A method for judging the anti-carburization performance of heat-resistant alloy furnace tubes

By conducting solid carburizing tests and multiple characterization analysis on heat-resistant alloy furnace pipes, the anti-carburizing performance coefficient is calculated, and the problem of lack of systematic evaluation methods in the existing technology is solved, and the accurate evaluation of the anti-carburizing performance of furnace pipes is achieved. , improves detection accuracy and reliability.

CN114659956BActive Publication Date: 2024-11-26HEFEI GENERAL MACHINERY RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210216625.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-07
Publication Date
2024-11-26
Estimated Expiration
2042-03-07

AI Technical Summary

Technical Problem

The existing technology lacks systematic, accurate and unified methods to judge the carburization resistance of heat-resistant alloy furnace tubes, which leads to easy damage to the ethylene cracking furnace tubes under high temperature, oxidation and carburization medium, and has a short service life, which brings petrochemical enterprises. Economic losses and safety hazards.

Method used

A method that includes cutting furnace tube samples, conducting solid carburization test, carbon content analysis, Vickers hardness test, low-magnitude etching test and metallographic microstructure observation is adopted to calculate the anti-carburization performance coefficient, and through various characterization methods Comprehensive analysis to judge the carburization resistance of furnace tubes.

Benefits of technology

By simulating the carburizing test during the service of the furnace tube, the anti-carburizing performance of the furnace tube is accurately judged, and the accidentality of a single characterization method is overcome, providing accurate judgments under different materials and temperature conditions, significantly improving the accuracy of the detection results. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114659956B_ABST
    Figure CN114659956B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for judging the anti-carburization performance of a heat-resistant alloy furnace tube. The method is mainly aimed at heat-resistant alloy furnace tubes for ethylene cracking furnaces. A carburization test is performed on furnace tube samples by a solid carburizing method. The furnace tube samples after the carburization test are sampled for carbon content analysis, Vickers hardness test, low-power acid etching test and metallographic microstructure observation to obtain the carburized layer thickness value of the furnace tube sample under each characterization method. The anti-carburization performance coefficient X of the furnace tube is obtained by weighted average comprehensive analysis of the carburized layer thickness values ​​obtained by the four characterization methods, which is used to judge the anti-carburization performance of the furnace tube. In the present invention, the carburized layer thickness is comprehensively characterized by four characterization methods, and the anti-carburization performance of the furnace tube can be accurately judged, overcoming the contingency brought by a single characterization method. The anti-carburization performance judging method of the present invention can be used for judging the anti-carburization performance of heat-resistant alloy furnace tubes of different materials under different temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carburizing test, and in particular relates to a method for judging the anti-carburizing performance of a heat-resistant alloy furnace tube. Background Art

[0002] The ethylene cracking furnace is the core equipment of the petrochemical ethylene unit, and the furnace tube is a key component in the ethylene cracking furnace. The cracking furnace tube has been in service for a long time in high temperature, oxidation and carburizing media and under various stress conditions, and is prone to various damages and failures. Among them, carburization of the cracking furnace tube is the most common and most harmful failure mode. Carburization will affect the strength of the furnace tube, causing the furnace tube material to deteriorate or even crack and fail, which will seriously affect the long-term safe operation of the entire unit. In recent years, in order to achieve high-temperature rapid heating and increase ethylene yield in the ethylene industry, there is a trend to reduce the tube diameter, which puts higher requirements on the anti-carburization performance of the furnace tube. However, the quality inspection process before the furnace tube products leave the factory does not examine the anti-carburization performance of the furnace tube. Many ethylene cracking furnace tubes put into use on the market have an actual service life of only one-third of the design life. Carburization failure accidents occur frequently, causing significant economic losses and safety hazards to petrochemical enterprises. Therefore, it is urgent to use anti-carburization performance as one of the inspection indicators in the purchase process of cracking furnace tubes.

