Resin composition, connection structure for solar power generation module, and junction box for solar power generation module
By adding specific proportions of polyphenylene ether resin, styrene resin, hydrogenated block copolymer and phosphate ester compound to the resin composition, a continuous phase structure is formed, which solves the problem of insufficient oil resistance of polyphenylene ether resin and realizes a resin composition with high oil resistance and flame retardancy, which is suitable for connection structure and junction box of solar power generation module.
Patent Information
- Application Number
- CN202111575787.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-01-07
- Filing Date
- 2021-12-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-21
AI Technical Summary
Existing polyphenylene ether resins have insufficient oil resistance and are prone to cracking or breaking when in contact with rust inhibitors, lubricants, etc. They also fall short in balancing high oil resistance and flame retardancy.
By adding specific proportions of polyphenylene ether resins, styrene resins, hydrogenated block copolymers, phosphate ester compounds, and polyolefin resins to a resin composition, a continuous phase structure is formed, optimizing the content of each component and the melt flow rate to improve oil resistance and flame retardancy.
This invention achieves a resin composition that balances high oil resistance and flame retardancy, making it suitable for connection structures and junction boxes of solar power generation modules.
Smart Images

Figure BDA0003423065800000021 
Figure BDA0003423065800000031 
Figure BDA0003423065800000051
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, a connection structure for a solar power generation module, and a junction box for a solar power generation module. Background Art
[0002] Conventionally, polyphenylene ether resins have excellent electrical insulation properties as well as heat resistance, hydrolysis resistance and flame retardancy, and therefore have been widely used in electrical and electronic components for secondary batteries or solar power generation, home appliances / OA equipment, and the like.
[0003] On the other hand, the polyphenylene ether resin composition has insufficient oil resistance, and may cause cracks or breakage due to contact with rust preventives attached to molds of molding machines, lubricating oils of various application parts, etc., which often becomes a problem.
[0004] To address such problems, Patent Document 1, for example, describes an oil-resistant resin composition having excellent heat resistance and flame retardancy, which is a resin composition composed of a polypropylene resin and a polyphenylene ether resin, wherein the continuous phase is the polypropylene resin.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2000-344974 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, there is still room for improvement in achieving both high oil resistance and flame retardancy.
[0010] Therefore, an object of the present invention is to provide a resin composition which can achieve both high oil resistance and flame retardancy.
[0011] Means for solving problems
[0012] The inventors have conducted intensive studies to solve the above-mentioned problems and have found that, in a resin composition containing (a) a polyphenylene ether resin or a mixed resin of a polyphenylene ether resin and a styrene resin, (b) a hydrogenated block copolymer, (c) a phosphate ester compound, and (d) a polyolefin resin having a specific melt flow rate, the above-mentioned problems can be advantageously solved by setting the content of each component within a specific range and forming a phase containing the component (a) as a continuous phase, thereby completing the present invention.
[0013] That is, the present invention is as follows.
[0014] A first aspect: A resin composition comprising:
[0015] (a) (a-1) a polyphenylene ether resin, or a mixed resin of (a-1) a polyphenylene ether resin and (a-2) a styrene resin;
[0016] (b) hydrogenated block copolymers;
[0017] (c) phosphate compounds; and
[0018] (d) polyolefin resins,
[0019] With respect to 100 parts by mass of the total of the above-mentioned component (a) and the above-mentioned component (b),
[0020] The amount of the component (a) is 60 to 90 parts by weight.
[0021] The amount of the component (b) is 10 to 40 parts by weight.
[0022] The amount of the component (c) is 8 to 25 parts by weight.
[0023] The amount of the component (d) is 1 to 10 parts by weight.
[0024] When the component (a) is the mixed resin, the amount of the polyphenylene ether resin (a-1) is 55 to 99.95 parts by mass based on 100 parts by mass of the mixed resin.
[0025] The melt flow rate of the component (d) is 30 g / 10 minutes or more,
[0026] The phase containing the above-mentioned component (a) forms a continuous phase.
[0027] Second aspect: The resin composition according to the first aspect, wherein the amount of the component (c) is 10 to 20 parts by mass based on 100 parts by mass of the total of the component (a) and the component (b).
[0028] A third aspect: The resin composition according to the first or second aspect, wherein the amount of the component (d) is 2 to 8 parts by mass based on 100 parts by mass of the total of the component (a) and the component (b).
[0029] A fourth aspect: The resin composition according to any one of the first to third aspects, wherein the component (c) is a phosphate ester compound represented by the following general formula (I) or (II).
[0030] [Chemistry 1]
[0031]
[0032] [Chemistry 2]
[0033]
[0034] (In the general formula (I), Q1, Q2, Q3 and Q4 independently represent an alkyl group having 1 to 6 carbon atoms, R11 and R12 represent a methyl group, and R13 and R14 independently represent a hydrogen atom or a methyl group.
[0035] In the general formula (II), Q1, Q2, Q3 and Q4 independently represent an alkyl group having 1 to 6 carbon atoms, and R11 and R12 represent a methyl group.
[0036] y is an integer greater than or equal to 1, n1 and n2 independently represent an integer from 0 to 2, and m1, m2, m3 and m4 independently represent an integer from 0 to 3.)
[0037] A fifth aspect: A connection structure for a solar power generation module, comprising a molded product of the resin composition according to any one of the first to fourth aspects.
[0038] A sixth aspect: A junction box for a solar power generation module, comprising a molded article of the resin composition according to any one of the first to fourth aspects.
