Hexagonal boron nitride powder and method for producing the same
After reduction nitridation and pickling treatment, combined with the magnetic separation technology of the electromagnetic sieve device, the content of magnetic foreign matter in hexagonal boron nitride powder was successfully reduced, solving the problem of low magnetic foreign matter removal efficiency in the existing technology, and achieving Preparation of hexagonal boron nitride powder with high electrical insulation and low cost, suitable for high-performance resin materials.
Patent Information
- Application Number
- CN202080078703.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-12-07
AI Technical Summary
The existing technology is difficult to effectively reduce the total content of magnetic foreign matter in hexagonal boron nitride powder, especially when the powder particle size is less than 0.5mm. The efficiency of the magnetic separation processor is low and may cause the magnetic foreign matter to be free, making it difficult to separate the hexagonal boron nitride particles. It is difficult to remove magnetic foreign matter inside the aggregate.
Hexagonal boron nitride powder is prepared by the reduction nitridation method, and through pickling, water washing and drying, the magnetic foreign matter is placed in a state that is easy to remove, and then an electromagnetic sieve device is used for magnetic separation, and a strong magnetic field and a multi-layer magnetic pole net are used to remove it Magnetic foreign matter on the surface and inside, reaching extremely low magnetic foreign matter content.
It achieves a high degree of removal of magnetic foreign matter in hexagonal boron nitride powder, improves electrical insulation and insulation strength, and makes it suitable for high-performance resin material fillers with low process cost and wide industrial applications.
Smart Images

Figure BDA0003639748180000131 
Figure BDA0003639748180000132
Abstract
Description
Technical Field
[0001] The present invention relates to hexagonal boron nitride powder having a reduced total content of magnetic foreign matter and a method for producing the same. Background Art
[0002] Hexagonal boron nitride is a ceramic having a hexagonal layered crystal structure, and hexagonal boron nitride powder having a high aspect ratio is used for cosmetic applications and as a processing aid in extrusion molding of resins (see Patent Document 1).
[0003] In addition, hexagonal boron nitride powder has high thermal conductivity, excellent heat dissipation, high electrical insulation, and excellent insulation strength. Therefore, it can be mixed into a resin material as a heat dissipation filler to produce an insulating sheet with excellent heat dissipation (see Patent Document 2).
[0004] Here, Patent Document 2 describes hexagonal boron nitride powders with excellent electrical insulation properties based on the fact that the concentration of iron contained as an impurity is 500 ppm or less, but the examples only disclose powders with an iron concentration of 70 ppm or more, which is limited in terms of improving electrical insulation properties.
[0005] It is also known that, when producing a sintered body of ceramic powder made of boron nitride or the like, a magnetic separator is used to minimize the amount of impurities mixed in a slurry in which the ceramic powder or the like and a solvent are mixed (see Patent Document 3).
[0006] However, although the conventional magnetic separation treatment machine has the function of removing magnetic foreign matter using a permanent magnet, it is a device in which a permanent magnet is combined in a cylindrical container or a grid-shaped frame, and is not suitable for processing powders below 0.5 mm, and it is difficult to further reduce the magnetic foreign matter of powders with a concentration of several hundred ppm to several thousand ppm. Furthermore, the wet magnetic separation treatment such as Patent Document 3 not only increases the process of removing the solvent, but also requires a flow rate above a certain level, so there is a concern that the magnetic foreign matter with weak magnetic force and small particle size temporarily captured by the magnet will become free.
