Polyimide composition, resin film, laminate, cover film, copper foil with resin, metal-clad laminate, and circuit board

The dielectric loss tangent of thermoplastic polyimide in high-frequency environments is solved by combining a high-quality aliphatic diamine and amino compounds by combining thermoplastic polyimide with low acid value polystyrene elastomer resin. The problem of properties is that the resin film with low loss tangent and high peel strength is achieved, which is suitable for high-frequency electronic equipment.

CN114656874BActive Publication Date: 2024-11-26NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111336066.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-23
Filing Date
2021-11-11
Publication Date
2024-11-26
Estimated Expiration
2041-11-11

AI Technical Summary

Technical Problem

The existing thermoplastic polyimide resins are difficult to meet the low dielectric loss tangent and excellent adhesion at the same time in high frequency environments, which affects the signal transmission performance of electronic devices.

Method used

A composition of thermoplastic polyimide and a polystyrene elastomer resin having an acid value of 10 mgKOH/g or less, containing 40 mol% or more of aliphatic diamine and an amino compound having at least two primary amino groups, and a specific Molar ratio and process processing form a resin film with low dielectric loss tangent and high peel strength.

Benefits of technology

It realizes low dielectric loss tangent and excellent adhesion of the resin film in high-frequency environment, and is suitable for electronic equipment for high-speed signal transmission, improving the reliability and structural stability of the electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003349149530000031
    Figure BDA0003349149530000031
  • Figure BDA0003349149530000181
    Figure BDA0003349149530000181
  • Figure BDA0003349149530000191
    Figure BDA0003349149530000191
Patent Text Reader

Abstract

The present invention provides a polyimide composition, a resin film, a laminate, a cover film, a copper foil with a resin, a metal-clad laminate and a circuit substrate, which use a thermoplastic polyimide to form a resin film having both low dielectric loss tangent and excellent adhesion. A polyimide composition contains (A) a thermoplastic polyimide and (B) a polystyrene elastomer resin having an acid value of less than 10 mgKOH / g, and relative to 100 parts by weight of the (A) component, the content of the (B) component is within the range of more than 10 parts by weight and less than 100 parts by weight. After the thermoplastic resin layer obtained by filming the polyimide composition is humidified under constant temperature and humidity conditions of 23°C and 50%RH for 24 hours, the dielectric loss tangent (Tanδ) at 10GHz measured by a separation dielectric resonator (SPDR) is less than 0.0020.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyimide composition which is effectively used as an adhesive in a circuit substrate such as a printed wiring board, a resin film, a laminate, a cover film, a copper foil with a resin, a metal-clad laminate, and a circuit substrate. Background Art

[0002] In recent years, with the development of miniaturization, lightness and space saving of electronic equipment, the demand for flexible printed circuits (FPC) that are thin, light, flexible and have excellent durability even when bent repeatedly has increased. FPC can be installed three-dimensionally and with high density even in a limited space, so its use is expanding to the wiring of the movable parts of electronic equipment such as hard disk drives (HDD), digital video disks (DVD), mobile phones, etc., or parts such as cables and connectors.

[0003] In addition to the high density, the high performance of the equipment is also constantly developing, so it is also necessary to deal with the high frequency of the transmission signal. In information processing or information communication, in order to transmit and process large-capacity information, efforts to improve the transmission frequency have been made, requiring the printed substrate material to reduce the transmission loss by the thinning of the insulating layer and the improvement of the dielectric properties of the insulating layer. In the future, for the insulating layer (including the adhesive layer) constituting the FPC, it is increasingly required to reduce the transmission loss and deal with the high frequency. About the improvement of the dielectric properties of the printed substrate material, a kind of adhesive composition containing acid-modified polystyrene elastomer resin, carbodiimide resin and epoxy resin (for example, patent documentation 1) is proposed. But, in patent documentation 1, if the acid value of the acid-modified polystyrene elastomer resin is low, then the compatibility with other components is reduced, resulting in not showing bonding strength. In addition, although it is related to the adhesive for fixing the semiconductor wafer on the support when grinding, a kind of adhesive composition containing acid-modified polystyrene elastomer resin (for example, patent documentation 2) is proposed.

[0004] In addition, it is proposed that a thermoplastic polyimide with a diamine compound derived from an aliphatic diamine such as dimer acid (dimer fatty acid) as a raw material and a cross-linked polyimide resin obtained by reacting an amino compound having at least two primary amino groups as a functional group is applied to the adhesive layer of the cover film (for example, patent document 3). In the embodiment of patent document 3, it is also disclosed that flaky talc is deployed in a thermoplastic polyimide composition with an aliphatic diamine as a raw material. Here, dimer acid is, for example, a dimerized fatty acid obtained by using natural fatty acids such as soybean oil fatty acid, tall oil fatty acid, rapeseed oil fatty acid and oleic acid, linoleic acid, linolenic acid, erucic acid, etc., which are refined from them, and performing Diels-Alder reaction, and it is known that the polyacid compound derived from dimer acid can be obtained as a raw material fatty acid or a composition of a fatty acid of trimerization or more (for example, patent document 4).

[0005] [Prior art literature]

[0006] [Patent Document]

[0007] [Patent Document 1] Japanese Patent No. 6705456

[0008] [Patent Document 2] International Publication No. WO2013 / 153904

[0009] [Patent Document 3] Japanese Patent No. 5777944

[0010] [Patent Document 4] Japanese Patent Application Publication No. 2017-137375 Summary of the invention

[0011] [Problems to be solved by the invention]

[0012] Thermoplastic polyimide made from aliphatic diamine is a resin material that can be effectively used as an adhesive because it is soluble in solvents, has excellent adhesion and good workability. However, in order to cope with the future development of high frequencies, in addition to satisfying the above-mentioned various characteristics, it is also required to further reduce the dielectric loss tangent.

[0013] Therefore, an object of the present invention is to provide a polyimide composition capable of forming a resin film having both low dielectric loss tangent and excellent adhesiveness using a thermoplastic polyimide.

[0014] [Technical means to solve the problem]

[0015] The polyimide composition of the present invention contains the following components (A) and (B);

[0016] (A) thermoplastic polyimide, and

[0017] (B) a polystyrene elastomer resin having an acid value of 10 mgKOH / g or less,

[0018] The content of the component (B) is in the range of 10 parts by weight or more and 100 parts by weight or less relative to 100 parts by weight of the component (A).

[0019] In the polyimide composition of the present invention, the content ratio of the styrene unit in the component (B) may be within a range of 10% by weight or more and 65% by weight or less.

[0020] In the polyimide composition of the present invention, the thermoplastic polyimide may be obtained by reacting a tetracarboxylic anhydride component with a diamine component, and may contain 40 mol % or more of an aliphatic diamine based on the diamine component.

[0021] The polyimide composition of the present invention may be a dimer diamine composition in which the aliphatic diamine is mainly composed of a dimer diamine in which both terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups.

[0022] The polyimide composition of the present invention may further contain an amino compound having at least two primary amino groups as functional groups.

[0023] The resin film of the present invention is a resin film comprising a thermoplastic resin layer, wherein:

[0024] The thermoplastic resin layer contains the following components (A) and (B);

[0025] (A) Thermoplastic polyimide,

[0026] and

[0027] (B) a polystyrene elastomer resin having an acid value of 10 mgKOH / g or less,

[0028] The content of the component (B) is in the range of 10 parts by weight or more and 100 parts by weight or less relative to 100 parts by weight of the component (A).

[0029] In the resin film of the present invention, the thermoplastic resin layer may have a dielectric loss tangent (Tanδ) of 0.0020 or less at 10 GHz measured by split post dielectric resonators (SPDR) after humidity conditioning at 23°C and 50% RH for 24 hours.

[0030] The laminated body of the present invention is a laminated body comprising a substrate and an adhesive layer laminated on at least one surface of the substrate, wherein the adhesive layer includes the resin film.

[0031] The cover film of the present invention is a cover film having a cover film material layer and an adhesive layer laminated on the cover film material layer, wherein the adhesive layer includes the resin film.

[0032] The resin-attached copper foil of the present invention is a copper foil with resin in which an adhesive layer and a copper foil are laminated, wherein the adhesive layer includes the resin film.

[0033] The metal-clad laminate of the present invention is a metal-clad laminate having an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, wherein at least one layer of the insulating resin layer includes the resin film.

[0034] The circuit board of the present invention is obtained by subjecting the metal layer of the metal-clad laminate to wiring processing.

[0035] [Effects of the Invention]

[0036] Polyimide composition of the present invention contains thermoplastic polyimide and polystyrene elastomer resin with specific acid number, therefore can be formed in maintaining low dielectric loss tangent with practical sufficient peel strength of excellent adhesiveness resin film.Therefore, polyimide composition of the present invention and resin film, for example, in the electronic equipment of needs high-speed signal transmission, can be particularly preferably used as the circuit substrate material of FPC etc.In addition, by improving the dielectric properties of resin film, can be applied to the receiver of direct conversion (direct conversion) mode.And then, owing to can improve the peel strength of resin film, therefore as the low dielectric adhesive with high reliability, can be applied to the electronic equipment of all structures. DETAILED DESCRIPTION

[0037] Hereinafter, embodiments of the present invention will be described.

[0038] [Polyimide composition]

[0039] The polyimide composition according to one embodiment of the present invention contains the following components (A) and (B);

[0040] (A) thermoplastic polyimide, and

[0041] (B) A polystyrene elastomer resin having an acid value of 10 mgKOH / g or less.