[0039] Effects of the Invention
[0040] According to the present invention, a resin composition having both high oil resistance and flame retardancy can be obtained. DETAILED DESCRIPTION
[0041] The specific implementation of the present invention (hereinafter referred to as "this implementation") is described in detail below. The following implementation is an example for illustrating the present invention and is not intended to limit the present invention to the following content. The present invention can be implemented by appropriately deforming within the scope of its main points.
[0042] In the present embodiment, (a-1) polyphenylene ether resin, (a-2) styrene resin, (b) hydrogenated block copolymer, (c) phosphate ester compound and (d) polyolefin resin are sometimes referred to as component (a-1), component (a-2), component (b), component (c) and component (d), respectively. In addition, in the present embodiment, component (a-1) alone or component (a-1) and component (a-2) together are sometimes referred to as component (a).
[0043] In the present embodiment, the number average molecular weight refers to a value measured using a gel permeation chromatography measuring apparatus equipped with an ultraviolet spectroscopic detector and converted using standard polystyrene.
[0044] In the present embodiment, the melt flow rate (hereinafter sometimes referred to as "MFR") refers to the value obtained by measuring in accordance with JIS K7210. In this specification, as long as it is not otherwise described in JIS K7210 and the JIS standard of each resin, the measurement load of MFR is 2.16 kg. For example, the measurement conditions of MFR of polypropylene, polyethylene, ethylene-vinyl acetate copolymer and polybutene are respectively described in JIS K6921-2, JIS K6922-2, JIS K6924-2 and JIS K6925-2. In addition, for example, MFR (230°C, 2.16 kg) refers to the MFR measured under the conditions of a temperature of 230°C and a load of 2.16 kg. Regarding the measurement temperature of the melt flow rate, it is preferred to select an appropriate temperature according to the type of resin to be measured, for example, 230°C for polypropylene and 190°C for polyethylene. When the component (d) contains two or more different polyolefin resins, the measurement temperature is the measurement temperature of the polyolefin resin accounting for 50% or more of the total mass of the polyolefin resins.
[0045] Resin composition
[0046] The resin composition of this embodiment includes:
[0047] (a) (a-1) a polyphenylene ether resin, or a mixed resin of (a-1) a polyphenylene ether resin and (a-2) a styrene resin;
[0048] (b) hydrogenated block copolymers;
[0049] (c) phosphate compounds; and
[0050] (d) polyolefin resins,
[0051] With respect to 100 parts by mass of the total of the above-mentioned component (a) and the above-mentioned component (b),
[0052] The amount of the component (a) is 60 to 90 parts by weight.
[0053] The amount of the component (b) is 10 to 40 parts by weight.
[0054] The amount of the component (c) is 8 to 25 parts by weight.
[0055] The amount of the component (d) is 1 to 10 parts by weight.
[0056] When the component (a) is the mixed resin, the amount of the polyphenylene ether resin (a-1) is 55 to 99.95 parts by mass relative to 100 parts by mass of the mixed resin.
[0057] The melt flow rate of the component (d) is 30 g / 10 minutes or more,
[0058] The phase containing the above-mentioned component (a) forms a continuous phase.
[0059] (a)Ingredients
[0060] The component (a) in the present embodiment is (a-1) a polyphenylene ether-based resin, or a mixture of (a-1) a polyphenylene ether-based resin and (a-2) a styrene-based resin.
[0061] The component (a) may be one kind only or a combination of two or more kinds.
[0062] ·(a-1) Ingredient
[0063] As the component (a-1) contained in the resin composition of the present embodiment, a homopolymer composed of a structural unit of the following general formula (III) and a copolymer having a structural unit of the general formula (III) (hereinafter sometimes simply referred to as "polyphenylene ether") can be used.
[0064] [Chemistry 3]
[0065]
[0066] In the general formula (III), O is an oxygen atom, and R21 to R24 independently represent any one selected from the group consisting of a hydrogen atom, a halogen atom, a primary or secondary alkyl group having 1 to 8 carbon atoms, a phenyl group, a halogenated alkyl group, an aminoalkyl group, a hydrocarbon group, and a halogenated hydrocarbon group (in which at least two carbon atoms separate the halogen atom and the oxygen atom).
[0067] Examples of the homopolymer of the polyphenylene ether resin include, but are not limited to, poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), and poly(2,6-dichloro-1,4-phenylene ether).
[0068] Examples of copolymers of polyphenylene ether-based resins include, but are not limited to, copolymers of 2,6-dimethylphenol and other phenols (eg, copolymers with 2,3,6-trimethylphenol and copolymers with 2-methyl-6-butylphenol).
[0069] Among these, as the polyphenylene ether-based resin, poly(2,6-dimethyl-1,4-phenylene ether), a copolymer of 2,6-dimethylphenol and 2,3,6-trimethylphenol, or a mixture thereof is preferred from the viewpoint of the balance of mechanical properties and productivity.
[0070] As a method for producing the polyphenylene ether resin used in the present embodiment, examples include, but are not limited to, known production methods described in, for example, U.S. Patent No. 3,306,874, U.S. Patent No. 3,306,875, U.S. Patent No. 3,257,357, and U.S. Patent No. 3,257,358, Japanese Patent Publication No. 50-51197, Japanese Patent Publication No. 52-17880, and Japanese Patent Publication No. 63-152628.
[0071] From the perspective of molding fluidity and physical property balance, the reduced viscosity of the polyphenylene ether resin is preferably in the range of 0.30 to 0.65 dL / g. More preferably, it is in the range of 0.40 to 0.60 dL / g, and further preferably in the range of 0.45 to 0.55 dL / g. When the reduced viscosity is 0.30 dL / g or more, the impact strength or oil resistance is excellent. In addition, when the reduced viscosity is 0.65 dL / g or less, the molding fluidity is excellent. In the present embodiment, the reduced viscosity of the polyphenylene ether resin is a value obtained by measuring using a 0.5 g / dL chloroform solution at 30°C using an Ubbelohde viscometer.