[0003] However, since carburization occurs during long-term service under complex working conditions, the current research on carburization of heat-resistant alloy furnace tubes mainly focuses on the detection and characterization of the carburization degree of in-service furnace tubes, while there is no systematic, accurate and unified measurement and evaluation method for the anti-carburization performance of newly manufactured heat-resistant alloy furnace tubes. Summary of the invention

[0004] In order to solve the above technical problems, one of the purposes of the present invention is to provide a method for evaluating the anti-carburization performance of a heat-resistant alloy furnace tube, which method can systematically and accurately evaluate the anti-carburization performance of a heat-resistant alloy furnace tube.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for evaluating the anti-carburization performance of a heat-resistant alloy furnace tube comprises the following steps:

[0007] S1. For the heat-resistant alloy furnace tube to be evaluated, cut at least 2 tube sections with a length of 100 to 150 mm, seal both ends of the tube section and reserve a circular hole on the sealing surface of one end for adding a solid carburizing agent to make a furnace tube sample;

[0008] S2. Take one furnace tube sample as the control group and do not perform the carburizing test. The rest are taken as the test group and perform the solid carburizing test at 1000-1150℃ for 20-200h.

[0009] S3. Take samples of furnace tubes from the test group and the control group for carbon content analysis, Vickers hardness test, low-power acid etching test and metallographic microstructure observation test, and calculate the carburized layer thickness d of the furnace tube samples. α , carburized layer thickness value d of furnace tube sample β , carburized layer thickness value d of furnace tube sample γ , carburized layer thickness of furnace tube sample d δ ;

[0010] S4. Perform comprehensive analysis and calculation on the carburized layer thickness value obtained in step S3 to obtain the anti-carburization performance coefficient X of the furnace tube, which is calculated as X=100*(αd α +βd β +γd γ +δd δ ) / t, where α, β, γ, and δ are weighting coefficients, t is the duration of the high temperature carburizing test, α∈[0.15,0.25], β∈[0.15,0.25], γ∈[0.25,0.35], δ∈[0.25,0.35] and α+β+γ+δ=1.

[0011] As a further improvement of the evaluation method of the anti-carburization performance of heat-resistant alloy furnace tubes:

[0012] Preferably, if X≥1, the heat-resistant alloy furnace tube to be judged has weak carburization resistance; if 0.1≤X<1, the heat-resistant alloy furnace tube to be judged has secondary carburization resistance; if X<0.1, the heat-resistant alloy furnace tube to be judged has high carburization resistance.

[0013] Preferably, the specific method of the solid carburizing test in step S2 is:

[0014] a. Fill the inner cavity of the furnace tube sample with solid carburizing agent with a particle size of 1.5 to 3 mm from the circular hole reserved on the sealing surface of the furnace tube sample;

[0015] b. Carburize the furnace tube sample in step a by keeping it at 1000-1150°C for 20-200h.

[0016] Preferably, in step b, a box-type resistance furnace with a maximum temperature of 1200° C., a temperature measurement accuracy of ±1° C., and a temperature control accuracy of ±0.1° C. is used to perform a carburizing test on the furnace tube sample in step a.

[0017] Preferably, the method for carbon content analysis in step S3 is:

[0018] a. Take chip-like chemical composition samples layer by layer from the inner wall to the outer wall of the furnace tube samples of the test group and the control group;

[0019] b. The carbon content of the chemical composition sample in step a was analyzed by using a CS-800 carbon-sulfur analyzer to obtain the carbon content distribution of the furnace tube samples in the test group and the control group along the wall thickness direction, and the carburized layer thickness d of the furnace tube samples in the test group was obtained by comparison. α .

[0020] Preferably, the method of the Vickers hardness test in step S3 is:

[0021] a. Take full-wall-thickness block specimens from the furnace tube samples of the test group and the control group respectively;

[0022] b. After the samples were mounted, roughly ground, finely ground and polished, the Vickers hardness of the samples was measured along the wall thickness direction using a DVK-1S Vickers hardness tester to obtain the distribution of Vickers hardness of the samples in the test group and the control group along the wall thickness direction. The carburized layer thickness d of the furnace tube samples in the test group was measured by comparison. β .