[0042] <Component (A): Thermoplastic Polyimide>

[0043] The thermoplastic polyimide as component (A) is a thermoplastic polyimide with solvent solubility, and is obtained by imidizing a polyamic acid as a precursor obtained by reacting a tetracarboxylic anhydride component with a diamine component. In addition, the so-called "thermoplastic polyimide" generally refers to a polyimide that softens by heating, solidifies by cooling, can repeat the above process, and can clearly confirm the glass transition temperature (Tg), but in the present invention, it refers to a polyimide in which the glass transition temperature can be clearly confirmed in a temperature range of less than 150°C. In addition, from the perspective of thermocompression bonding at low temperatures, it is preferably a polyimide in which the glass transition temperature can be clearly confirmed in a temperature range of less than 100°C, and more preferably a storage elastic coefficient of 1.0×10 at 30°C measured using a dynamic viscoelasticity measuring device (dynamic mechanical analyzer (dynamic mechanical analyzer, DMA)). 8 Pa or above, and the storage elastic coefficient at the glass transition temperature + 30°C is less than 3.0×10 7 In addition, the so-called "non-thermoplastic polyimide" generally refers to a polyimide that does not show softening and adhesiveness even when heated, but in the present invention, it refers to a polyimide having a storage elastic modulus of 1.0×10 at 30°C measured using a dynamic viscoelasticity measuring device (DMA). 9 Pa or more, and the storage elastic modulus at 300°C is 3.0×10 8 Pa or more polyimide.

[0044] (Tetracarboxylic anhydride component)

[0045] The thermoplastic polyimide as the component (A) may contain tetracarboxylic acid residues derived from tetracarboxylic anhydride generally used in thermoplastic polyimide without particular limitation, but preferably contains 90 mol% or more of tetracarboxylic acid residues derived from tetracarboxylic anhydride represented by the following general formula (1) relative to all tetracarboxylic acid residues. By containing 90 mol% or more of tetracarboxylic acid residues derived from tetracarboxylic anhydride represented by the following general formula (1) relative to all tetracarboxylic acid residues, it is easy to achieve a balance between the flexibility and heat resistance of the polyimide and it is preferred. When the total amount of tetracarboxylic acid residues derived from tetracarboxylic anhydride represented by the following general formula (1) is less than 90 mol%, there is a tendency for the solvent solubility of the polyimide to decrease.

[0046] [Chemistry 1]

[0047]

[0048] In the general formula (1), X represents a single bond or a divalent group selected from the following formulae.

[0049] [Chemistry 2]

[0050] -CO-, -SO2-, -O-,

[0051] -C(CF3)2-,

[0052] -COO- or -COO-Z-OCO-

[0053] In the above formula, Z represents -C6H4-, -(CH2)n- or -CH2-CH(-OC(=O)-CH3)-CH2-, and n represents an integer of 1 to 20.

[0054] Examples of the tetracarboxylic anhydride represented by the general formula (1) include 3,3′,4,4′-biphenyltetracarboxylic dianhydride (BPDA), 3,3′,4,4′-benzophenonetetracarboxylic dianhydride (BTDA), 3,3′,4,4′-diphenylsulfonetetracarboxylic dianhydride (DSDA), 4,4′-oxydiphthalic anhydride (ODPA), 4,4′-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), p-phenylenebis(trimellitic acid monoester anhydride) (TAHQ), and ethylene glycol bis(trimellitic acid monoester anhydride) (TMEG). Among these, when 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) is used, the adhesion of the polyimide can be improved. In addition, when the ketone group present in the molecular skeleton reacts with the amino group of the amino compound used for crosslinking formation described later to form a C=N bond, the effect of improving heat resistance is easily exhibited. From this viewpoint, it is preferable to contain a tetravalent tetracarboxylic acid residue (BTDA residue) derived from BTDA in an amount of preferably 50 mol% or more, more preferably 60 mol% or more, relative to all tetracarboxylic acid residues.

[0055] The thermoplastic polyimide as the component (A) may contain a tetracarboxylic acid residue derived from an acid anhydride other than the tetracarboxylic acid anhydride represented by the general formula (1) as long as the effect of the invention is not impaired. Such a tetracarboxylic acid residue is not particularly limited, and examples thereof include pyromellitic acid dianhydride, 2,3′,3,4′-biphenyltetracarboxylic acid dianhydride, 2,2′,3,3′-benzophenonetetracarboxylic acid dianhydride or 2,3,3′,4′-benzophenonetetracarboxylic acid dianhydride, 2,3′,3,4′-diphenylethertetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, 3,3″,4,4″-triphenylenetetracarboxylic acid dianhydride, 2,3,3″,4″-triphenylenetetracarboxylic acid dianhydride or 2,2″,3,3″-triphenylenetetracarboxylic acid dianhydride, 2,2-bis(2,3-dicarboxyphenyl)ether dianhydride 1,2,7,8-phenanthrene-tetracarboxylic dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride, 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 2,3,6,7-anthracene-tetracarboxylic dianhydride, 1,2,4-dicarboxyphenyl-propane dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride, 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-phenanthrene-tetracarboxylic dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride, 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 1,2,3,6,7-anthracene-tetracarboxylic dianhydride, 1,2,4-dicarboxyphenyl-propane ...7,8-phenanthrene-tetracarboxylic dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride, 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 1,2,3,6,7-anthracene-tetracar acid dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 2,3,5,6-cyclohexane dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-(or 1,4,5,8-)tetrachloronaphthalene-1,4,5,8- A tetracarboxylic acid residue derived from an aromatic tetracarboxylic acid dianhydride such as cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride and 4,4′-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride.

[0056] (Diamine component)

[0057] Thermoplastic polyimide as (A) component preferably uses a diamine component containing preferably 40 mol % or more, more preferably 60 mol % or more aliphatic diamine as raw material relative to all diamine components. That is, the thermoplastic polyimide as (A) component preferably contains diamine residues derived from aliphatic diamines preferably 40 mol % or more, more preferably 60 mol % or more relative to all diamine residues. By containing diamine residues derived from aliphatic diamines with the amount, the dielectric properties of polyimide can be improved, and the improvement of the thermocompression bonding properties brought about by the low temperature (low Tg) of the glass transition temperature of polyimide and the low elastic coefficient can be relaxed to internal stress. When the diamine residue derived from aliphatic diamines relative to all diamine residues is less than 40 mol %, there is a situation where the improvement effect of dielectric loss tangent and thermocompression bonding properties cannot be fully obtained. Here, as the aliphatic diamine, for example, a dimer diamine composition mainly composed of a dimer diamine in which both terminal carboxylic acid groups of a dimer acid are substituted with a primary aminomethyl group or an amino group, hexamethylenediamine, dodecanediamine, cyclohexanediamine, polyoxyalkyleneamine, 4,4-diaminodicyclohexylmethane, etc. can be used, and a dimer diamine composition is particularly preferred.

[0058] (Dimer diamine composition)

[0059] The dimer diamine composition contains the following component (a) as a main component, and the amounts of the component (b) and the component (c) are controlled.

[0060] (a) Dimer diamine

[0061] The so-called dimer diamine as component (a) refers to a diamine in which the two terminal carboxylic acid groups (-COOH) of the dimer acid are substituted with primary aminomethyl groups (-CH2-NH2) or amino groups (-NH2). Dimer acid is a known dibasic acid obtained by intermolecular polymerization of unsaturated fatty acids. Its industrial production process has been roughly standardized in the industry, and is obtained by dimerizing unsaturated fatty acids with carbon numbers of 11 to 22 using clay catalysts, etc. Regarding the industrially obtained dimer acid, the main component is a dibasic acid with a carbon number of 36 obtained by dimerizing unsaturated fatty acids with a carbon number of 18 such as oleic acid, linoleic acid, and linolenic acid, and contains any amount of monomer acid (carbon number 18), trimer acid (carbon number 54), and other polymerized fatty acids with carbon numbers of 20 to 54, depending on the degree of purification. In addition, after the dimerization reaction, double bonds remain, but in the present invention, it is assumed that the dimer acid also contains an acid that is further hydrogenated to reduce the unsaturation. The dimer diamine as the component (a) can be defined as a diamine compound obtained by substituting the terminal carboxylic acid group of a dibasic acid compound having a carbon number of 18 to 54, preferably 22 to 44, with a primary aminomethyl group or an amino group.

[0062] As the characteristic of dimer diamine, the characteristic derived from dimer acid skeleton can be given. That is, dimer diamine is a huge molecule aliphatic with a molecular weight of about 560 to 620, so the molar volume of the molecule can be increased, and the polar group of the polyimide can be relatively reduced. It is believed that the characteristics of this dimer acid type diamine contribute to suppressing the reduction of the heat resistance of polyimide, while reducing relative dielectric constant and dielectric loss tangent, and improving dielectric properties. In addition, due to having two hydrophobic chains with two freely movable carbon numbers 7 to 9 and two chain aliphatic amino groups with a length close to carbon number 18, it is not only possible to give flexibility to polyimide, but also polyimide is set to an asymmetric chemical structure or a non-planar chemical structure, so it is believed that the low dielectric constant and low dielectric loss tangent of polyimide can be realized.