[0007] On the other hand, it is believed that the magnetic foreign matter is mixed into the hexagonal boron nitride powder through the following paths: mixing from the raw materials when synthesizing the hexagonal boron nitride; and mixing from the manufacturing device when the synthesized hexagonal boron nitride is subjected to treatments such as pulverization and classification. Among them, when the magnetic foreign matter from the raw materials is firmly attached to the hexagonal boron nitride powder, especially when the hexagonal boron nitride powder is a particle aggregate, it is difficult to remove the magnetic foreign matter present in the aggregate, and there is a problem that the hexagonal boron nitride powder obtained by the conventional magnetic separation treatment cannot obtain a hexagonal boron nitride powder with a highly reduced total content of magnetic foreign matter.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2008-280243
[0011] Patent Document 2: Japanese Patent Application Publication No. 2011-098882
[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 7-082033 Summary of the invention
[0013] Problem that the invention aims to solve
[0014] The present inventors conducted intensive research and found that, for hexagonal boron nitride powder obtained by reduction nitridation, impurity metals constituting magnetic foreign matter originating from the raw material are easily sublimated at high temperatures and are easily present on the surface of the hexagonal boron nitride particles in the form of granular magnetic foreign matter. In addition, by subjecting the hexagonal boron nitride powder to an acid treatment, the magnetic foreign matter can be easily removed. Furthermore, by subjecting the hexagonal boron nitride powder to a special magnetic separation treatment that has not been used before, the magnetic foreign matter attached to the surface of the hexagonal boron nitride particles can be effectively removed, or the magnetic foreign matter present in the particles of the particle aggregate of the hexagonal boron nitride powder can be removed together with the particles. Thus, a high degree of removal of magnetic foreign matter that has not been achieved before was successfully achieved, thereby completing the present invention.
[0015] Therefore, an object of the present invention is to provide a hexagonal boron nitride powder in which magnetic foreign matter is removed to an extremely high degree and which has excellent electrical insulating properties.
[0016] Solutions for solving problems
[0017] The present invention provides a hexagonal boron nitride powder, characterized in that it is a powder formed by single particles and / or aggregated particles of hexagonal boron nitride, and the total content of Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn, and Al elements is within a range of less than 20 ppm.
[0018] Here, the aforementioned Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn, and Al elements are elements that are often contained in the hexagonal boron nitride powder raw material or its manufacturing device, and the compounds containing these elements themselves will form magnetic foreign matter, or may be contained in magnetic foreign matter.
[0019] The magnetic foreign matter refers to all foreign matter having magnetic properties contained in the hexagonal boron nitride powder.
[0020] The average particle size of the hexagonal boron nitride powder is preferably 2 to 90 μm.
[0021] The above-mentioned hexagonal boron nitride powder is preferably: after the hexagonal boron nitride is immersed in a 0.02 mol / L sulfuric acid aqueous solution at 25°C for 120 minutes, the amount of boron dissolved converted to B2O3 is less than 200 ppm, the amount of calcium dissolved is less than 50 ppm, and the amount of sodium and silicon dissolved is less than 20 ppm respectively. The amount of chlorine dissolved after the hexagonal boron nitride powder is immersed in water at 25°C for 120 minutes is less than 10 ppm.
[0022] In addition, the hexagonal boron nitride powder with reduced magnetic foreign matter of the present invention can be obtained by the following production method, which includes the following steps:
[0023] A process for preparing hexagonal boron nitride powder by reduction nitridation;
[0024] The hexagonal boron nitride powder is acid-washed, water-washed and dried; and
[0025] The step of preparing an electromagnetic sieve device to magnetically separate the powder after the particle size adjustment, wherein the electromagnetic sieve device has 20 or more overlapping openings of 5 mm or less and 8 mm or less and a 30 cm 2 The magnetic pole area is above and the mesh is magnetized to above 1.2T.
[0026] Effects of the Invention
[0027] The hexagonal boron nitride powder of the present invention has a very low content of magnetic foreign matter and therefore has high electrical insulation and excellent dielectric strength, and is therefore suitable for use as a heat dissipating filler or the like to be blended into a resin material.
[0028] In addition, the production method of the present invention can produce hexagonal boron nitride powder having a reduced total content of magnetic foreign matter at low cost, and is therefore extremely useful industrially. DETAILED DESCRIPTION
[0029] The greatest feature of the hexagonal boron nitride powder of the present invention is that the content of Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn, and Al elements is extremely significantly reduced compared with the conventional hexagonal boron nitride powder. The Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn, and Al are elements that are often contained in the raw materials of hexagonal boron nitride powder and its manufacturing equipment, and the compounds containing the elements themselves will form magnetic foreign matter, or may be contained in the magnetic foreign matter.
[0030] That is, the content of Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn, and Al elements in the hexagonal boron nitride powder of the present invention is 20 ppm or less, preferably 15 ppm or less.