[0072] In the present embodiment, a mixture of two or more polyphenylene ether-based resins having different reduced viscosities can also be preferably used.
[0073] In addition, the (a-1) polyphenylene ether resin of the present embodiment may also include a modified polyphenylene ether that has been modified in whole or in part. The modified polyphenylene ether referred to herein refers to a polyphenylene ether modified by a modified compound having at least one carbon-carbon double bond or carbon-carbon triple bond in the molecule and at least one group selected from the group consisting of a carboxylic acid group, anhydride group, amino group, hydroxyl group and glycidyl group (hereinafter sometimes referred to as a "modified compound"). Only one modified compound may be used, or two or more modified compounds may be used in combination.
[0074] Examples of methods for producing modified polyphenylene ether include, but are not limited to, (1) a method of reacting with a modifying compound at a temperature in the range of 100° C. or higher and lower than the glass transition temperature of polyphenylene ether in the presence or absence of a free radical initiator, (2) a method of melt-kneading and reacting with a modifying compound at a temperature in the range of 360° C. or higher than the glass transition temperature of polyphenylene ether, and (3) a method of reacting polyphenylene ether with a modifying compound in a solution at a temperature lower than the glass transition temperature of polyphenylene ether. From the viewpoint of productivity, method (1) or (2) is preferred.
[0075] Next, the modifying compound used for producing the modified polyphenylene ether will be described.
[0076] As the modified compound having a carbon-carbon double bond in the molecule and a carboxylic acid group or an acid anhydride group, there can be mentioned, but not limited to, unsaturated dicarboxylic acids such as maleic acid, fumaric acid, chloromaleic acid, cis-4-cyclohexene-1,2-dicarboxylic acid, and their anhydrides, etc. In particular, from the aspect of reactivity with the polyphenylene ether resin, fumaric acid, maleic acid, and maleic anhydride are preferred, and fumaric acid and maleic anhydride are more preferred.
[0077] Furthermore, a compound in which one or both of the two carboxyl groups of the above unsaturated dicarboxylic acid form an ester can also be used as the modified compound.
[0078] Examples of the modified compound having a carbon-carbon double bond and a glycidyl group in the molecule include, but are not limited to, allyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, epoxidized natural oils and fats, etc. Among these, glycidyl acrylate and glycidyl methacrylate are preferred.
[0079] Examples of modified compounds having a carbon-carbon double bond and a hydroxyl group in the molecule include, but are not limited to, allyl alcohol, 4-penten-1-ol, 1,4-pentadien-3-ol, and the like. n H 2n-1 OH, C n H 2n-3 OH (where n is a positive integer), an unsaturated alcohol of the general formula C n H 2n-5 OH, C n H 2n-7 OH (wherein n is a positive integer) and other unsaturated alcohols.
[0080] The above-mentioned modifying compounds may be used alone or in combination of two or more.
[0081] The amount of the modifying compound added when producing the modified polyphenylene ether is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, and even more preferably 0.5 to 3 parts by mass based on 100 parts by mass of the polyphenylene ether, for example, from the viewpoint of modification efficiency.
[0082] The amount of the radical initiator added when producing the modified polyphenylene ether using the radical initiator is preferably 0.001 to 1 part by mass, more preferably 0.01 to 0.5 part by mass, and even more preferably 0.05 to 0.3 part by mass relative to 100 parts by mass of the polyphenylene ether from the viewpoint of the balance between the modification rate and the physical properties.
[0083] The addition rate of the modifying compound to the modified polyphenylene ether is preferably 0.01 to 5% by mass, more preferably 0.05 to 3% by mass, and even more preferably 0.1 to 1% by mass, relative to 100% by mass of the modified polyphenylene ether.
[0084] Unreacted modifying compounds and polymers of modified compounds may remain in the modified polyphenylene ether. When unreacted modifying compounds and polymers of modified compounds remain, the amount of the residue is preferably less than 5% by mass, more preferably 3% by mass or less, and further preferably 1% by mass or less.
[0085] ·(a-2)Ingredients
[0086] In the present embodiment, (a-2) styrene resin refers to a copolymer obtained by polymerizing a styrene compound or a styrene compound and a compound copolymerizable with a styrene compound (hereinafter, "compound copolymerizable with a styrene compound" is sometimes referred to as "copolymerizable compound") in the presence or absence of a rubber polymer. The styrene resin also belonging to the hydrogenated block copolymer (b) described later is not the (a-2) component but the (b) component.
[0087] Examples of the styrene-based compound include, but are not limited to, styrene, α-methylstyrene, 2,4-dimethylstyrene, monochlorostyrene, p-methylstyrene, p-tert-butylstyrene, and ethylstyrene, among which styrene is preferred.
[0088] Examples of the copolymerizable compound include, but are not limited to, methacrylic acid esters such as methyl methacrylate and ethyl methacrylate; unsaturated nitrile compounds such as acrylonitrile and methacrylonitrile; acid anhydrides such as maleic anhydride; and the like.
[0089] The amount of the copolymerizable compound used is preferably 20% by mass or less, more preferably 15% by mass or less, based on 100% by mass of the total amount of the styrene-based compounds.
[0090] Examples of the rubber polymer include conjugated diene rubbers, copolymers of conjugated dienes and aromatic vinyl compounds, ethylene-propylene copolymer rubbers, etc. Preferred among these are polybutadiene, styrene-butadiene random copolymers, styrene-butadiene block copolymers, and rubber components obtained by partially, substantially completely, or completely hydrogenating these (e.g., rubber components having a hydrogenation rate of 50 to 100%).