[0023] Preferably, the method of the low-magnification acid etching test in step S3 is:

[0024] a. Cut a 10-15mm thick ring sample from the furnace tube sample of the test group by radial ring cutting;

[0025] b. According to the NACE TM0498-2014 standard, the ring sample was immersed in a mixed acid solution of 20wt.% HNO3 and 4wt.% HF for 2h, the carburized layer of the sample was observed, and the carburized layer thickness of the furnace tube sample was measured. γ .

[0026] Preferably, the method of the metallographic observation test in step S3 is:

[0027] a. Take full-wall-thickness block specimens from the furnace tube samples of the test group and the control group respectively;

[0028] b. After the sample cross section is coarsely ground, finely ground and polished, it is electrolytically etched with 10% oxalic acid solution for 15 to 30 seconds;

[0029] c. The ZEISS Supra40 scanning electron microscope was used to observe the metallographic structure of the entire cross section of the sample and the carburized layer thickness of the furnace tube sample was measured. δ .

[0030] The beneficial effects of the present invention are:

[0031] 1) In the present invention, a furnace tube sample is made to carry out a carburizing test, which accurately simulates the carburizing process of the inner wall of the furnace tube during service, and the accuracy of the test result is significantly better than that of the traditional test method.

[0032] 2) In the present invention, the carburized layer thickness is comprehensively characterized by four characterization methods, which can accurately determine the anti-carburization performance of the furnace tube and overcome the randomness caused by a single characterization method.

[0033] 3) The anti-carburization performance evaluation method of the present invention can be used to evaluate the anti-carburization performance of heat-resistant alloy furnace tubes of different materials under different temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a macroscopic schematic diagram of the furnace tube samples of Examples 1, 2 and 3.

[0035] Figure 2 This is the metallographic observation test result of the original state of the 1# furnace tube sample.

[0036] Figure 3 This is the carbon content distribution diagram of the cross section of the No. 1 furnace tube sample after carburizing test.

[0037] Figure 4 This is the Vickers hardness distribution diagram of the cross section of the 1# furnace tube sample after carburizing test.

[0038] Figure 5 The depth of the gray-black area on the cross section of the annular sample measured by low-power acid etching after the carburizing test of the furnace tube samples of Examples 1, 2, and 3 is the carburized layer thickness value d of the furnace tube sample γ .

[0039] Figure 6a This is the metallographic structure diagram of the No. 1 furnace tube sample after carburizing test, magnified 100 times; Figure 6b This is the metallographic structure diagram of the No. 1 furnace tube sample after carburizing test, magnified 1000 times.

[0040] Figure 7 The metallographic observation test results of the original state of the 2# furnace tube sample.

[0041] Figure 8 This is the carbon content distribution diagram of the cross section of the 2# furnace tube sample after carburizing test.

[0042] Fig. 9 This is the Vickers hardness distribution diagram of the cross section of the 2# furnace tube sample after carburizing test.

[0043] Fig.10a This is the metallographic structure diagram of the No. 2 furnace tube sample after carburizing test, magnified 100 times; Fig.10b This is the metallographic structure diagram of the 2# furnace tube sample after carburizing test, magnified 1000 times.

[0044] Fig.11 The metallographic observation test results of the original state of the 3# furnace tube sample.

[0045] Fig.12 This is the carbon content distribution diagram of the cross section of the 3# furnace tube sample after carburizing test.

[0046] Fig.13 This is the Vickers hardness distribution diagram of the cross section of the 3# furnace tube sample after carburizing test.

[0047] Fig.14a This is the metallographic structure diagram of the 3# furnace tube sample after carburizing test, magnified 100 times; Fig.14b This is the metallographic structure diagram of the 3# furnace tube sample after carburizing test, magnified 1000 times. DETAILED DESCRIPTION

[0048] The technical solution of the present invention will be clearly and completely described below in conjunction with an analysis example of the anti-carburization performance test of the traditional heat-resistant alloy furnace tubes and the new aluminum-containing heat-resistant alloy furnace tubes produced by Qingdao Xinlitong Industrial Co., Ltd.