[0031] Here, when the content of the above-mentioned element exceeds 20 ppm, there is a possibility that the electrical insulation property may not necessarily be excellent.
[0032] The content of Fe, which is a main element forming the magnetic foreign matter, is preferably 10 ppm or less, more preferably 8 ppm or less.
[0033] The hexagonal boron nitride powder obtained by the compound containing the element itself forming magnetic foreign matter or by highly removing the elements possibly contained in the magnetic foreign matter is first proposed by the present invention. When it is filled into a resin as a filler, it can impart extremely high insulation resistance to the obtained resin composition.
[0034] As long as the hexagonal boron nitride powder of the present invention has the above-mentioned properties, other properties are not particularly limited.
[0035] For example, the particles constituting the hexagonal boron nitride powder may be single particles, aggregated particles, or a mixture thereof.
[0036] The average particle size of the hexagonal boron nitride powder of the present invention is 2 to 90 μm, and particularly preferably 5 to 70 μm.
[0037] Here, when the average particle size is less than 2 μm, the particle size may be too small to be handled, and when it exceeds 90 μm, the particle size may be too large to be handled.
[0038] In addition, for the hexagonal boron nitride powder of the present invention, in order to further improve the insulation resistance of the obtained resin composition when used as a filler, it is preferred that: after immersion in a 0.02 mol / L sulfuric acid aqueous solution at 25°C for 120 minutes, the amount of eluted boron converted to B2O3 is less than 200 ppm, the amount of eluted calcium is less than 50 ppm, the amount of eluted sodium and silicon is less than 20 ppm respectively, and the amount of eluted chlorine after immersion in water at 25°C for 120 minutes is less than 10 ppm.
[0039] Here, in at least any one of the following cases, the acid cleaning of the hexagonal boron nitride powder is insufficient, and the hexagonal boron nitride powder of the present invention may not be obtained, wherein: the amount of the aforementioned dissolved boron converted to B2O3 exceeds 200 ppm; the amount of the aforementioned dissolved calcium exceeds 50 ppm; the amount of at least one of the aforementioned dissolved sodium and silicon exceeds 20 ppm; or the amount of the aforementioned dissolved chlorine exceeds 10 ppm.
[0040] <Process for producing hexagonal boron nitride powder of the present invention>
[0041] If a typical method for producing the hexagonal boron nitride powder of the present invention is exemplified, the method for producing the hexagonal boron nitride powder includes the following steps:
[0042] A process for preparing hexagonal boron nitride powder by reduction nitridation;
[0043] The hexagonal boron nitride powder is acid-washed, water-washed and dried;
[0044] A step of classifying the dried powder obtained in the above step to adjust the particle size;
[0045] The step of preparing an electromagnetic sieve device to magnetically separate the powder after the particle size adjustment, wherein the electromagnetic sieve device has 20 or more overlapping openings of 5 mm or less and 8 mm or less and a 30 cm 2 A mesh having a magnetic pole area of more than 1.2 T and magnetized to more than 1.2 T; and
[0046] The process of filling magnetically separated powder into packaging bags.
[0047] Here, the electromagnetic sieve device may not be able to perform sufficient magnetic separation in at least any of the following situations: the opening is larger than 5 mm or less × 8 mm or less; the magnetic pole area is less than 30 cm 2 or the number of overlapping sheets of the net magnetized to 1.2T or more is less than 20 sheets.
[0048] The term "magnetic separation" means to remove magnetic foreign matter from powder, thereby reducing the content of magnetic foreign matter in the powder.
[0049] <Process for preparing hexagonal boron nitride powder by reduction nitridation method>
[0050] The invention comprises a process of preparing hexagonal boron nitride powder by a reduction nitridation method.
[0051] For example, the production of hexagonal boron nitride (hereinafter also referred to as "h-BN") based on the reduction nitridation method can be implemented as follows. That is, an oxygen-containing boron compound such as boron oxide (B2O3) is used as a boron source, a powder of the oxygen-containing boron compound, a mixed powder of carbon powder and an auxiliary agent are used as a reaction raw material, nitrogen is supplied in a nitridation reactor, and h-BN is obtained by reduction and nitridation of the oxygen-containing boron compound. It should be noted that there is no particular limitation on the mixing device used to prepare the aforementioned mixed powder as a reaction raw material as long as the components are uniformly mixed, and a mixing device such as a vibration mill, a ball mill, a drum mixer, a vibration agitator, etc. can be used for the preparation.