[0091] As the component (a-2), for example, homopolystyrene, rubber modified polystyrene (HIPS), styrene-acrylonitrile copolymer (AS resin), styrene-rubber polymer-acrylonitrile copolymer (ABS resin), other styrene copolymers, etc. can be cited, but are not limited to. Among them, as the component (a-2), from the aspect of compatibility with the polyphenylene ether resin, at least one selected from the group consisting of homopolystyrene and rubber modified polystyrene (HIPS) is preferred.
[0092] (b) Ingredients
[0093] The resin composition of the present embodiment contains (b) a hydrogenated block copolymer.
[0094] The (b) hydrogenated block copolymer of the present embodiment is a block copolymer of an aromatic vinyl compound (eg, styrene) and a conjugated diene compound, that is, a hydrogenated block copolymer obtained by hydrogenating a block copolymer containing a polystyrene block and a conjugated diene compound polymer block.
[0095] The hydrogenation rate (hydrogenation rate) of the unsaturated bonds derived from the conjugated diene compound by hydrogenation is preferably 60% or more, more preferably 80% or more, and even more preferably 95% or more, from the viewpoint of heat resistance stability.
[0096] As the structure of the block copolymer before hydrogenation, when the block copolymer is a block copolymer of styrene and a conjugated diene compound, when the styrene block chain is represented by S and the diene compound block chain is represented by B, for example, SBS, SBSB, (SB-)4-S, SBSBS, etc. can be mentioned.
[0097] In addition, the microstructure of the polymer block of the conjugated diene compound (bonding form of the conjugated diene compound) can be arbitrarily selected. The vinyl bonding amount (total of 1,2-vinyl bonding and 3,4-vinyl bonding) of the conjugated diene compound polymer block is preferably 2 to 60%, more preferably 8 to 40%, relative to the total bonding amount (total of 1,2-vinyl bonding, 3,4-vinyl bonding and 1,4-conjugated bonding) of the conjugated diene compound polymer.
[0098] The number average molecular weight of the component (b) is preferably 100,000 to 400,000, more preferably 150,000 to 350,000, and further preferably 200,000 to 300,000. When the number average molecular weight of the component (b) is 100,000 or more, a resin composition having excellent impact resistance can be obtained. The impact resistance of the resin composition of the present embodiment is increased in proportion to the number average molecular weight of the component (b), and when the number average molecular weight of the component (b) is 400,000 or less, a resin composition having a low load during melt extrusion and excellent processing fluidity can be obtained, and the component (b) has excellent dispersibility in the resin composition.
[0099] When the component (b) has a styrene polymer block chain, the number average molecular weight of at least one styrene polymer block chain is preferably 15,000 or more, more preferably 20,000 to 50,000, and even more preferably the number average molecular weight of all styrene polymer block chains is 15,000 or more.
[0100] When the component (b) has a styrene polymer block chain, the proportion of the styrene polymer block chain of the component (b) is not particularly limited as long as the number average molecular weight of the styrene polymer block chain is within the above range, but is preferably 10 to 70% by mass, more preferably 20 to 50% by mass, and even more preferably 30 to 40% by mass from the perspective of impact resistance.
[0101] As component (b), two or more hydrogenated block copolymers having different compositions or structures may be used in combination. For example, a hydrogenated block copolymer having a bound styrene polymer block content of 50% by mass or more and a hydrogenated block copolymer having a bound styrene polymer block content of 30% by mass or less, a combination of hydrogenated block copolymers having different molecular weights, and a combination of the above-mentioned block copolymer of styrene and a conjugated diene compound and a hydrogenated random block copolymer (the hydrogenated random block copolymer is obtained by hydrogenating a block copolymer containing a random copolymer block of styrene and a conjugated diene compound).
[0102] The "bound styrene polymer block content" refers to the ratio of the styrene polymer block chains in the component (b).
[0103] (c) Ingredients
[0104] The component (c) contained in the resin composition of the present embodiment may be any component as long as it is an organic phosphate ester generally used as a flame retardant.
[0105] The component (c) may be one kind only or a combination of two or more kinds.
[0106] As the component (c), for example, but not limited to, triphenyl phosphate, trisnonylphenyl phosphate, resorcinol bis(diphenyl phosphate), resorcinol bis[di(2,6-dimethylphenyl) phosphate], 2,2-bis{4-[bis(phenoxy)phosphoryloxy]phenyl}propane, 2,2-bis{4-[bis(methylphenoxy)phosphoryloxy]phenyl}propane, etc. Further, as the component (c), for example, phosphate ester flame retardants such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, tricresyl phosphate, cresylphenyl phosphate, octyldiphenyl phosphate, and diisopropylphenyl phosphate; diphenyl-4-hydroxy-2,3,5,6-tetrabromobenzyl phosphate, dimethyl-4-hydroxy-3,5-dibromobenzyl phosphate, diphenyl-4-hydroxy-3 ,5-dibromobenzyl phosphate, tris(chloroethyl) phosphate, tris(dichloropropyl) phosphate, tris(chloropropyl) phosphate, bis(2,3-dibromopropyl)-2,3-dichloropropyl phosphate, tris(2,3-dibromopropyl) phosphate, bis(chloropropyl) monooctyl phosphate, hydroquinone diphenyl phosphate, phenyl nonylphenyl hydroquinone phosphate, phenyl dinonylphenyl phosphate and other monophosphate compounds; and aromatic condensed phosphate compounds, etc. Among these, aromatic condensed phosphate compounds are preferred from the aspects of less gas generation during processing and excellent thermal stability.