[0063] The dimer diamine composition is preferably one in which the content of the dimer diamine as the component (a) is increased to 96% by weight or more, preferably 97% by weight or more, and more preferably 98% by weight or more by a purification method such as molecular distillation. By setting the content of the dimer diamine as the component (a) to 96% by weight or more, the spread of the molecular weight distribution of the polyimide can be suppressed. In addition, if technically feasible, it is most preferred that the entirety (100% by weight) of the dimer diamine composition includes the dimer diamine as the component (a).

[0064] (b) a monoamine compound obtained by substituting the terminal carboxylic acid group of a monobasic acid compound having 10 to 40 carbon atoms with a primary aminomethyl group or an amino group;

[0065] The monoacid compound having a carbon number of 10 to 40 is a mixture of a monobasic unsaturated fatty acid having a carbon number of 10 to 20, which is derived from a raw material of dimer acid, and a monoacid compound having a carbon number of 21 to 40, which is a byproduct when producing dimer acid. The monoamine compound is a compound obtained by substituting the terminal carboxylic acid group of the monoacid compound with a primary aminomethyl group or an amino group.

[0066] The monoamine compound as component (b) is a component that suppresses the increase in molecular weight of polyimide. During the polymerization of polyamic acid or polyimide, the monofunctional amino group of the monoamine compound reacts with the terminal anhydride group of polyamic acid or polyimide, thereby sealing the terminal anhydride group and suppressing the increase in molecular weight of polyamic acid or polyimide.

[0067] (c) an amine compound obtained by substituting the terminal carboxylic acid group of a polyacid compound having a hydrocarbon group in the range of 41 to 80 carbon atoms with a primary aminomethyl group or an amino group (except the dimer diamine);

[0068] The polybasic acid compound having a hydrocarbon group in the range of 41 to 80 carbon atoms is a polybasic acid compound having as a main component a tribasic acid compound in the range of 41 to 80 carbon atoms, which is a byproduct when producing dimer acid. In addition, a polymerized fatty acid other than the dimer acid in the range of 41 to 80 carbon atoms may be contained. The amine compound is a compound obtained by substituting the terminal carboxylic acid group of the polybasic acid compound with a primary aminomethyl group or an amino group.

[0069] The amine compound as component (c) is a component that promotes the increase in the molecular weight of the polyimide. The triamine body derived from trimer acid as the main component of the trifunctional or higher amino group reacts with the terminal acid anhydride group of the polyamic acid or polyimide to increase the molecular weight of the polyimide sharply. In addition, the amine compound derived from the polymerized fatty acid other than the dimer acid having 41 to 80 carbon atoms also increases the molecular weight of the polyimide and becomes the cause of the gelation of the polyamic acid or polyimide.

[0070] When the dimer diamine composition is quantitatively measured by gel permeation chromatography (GPC), a sample treated with acetic anhydride and pyridine is used to easily confirm the peak start, peak top and peak end of each component of the dimer diamine composition, and cyclohexanone is used as an internal standard substance. The sample prepared in the above manner is used to quantify each component by the area percentage of the chromatogram of GPC. The peak start and peak end of each component can be used as the minimum value of each peak curve and used as a reference to calculate the area percentage of the chromatogram.

[0071] In addition, in the dimer diamine composition used in the present invention, the total content of component (b) and component (c) is preferably 4% or less, preferably less than 4%, in terms of area percentage of the chromatogram obtained by GPC measurement. By setting the total content of component (b) and component (c) to 4% or less, the spread of the molecular weight distribution of the polyimide can be suppressed.

[0072] In addition, the area percentage of the chromatogram of the component (b) is preferably 3% or less, more preferably 2% or less, and further preferably 1% or less. By setting it to such a range, the decrease in the molecular weight of the polyimide can be suppressed, and the range of the molar ratio of the tetracarboxylic anhydride component and the diamine component can be expanded. In addition, the component (b) may not be included in the dimer diamine composition.

[0073] In addition, the area percentage of the chromatogram of the component (c) is preferably 2% or less, preferably 1.8% or less, and more preferably 1.5% or less. By setting it to this range, the molecular weight of the polyimide can be suppressed from increasing sharply, and the dielectric loss tangent of the resin film can be suppressed from rising at a frequency in a wide region. In addition, the component (c) may not be included in the dimer diamine composition.

[0074] In addition, when the ratio (b / c) of the area percentage of the chromatogram of component (b) and component (c) is 1 or more, the molar ratio of the tetracarboxylic anhydride component and the diamine component (tetracarboxylic anhydride component / diamine component) is preferably set to 0.97 or more and less than 1.0. By setting such a molar ratio, it is easier to control the molecular weight of the polyimide.

[0075] In addition, when the ratio (b / c) of the area percentage of the chromatogram of the component (b) and the component (c) is less than 1, the molar ratio of the tetracarboxylic anhydride component and the diamine component (tetracarboxylic anhydride component / diamine component) is preferably set to 0.97 or more and 1.1 or less. By setting such a molar ratio, it is easier to control the molecular weight of the polyimide.

[0076] The weight average molecular weight of the polyimide is preferably in the range of 10,000 to 200,000, for example. In addition, for example, when used as an adhesive for FPC, the weight average molecular weight of the polyimide is more preferably in the range of 20,000 to 150,000, and further preferably in the range of 40,000 to 150,000. When the weight average molecular weight of the polyimide is less than 20,000, there is a tendency for the resistance to fluidity to deteriorate. On the other hand, if the weight average molecular weight of the polyimide exceeds 150,000, the viscosity increases excessively and becomes insoluble in the solvent, and there is a tendency that the thickness of the adhesive layer is uneven, streaks, and other defects are easily generated during the coating operation.

[0077] The dimer diamine composition is preferably refined for the purpose of reducing the components other than the dimer diamine as (a) component. As a refining method, there is no particular limitation, and it is preferably a known method such as distillation or precipitation refining. The dimer diamine composition before refining can be obtained as a commercially available product, for example, PRIAMINE 1073 (trade name) manufactured by Croda Japan, PRIAMINE 1074 (trade name) manufactured by Croda Japan, PRIAMINE 1075 (trade name) manufactured by Croda Japan, etc.

[0078] Examples of diamine compounds other than aliphatic diamines used in polyimide include aromatic diamine compounds. Specific examples thereof include 1,4-diaminobenzene (p-PDA; p-phenylenediamine), 2,2′-dimethyl-4,4′-diaminobiphenyl (m-TB), 2,2′-n-propyl-4,4′-diaminobiphenyl (m-NPB), 4-aminophenyl-4′-aminobenzoate (APAB), 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)phenyl] methane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)]benzophenone, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 2,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3-aminophenoxy)phenyl]hexafluoropropane, 3,3′-dimethyl-4,4′-diaminobiphenyl, 4,4′-methylenebis-o-toluidine, 4,4′-methylenebis-2,6-dimethylaniline, 4,4′-methylenebis-2,6-diethylaniline, 3,3′-diaminodiphenylethane, 3 , 3′-diaminobiphenyl, 3,3′-dimethoxybenzidine, 3,3″-diamino-p-terphenyl, 4,4′-[1,4-phenylenebis(1-methylethylidene)]dianiline, 4,4′-[1,3-phenylenebis(1-methylethylidene)]dianiline, bis(p-aminocyclohexyl)methane, bis(p-β-amino-tert-butylphenyl) ether, bis(p-β-methyl-8-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis( diamine compounds such as β-amino-tert-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-phenylenediamine, p-phenylenediamine, 2,6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4-oxadiazole, piperazine, 2′-methoxy-4,4′-diaminobenzanilide, 4,4′-diaminobenzanilide, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 6-amino-2-(4-aminophenoxy)benzoxazole, and 1,3-bis(3-aminophenoxy)benzene.

[0079] Polyimide can be manufactured by reacting the tetracarboxylic anhydride component with a diamine component in a solvent to generate a polyamic acid and then heating the closed loop. For example, the tetracarboxylic anhydride component and the diamine component are dissolved in an organic solvent in approximately equimolar amounts, and the polymerization reaction is carried out by stirring for 30 minutes to 24 hours at a temperature in the range of 0°C to 100°C, thereby obtaining a polyamic acid as a precursor of the polyimide. During the reaction, the reaction components are dissolved in a manner such that the generated precursor becomes within the range of 5% by weight to 50% by weight, preferably within the range of 10% by weight to 40% by weight in the organic solvent. As the organic solvent used in the polymerization reaction, for example, N, N-dimethylformamide (DMF), N, N-dimethylacetamide (DMAc), N, N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethyl sulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, methylcyclohexane, dioxane, tetrahydrofuran, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), methanol, ethanol, benzyl alcohol, cresol etc. can be listed. These solvents can also be used in combination with two or more, and then the aromatic hydrocarbons such as xylene and toluene can also be used in combination. In addition, as the usage amount of this organic solvent, there is no particular restriction, and it is preferably adjusted to the usage amount of about 5 weight % to 50 weight % to be used in the concentration of the polyamic acid solution obtained by the polymerization reaction.

[0080] The synthesized polyamic acid is usually advantageously used as a reaction solvent solution, and can be concentrated, diluted or replaced with other organic solvents as needed. In addition, polyamic acid is generally advantageously used due to its excellent solvent solubility. The viscosity of the polyamic acid solution is preferably within the range of 500cps to 100,000cps. If it deviates from this range, it is easy to produce uneven thickness, stripes and other defects in the film when a coating operation is performed using a coating machine or the like.