[0052] Here, the oxygen-containing boron compound is not particularly limited, and for example, boric acid, anhydrous boric acid, metaboric acid, perboric acid, hypoboric acid, sodium tetraborate, sodium perborate, etc. Boric acid and boron oxide, which are generally readily available, are preferably used.
[0053] In addition, the nitrogen atmosphere can be formed by a known method. As the gas used, there is no particular limitation as long as it is a gas that can provide nitrogen to boron in the above-mentioned nitridation reaction. It can be nitrogen, ammonia, or a gas in which a non-oxidizing gas such as hydrogen, argon, or helium is mixed in nitrogen or ammonia.
[0054] Furthermore, the reduction nitridation reaction step can be performed using a known device capable of controlling the reaction atmosphere, for example, an atmosphere-controlled high-temperature furnace that performs heat treatment by high-frequency induction heating or heater heating, and in addition to a batch furnace, a continuous furnace such as a pusher tunnel furnace or a vertical reaction furnace can also be used.
[0055] The above reaction is represented by the following formula, and the reaction is usually carried out at a temperature above 1200°C.
[0056] B2O3B+3C→2B+3CO
[0057] 2B+N2→2BN
[0058] The above reaction is usually preferably carried out at a temperature below 1550°C. If a calcium auxiliary agent is used at a temperature exceeding 1550°C and more than 5% by mass of carbon remains, black impurities such as CaB6 will be generated, which is not preferred. For example, it is preferred to maintain the temperature at about 1500°C for 2 to 10 hours to allow the reaction to proceed sufficiently.
[0059] After the above reaction, the temperature in the nitriding reactor is usually maintained at 1700-2000°C, preferably 1750-1950°C. It is presumed that the crystal growth of h-BN progresses and the metal constituting the magnetic foreign matter contained in the raw material volatilizes or exists in particles outside the crystal.
[0060] In addition, the oxygen-containing calcium compound as an auxiliary agent in the reaction raw material is used to promote the above-mentioned crystal growth. As the oxygen-containing calcium compound, calcium oxide (CaO) can be used, for example. Usually, an excess of boron oxide (B2O3) is added on the basis of reduction nitridation, and a two-component system liquid phase (B2O3-CaO) exists at the stage of crystal growth at 1700°C to 2000°C, and crystal growth is carried out in this liquid phase.
[0061] Here, the oxygen-containing calcium compound is not particularly limited, and for example, calcium oxide, calcium carbonate, calcium hydrogen carbonate, calcium hydroxide, calcium nitrate, calcium sulfate, calcium phosphate, calcium oxalate, etc. can be used, and two or more of these can be used in combination.
[0062] In the production method of the present invention, boron carbide can be used as a raw material B source auxiliary agent for aggregates, and known boron carbide can be used without particular limitation. Aggregates can be produced with high selectivity by mixing boron carbide with the above-mentioned reduction nitridation reaction raw materials.
[0063] In addition, the average particle size of the hexagonal boron carbide is preferably 20 to 250 μm, more preferably 50 to 180 μm, and particularly preferably 70 to 150 μm. That is, by setting the average particle size of the boron carbide to 250 μm or less, the formation of coarse aggregates is suppressed. In addition, by setting it to 20 μm or more, it is easy to produce aggregates of a moderate particle size for ensuring high thermal conductivity. Boron carbide contains metal impurities represented by Fe, and will contain about 0.05 to 0.5 weight % of Fe. In the reduction nitridation reaction raw material, the higher the content of boron carbide, the more the amount of metal impurities remaining in the generated boron nitride powder.