[0049] The traditional heat-resistant alloy furnace tube samples and the new aluminum-containing heat-resistant alloy furnace tube samples produced by Qingdao Xinlitong Industrial Co., Ltd. are used as test objects. The materials of the traditional heat-resistant alloy furnace tube samples are 25Cr35NiNb+MA and 35Cr45NiNb+MA, and the material of the new aluminum-containing heat-resistant alloy furnace tube samples is named NH1949. The present invention simulates the carburization of the ethylene cracking furnace tube in the service process by filling a solid carburizing agent inside the furnace tube sample with one end sealed and the other end left with a hole, and then samples the furnace tube samples of the control group without carburizing test and the test group after carburizing test, respectively, and perform characterization analysis such as carbon content analysis, low-power acid etching test, metallographic observation test and Vickers hardness test, and comprehensively determine the anti-carburization performance coefficient of the furnace tube by combining multiple characterization analysis results, and then judge the anti-carburization performance of the sample furnace tube.

[0050] The calculation method of the anti-carburization performance coefficient is as follows: First, the carbon content analysis, Vickers hardness test and metallographic observation test of the control group furnace tube samples that have not been subjected to the carburizing test are carried out to obtain the initial carbon content C0, cross-sectional Vickers hardness value H0 and original cast structure photos of the control group furnace tube samples. Then, the carbon content analysis, low-power acid etching test, metallographic observation test and Vickers hardness test and other characterization analyses are carried out on the test group furnace tube samples after the carburizing test.

[0051] Carbon content analysis: Carbon content analysis was performed on the furnace tube samples of the test group. Chemical composition samples were taken at 1mm, 2mm, 3mm and 4mm from the inner wall of the furnace tube samples. The carbon content of these chemical composition samples was analyzed using a CS-800 carbon-sulfur analyzer to obtain the carbon content distribution of the furnace tube samples of the test group along the wall thickness direction. The carbon content of different parts of the furnace tube samples of the test group was compared with the initial carbon content C0 of the furnace tube samples of the control group to obtain the carburized layer thickness value d of the furnace tube samples of the test group. α The carburized layer thickness obtained by carbon content analysis test is not very accurate and can only be accurate to 1.0mm.

[0052] Vickers hardness test: Take full-wall block specimens from the test group furnace tube samples. After mounting, rough grinding, fine grinding and polishing, use DVK-1S Vickers hardness tester to measure the Vickers hardness of the specimen along the wall thickness direction. The Vickers hardness distribution of the specimen along the wall thickness direction is obtained, and compared with the Vickers hardness value H0 of the control group furnace tube sample to obtain the carburized layer thickness value d of the furnace tube sample. β .

[0053] Low-power acid etching test: A ring sample is obtained by radially cutting the furnace tube sample of the test group, and it is immersed in a mixed acid solution of 20wt.% HNO3 and 4wt.% HF for 2h. The carburized area on the sample will appear gray-black, while the non-carburized area still maintains a metallic luster. The carburized layer thickness value d of the furnace tube sample is obtained by measuring the depth of the gray-black area on the cross section of the ring sample. γ The carburized layer thickness obtained by low-magnification acid etching test has high accuracy, which can be accurate to 0.05mm.

[0054] Metallographic observation test: Take full-wall block metallographic specimens from the test group furnace tube samples. After rough grinding, fine grinding and polishing, use 10% oxalic acid solution for electrolytic etching for 15 to 30 seconds. Use ZEISS Supra40 scanning electron microscope to observe the metallographic structure of the full cross section of the specimen. Under the scanning electron microscope, the grain boundary carbides in the carburized area are coarse and massive, and there are fine white precipitation phases inside the coarse and massive grain boundary carbides. There is a certain boundary between the carburized layer and the uncarburized area. Based on this, the carburized layer thickness value d of the furnace tube sample can be measured. δ The thickness of the carburized layer obtained by metallographic observation test is highly accurate and can be accurate to micron level.

[0055] The carburized layer thickness values ​​obtained by the four characterization methods have large differences in accuracy. It is inaccurate to use the carburized layer thickness value obtained by a single characterization method to judge the anti-carburization performance of the furnace tube material. Considering the advantages and disadvantages of the four characterization methods, the calculation formula for determining the anti-carburization performance coefficient is X=100*(αd α +βd β +γd γ +δd δ ) / t, where α, β, γ, and δ are weighting coefficients, α∈[0.15,0.25], β∈[0.15,0.25], γ∈[0.25,0.35], δ∈[0.25,0.35] and α+β+γ+δ=1, and t is the duration of the carburizing test.

