obtained in the same manner as in Example 1, except that the MD orientation ratio and the TD orientation ratio in the orientation step were controlled to 5.5 times and 6 times, respectively. The obtained separator had a thickness of 9 μm and an air permeation time of 74 seconds / 100 cc.
[0215] Example 3
[0216] A cross-linked polyolefin separator was obtained in the same manner as in Example 1, except that the orientation was further performed in the width direction in the heat fixing bath at a ratio of 70% based on the width of the initially introduced porous film, and relaxation was performed in the later stage of the heat fixing bath, and the porous film with a width increased by 40% compared with the width of the initial porous film was wound. The obtained separator had a thickness of 9 μm and an air permeation time of 70 seconds / 100 cc.
[0217] Comparative Example 1
[0218] A crosslinked polyolefin separator was obtained in the same manner as in Example 1, except that no initiator and alkoxysilane containing a carbon-carbon double bond group were added. In other words, the obtained separator was a non-crosslinked polyolefin separator. The obtained separator had a thickness of 9 μm and an air permeation time of 89 seconds / 100 cc.
[0219] Example 4
[0220] First, 2-isopropylthioxanthone (ITX, available from Sigma Aldrich) as a Type 2 photoinitiator was dissolved in acetone to a concentration of 0.5 wt % to prepare a Type 2 photoinitiator composition.
[0221] Next, the Type 2 photoinitiator composition was applied to the surface of the non-crosslinked polyolefin separator according to Comparative Example 1 by a dip coating process. Then, the acetone was dried at a temperature of 60°C.
[0222] Then, the cumulative light dose, i.e., the UV irradiation light dose, was 500 mJ / cm 2 , irradiating ultraviolet rays to the top surface of the uncrosslinked polyolefin separator coated with the Type 2 photoinitiator composition, wherein the UV irradiation intensity (intensity) is set to 80% of the UV light source and the line speed (line speed) is set to 10m / min. In this way, a crosslinked polyolefin separator is obtained. The obtained separator has a thickness of 9μm and an air permeation time of 90 seconds / 100cc.
[0223] Comparative Example 2
[0224] A non-crosslinked polyolefin separator (S10W, available from Asahi) including ultra-high molecular weight polyethylene and a small amount of polypropylene was prepared. The separator had a thickness of 9 μm and an air permeation time of 92 seconds / 100 cc.
[0225] Example 5
[0226] First, 2-isopropylthioxanthone (ITX, available from Sigma Aldrich) as a Type 2 photoinitiator was dissolved in acetone to a concentration of 0.5 wt % to prepare a Type 2 photoinitiator composition.
[0227] Next, the Type 2 photoinitiator composition was applied by a dip coating process onto the non-crosslinked polyolefin separator according to Comparative Example 2. Then, acetone was dried at a temperature of 60°C.
[0228] Then, the cumulative light dose, i.e., the UV irradiation light dose, was 500 mJ / cm 2 , irradiating ultraviolet rays to the top surface of the uncrosslinked polyolefin separator coated with the Type 2 photoinitiator composition, wherein the UV irradiation intensity (intensity) is set to 80% of the UV light source and the line speed (line speed) is set to 10m / min. In this way, a crosslinked polyolefin separator is obtained. The resulting separator has a thickness of 9μm and an air permeation time of 91 seconds / 100cc.
[0229] Comparative Example 3
[0230] An uncrosslinked polyolefin separator (DB0905, available from Toray) having a three-layer structure including a core layer having a low shutdown temperature and skin layers applied to both surfaces of the core layer and having a high melting temperature and having a thickness of 9 μm was prepared. The separator had a thickness of 9 μm and an air permeation time of 88 seconds / 100 cc.
[0231] Comparative Example 4
[0232] First, 2-isopropylthioxanthone (ITX, available from Sigma Aldrich) as a Type 2 photoinitiator was dissolved in acetone to a concentration of 0.5 wt % to prepare a Type 2 photoinitiator composition.
[0233] Next, the Type 2 photoinitiator composition was applied to the non-crosslinked polyolefin separator according to Comparative Example 3 by a dip coating process. Then, acetone was dried at a temperature of 60°C.
[0234] Then, the cumulative light dose, i.e., the UV irradiation light dose, was 5,000 mJ / cm2 , irradiate ultraviolet rays to the top surface of the uncrosslinked polyolefin separator coated with the Type 2 photoinitiator composition, wherein the UV irradiation intensity is set to 80% of the UV light source and the line speed is set to 10 m / min. In this way, a crosslinked polyolefin separator is obtained. The resulting separator has a thickness of 9 μm and an air permeation time of 88 seconds / 100 cc. It can be seen from Comparative Example 4 that due to such an excessively high UV irradiation light dose, the polyolefin chain is broken.