[0081] The method for imidizing the polyamic acid to form the polyimide is not particularly limited, and for example, a heat treatment such as heating in the solvent at a temperature condition in the range of 80° C. to 400° C. for 1 to 24 hours can be preferably adopted. In addition, the temperature can be heated at a fixed temperature condition or the temperature can be changed in the middle of the step.

[0082] In the thermoplastic polyimide as the component (A), by selecting the types of the tetracarboxylic anhydride component and the diamine component, or the respective molar ratios when two or more tetracarboxylic anhydride components or diamine components are used, dielectric properties, thermal expansion coefficient, tensile elastic coefficient, glass transition temperature, etc. can be controlled. In addition, in the thermoplastic polyimide as the component (A), when there are a plurality of structural units of polyimide, they may exist in the form of blocks or randomly, preferably randomly.

[0083] The imide group concentration of the thermoplastic polyimide as component (A) is preferably 22% by weight or less, more preferably 20% by weight or less. Here, "imide group concentration" refers to the value obtained by dividing the molecular weight of the imide group (-(CO)2-N-) in the polyimide by the molecular weight of the entire structure of the polyimide. If the imide group concentration exceeds 22% by weight, the molecular weight of the resin itself becomes smaller, and the low hygroscopicity is also deteriorated due to the increase of polar groups, and Tg and tensile elastic coefficient increase.

[0084] The thermoplastic polyimide as component (A) is most preferably a fully imidized structure. Part of the polyimide may be amic acid. The imidization rate can be measured by using a Fourier transform infrared spectrophotometer (commercially available: manufactured by JASCO Corporation, trade name: FT / IR620) and using the attenuated total reflection (ATR) method to measure the infrared absorption spectrum of the polyimide film. -1 The benzene ring absorber nearby is used as the reference, starting from 1780cm -1 The absorbance derived from the C=O expansion and contraction of the imide group was calculated.

[0085] <Component (B): Polystyrene Elastomer Resin>

[0086] The polystyrene elastomer resin as component (B) is a copolymer of styrene or its derivatives and a conjugated diene compound, and includes hydrogenated products thereof. Here, styrene or its derivatives are not particularly limited, and examples thereof include styrene, methyl styrene, butyl styrene, divinyl benzene, vinyl toluene, etc. In addition, the conjugated diene compound is not particularly limited, and examples thereof include butadiene, isoprene, 1,3-pentadiene, etc.

[0087] The polystyrene elastomer resin is preferably hydrogenated. Hydrogenation further improves thermal stability, makes it less likely to undergo decomposition, polymerization, or other changes, and improves aliphatic properties, thereby improving compatibility with the thermoplastic polyimide as the component (A).

[0088] The copolymer structure of the polystyrene elastomer resin as the component (B) may be a block structure or a random structure. Preferred specific examples of the polystyrene elastomer resin include styrene-butadiene-styrene block copolymer (SBS), styrene-butadiene-butylene-styrene block copolymer (SBBS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-ethylene-ethylene / propylene-styrene block copolymer (SEEPS), etc., but are not limited to these specific examples.

[0089] The acid value of the polystyrene elastomer resin as (B) component is below 10mgKOH / g, preferably below 1mgKOH / g, more preferably 0mgKOH / g. By allocating the polystyrene elastomer resin with an acid value of below 10mgKOH / g in the polyimide composition, the dielectric loss tangent when forming the resin film can be reduced, and good peel strength can be maintained. On the other hand, if the acid value exceeds 10mgKOH / g, the dielectric properties deteriorate due to the increase of the polar group, and the compatibility variation with the (A) component deteriorates, and the adhesion when forming the resin film is reduced. Therefore, the lower the acid value, the better, and the resin (that is, the resin with an acid value of 0mgKOH / g) not modified by acid is most suitable as (B) component of the present invention. In the present invention, when the thermoplastic polyimide as the component (A) contains a residue derived from an aliphatic diamine, excellent adhesion can be exhibited. Therefore, even if a polystyrene elastomer resin that has not been acid-modified (i.e., having strong aliphatic properties) is used, a decrease in adhesive strength as is feared in Patent Document 1 can be avoided.

[0090] The polystyrene elastomer resin as component (B) preferably has a styrene unit [-CH2CH(C6H5)-] content ratio in the range of 10 wt% to 65 wt%, more preferably in the range of 20 wt% to 65 wt%, and most preferably in the range of 30 wt% to 60 wt%. When the content ratio of the styrene unit in the polystyrene elastomer resin is less than 10 wt%, the elastic modulus of the resin decreases, and the operability as a film deteriorates. If it increases to more than 65 wt%, the resin becomes rigid and difficult to use as an adhesive. In addition, the rubber component in the polystyrene elastomer resin decreases, resulting in deterioration of dielectric properties.

[0091] In addition, by making the content ratio of styrene units within the above range, the proportion of aromatic rings in the resin film becomes higher. Therefore, when through holes (through holes) and blind holes are formed by laser processing in the process of using the resin film to manufacture circuit substrates, the absorption in the ultraviolet region can be improved, and the laser processability can be further improved.

[0092] The weight average molecular weight of the polystyrene elastomer resin as the component (B) is, for example, preferably in the range of 50,000 to 300,000, and more preferably in the range of 80,000 to 270,000. If the weight average molecular weight of the component (B) is lower than the above range, the effect of improving the dielectric properties may be reduced. On the contrary, if it is higher than the above range, the viscosity of the polyimide composition becomes high, and the production of the resin film may become difficult.

[0093] The polystyrene elastomer resin as the component (B) may be a commercially available product as long as the acid value is 10 mgKOH / g or less. As such commercially available polystyrene elastomer resin, for example, A1535HU (trade name), G1652MU (trade name), G1726VS (trade name), G1645VS (trade name), FG1901GT (trade name), G1650MU (trade name), G1654HU (trade name), G1730VO (trade name), MD1653MO (trade name), etc. manufactured by KRATON can be preferably used.

[0094] [Amount]

[0095] In the polyimide composition, (B) component is in the range of more than 10 parts by weight and less than 100 parts by weight relative to the content of (A) component 100 parts by weight, preferably in the range of more than 20 parts by weight and less than 90 parts by weight, more preferably in the range of more than 30 parts by weight and less than 80 parts by weight. If (B) component is less than 10 parts by weight relative to the content of (A) component 100 parts by weight, there is a situation where the effect of reducing dielectric loss tangent is not fully shown. On the other hand, if the weight ratio of (B) component exceeds 100 parts by weight, the adhesion when forming resin film is reduced, and the solid content concentration in the polyimide composition becomes too high and viscosity rises, and there is a situation where operability is reduced.

[0096] [Optional Ingredients]

[0097] When the thermoplastic polyimide as component (A) has a ketone group, a crosslinked structure can be formed by reacting the ketone group with an amino group of an amino compound having at least two primary amino groups as functional groups (sometimes referred to as "crosslinking forming amino compound" in this specification) to form a C=N bond. By forming a crosslinked structure, the heat resistance of the thermoplastic polyimide forming the adhesive layer can be improved. Therefore, the polyimide composition of the present embodiment can contain a crosslinking forming amino compound as an optional component.

[0098] As a tetracarboxylic anhydride preferred for forming a polyimide having a keto group, for example, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) can be mentioned, and as a diamine compound, for example, aromatic diamines such as 4,4'-bis(3-aminophenoxy)benzophenone (BABP) and 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene (BABB) can be mentioned. For the purpose of forming a crosslinked structure, the polyimide composition of the present embodiment is particularly preferably composed of a thermoplastic polyimide as the (A) component and an amino compound for crosslink formation, wherein the thermoplastic polyimide contains BTDA residues derived from BTDA in an amount of preferably 50 mol% or more, more preferably 60 mol% or more, relative to all tetracarboxylic acid residues.

[0099] As the amino compound for crosslinking formation, there can be exemplified: (I) dihydrazide compounds, (II) aromatic diamines, (III) aliphatic amines, etc. Among them, dihydrazide compounds are preferred. Aliphatic amines other than dihydrazide compounds are easy to form crosslinked structures even at room temperature, which is worrying about the storage stability of varnishes. On the other hand, aromatic diamines need to be set to high temperature in order to form crosslinked structures. In this way, when using dihydrazide compounds, both the storage stability of varnishes and the shortening of curing time can be taken into account. As the dihydrazide compound, for example, dihydrazide compounds such as oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, diglycolic acid dihydrazide, tartaric acid dihydrazide, malic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, 2,6-naphthoic acid dihydrazide, 4,4-diphenyl dihydrazide, 1,4-naphthoic acid dihydrazide, 2,6-pyridine dihydrazide, and itaconic acid dihydrazide are preferred. The above dihydrazide compounds may be used alone or in combination of two or more.

[0100] Furthermore, the amino compounds such as (I) dihydrazide compounds, (II) aromatic diamines, and (III) aliphatic amines may be used in combination of two or more, for example, a combination of (I) and (II), a combination of (I) and (III), and a combination of (I) and (II) and (III).

[0101] In addition, from the viewpoint of making the network structure formed by crosslinking using the crosslinking amino compound denser, the molecular weight of the crosslinking amino compound used in the present invention (the weight average molecular weight when the crosslinking amino compound is an oligomer) is preferably 5,000 or less, more preferably 90 to 2,000, and further preferably 100 to 1,500. Among them, a crosslinking amino compound having a molecular weight of 100 to 1,000 is particularly preferred. If the molecular weight of the crosslinking amino compound is less than 90, one amino group of the crosslinking amino compound is limited to forming a C=N bond with the ketone group of the polyimide resin, and the surrounding of the remaining amino group becomes sterically bulky, so there is a tendency that the remaining amino group is not easy to form a C=N bond.