[0056] Example 1

[0057] 1) Qingdao Xinlitong Industrial Co., Ltd. produces a traditional heat-resistant alloy furnace tube made of 25Cr35NiNb+MA. In order to test its anti-carburization performance, a The furnace tube sample is numbered 1#. One end of the furnace tube sample is sealed and a hole is left on the other end. Figure 1 The carbon content of the original furnace tube sample is C0 = 0.532wt.%, and the cross-sectional Vickers hardness value is H0 = 218.5HV10. The original cast structure is as shown in Figure 2 shown.

[0058] 2) Fill the inner cavity of the furnace tube sample with solid carburizing agent, load it into the KSL-1200X-5L box-type resistance furnace, and carry out a solid carburizing test at 1100°C for a test time of t=200h.

[0059] 3) Carbon content analysis test results: The carbon content analysis results of different parts of the furnace tube samples after carburizing at 1100℃ for 200h are shown in Table 1 and Figure 3 As shown in the figure, it can be seen that the carbon content within 2mm of the inner wall of the 25Cr35NiNb+MA furnace tube sample increased significantly after carburizing at 1100℃ for 200h, that is, the carburized layer thickness d of the 25Cr35NiNb+MA furnace tube sample α =2.0mm.

[0060] Table 1 Carbon content analysis results of 1# furnace tube samples before and after carburizing test

[0061]

[0062] 4) Vickers hardness test results: The Vickers hardness test results of the radial cross section of the furnace tube sample after carburizing for 200 hours at 1100℃ are as follows: Figure 4 As shown in the figure, it can be seen that the Vickers hardness value within the 3.0mm range of the inner wall of the 25Cr35NiNb+MA furnace tube sample increases significantly after carburizing at 1100℃ for 200h, that is, the carburized layer thickness d of the 25Cr35NiNb+MA furnace tube sample β =3.0mm.

[0063] 5) Low-power acid etching test results: After carburizing for 200 hours at 1100℃, the furnace tube sample was cut along the radial direction to obtain a ring sample. The carburized layer thickness of the ring sample after low-power acid etching test was tested as follows: Figure 5 As shown, the carburized layer thickness d of the 25Cr35NiNb+MA furnace tube sample γ =2.5mm.

[0064] 6) Metallographic observation test results: The metallographic observation test results of the furnace tube sample after carburizing at 1100℃ for 200h are as follows: Figure 6a , Figure 6b As shown in Figure 6, the carbides at the grain boundaries in the carburized zone are coarser than those in the original cast structure, and white fine precipitates are found on the coarse carbides. Figure 6a , Figure 6bIt can be seen that the carburized layer thickness d of the 25Cr35NiNb+MA furnace tube sample is δ =1.75mm.

[0065] 7) The anti-carburization performance coefficient is calculated as follows:

[0066] Take α=0.2, β=0.2, γ=0.3, δ=0.3,

[0067] X=100*(αd α +βd β +γd γ +δd δ ) / t

[0068] =100*(0.2*2.0+0.2*3.0+0.3*2.5+0.3*1.75) / 200

[0069] =1.14

[0070] Since the anti-carburization performance coefficient X>1, it indicates that the 25Cr35NiNb+MA alloy furnace tube produced by the furnace tube manufacturer has weak anti-carburization performance at 1100℃.

[0071] The carburization degree of 6 first-pass tubes of BA-104 cracking furnace of Zhenhai Refining and Chemical Company of China Petroleum and Chemical Corporation, which have been in service for 4 years, were tested. The material of the first-pass tubes is 25Cr35NiNb+MA, which is supplied by Qingdao Xinlitong Industrial Co., Ltd. The test results show that the carburization degree of the 6 25Cr35NiNb+MA alloy furnace tubes in service is between 58% and 100%, indicating that the anti-carburization performance of 25Cr35NiNb+MA alloy furnace tubes is weak.