[0107] Aromatic condensed phosphate compounds are commercially available, and examples thereof include, but are not limited to, trade names "CR741", "CR733S", "PX200", and "E890" from Daihachi Chemical Industry Co., Ltd. and trade names "FP600", "FP700", and "FP800" from ADEKA Corporation.
[0108] As the component (c) used in the present embodiment, an aromatic condensed phosphate ester represented by the following general formula (I) or the following general formula (II) is preferred, and an aromatic condensed phosphate ester represented by the general formula (I) is more preferred.
[0109] [Chemistry 4]
[0110]
[0111] [Chemistry 5]
[0112]
[0113] In the general formula (I), Q1, Q2, Q3 and Q4 independently represent an alkyl group having 1 to 6 carbon atoms, R11 and R12 represent a methyl group, and R13 and R14 independently represent a hydrogen atom or a methyl group. In the general formula (II), Q1, Q2, Q3 and Q4 independently represent an alkyl group having 1 to 6 carbon atoms, and R11 and R12 represent a methyl group. y is an integer greater than 1, n1 and n2 independently represent an integer of 0 to 2, and m1, m2, m3 and m4 independently represent an integer of 0 to 3.
[0114] In the general formulae (I) and (II), y is preferably an integer of 1, 2 or 3, and more preferably 1.
[0115] In a preferred example of the general formula (I), m1, m2, m3, m4, n1 and n2 are 0, R13 and R14 are methyl groups, and y is 1, 2 or 3. In another preferred example of the general formula (I), Q1, Q2, Q3, Q4, R13 and R14 are methyl groups, n1 and n2 are 0, m1, m2, m3 and m4 are 1, 2 or 3, and y is 1, 2 or 3.
[0116] The component (c) preferably contains 50 to 100% by mass of the aromatic condensed phosphoric acid ester of the formula (I) based on 100% by mass of the component (c).
[0117] In one preferred example of the general formula (II), m1, m2, m3, m4, n1 and n2 are 0, and y is 1, 2 or 3. In another preferred example of the general formula (II), Q1, Q2, Q3 and Q4 are methyl groups, n1 and n2 are 0, m1, m2, m3 and m4 are 1, 2 or 3, and y is 1, 2 or 3.
[0118] In the component (c), the aromatic condensed phosphoric acid ester of the formula (II) is preferably contained in an amount of 50 to 100% by mass based on 100% by mass of the component (c).
[0119] The aromatic condensed phosphate compound more preferably has an acid value of 0.1 or less (value obtained in accordance with JIS K2501).
[0120] (d) Ingredients
[0121] (d) component is a polymer obtained by polymerizing monomer units containing olefins (e.g., α-olefins). Examples of (d) component include homopolymers of ethylene, propylene, and other olefinic hydrocarbons, and copolymers thereof. (d) component may be only one kind or a combination of two or more kinds. (d) component includes, for example, polyethylene such as low-density polyethylene, polypropylene, ethylene-vinyl acetate copolymer, polybutene, etc. As preferred (d) component, for example, polyethylene and polypropylene may be included from the aspects of oil resistance and impact resistance.
[0122] The melt flow rate of the component (d) is 30 g / 10 minutes or more, preferably 40 g / 10 minutes or more, and more preferably 50 g / 10 minutes or more. The MFR of the component (d) is preferably 200 g / 10 minutes or less, more preferably 150 g / 10 minutes or less, and further preferably 100 g / 10 minutes or less. By making the MFR of the component (d) 30 g / 10 minutes or more, the polyolefin resin is easily present on the surface portion (e.g., within 2 μm from the surface) of the resin composition molded body, and the oil resistance is excellent.
[0123] (d) When the component is polyethylene, the MFR is suitable for measurement under the conditions of a temperature of 190°C and a load of 2.16kg. In one embodiment, the MFR (190°C, 2.16kg) of polyethylene is 30g / 10 minutes or more, 40g / 10 minutes or more, or 50g / 10 minutes or more. In another embodiment, the MFR (190°C, 2.16kg) of polyethylene is 200g / 10 minutes or less, 150g / 10 minutes or less, or 100g / 10 minutes or less. By making the MFR (190°C, 2.16kg) of polyethylene 30g / 10 minutes or more, the polyolefin resin is easily present in the surface portion (e.g., within 2μm from the surface) of the resin composition molded body. In particular, when the MFR (190°C, 2.16kg) of polyethylene is 100g / 10 minutes or less, there is a tendency to significantly improve the flame retardancy of the resin composition.
[0124] (d) When the component is polypropylene, the MFR is suitably measured under the conditions of a temperature of 230°C and a load of 2.16kg. In one embodiment, the MFR (230°C, 2.16kg) of polypropylene is 30g / 10 minutes or more, 40g / 10 minutes or more, or 50g / 10 minutes or more. In another embodiment, the MFR (230°C, 2.16kg) of polypropylene is 200g / 10 minutes or less, 150g / 10 minutes or less, or 100g / 10 minutes or less. By making the MFR (230°C, 2.16kg) of polypropylene 30g / 10 minutes or more, the polyolefin resin is easily present in the surface portion (e.g., within 2μm from the surface) of the resin composition molded body.
[0125] In one embodiment, the amount of the polyethylene wax in the component (d) is greater than 0 mass % and 5 mass % or less.
[0126] Other flame retardants
[0127] Various conventionally known flame retardants and flame retardant aids may be added to the resin composition of the present embodiment. Examples of other flame retardants include phosphinates, alkaline earth metal hydroxides such as magnesium hydroxide, aluminum hydroxide, alkali metal hydroxides, zinc borate compounds, and zinc stannate compounds.