[0102] In the case of crosslinking the ketone group in the thermoplastic polyimide as the component (A) with the crosslinking amino compound, the crosslinking amino compound is added to the resin solution containing the component (A) to cause the ketone group in the thermoplastic polyimide to undergo a condensation reaction with the primary amino group of the crosslinking amino compound. Through the condensation reaction, the resin solution is cured to become a cured product. In the case, the amount of the crosslinking amino compound added can be 0.004 mol to 1.5 mol, preferably 0.005 mol to 1.2 mol, more preferably 0.03 mol to 0.9 mol, and most preferably 0.04 mol to 0.6 mol, relative to 1 mol of the ketone group. Regarding the addition amount of the cross-linking amino compound such that the total primary amino group is less than 0.004 mol relative to 1 mol of keto group, since the cross-linking by the cross-linking amino compound is insufficient, there is a tendency that the heat resistance after curing is difficult to exhibit. If the addition amount of the cross-linking amino compound exceeds 1.5 mol, the unreacted cross-linking amino compound acts as a thermoplastic agent, and there is a tendency to reduce the heat resistance of the adhesive layer.

[0103] The conditions for the condensation reaction for crosslink formation are not particularly limited as long as the ketone group in the thermoplastic polyimide as component (A) reacts with the primary amino group of the amino compound for crosslink formation to form an imine bond (C=N bond). Regarding the temperature of the heating condensation, for reasons such as releasing the water generated by the condensation to the outside of the system or simplifying the condensation step when the heating condensation reaction is carried out after the synthesis of the thermoplastic polyimide as component (A), it is preferably in the range of 120°C to 220°C, and more preferably in the range of 140°C to 200°C. The reaction time is preferably about 30 minutes to 24 hours. The end point of the reaction can be determined, for example, by using a Fourier transform infrared spectrophotometer (commercially available product: FT / IR620 manufactured by JASCO Corporation) to measure the infrared absorption spectrum and using 1670cm -1 The absorption peaks at 1635 cm-1 and 1635 cm-2 derived from the ketone groups in the polyimide resin decrease or disappear. -1 This was confirmed by the appearance of an absorption peak derived from an imine group nearby.

[0104] The heat condensation of the ketone group of the thermoplastic polyimide as the component (A) and the primary amino group of the crosslink-forming amino compound can be performed, for example, by the following method.

[0105] (1) A method in which an amino compound for crosslinking is added immediately after the synthesis (imidization) of the thermoplastic polyimide as the component (A) and heating is performed;

[0106] (2) A method in which an excess amount of an amino compound is added as a diamine component in advance, and immediately after the synthesis (imidization) of the thermoplastic polyimide as the component (A), the remaining amino compound that does not participate in the imidization or amidation is used as an amino compound for crosslinking formation and heated together with the thermoplastic polyimide; or

[0107] (3) A method of heating a polyimide composition to which a crosslink-forming amino compound is added after processing it into a predetermined shape (for example, after coating it on an arbitrary substrate or forming it into a film).

[0108] The case where an imide bond is formed in the formation of a cross-linked structure in order to impart heat resistance to the thermoplastic polyimide as the component (A) has been described, but the present invention is not limited to this. Regarding the method for curing the thermoplastic polyimide as the component (A), for example, a compound having an unsaturated bond such as an epoxy resin, an epoxy resin hardener, maleimide or an activated ester resin or a resin having a styrene skeleton may be formulated for curing.

[0109] In the polyimide composition of the present embodiment, inorganic fillers, organic fillers, plasticizers, hardening accelerators, coupling agents, pigments, flame retardants, etc. can be appropriately prepared as arbitrary components within the scope of the effect of the invention as needed. Here, as inorganic fillers, for example, silicon dioxide, aluminum oxide, beryllium oxide, niobium oxide, titanium oxide, magnesium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum fluoride, calcium fluoride, magnesium fluoride, gallium silicofluoride, phosphinate metal salts, etc. can be listed. They can be used one or mixed with two or more. In addition, as an arbitrary component, for example, other resin components such as epoxy resin, fluororesin, olefin resin, etc. can also be prepared.

[0110] And then, the polyimide composition of the present embodiment can contain organic solvents and other solvents.Because the thermoplastic polyimide as (A) component has solvent solubility, and the polystyrene elastomer resin as (B) component also shows good solubility in aromatic hydrocarbon solvents such as dimethylbenzene and toluene, the polyimide composition of the present embodiment can be prepared into a polyimide solution (varnish) containing solvent.As organic solvent, for example, preferably use will be selected from N, N-dimethylformamide (DMF), N, N-dimethylacetamide (DMAc), N, N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethyl sulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, cresol etc. one or more and the aromatic hydrocarbon solvent mixed with any ratio mixed solvent.

[0111] The content of the solvent is not particularly limited, but is preferably adjusted so that the concentration of the polyamic acid or polyimide becomes approximately 5% by weight to 30% by weight.

[0112] [Viscosity]

[0113] The viscosity of the polyimide composition is preferably within a range of 3000 cps to 100000 cps, more preferably within a range of 5000 cps to 50000 cps, as a viscosity range that improves the workability when applying the polyimide composition and facilitates forming a coating film of uniform thickness. If the viscosity deviates from the above range, defects such as uneven thickness and streaks are likely to occur in the film when applying the composition using a coater or the like.

[0114] [Preparation of polyimide composition]

[0115] The polyimide composition can be prepared, for example, by mixing a polystyrene elastomer resin with a resin solution of a thermoplastic polyimide prepared using an arbitrary solvent. At this time, in order to uniformly mix the thermoplastic polyimide and the polystyrene elastomer resin, the polystyrene elastomer resin may be mixed in a state where the polystyrene elastomer resin is dissolved in a solvent, or a solvent having high solubility in the polystyrene elastomer resin may be added.

[0116] The polyimide composition of the present embodiment is a polyimide composition having excellent flexibility and thermoplasticity when used to form an adhesive layer. Therefore, for example, in FPC, rigid / flexible circuit substrates, etc., it has preferred properties in applications such as adhesive layer materials and adhesives for cover films to protect wiring portions.

[0117] [Resin film]

[0118] The resin film of this embodiment is a single-layer or multi-layer resin film including a thermoplastic resin layer, wherein the thermoplastic resin layer is formed by filming the solid content (remaining part after removing the solvent) of the polyimide composition as a main component. That is, the thermoplastic resin layer contains component (A) and component (B);

[0119] (A) Thermoplastic polyimide,

[0120] and

[0121] (B) a polystyrene elastomer resin having an acid value of 10 mgKOH / g or less,

[0122] The content of the component (B) is in the range of 10 parts by weight to 100 parts by weight based on 100 parts by weight of the component (A). The resin film of this embodiment has excellent high frequency characteristics and excellent adhesion (particularly peel strength).

[0123] The resin film of this embodiment is not particularly limited as long as it is a film of an insulating resin containing the thermoplastic resin layer. It may be a film (sheet) containing only an insulating resin, or a film of an insulating resin in a state of being laminated on a substrate such as a resin sheet such as a copper foil, a glass plate, a polyimide film, a polyamide film, or a polyester film.

[0124] (Relative dielectric constant)

[0125] The resin film of this embodiment preferably has a relative dielectric constant (ε) of 3.3 or less, more preferably 3.1 or less at 10 GHz after being conditioned at a constant temperature and humidity of 23°C and 50% RH for 24 hours in order to ensure impedance matching when used in a circuit substrate such as an FPC and to reduce the loss of electric signals. If the relative dielectric constant exceeds 3.3, for example, when used in a circuit substrate such as an FPC, it is easy to cause an undesirable situation such as loss of electric signals in the transmission path of high-frequency signals.

[0126] (Dielectric loss tangent)

[0127] In addition, in order to reduce the loss of electric signals when used in circuit substrates such as FPC, the resin film of the present embodiment preferably has a dielectric loss tangent (Tanδ) of 0.0020 or less, and more preferably 0.0018 or less at 10 GHz after humidity adjustment for 24 hours under constant temperature and humidity conditions of 23°C and 50%RH, in order to reduce the loss of electric signals when used in circuit substrates such as FPC. If the dielectric loss tangent exceeds 0.0020, for example, when used in circuit substrates such as FPC, it is easy to cause disadvantages such as loss of electric signals in the transmission path of high-frequency signals.

[0128] (Glass transition temperature)

[0129] The glass transition temperature (Tg) of the resin film of this embodiment is preferably 250°C or less, and more preferably in the range of 40°C or more and 200°C or less. When the Tg of the resin film is 250°C or less, thermocompression bonding can be performed at low temperatures, thereby relieving the internal stress generated during lamination and suppressing dimensional changes after circuit processing. If the Tg of the resin film exceeds 250°C, the temperature will then increase, and there is a concern that the dimensional stability after circuit processing will be impaired.

[0130] (thickness)

[0131] The thickness of the resin film of the present embodiment is preferably within a range of 5 μm to 125 μm, and more preferably within a range of 8 μm to 100 μm. If the thickness of the resin film is less than 5 μm, there is a concern that wrinkles and other defects may occur during the transportation of the resin film during the manufacture of the resin film, while on the other hand, if the thickness of the resin film exceeds 125 μm, there is a concern that the productivity of the resin film may be reduced.