[0072] Example 2

[0073] 1) Qingdao Xinlitong Industrial Co., Ltd. produces a traditional heat-resistant alloy furnace tube made of 35Cr45NiNb+MA. In order to test its anti-carburization performance, a The furnace tube sample is numbered 2#. One end of the furnace tube sample is sealed and a hole is left on the other end. The schematic diagram is as follows Figure 1 The carbon content of the original furnace tube sample is C0 = 0.515wt.%, and the cross-sectional Vickers hardness value is H0 = 249.0HV10. The original cast structure is as follows Figure 7 shown.

[0074] 2) Fill the inner cavity of the furnace tube sample with solid carburizing agent, load it into the KSL-1200X-5L box-type resistance furnace, and carry out a solid carburizing test at 1100°C for a test time of t=200h.

[0075] 3) Carbon content analysis test results: The carbon content analysis results of different parts of the furnace tube samples after carburizing at 1100℃ for 200h are shown in Table 2 and Figure 8 As shown in the figure, it can be seen that the carbon content within the 2mm range of the inner wall of the 35Cr45NiNb+MA furnace tube sample increased significantly after carburizing at 1100℃ for 200h, that is, the carburized layer thickness d of the 35Cr45NiNb+MA furnace tube sample α =2.0mm.

[0076] Table 2 Carbon content analysis results of 2# furnace tube samples before and after carburizing test

[0077]

[0078] 4) Vickers hardness test results: The Vickers hardness test results of the radial cross section of the furnace tube sample after carburizing for 200 hours at 1100℃ are as follows: Fig. 9 As shown in the figure, it can be seen that the Vickers hardness value within the 2.0mm range of the inner wall of the 35Cr45NiNb+MA furnace tube sample increases significantly after carburizing for 200h at 1100℃, that is, the carburized layer thickness d of the 35Cr45NiNb+MA furnace tube sample β =2.0mm.

[0079] 5) Low-power acid etching test results: After carburizing for 200 hours at 1100℃, the furnace tube sample was cut along the radial direction to obtain a ring sample. The carburized layer thickness of the ring sample after low-power acid etching test was tested as follows: Figure 5 As shown, the carburized layer thickness d of the 35Cr45NiNb+MA furnace tube sample γ =2.0mm.

[0080] 6) Metallographic observation test results: The metallographic observation test results of the furnace tube sample after carburizing at 1100℃ for 200h are as follows: Fig.10a , Fig.10b As shown in Figure 10, the carbides at the grain boundaries in the carburized zone are coarser than those in the original cast structure, and white fine precipitates are found on the coarse carbides. Fig.10a , Fig.10b It can be seen that the carburized layer thickness d of the 35Cr45NiNb+MA furnace tube sample is δ =1.55mm.

[0081] 7) The anti-carburization performance coefficient is calculated as follows:

[0082] Take α=0.2, β=0.2, γ=0.3, δ=0.3,

[0083] X=100*(αd α +βd β +γd γ +δd δ ) / t

[0084] =100*(0.2*2.0+0.2*2.0+0.3*2.0+0.3*1.55) / 200

[0085] =0.93

[0086] Since the anti-carburization performance coefficient X is less than 1, it indicates that the 35Cr45NiNb+MA alloy furnace tube produced by the furnace tube manufacturing enterprise is anti-carburization at 1100°C. The carburization degree of 6 BA-104 cracking furnace second-pass tubes of the Zhenhai Refining and Chemical Company of China Petrochemical Corporation, which have been in service for 4 years, were tested. The second-pass tubes were made of 35Cr45NiNb+MA and supplied by Qingdao Xinlitong Industrial Co., Ltd. The test results showed that the carburization degree of the 6 35Cr45NiNb+MA service furnace tubes was between 16 and 43%, which was significantly better than the 58% to 100% of the 25Cr35NiNb+MA service furnace tubes, indicating that the anti-carburization performance of the 35Cr45NiNb+MA alloy furnace tube is better than that of the 25Cr35NiNb+MA alloy furnace tube.