[0128] ·additive
[0129] In the resin composition of the present embodiment, in order to further impart other characteristics, additives such as resins other than components (a), (b) and (d), plasticizers, antioxidants, stabilizers such as ultraviolet absorbers, antistatic agents, anti-sticking agents, dyes, pigments, fillers, reinforcing materials, spreading agents, etc. may be added within the range that does not impair the effects of the present invention.
[0130] Content of each ingredient
[0131] In the resin composition of the present embodiment, the amounts of components (a) to (d) are, relative to 100 parts by mass of the total of components (a) and (b), 60 to 90 parts by mass of component (a), 10 to 40 parts by mass of component (b), 8 to 25 parts by mass of component (c), and 1 to 10 parts by mass of component (d).
[0132] In the resin composition of the present embodiment, regarding the content of component (a) and component (b), from the aspects of flame retardancy and oil resistance, relative to a total of 100 parts by mass of component (a) and component (b), preferably component (a) is 65 to 90 parts by mass, component (b) is 10 to 35 parts by mass, more preferably component (a) is 65 to 85 parts by mass, component (b) is 15 to 35 parts by mass, and further preferably component (a) is 70 to 85 parts by mass, component (b) is 15 to 30 parts by mass. Specifically, when the amount of component (a) is 60 parts by mass or more, flame retardancy and rigidity are excellent; when the amount of component (b) is 10 parts by mass or more, there is a tendency to have excellent oil resistance and impact resistance.
[0133] The component (a) may be only the component (a-1) or a mixed resin of the component (a-1) and the component (a-2).
[0134] When the component (a) is a mixed resin of the components (a-1) and (a-2), the amount of the component (a-1) is 55 to 99.95 parts by mass, and the amount of the component (a-2) is 0.05 to 45 parts by mass, relative to 100 parts by mass of the mixed resin. When the amount of the component (a-1) is 55 parts by mass or more, there is a tendency to have excellent flame retardancy. In particular, in order to obtain a resin composition with excellent flame retardancy, it is preferred that the component (a) is only the component (a-1). Alternatively, in order to obtain a resin composition with excellent flame retardancy, it is preferred that the component (a) is a mixed resin, and the amount of the component (a-1) is 60 to 99.95 parts by mass relative to 100 parts by mass of the mixed resin, more preferably the amount of the component (a-1) is 65 to 99.95 parts by mass, and further preferably the amount of the component (a-1) is 85 to 95 parts by mass.
[0135] From the perspective of flame retardancy and oil resistance, the content of component (c) is 8 to 25 parts by mass relative to 100 parts by mass of the total of components (a) and (b). It is preferably 10 to 21 parts by mass, and more preferably 10 to 20 parts by mass. When the amount of component (c) is 8 parts by mass or more, flame retardancy is excellent; when it is 25 parts by mass or less, oil resistance tends to be excellent.
[0136] From the perspective of flame retardancy and oil resistance, the content of component (d) is 1 to 10 parts by mass relative to 100 parts by mass of the total of components (a) and (b). It is preferably 2 to 8 parts by mass, and more preferably 3 to 7 parts by mass. When the content of the polyolefin resin (d) is 1 part by mass or more, oil resistance is excellent; when it is 10 parts by mass or less, flame retardancy tends to be excellent.
[0137] When other flame retardants are included, from the aspects of fluidity and appearance, the content of other flame retardants is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and further preferably 20 parts by mass or less relative to 100 parts by mass of the total of components (a) and (b). When the content of other flame retardants is 40 parts by mass or less, there is a tendency for fluidity and appearance to be excellent.
[0138] The content of the total of the additives is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, relative to 100% by mass of the resin composition.
[0139] ·morphology
[0140] As the morphology of the resin composition of the present embodiment, from the aspect of flame retardancy, the phase containing the component (a) forms a continuous phase. The morphology can be determined by staining with a known dye such as ruthenium tetroxide or osmium tetroxide according to the type of thermoplastic resin and observing an image at a magnification of 10,000 times using a transmission microscope or the like.
[0141] (Method for producing resin composition)
[0142] The resin composition of the present embodiment can be produced by, for example, melt-kneading the components (a) to (d) and the like using a twin-screw extruder.
[0143] Examples of the twin-screw extruder include the "ZSK" series manufactured by Coperion, the "TEM" series manufactured by Toshiba Machine, and the "TEX" series manufactured by The Nippon Steel Works, Ltd.
[0144] The melt-kneading temperature and the screw speed in the method for producing the resin composition of the present embodiment can be appropriately selected from the ranges of 100 to 370° C. for the melt-kneading temperature and 100 to 1200 rpm for the screw speed.
[0145] As a raw material supply device for supplying raw materials to a twin-screw extruder, for example, there can be mentioned a loss-in-weight feeder, a single-screw feeder, a twin-screw feeder, a table feeder, a rotary feeder, etc. Among them, a loss-in-weight feeder is preferred from the perspective of less variation error in raw material supply.
[0146] (Molding body)
[0147] The resin composition of the present embodiment can be molded into a molded product. The molded product contains at least the resin composition of the present embodiment.
[0148] As the molding method, for example, known molding methods such as injection molding, hollow molding, extrusion molding, sheet molding, and film molding can be used, and injection molding is particularly preferred. As an injection molding machine, for example, the trade name "SH100C" manufactured by Sumitomo Heavy Industries, Ltd. can be cited.
[0149] The melt temperature and the mold temperature in the molding method of the resin composition of the present embodiment can be appropriately selected from the ranges of 200 to 320°C for the melt temperature and 30 to 100°C for the mold temperature.