[0235] Comparative Example 5
[0236] A cross-linked polyolefin separator was obtained in the same manner as in Example 1, except that: orientation was further performed in the width direction in a heat fixing bath, the ratio was 85% based on the width of the porous film initially introduced, and relaxation was performed in the later stage of the heat fixing bath, and the porous film with a width increased by 55% compared to the width of the initial porous film was wound. The resulting separator had a thickness of 9 μm and an air permeation time of 66 seconds / 100 cc. In other words, Comparative Example 5 was performed in the same manner as in Example 1, except that: the orientation rate in the heat fixing bath was 185%. In the case of Comparative Example 5, the porous film was excessively oriented and caused fibril breakage, resulting in cross-linking failure.
[0237] Comparative Example 6
[0238] An uncrosslinked polyolefin separator was obtained in the same manner as in Comparative Example 1, except that each of the first antioxidant (Irganox 1010, available from BASF) and the second antioxidant (Irgafos 168, available from 168) was introduced at 8,000 ppm. Then, a UV crosslinked polyolefin separator was obtained in the same manner as in Example 4. The resulting separator had a thickness of 9 μm and an air permeation time of 92 seconds / 100 cc. In the case of Comparative Example 6, the porous film contained an excessively high content of the antioxidant, so crosslinking could not occur smoothly.
[0239] Test Case
[0240] Determination of storage modulus and loss modulus
[0241] Each separator according to the embodiment and the comparative example was analyzed by a frequency sweep test at a temperature of 190° C. using a rheological performance analyzer (ARES-G2, available from TA Instruments) to determine the storage modulus (G′, storage modulus) at a frequency of 1 rad / s, the loss modulus (G″, loss modulus) at a frequency of 1 rad / s, and the -1The gradient of the storage modulus (G') at a frequency of 1 rad / s is shown in Table 1. At the same time, the fluidity of each separator can be determined by G' and G".
[0242] Determination of the melting temperature of the separator
[0243] Each separator according to the Examples and Comparative Examples was evaluated in terms of meltdown temperature via thermomechanical analysis (TMA) using a Q400 instrument available from TA. The results are shown in Table 1 below.
[0244] [Table 1]
[0245] G'(Pa)(A) G”(Pa)(B) A / B(G' / G') G' Gradient Melting temperature(℃) Example 1 351,229 76,336 4.60 0.165 192 Example 2 347,717 77,099 4.51 0.160 188 Example 3 376,681 80,548 4.68 0.133 195 Example 4 193,176 83,969 2.30 0.165 177 Example 5 218,867 100,190 2.18 0.267 172 Comparative Example 1 98,838 92,341 1.07 0.620 148 Comparative Example 2 158,599 119,124 1.33 0.550 150 Comparative Example 3 139,576 87,239 1.60 0.415 158 Comparative Example 4 122,827 79,823 1.54 0.430 161 Comparative Example 5 96,861 86,801 1.12 0.634 155 Comparative Example 6 99,471 90,427 1.10 0.544 151
[0246] Referring to Table 1, compared with the separator according to Comparative Examples 1-6, at a frequency of the cross-linked polyolefin separator of 1 rad / s or less, each cross-linked polyolefin separator obtained by Examples 1-5 satisfying a ratio (A / B) of 2 or more of the storage modulus (G', storage modulus) (A) to the loss modulus (G', loss modulus) (B) or a gradient of the storage modulus (G', storage modulus) (A) with respect to the frequency of 0.05-0.4 shows a significantly higher melting temperature. Therefore, it can be seen that each cross-linked polyolefin separator according to Examples 1-5 shows significantly improved thermal safety.
Claims
1. A cross-linked polyolefin separator, wherein in a frequency-loss / storage modulus curve, within a frequency range of the cross-linked polyolefin separator of 1 rad / s or less, the cross-linked polyolefin separator shows a ratio (A / B) of 2 or more of a storage modulus (G', storage modulus) (A) to a loss modulus (G", loss modulus) (B), the horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted to a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and the loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted to a logarithmic scale, and the storage modulus is 1.2×10 5 to 1.0×10 7 Pa.
2. A cross-linked polyolefin separator, wherein in a frequency-loss modulus curve, -1 In the frequency range of the cross-linked polyolefin separator of 1 rad / s to 1 rad / s, the cross-linked polyolefin separator shows a storage modulus (G') versus frequency curve with a gradient of 0.05-0.4, the horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, the vertical axis of the curve is the storage modulus (G') (A) and the loss modulus (G', loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale, and the storage modulus is 1.2×10 5 to 1.0×10 7 Pa.
3. The cross-linked polyolefin separator according to claim 1 or 2, wherein the storage modulus is 1.9×10 5 to 3.8×10 5 Pa.
4. The cross-linked polyolefin separator according to claim 1 or 2, wherein the loss modulus is 3.0×10 5 Pa or less.
5. The cross-linked polyolefin separator according to claim 1, wherein the cross-linked polyolefin separator exhibits a ratio (A / B) of storage modulus (G', storage modulus) (A) to loss modulus (G") (B) of 2-7, 2-5, 2.1-4.7, or 2.18-4.
68.