[0132] (tensile elastic coefficient)

[0133] The tensile modulus of elasticity of the resin film of the present embodiment is preferably within a range of 0.1 GPa to 3.0 GPa, more preferably within a range of 0.2 GPa to 2.0 GPa, from the viewpoints of reducing wrinkles, preventing inclusion of bubbles during lamination, and handling properties.

[0134] (Maximum elongation)

[0135] From the viewpoint of flexibility and crack prevention when used as an insulating resin layer of an FPC, the maximum elongation of the resin film of the present embodiment is preferably within a range of 30% to 200%, more preferably within a range of 60% to 160%.

[0136] The resin film of this embodiment has low dielectric loss tangent and excellent adhesion, and is therefore effectively used as an adhesive layer in a cover film, an adhesive layer in a circuit substrate, a multilayer circuit substrate, a copper foil with a resin, a substrate bonding sheet, a pure adhesive bonding sheet, etc.

[0137] [Laminated body]

[0138] The laminated body of one embodiment of the present invention comprises a substrate and an adhesive layer laminated on at least one surface of the substrate, wherein the adhesive layer comprises the resin film. In addition, the laminated body may comprise any layer other than the above. As the substrate in the laminated body, for example, a substrate of an inorganic material such as copper foil and a glass plate; or a substrate of a resin material such as a polyimide film, a polyamide film, and a polyester film can be cited.

[0139] Preferred embodiments of the laminate include a coverlay film, a copper foil with resin, and the like.

[0140] [Cover film]

[0141] A cover film as one embodiment of the laminate includes a cover film material layer as a base material and an adhesive layer laminated on one side of the cover film material layer, wherein the adhesive layer includes the resin film. The cover film may include any layer other than the above.

[0142] The material of the covering film material layer is not particularly limited, and for example, polyimide films such as polyimide resin, polyetherimide resin, polyamide-imide resin, or polyamide films, polyester films, etc. can be used. Among them, it is preferred to use a polyimide film with excellent heat resistance. In addition, in order to effectively show light-shielding properties, concealment, design, etc., the covering film material may also contain a black pigment, and in addition, any component such as a matte pigment that suppresses the surface gloss can be included within the range that does not damage the improvement effect of the dielectric properties.

[0143] The thickness of the covering film material layer is not particularly limited, but is preferably within a range of 5 μm to 100 μm, for example.

[0144] The thickness of the adhesive layer is not particularly limited, but is preferably within a range of 10 μm to 75 μm, for example.

[0145] The cover film of the present embodiment can be produced by the method exemplified below.

[0146] First, as a first method, a varnish-like polyimide composition containing a solvent is applied to one surface of a covering film material layer and then dried at a temperature of, for example, 80° C. to 180° C. to form an adhesive layer, thereby forming a covering film having a covering film material layer and an adhesive layer.

[0147] In addition, as a second method, a varnish-like polyimide composition containing a solvent is coated on an arbitrary substrate, and then dried at a temperature of, for example, 80°C to 180°C and then peeled off to form a resin film for an adhesive layer. The resin film and a covering film material layer are heat-pressed together at a temperature of, for example, 60°C to 220°C to form a covering film.

[0148] [Copper foil with resin]

[0149] The copper foil with resin as another embodiment of the laminate is formed by laminating an adhesive layer on at least one side of a copper foil as a base material, and the adhesive layer includes the resin film. In addition, the copper foil with resin of this embodiment may include any layer other than the above.

[0150] The thickness of the adhesive layer in the copper foil with resin is preferably in the range of 2μm to 125μm, and more preferably in the range of 2μm to 100μm. If the thickness of the adhesive layer is less than the lower limit, problems such as insufficient adhesion may occur. On the other hand, if the thickness of the adhesive layer exceeds the upper limit, undesirable conditions such as reduced dimensional stability may occur. In addition, from the perspective of low dielectric constant and low dielectric loss tangent, it is preferred that the thickness of the adhesive layer be set to 3um or more.

[0151] The material of the copper foil in the copper foil with resin is preferably a material with copper or copper alloy as the main component. The thickness of the copper foil is preferably 35 μm or less, and more preferably in the range of 5 μm to 25 μm. From the viewpoint of production stability and handling properties, the lower limit of the thickness of the copper foil is preferably set to 5 μm. In addition, the copper foil may be a rolled copper foil or an electrolytic copper foil. In addition, as the copper foil, a commercially available copper foil may also be used.

[0152] The copper foil with resin can be prepared, for example, by sputtering a metal on a resin film to form a seed layer, and then forming a copper layer by copper plating, or by laminating a resin film and a copper foil by a method such as thermocompression bonding. Furthermore, the copper foil with resin can be prepared by casting a coating liquid of a polyimide composition, drying to form a coating film, and then performing a desired heat treatment in order to form an adhesive layer on the copper foil.

[0153] [Metal-clad laminate]

[0154] (First Embodiment)

[0155] The metal-clad laminate according to one embodiment of the present invention includes an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, wherein at least one insulating resin layer includes the resin film. The metal-clad laminate according to this embodiment may include any layer other than the above.

[0156] (Second Embodiment)

[0157] The metal-clad laminate of another embodiment of the present invention is, for example, a so-called three-layer metal-clad laminate including an insulating resin layer, an adhesive layer laminated on at least one side of the insulating resin layer, and a metal layer laminated on the insulating resin layer via the adhesive layer, and the adhesive layer includes the resin film. In addition, the three-layer metal-clad laminate may include any layer other than the above. The adhesive layer of the three-layer metal-clad laminate can be arranged on one side or both sides of the insulating resin layer, and the metal layer can be arranged on one side or both sides of the insulating resin layer via the adhesive layer. That is, the three-layer metal-clad laminate may be a single-sided metal-clad laminate or a double-sided metal-clad laminate. A single-sided FPC or a double-sided FPC can be manufactured by etching the metal layer of the three-layer metal-clad laminate and performing wiring circuit processing.

[0158] The insulating resin layer in the three-layer metal-clad laminate is not particularly limited as long as it is composed of a resin having electrical insulation properties, and examples thereof include polyimide, epoxy resin, phenolic resin, polyethylene, polypropylene, polytetrafluoroethylene, silicone, ethylene-tetrafluoroethylene copolymer (ETFE), etc., preferably including polyimide. The polyimide layer constituting the insulating resin layer may be a single layer or a multilayer, and preferably includes a non-thermoplastic polyimide layer.

[0159] The thickness of the insulating resin layer in the three-layer metal-clad laminate is preferably in the range of 1 μm to 125 μm, and more preferably in the range of 5 μm to 100 μm. If the thickness of the insulating resin layer is less than the lower limit, problems such as failure to ensure sufficient electrical insulation may occur. On the other hand, if the thickness of the insulating resin layer exceeds the upper limit, the metal-clad laminate may be easily warped.

[0160] The thickness of the adhesive layer in the three-layer metal-clad laminate is preferably in the range of 0.1μm to 125μm, and more preferably in the range of 0.3μm to 100μm. In the three-layer metal-clad laminate of the present embodiment, if the thickness of the adhesive layer is less than the lower limit, problems such as insufficient adhesion may sometimes occur. On the other hand, if the thickness of the adhesive layer exceeds the upper limit, undesirable conditions such as reduced dimensional stability may occur. In addition, from the perspective of low dielectric constant and low dielectric loss tangent of the entire insulating layer of the laminate of the insulating resin layer and the adhesive layer, the thickness of the adhesive layer is preferably set to 3μm or more.

[0161] In addition, the ratio of the thickness of the insulating resin layer to the thickness of the adhesive layer (the thickness of the insulating resin layer / the thickness of the adhesive layer) is preferably in the range of 0.1 to 3.0, and more preferably in the range of 0.15 to 2.0. By setting such a ratio, the warping of the three-layer metal-clad laminate can be suppressed. In addition, the insulating resin layer may contain fillers as needed. As fillers, for example, silicon dioxide, aluminum oxide, magnesium oxide, beryllium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum fluoride, calcium fluoride, metal salts of organic phosphinates, etc. They can be used alone or in a mixture of two or more.

[0162] [Circuit board]

[0163] The circuit substrate of the embodiment of the present invention is formed by wiring the metal layer of the metal-clad laminate of any of the above-mentioned embodiments. One or more metal layers of the metal-clad laminate are processed into a pattern by conventional methods to form a wiring layer (conductor circuit layer), thereby manufacturing a circuit substrate such as an FPC. In addition, the circuit substrate may also include a cover film covering the wiring layer.

[0164] [Example]

[0165] The following examples are shown to more specifically describe the features of the present invention. Wherein, the scope of the present invention is not limited to the examples. In addition, in the following examples, unless otherwise specified, various measurements and evaluations are performed based on the following.

[0166] [Measurement of Weight Average Molecular Weight (Mw) of Polyimide]

[0167] The weight average molecular weight was measured by gel permeation chromatography (manufactured by Tosoh Corporation, trade name: HLC-8220GPC). Polystyrene was used as a standard substance, and tetrahydrofuran (THF) was used as a developing solvent.

[0168] [Determination of storage elastic modulus]

[0169] The measurement was performed using a dynamic viscoelasticity measuring apparatus (DMA: manufactured by TA Instruments, trade name: RSA-G2).