[0150] The molded article can be used in the form of various molded articles and can be used in a wide range of fields such as industrial parts, electrical / electronic parts, office equipment housings, automobile parts, precision parts, etc., and can be particularly suitably used in connection structures for solar power generation modules such as module connectors for solar power generation and junction boxes for solar cells.
[0151] (Connection structure for solar power generation module)
[0152] The connection structure for a photovoltaic power generation module according to the present embodiment includes a molded product of the resin composition according to the present embodiment.
[0153] (junction box for solar power generation module)
[0154] The junction box for a solar power generation module according to the present embodiment includes a molded product of the resin composition according to the present embodiment.
[0155] Example
[0156] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.
[0157] The raw materials used in the resin compositions of Examples and Comparative Examples are as follows.
[0158] ·(a)Ingredients
[0159] (a-1) Component: Poly(2,6-dimethyl-1,4-phenylene ether) having a reduced viscosity of 0.5 dL / g
[0160] (a-2) Component: Rubber-modified polystyrene (HIPS), manufactured by Petrochemicals, trade name "CT60", content of rubber polymer: 10% by mass
[0161] (b) Ingredients
[0162] TSRC manufactured product, trade name "TAIPOL6151", number average molecular weight: about 280,000
[0163] (c) Ingredients
[0164] (c-1) Component: Aromatic condensed phosphate compound, manufactured by Daihachi Chemical Industry Co., Ltd., trade name "E890"
[0165] (d) Ingredients
[0166] (d-1) Component: Polypropylene having an MFR (230°C, 2.16 kg) of 100 g / 10 min.
[0167] (d-2) Component: low-density polyethylene having an MFR (190°C, 2.16 kg) of 55 g / 10 min.
[0168] (d-3) Component: Polypropylene having an MFR (230°C, 2.16 kg) of 0.4 g / 10 min
[0169] (d-4) Component: low-density polyethylene having an MFR (190°C, 2.16 kg) of 0.4 g / 10 min
[0170] (d-5) Component: low-density polyethylene having an MFR (190°C, 2.16 kg) of 20 g / 10 min
[0171] Other flame retardants: Clariant, trade name "Exolit (registered trademark) OP 930"
[0172] Other materials used in the examples are shown below.
[0173] Processing oil: Nippon Hydraulic Oil Manufacturing, trade name "G-6280"
[0174] The apparatus used in the examples are as follows.
[0175] Twin-screw extruder: Coperion, trade name "ZSK-25WLE"
[0176] Small injection molding machine: Sumitomo Heavy Industries, Ltd., trade name "SH100C"
[0177] Microscope: Made by KEYENCE Corporation, trade name "VHX-5000"
[0178] Transmission electron microscope (TEM): manufactured by Hitachi High-Technologies Corporation, trade name "HT7700"
[0179] (Examples 1 to 6, Comparative Examples 1 to 11)
[0180] The components (a) to (d) and other flame retardants were supplied to a twin-screw extruder in the compositions shown in Tables 1 and 2, and melt-kneaded under the conditions of an extrusion temperature of 300 to 320°C, a screw speed of 300 rpm, and a discharge rate of 15 kg / hour to obtain pellets of a resin composition. The twin-screw extruder was set as follows: the number of barrels was 12, and in the flow direction of the raw materials, from the upstream, an upstream supply port was set in the first barrel, a liquid addition pump was set in the seventh barrel, and a vacuum exhaust port was set in the fifth barrel and the eleventh barrel.
[0181] The methods for measuring physical properties in Examples and Comparative Examples are as follows.
[0182] Oil resistance
[0183] The resin composition pellets were fed into a small injection molding machine with the barrel temperature set at 280°C, and a 120mm×80mm×3mm flat plate was molded at a mold temperature of 80°C. A test piece (80mm×12.5mm×3mm) with the length direction perpendicular to the flow direction was cut from the flat plate. The test piece was mounted on a rod with the horizontal direction as the x-axis, the vertical direction as the y-axis, and the vertical section as the y-axis in a manner that there was no gap between the rod and the test piece. 2 =6x(x≧0, y≧0) on the curved surface of the parabola bending rod. In addition, in the bending rod, the position of x=0, y=0 on its vertical section is used as the configuration position of the end portion on the measurement starting point side of the test piece, and the position of x>0 and y>0 is used as the configuration position of the end portion on the measurement end side of the test piece.
[0184] Next, machining oil was applied to the surface of the test piece and left at 40° C. for 24 hours. If cracks occurred on the surface of the test piece after 24 hours, the critical position of crack generation (the position where the x value of the bending rod in the x-axis direction reached the maximum) was read.
[0185] When reading the critical position of crack generation, the scale of the x-axis coordinate of the bending rod is transferred to the test piece while it is installed on the bending rod. After the test piece is removed from the bending rod, the existence of the crack is confirmed, and the position where the crack exists is compared with the transferred scale and read (because the critical position is the position corresponding to the x-axis coordinate of the bending rod, it is not the circumferential length of the test piece). It should be noted that in the present disclosure, cracks refer to cracks in the flow direction of more than 200 μm observed when the surface of the test piece is observed using a microscope.
[0186] After that, the critical deformation (%) was calculated by the following formula based on the thickness of the test piece and the critical position of crack generation. The critical deformation (%) of Comparative Example 1 was set to 100, and the critical deformation of each embodiment and comparative example was indexed. The larger the index value, the better the oil resistance was judged to be.
[0187] Critical deformation (%) = d × 3 1 / 2 / 2(3+2x) 3 / 2 ×100
[0188] d: Thickness of the test piece (inch)
[0189] x: Critical position of crack generation (inch)
[0190] Flame retardant
[0191] The flame retardancy was evaluated based on the UL-94 vertical burning test using an injection molded test piece having a thickness of 0.75 mm.