6. The cross-linked polyolefin separator according to claim 2, wherein the cross-linked polyolefin separator exhibits a storage modulus (G') versus frequency curve with a gradient of 0.07-0.35, 0.1-0.3, 0.12-0.28, or 0.133-0.
267. 7 . The cross-linked polyolefin separator according to claim 1 or 2 , which is formed by aqueous cross-linking or UV cross-linking.
8. The cross-linked polyolefin separator according to claim 7, which is formed by aqueous cross-linking, comprises Si-O-Si bonds, and has a silicon (Si) content of 0.01-20 parts by weight based on 100 parts by weight of the cross-linked polyolefin separator.
9. The cross-linked polyolefin separator according to claim 7, which is formed by UV cross-linking and comprises a plurality of fibrils and pores formed by entanglement of the fibrils with each other, wherein polyolefin chains forming the fibrils are directly cross-linked with each other.
10. A lithium secondary battery comprising: a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is a cross-linked polyolefin separator as defined in claim 1 or 2, and The positive electrode comprises: a current collector; and a layer of positive electrode active material disposed on the current collector, The positive electrode active material comprises Li[Ni a Co b Mn c M1 d M2 e ]O2 (wherein M1 and M2 are each independently any one selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg and Mo, a, b, c, d and e each independently represent the atomic fraction of each element forming the oxide, a≥0.5, a+b+c+d+e=1, and b>d>e).
11. A method for manufacturing a cross-linked polyolefin separator, comprising the steps of: (S1) introducing a polyolefin, a diluent, an initiator, a crosslinking catalyst and an alkoxysilane containing a carbon-carbon double bond group into an extruder, followed by mixing, to perform reactive extrusion of a silane-grafted polyolefin composition; (S2) forming and orienting the reactively extruded silane-grafted polyolefin composition into a sheet form; (S3) extracting the diluent from the oriented sheet to obtain a porous membrane; (S4) thermally fixing the porous film, wherein the porous film is subjected to a first orientation at 100-180% based on the width of the porous film initially introduced into a thermal fixing bath, and then the porous film is subjected to a second orientation at a reduced orientation ratio of 100-150% based on the width of the porous film initially introduced into a thermal fixing bath; and (S5) performing aqueous crosslinking of the porous membrane by thermal fixation, Wherein in the frequency-loss / storage modulus curve, within the frequency range of the cross-linked polyolefin separator of 1 rad / s or less, the cross-linked polyolefin separator shows a ratio (A / B) of storage modulus (G', storage modulus) (A) to loss modulus (G", loss modulus) (B) of 2 or greater, the horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted to a logarithmic scale, and the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted to a logarithmic scale.
12. The method for manufacturing a cross-linked polyolefin separator according to claim 11, wherein the ratio (t2 / t1) of the time (t2) at which the second orientation starts after the porous membrane is initially introduced into a heat fixing bath to the time (t1) at which the first orientation starts after the porous membrane is initially introduced into a heat fixing bath is 0.5-1.
5.
13. The method for manufacturing a cross-linked polyolefin separator according to claim 11, wherein the temperature of the heat fixing is 100-140°C, and the time of the heat fixing is 10-120 seconds.
14. A method for manufacturing a cross-linked polyolefin separator, the cross-linked polyolefin separator comprising a cross-linked polyolefin porous substrate, the cross-linked polyolefin porous substrate comprising a plurality of fibrils and pores formed by entanglement of the fibrils with each other, wherein polyolefin chains forming the fibrils are directly cross-linked with each other, the method comprising the following steps: applying a Type 2 photoinitiator composition including a Type 2 photoinitiator to an uncrosslinked polyolefin porous substrate; and The polyolefin porous substrate coated with the type 2 photoinitiator composition is irradiated with ultraviolet light at a rate of 10-2500 mJ / cm 2 dose of UV radiation, and In the frequency-loss / storage modulus curve, within the frequency range of the cross-linked polyolefin separator of 1 rad / s or less, the cross-linked polyolefin separator shows a ratio (A / B) of storage modulus (G', storage modulus) (A) to loss modulus (G", loss modulus) (B) of 2 or more, the horizontal axis of the curve is the frequency (rad / s) of the cross-linked polyolefin separator converted into a logarithmic scale, the vertical axis of the curve is the storage modulus (G', storage modulus) (A) and loss modulus (G", loss modulus) (B) of the cross-linked polyolefin separator converted into a logarithmic scale, and the storage modulus is 1.2×10 5 to 1.0×10 7 Pa.
15. The method for manufacturing a cross-linked polyolefin separator according to claim 14, wherein the type 2 photoinitiator comprises thioxanthone (TX), thioxanthone derivatives, benzophenone (BPO), benzophenone derivatives, or a mixture of two or more thereof. 16 . The method for manufacturing a cross-linked polyolefin separator according to claim 14 , wherein the concentration of the type 2 photoinitiator in the type 2 photoinitiator composition is 0.01-0.3 wt %.