[0170] [Evaluation of Dielectric Properties]

[0171] Using a vector network analyzer (manufactured by Agilent, trade name: Vector Network Analyzer E8363C) and an SPDR resonator, the polyimide film (cured polyimide film) was placed under temperature: 23°C and humidity: 50% RH for 24 hours, and then the relative dielectric constant (ε) and dielectric loss tangent (Tanδ) at a frequency of 10 GHz were measured.

[0172] [Glass transition temperature (Tg)]

[0173] The adhesive sheet pressed under the conditions of temperature: 160°C, pressure: 3.5 MPa, and time: 60 minutes was cut into a test piece of 5 mm×20 mm size, and measured using a dynamic viscoelasticity measuring device (DMA: manufactured by TA Instrument, trade name: RSA-G2) from 30°C to 200°C at a heating rate of 4°C / min and a frequency of 11 Hz. The temperature at which the elastic modulus change (tanδ) was the maximum was defined as the glass transition temperature.

[0174] [Tensile elastic modulus and maximum elongation]

[0175] A tensile test was performed on a test piece of the resin film (width: 12.7 mm, length: 127 mm) at 50 mm / min using a tension tester (Tensilon manufactured by Orientec) to determine the tensile modulus of elasticity and the maximum elongation at 25°C.

[0176] [Solder heat resistance test (dry)]

[0177] The single copper foil of the double-sided copper-clad laminate (manufactured by NIPPON STEEL Chemical & Material, trade name: Espanex MB12-25-12UEG) was etched away, and the other copper foil surface was laminated with an adhesive sheet in the form of being sandwiched by copper foil, and pressed under the conditions of temperature: 160°C, pressure: 3.5MPa, and time: 60 minutes. After the test piece with copper foil was dried at 135°C / 60 minutes, it was immersed in a solder bath set to each evaluation temperature from 260°C in units of 10°C to 300°C for 10 seconds, and its bonding state was observed to confirm whether there were any adverse conditions such as foaming, expansion, and peeling. As a judgment, it was set as ○ (good) when no adverse conditions were confirmed at 280°C, and it was set as × (bad) when an adverse condition was confirmed.

[0178] [Solder heat resistance test (moisture absorption)]

[0179] The copper foil on one side of the double-sided copper-clad laminate (manufactured by NIPPON STEEL Chemical & Material, trade name: Espanex MB12-25-12UEG) was etched away, and the other copper foil surface was laminated with an adhesive sheet in the form of being sandwiched by copper foil, and pressed under the conditions of temperature: 160°C, pressure: 3.5MPa, and time: 60 minutes. After the test piece with copper foil was placed at 40°C and relative humidity: 90% RH for 72 hours, it was immersed in a solder bath set at each evaluation temperature from 240°C to 300°C in units of 10°C for 10 seconds, and its bonding state was observed to confirm whether there were any defects such as foaming, expansion, and peeling. As a judgment, it was set as ○ (good) when no defect was confirmed at 260°C, and × (bad) when a defect was confirmed.

[0180] [Determination of peel strength]

[0181] A double-sided copper-clad laminate (manufactured by NIPPON STEEL Chemical & Material Co., Ltd., trade name: Espanex MB12-25-12UEG) was cut into a width of 50 mm and a length of 100 mm, and then an adhesive sheet was placed on the copper foil side of the sample after etching away the copper foil on one side, and then a polyimide film (manufactured by Toray-Dupont Co., Ltd., trade name: Kapton 50EN-S) was laminated on the adhesive sheet, and pressed under the conditions of temperature: 160°C, pressure: 3.5 MPa, and time: 60 minutes to prepare a laminate. The laminate was cut into a 5 mm width test piece, and the test piece was stretched in a 180° direction at a speed of 50 mm / min using a tensile tester (manufactured by Toyo Seiki Seisaku-sho, trade name: Strograph VE). The peel strength between the adhesive layer and the copper foil at this time was measured and used as the peel strength.

[0182] [Evaluation method of film retention]

[0183] Cut the adhesive sheet into test pieces with a width of 20 mm and a length of 20 mm, fold it along the diagonal line to form a crease, and then unfold it to observe the state of the film. At this time, if there is no crack in the test piece after opening with the crease, it will be rated as "good", and if there is crack in part, it will be rated as "unacceptable".

[0184] [Evaluation method of film defects]

[0185] The polyimide varnish was applied to one side of a release-treated PET film, dried at 100°C for 5 minutes, and then dried at 120°C for 10 minutes, and the state of the film after peeling was observed. At this time, a film without interruptions (drag marks) caused by coagulation or poor solubility of the elastomer resin was rated as "good", and a film with interruptions was rated as "unacceptable".

[0186] [Acid value]

[0187] The acid value is the number of mg of potassium hydroxide (KOH) required to neutralize 1 g of sample. It is measured, for example, by the following method. First, accurately weigh the sample and put it into a 250 mL flask, add 50 mL of an equal volume mixture of ethanol or ethanol and ether, heat it to dissolve it, and titrate it with 0.1 N potassium hydroxide solution while shaking and mixing as needed (indicator: phenolphthalein). The endpoint of the titration is set to the point where the light red color of the liquid lasts for 30 seconds. Then, a blank test is performed by the same method for correction, and the value of the acid value is calculated according to the following formula.

[0188] Acid value = [0.1N potassium hydroxide solution consumption (mL) × 5.611] / [sample amount (g)]

[0189] The abbreviations used in the present examples represent the following compounds.

[0190] BTDA: 3,3',4,4'-benzophenonetetracarboxylic dianhydride

[0191] DDA: Distilled and purified PRIAMINE 1075 (trade name: Croda Japan Co., Ltd.) (component a: 99.2 wt%, component b: 0%, component c: 0.8%, amine value: 210 mgKOH / g)

[0192] N-12: Dodecanedioic acid dihydrazide

[0193] NMP: N-methyl-2-pyrrolidone

[0194] Elastomer resin 1: manufactured by Kraton Corporation, trade name: A1535HU (hydrogenated polystyrene elastomer resin, styrene unit content ratio 58% by weight, specific gravity: 0.96, no acid value)

[0195] Elastomer resin 2: manufactured by Kraton, trade name: G1652MU (hydrogenated polystyrene elastomer resin, styrene unit content 30% by weight, specific gravity: 0.91, no acid value)

[0196] Elastomer resin 3: manufactured by Kraton, trade name: G1726VS (hydrogenated polystyrene elastomer resin, styrene unit content ratio 30% by weight, specific gravity: 0.91, no acid value)

[0197] Elastomer resin 4: manufactured by Kraton, trade name: G1645VS (hydrogenated polystyrene elastomer resin, styrene unit content ratio 13% by weight, specific gravity: 0.89, no acid value)

[0198] Elastomer resin 5: manufactured by Kraton, trade name: FG1901GT (hydrogenated polystyrene elastomer resin, styrene unit content ratio 30% by weight, specific gravity: 0.91, acid value 10 mgKOH / g)

[0199] Elastomer resin 6: manufactured by Asahi Kasei Corporation, trade name: Tuftec M1913 (hydrogenated polystyrene elastomer resin, styrene unit content ratio 30% by weight, specific gravity: 0.91, acid value 11 mgKOH / g)

[0200] Elastomer resin 7: manufactured by Asahi Kasei Corporation, trade name: Tuftec M1943 (hydrogenated polystyrene elastomer resin, styrene unit content ratio 20% by weight, specific gravity: 0.91, acid value 11 mgKOH / g)

[0201] In the above-mentioned DDA, "%" of component a, component b, and component c refers to the area percentage of the chromatogram in the GPC measurement. The molecular weight of DDA is calculated by the following formula (1).

[0202] Molecular weight = 56.1 × 2 × 1000 / amine value (1)

[0203] (Synthesis example 1)

[0204] 55.51 g of BTDA (0.1721 mol), 94.49 g of DDA (0.1735 mol), 210 g of NMP and 140 g of xylene were placed in a 1000 ml separable flask and mixed thoroughly at 40° C. for 1 hour to prepare a polyamic acid solution. The polyamic acid solution was heated to 190° C., heated and stirred for 10 hours, and 125 g of xylene was added to prepare a polyimide solution 1 (solid content: 31% by weight, weight average molecular weight: 80,900, thermoplastic polyimide) after imidization.

[0205] [Example 1]

[0206] 1.12 g of N-12 and 7.8 g of elastomer resin 1 were mixed with 100 g of polyimide solution 1 prepared in Synthesis Example 1, and xylene was added to dilute and stir the mixture so that the solid content became 27 wt %, thereby preparing polyimide varnish 1a.

[0207] [Example 2 to Example 8]

[0208] Polyimide varnishes 2a to 8a were prepared in the same manner as in Example 1 except that elastomer resin 1, elastomer resin 2, elastomer resin 3, elastomer resin 4, and elastomer resin 5 were used and the blending amounts were changed as shown in Table 1.

[0209] Comparative Example 1, Comparative Example 2

[0210] Polyimide varnish 9a and polyimide varnish 10a were prepared in the same manner as in Example 1 except that the elastomer resin 6 and the elastomer resin 7 were used, the blending amounts were changed as shown in Table 1, and the solid content concentration of the polyimide varnish was set to 31% by weight.

[0211] Comparative Example 3

[0212] A polyimide varnish 11 a was prepared in the same manner as in Example 1 except that no elastomer was used and the solid content concentration of the polyimide varnish was changed to 31% by weight.