[0192] First, the resin composition pellets are supplied to a small injection molding machine with the barrel temperature set at 300°C to 320°C, and injection molding is performed under the conditions of injection speed 20%, injection pressure 99%, and mold temperature 90°C to mold 5 test pieces of the dimensions specified in the standard (length 125 mm × width 13 mm, thickness 0.75 mm).
[0193] The test piece is exposed to the flame of a gas lamp to evaluate the degree of its burning. It should be noted that the flame retardancy grade shows the grade of flame retardancy classified by the UL94 vertical test. For all test pieces, 5 pieces are tested for determination. The outline of the classification method is as follows.
[0194] Flame retardancy evaluation criteria
[0195] V-0 (pass): The total burning time of 5 pieces is less than 50 seconds, the maximum burning time is less than 10 seconds, and no flaming droplets occur.
[0196] Vоut: The total burning time of 5 pieces is greater than 250 seconds, the maximum burning time is greater than 30 seconds, and flaming droplets occur.
[0197] ·morphology
[0198] Ultrathin sections with a thickness of several 10 to 100 nm were prepared from the molded body prepared in the same manner as the test piece for oil resistance evaluation using an ultrathin microtome. The ultrathin sections were then stained with osmium tetroxide and ruthenium tetroxide, and the stained ultrathin sections were observed using a transmission electron microscope to obtain an image with a magnification of 10,000 times. The obtained image was used to determine whether the phase containing component (a) formed a continuous phase.
[0199] The morphology of the molded articles produced from the resin compositions of Examples 1 to 6 and Comparative Examples 1 to 11 was observed. As a result, the phase containing the component (a) formed a continuous phase in all of them.
[0200] [Table 1]
[0201]
[0202] In Table 1, "CP" means that the phase containing the component (a) forms a continuous phase.
[0203]
[0204] All of Examples 1 to 6 were excellent in oil resistance and flame retardancy. The resin composition of the present embodiment was molded into a molded body having both high oil resistance and flame retardancy.
[0205] Industrial Applicability
[0206] The resin composition of the present invention can be used for a molded product requiring high oil resistance and flame retardancy.
Claims
1. A resin composition comprising: (a) (a-1) a polyphenylene ether resin, or a mixed resin of (a-1) a polyphenylene ether resin and (a-2) a styrene resin; (b) hydrogenated block copolymers; (c) phosphate compounds; and (d) polyolefin resins, With respect to 100 parts by mass of the total of the component (a) and the component (b), The amount of the component (a) is 60 to 90 parts by mass, The amount of the component (b) is 10 to 40 parts by mass, The amount of the component (c) is 8 to 25 parts by mass, The amount of the component (d) is 1 to 10 parts by mass, When the component (a) is the mixed resin, the amount of the polyphenylene ether-based resin (a-1) is 55 to 99.95 parts by mass relative to 100 parts by mass of the mixed resin. The melt flow rate of the component (d) is 30 g / 10 minutes or more, The phase containing the component (a) forms a continuous phase.
2. The resin composition according to claim 1, in, The amount of the component (c) is 10 to 20 parts by mass based on 100 parts by mass of the total of the components (a) and (b).
3. The resin composition according to claim 1 or 2, in, The amount of the component (d) is 2 to 8 parts by mass based on 100 parts by mass of the total of the components (a) and (b).
4. The resin composition according to claim 1 or 2, in, The component (c) is an aromatic condensed phosphate compound.
5. The resin composition according to claim 1 or 2, in, The component (c) is a phosphate compound represented by the following general formula (I) or (II), [Chemistry 1] [Chemistry 2] In the general formula (I), Q1, Q2, Q3 and Q4 independently represent an alkyl group having 1 to 6 carbon atoms, R11 and R12 represent a methyl group, and R13 and R14 independently represent a hydrogen atom or a methyl group; In the general formula (II), Q1, Q2, Q3 and Q4 independently represent an alkyl group having 1 to 6 carbon atoms, and R11 and R12 represent a methyl group; y is an integer greater than or equal to 1, n1 and n2 independently represent an integer of 0-2, and m1, m2, m3, and m4 independently represent an integer of 0-3.
6. The resin composition according to claim 5, in, The component (c) is a phosphate compound represented by the general formula (I).
7. The resin composition according to claim 1 or 2, in, The component (d) is selected from the group consisting of polyethylene and polypropylene.
8. The resin composition according to claim 1 or 2, in, The melt flow rate of the component (d) is 50 g / 10 min or more and 150 g / 10 min or less.
9. The resin composition according to claim 1 or 2, in, The reduced viscosity of the polyphenylene ether-based resin (a-1) is in the range of 0.30 dL / g to 0.65 dL / g.
10. The resin composition according to claim 1 or 2, in, With respect to 100 parts by mass of the total of the component (a) and the component (b), The amount of the component (a) is 65 to 90 parts by mass, The amount of the component (b) is 10 to 35 parts by mass.
11. The resin composition according to claim 1 or 2, in, When the component (a) is the mixed resin, the amount of the (a-1) polyphenylene ether-based resin is 65 parts by mass to 99.95 parts by mass based on 100 parts by mass of the mixed resin.
12. The resin composition according to claim 1 or 2, in, The content of the total additives is 10% by mass or less relative to 100% by mass of the resin composition. 13 . A connection structure for a solar power generation module, comprising a molded body of the resin composition according to claim 1 . 14 . A junction box for a solar power generation module, comprising a molded article of the resin composition according to claim 1 .