[0087] Example 3

[0088] 1) Qingdao Xinlitong Industrial Co., Ltd. produces a new type of aluminum-containing heat-resistant alloy furnace tube, named NH1949. In order to test its anti-carburization performance, a The furnace tube sample is numbered 3#. One end of the furnace tube sample is sealed and a hole is left on the other end. The schematic diagram is as follows Figure 1 The carbon content of the original furnace tube sample is C0 = 0.460wt.%, and the cross-sectional Vickers hardness value is H0 = 368.2HV10. The original cast structure is as follows Fig.11 shown.

[0089] 2) Fill the inner cavity of the 3# furnace tube sample with solid carburizing agent, load it into the KSL-1200X-5L box-type resistance furnace, and conduct a solid carburizing test at 1100°C for a test time of t=200h.

[0090] 3) Carbon content analysis test results: The carbon content analysis results of different parts of the 3# furnace tube sample after carburizing at 1100℃ for 200h are shown in Table 3 and Fig.12 As shown in the figure, it can be seen that the carbon content within 1mm of the inner wall of the 3# furnace tube sample increased significantly after carburizing at 1100℃ for 200h, that is, the carburized layer thickness d of the 3# furnace tube sample α =1.0mm.

[0091] Table 3 Carbon content analysis results of 3# furnace tube samples before and after carburizing test

[0092]

[0093] 4) Vickers hardness test results: The Vickers hardness test results of the radial cross section of the furnace tube sample after carburizing for 200 hours at 1100℃ are as follows: Fig.13 As shown in the figure, it can be seen that the Vickers hardness value within the 1.5mm range of the inner wall of the 3# furnace tube sample increased significantly after carburizing at 1100℃ for 200h, that is, the carburized layer thickness d of the 3# furnace tube sample β =1.5mm.

[0094] 5) Low-power acid etching test results: The carburized layer thickness of the furnace tube ring specimen after carburizing at 1100℃ for 200h was measured by low-power acid etching test. Figure 5 As shown, the carburized layer thickness d of the 2# furnace tube sample γ =1.5mm.

[0095] 6) Metallographic observation test results: The metallographic observation test results of the furnace tube sample after carburizing at 1100℃ for 200h are as follows: Fig.14a , Fig.14b As shown in Figure 14, the carbides at the grain boundaries in the carburized zone are coarser than those in the original cast structure, and white fine precipitates are found on the coarse carbides. Fig.14a , Fig.14b It can be seen that the carburized layer thickness d of the 3# furnace tube sample is δ =1.44mm.

[0096] 7) The anti-carburization performance coefficient is calculated as follows:

[0097] Take α=0.2, β=0.2, γ=0.3, δ=0.3,

[0098] X=100*(αd α +βd β +γd γ +δd δ ) / t

[0099] =100*(0.2*1.0+0.2*1.5+0.3*1.5+0.3*1.44) / 200

[0100] =0.69

[0101] Since the anti-carburization performance coefficient is 0.1≤X<1, it indicates that the new aluminum-containing heat-resistant alloy furnace tube has secondary anti-carburization at 1100℃.

[0102] Those skilled in the art should understand that the above are only some specific embodiments of the present invention, rather than all embodiments. It should be noted that for those of ordinary skill in the art, many modifications and improvements can be made, and all modifications or improvements that do not exceed the scope of protection of the present invention should be regarded as.

Claims

1. A method for evaluating the anti-carburization performance of a heat-resistant alloy furnace tube, characterized in that The following steps are involved: S1. For the heat-resistant alloy furnace tube to be evaluated, cut at least 2 tube sections with a length of 100 to 150 mm, seal both ends of the tube section and reserve a circular hole on the sealing surface of one end for adding a solid carburizing agent to make a furnace tube sample; S2. Take one furnace tube sample as the control group and do not perform the carburizing test. The rest are taken as the test group and perform the solid carburizing test at 1000-1150℃ for 20-200h. S3. Take samples of furnace tubes from the test group and the control group for carbon content analysis, Vickers hardness test, low-power acid etching test and metallographic microstructure observation test, and calculate the carburized layer thickness d of the furnace tube samples. α , carburized layer thickness value d of furnace tube sample β , carburized layer thickness value d of furnace tube sample γ , carburized layer thickness of furnace tube sample d δ ; S4. Perform comprehensive analysis and calculation on the carburized layer thickness value obtained in step S3 to obtain the anti-carburization performance coefficient X of the furnace tube, which is calculated as X=100*(αd α +βd β +γd γ +δd δ ) / t, where α, β, γ, and δ are weighting coefficients, t is the duration of the high temperature carburizing test, α∈[0.15,0.25], β∈[0.15,0.25], γ∈[0.25,0.35], δ∈[0.25,0.35] and α+β+γ+δ=1.