[0213] Tables 1 and 2 show the formulations of Examples 1 to 8 and Comparative Examples 1 to 3.

[0214] [Table 1]

[0215]

[0216]

[0217] [Example 9]

[0218] The polyimide varnish 1a prepared in Example 1 was applied to one surface of a release-treated PET film, dried at 100°C for 5 minutes, then dried at 120°C for 10 minutes and peeled off to prepare an adhesive sheet 1b (thickness: 25 μm).

[0219] Various evaluation results of the adhesive sheet 1b are as follows.

[0220] Relative dielectric constant: 2.5, dielectric loss tangent: 0.0018, tensile elastic modulus: 0.3GPa, maximum elongation: 136%, Tg: 41°C, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.5kN / m, film defects: good

[0221] [Example 10]

[0222] An adhesive sheet 2b was prepared in the same manner as in Example 9 using the polyimide varnish 2a.

[0223] Various evaluation results of the adhesive sheet 2b are as follows.

[0224] Relative dielectric constant: 2.5, dielectric loss tangent: 0.0015, tensile elastic modulus: 0.3GPa, maximum elongation: 195%, Tg: 43℃, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.4kN / m, film defects: good

[0225] [Example 11]

[0226] An adhesive sheet 3b was prepared in the same manner as in Example 9 using the polyimide varnish 3a.

[0227] Various evaluation results of the adhesive sheet 3b are as follows.

[0228] Relative dielectric constant: 2.5, dielectric loss tangent: 0.0013, tensile elastic modulus: 0.3GPa, maximum elongation: 230%, Tg: 42℃, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.3kN / m, film defects: good

[0229] [Example 12]

[0230] An adhesive sheet 4b was prepared in the same manner as in Example 9 using the polyimide varnish 4a.

[0231] Various evaluation results of the adhesive sheet 4b are as follows.

[0232] Relative dielectric constant: 2.6, dielectric loss tangent: 0.0018, tensile elastic modulus: 0.4GPa, maximum elongation: 118%, Tg: 40℃, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.5kN / m, film defects: good

[0233] [Example 13]

[0234] An adhesive sheet 5b was prepared in the same manner as in Example 9 using the polyimide varnish 5a.

[0235] Various evaluation results of the adhesive sheet 5b are as follows.

[0236] Relative dielectric constant: 2.8, dielectric loss tangent: 0.0017, tensile elastic modulus: 0.3GPa, maximum elongation: 144%, Tg: 40℃, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.6kN / m, film defects: good

[0237] [Example 14]

[0238] An adhesive sheet 6b was prepared in the same manner as in Example 9 using the polyimide varnish 6a.

[0239] Various evaluation results of the adhesive sheet 6b are as follows.

[0240] Relative dielectric constant: 2.6, dielectric loss tangent: 0.0018, tensile elastic modulus: 0.3GPa, maximum elongation: 103%, Tg: 42℃, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.4kN / m, film defects: good

[0241] [Example 15]

[0242] An adhesive sheet 7b was prepared in the same manner as in Example 9 using the polyimide varnish 7a.

[0243] Various evaluation results of the adhesive sheet 7b are as follows.

[0244] Relative dielectric constant: 2.6, dielectric loss tangent: 0.0020, tensile elastic modulus: 0.2GPa, maximum elongation: 103%, Tg: 41°C, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.4kN / m, film defects: good

[0245] [Example 16]

[0246] An adhesive sheet 8b was prepared in the same manner as in Example 9 using the polyimide varnish 8a.

[0247] Various evaluation results of the adhesive sheet 8b are as follows.

[0248] Relative dielectric constant: 2.6, dielectric loss tangent: 0.0019, tensile elastic modulus: 0.3GPa, maximum elongation: 122%, Tg: 41°C, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.2kN / m, film defects: good

[0249] Comparative Example 4

[0250] An adhesive sheet 9b was prepared in the same manner as in Example 9 using the polyimide varnish 9a.

[0251] Various evaluation results of the adhesive sheet 9b are as follows.

[0252] Relative dielectric constant: 2.8, dielectric loss tangent: 0.0022, tensile elastic modulus: 0.3GPa, maximum elongation: 201%, Tg: 43℃, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.6kN / m, film defect: unacceptable

[0253] Comparative Example 5

[0254] An adhesive sheet 10b was prepared in the same manner as in Example 9 using the polyimide varnish 10a.

[0255] Various evaluation results of the adhesive sheet 10b are as follows.

[0256] Relative dielectric constant: 2.8, dielectric loss tangent: 0.0022, tensile elastic modulus: 0.2GPa, maximum elongation: 185%, Tg: 41℃, film retention: good, solder heat resistance test (dry): ○, solder heat resistance test (moisture absorption): ○, peel strength: 1.4kN / m, film defect: unacceptable

[0257] Comparative Example 6

[0258] An adhesive sheet 11b was prepared in the same manner as in Example 9 using the polyimide varnish 11a.

[0259] Various evaluation results of the adhesive sheet 11b are as follows.

[0260] Relative dielectric constant: 2.6, dielectric loss tangent: 0.0021, tensile elastic modulus: 0.5GPa, maximum elongation: 119%, Tg: 44℃, film retention: good, solder heat resistance test (dry): ×, solder heat resistance test (moisture absorption): ×, peel strength: 1.0kN / m, film defects: good

[0261] The above results are summarized in Table 3.

[0262] [Table 3]

[0263]

[0264] According to Table 3, it is confirmed that the dielectric loss tangent of the adhesive sheets 1b to 8b of Examples 9 to 16 to which the elastomer resin 1, 2, 3, 4, and 5 are added is 0.0020 or less, and a high peel strength is obtained, and there is no film defect. According to such results, it is confirmed that the adhesive sheet as the resin film of the present embodiment can be expected to reduce the transmission loss in the high frequency band of about 10 GHz to 20 GHz, for example, and has excellent peel strength while maintaining flexibility and film retention.

[0265] As shown in the above examples, by adding a hydrogenated polystyrene elastomer resin having an acid value of 10 mgKOH / g or less to a polyimide made of an aliphatic diamine as a raw material, a clear improvement in dielectric properties and an improvement in peel strength are observed.

[0266] Furthermore, it was also confirmed that the adhesive sheet obtained in each Example maintained its film shape by using the hydrogenated polystyrene elastomer resin having an acid value of 10 mgKOH / g or less in a formulation amount within a practical range.

[0267] From the above results, it was confirmed that the resin film of the present embodiment can be suitably used as a material for a circuit board such as a high-frequency compatible FPC.

[0268] As mentioned above, although embodiment of this invention was described in detail for the purpose of illustration, this invention is not limited to the said embodiment, Various deformation|transformation is possible.

Claims

1. A polyimide composition comprising the following components (A) and (B); (A) thermoplastic polyimide, and (B) a polystyrene elastomer resin having an acid value of 10 mgKOH / g or less, The content of the component (B) is within a range of 10 parts by weight or more and 100 parts by weight or less relative to 100 parts by weight of the component (A). The content ratio of the styrene unit in the component (B) is within the range of 10 wt % or more and 65 wt % or less, The thermoplastic polyimide is obtained by reacting a tetracarboxylic anhydride component and a diamine component, and contains 40 mol % or more of an aliphatic diamine based on the diamine component.

2. The polyimide composition according to claim 1, wherein The aliphatic diamine is a dimer diamine composition having as a main component a dimer diamine in which both terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups. 3 . The polyimide composition according to claim 1 , further comprising an amino compound having at least two primary amino groups as functional groups.

4. A resin film comprising a thermoplastic resin layer, wherein the resin film is characterized in that: The thermoplastic resin layer contains the following components (A) and (B); (A) thermoplastic polyimide, and (B) a polystyrene elastomer resin having an acid value of 10 mgKOH / g or less, The content of the component (B) is within a range of 10 parts by weight or more and 100 parts by weight or less relative to 100 parts by weight of the component (A). The content ratio of the styrene unit in the component (B) is within the range of 10 wt % or more and 65 wt % or less, The thermoplastic polyimide is obtained by reacting a tetracarboxylic anhydride component and a diamine component, and contains 40 mol % or more of an aliphatic diamine based on the diamine component.

5. The resin film according to claim 4, wherein The thermoplastic resin layer has a dielectric loss tangent (Tan δ) of 0.0020 or less at 10 GHz measured by a separation dielectric resonator (SPDR) after humidity control for 24 hours at a constant temperature and humidity of 23° C. and 50% RH.

6. A laminate comprising: a substrate; and an adhesive layer laminated on at least one surface of the substrate, wherein the laminate is characterized in that: The adhesive layer includes the resin film according to claim 4 .

7. A covering film comprising: a covering film material layer; and an adhesive layer laminated on the covering film material layer, wherein the covering film is characterized in that: The adhesive layer includes the resin film according to claim 4 .

8. A copper foil with resin, which is formed by laminating an adhesive layer and a copper foil, wherein the copper foil with resin is characterized in that: The adhesive layer includes the resin film according to claim 4 .

9. A metal-clad laminate comprising: an insulating resin layer; and a metal layer laminated on at least one surface of the insulating resin layer, wherein: At least one layer of the insulating resin layer includes the resin film according to claim 4 . 10 . A circuit board obtained by subjecting the metal layer of the metal-clad laminate according to claim 9 to wiring processing.