2. The method for judging the anti-carburization performance of a heat-resistant alloy furnace tube according to claim 1, characterized in that: If X≥1, the heat-resistant alloy furnace tube to be judged is weakly anti-carburization; if 0.1≤X<1, the heat-resistant alloy furnace tube to be judged is secondary anti-carburization; if X<0.1, the heat-resistant alloy furnace tube to be judged is anti-carburization.

3. The method for judging the anti-carburization performance of a heat-resistant alloy furnace tube according to claim 1, characterized in that: The specific method of the solid carburizing test in step S2 is: a. Fill the inner cavity of the furnace tube sample with solid carburizing agent with a particle size of 1.5 to 3 mm from the circular hole reserved on the sealing surface of the furnace tube sample; b. Carburize the furnace tube sample in step a by keeping it at 1000-1150°C for 20-200h.

4. The method for judging the anti-carburization performance of a heat-resistant alloy furnace tube according to claim 3, characterized in that: In step b, a box-type resistance furnace with a maximum temperature of 1200°C, a temperature measurement accuracy of ±1°C, and a temperature control accuracy of ±0.1°C is used to perform a carburizing test on the furnace tube sample in step a.

5. The method for judging the anti-carburization performance of a heat-resistant alloy furnace tube according to claim 1, characterized in that: The method for carbon content analysis in step S3 is: a. Take chip-like chemical composition samples layer by layer from the inner wall to the outer wall of the furnace tube samples of the test group and the control group; b. The carbon content of the chemical composition sample in step a was analyzed by using a CS-800 carbon-sulfur analyzer to obtain the carbon content distribution of the furnace tube samples in the test group and the control group along the wall thickness direction, and the carburized layer thickness d of the furnace tube samples in the test group was obtained by comparison. α .

6. The method for judging the anti-carburization performance of a heat-resistant alloy furnace tube according to claim 1, characterized in that: The method of the Vickers hardness test in step S3 is: a. Take full-wall-thickness block specimens from the furnace tube samples of the test group and the control group respectively; b. After the samples were mounted, roughly ground, finely ground and polished, the Vickers hardness of the samples was measured along the wall thickness direction using a DVK-1S Vickers hardness tester to obtain the distribution of Vickers hardness of the samples in the test group and the control group along the wall thickness direction. The carburized layer thickness d of the furnace tube samples in the test group was measured by comparison. β .

7. The method for judging the anti-carburization performance of a heat-resistant alloy furnace tube according to claim 1, characterized in that: The method of the low-magnification acid etching test in step S3 is: a. Cut a 10-15mm thick ring sample from the furnace tube sample of the test group by radial ring cutting; b. According to the NACE TM0498-2014 standard, the ring sample was immersed in a mixed acid solution of 20wt.% HNO3 and 4wt.% HF for 2h, the carburized layer of the sample was observed, and the carburized layer thickness of the furnace tube sample was measured. γ .

8. The method for judging the anti-carburization performance of a heat-resistant alloy furnace tube according to claim 1, characterized in that: The method of the metallographic observation test in step S3 is: a. Take full-wall-thickness block specimens from the furnace tube samples of the test group and the control group respectively; b. After the sample cross section is coarsely ground, finely ground and polished, it is electrolytically etched with 10% oxalic acid solution for 15 to 30 seconds; c. The ZEISS Supra40 scanning electron microscope was used to observe the metallographic structure of the entire cross section of the sample and the carburized layer thickness of the furnace tube sample was measured. δ .