[0064] In the case where single-particle boron nitride particles are to be obtained with high selectivity, it is preferred that the ratio of the B source contained in the oxygen-containing boron compound to the C source contained in the carbon source in the reaction raw material is 0.75 to 1.05 in terms of B / C (element ratio), and the oxygen-containing calcium compound is 5 to 20 parts by mass in terms of CaO relative to 100 parts by mass of the total amount of the oxygen-containing boron compound and the carbon source (B2O3, C conversion value). In the case where aggregates are to be obtained with high selectivity, it is preferred that the above-mentioned boron carbide is mixed in a ratio of 10 to 45 parts by mass relative to 100 parts by mass of the total amount of B2O3, C, and CaO conversion mass of the oxygen-containing boron compound, carbon source, and oxygen-containing calcium compound in the above ratio.
[0065] Here, the carbon source is not particularly limited, and for example, in addition to amorphous carbon such as carbon black, activated carbon, and carbon fiber, crystalline carbon such as diamond, graphite, and nanocarbon, pyrolytic carbon obtained by pyrolyzing monomers and polymers, etc. can also be used. Inexpensive carbon black is usually used.
[0066] In the above reaction step, the nitriding reactor is filled with nitrogen atmosphere at atmospheric pressure, and nitrogen is usually supplied / exhausted at a flow rate of 0.1 to 100 L / hr, preferably 10 to 80 L / hr, per 1 L of the volume of the nitriding reactor.
[0067] For the hexagonal boron nitride powder obtained by the reduction nitridation method, the particles are usually lightly sintered to form aggregates, and it is preferred to crush them into single particles or aggregated particles of appropriate particle size. The crushing is preferably carried out in a manner that the average particle size becomes 2 to 90 μm, especially 10 to 70 μm.
[0068] <Steps of acid washing, water washing and drying hexagonal boron nitride powder>
[0069] The present invention includes the steps of subsequently acid washing, water washing and drying the hexagonal boron nitride powder.
[0070] By acid washing (also called acid cleaning) the hexagonal boron nitride powder, the byproducts contained in the hexagonal boron nitride powder can be removed, and the particle size of the magnetic foreign matter can be reduced, so that it can be made easier to remove in the subsequent magnetic separation. In addition, the fine magnetic foreign matter can be completely dissolved and disappear by the acid washing.
[0071] For the above treatment, for example, the following method is appropriate: the hexagonal boron nitride powder is placed in a polyethylene cylindrical container, an aqueous hydrochloric acid solution (hydrochloric acid concentration of about 5 to 15% by weight) of 10 times or more of the hexagonal boron nitride powder is added, and the container is stirred at a speed of 100 to 400 rpm for preferably more than 4 hours. Here, as the acid used in the pickling, in addition to hydrochloric acid, nitric acid, sulfuric acid, acetic acid, etc. can also be used.
[0072] After the acid washing, the acid is preferably filtered and washed with water (also referred to as pure water washing). Specifically, there can be mentioned a method in which the steps of dispersing the acid-washed hexagonal boron nitride powder in pure water and filtering again are repeated until the filtrate becomes neutral.
[0073] After the water washing, the obtained powder is dried in air at 50 to 250° C. or under reduced pressure, thereby obtaining a high-purity hexagonal boron nitride powder.
[0074] <Step of Classifying the Dried Powder to Adjust Particle Size>
[0075] The present invention preferably includes a step of classifying the dried hexagonal boron nitride powder obtained in the above step to adjust the particle size.
[0076] This is an appropriate pre-treatment because after this process, there is a process of magnetically separating the aforementioned powder whose particle size has been adjusted using a specific electromagnetic sieve device. The particle size adjustment can be performed using a common classifier such as a classifier using a sieve, a wind classifier, etc. Regarding the range of particle size to be adjusted, it is preferably set in a manner that removes particles larger than the mesh size of the net used in the aforementioned electromagnetic sieve device. That is, this is because: when there is powder larger than the mesh size, it cannot pass through the aforementioned mesh size, so it will be clogged and the electromagnetic sieve device will not be able to function. In the worst case, it will become the cause of adverse conditions such as device failure.
[0077] The present invention includes a step of preparing an electromagnetic sieve device to magnetically separate the powder after the particle size is adjusted, wherein the electromagnetic sieve device has 20 or more overlapping openings of 5 mm or less and 8 mm or less and a 30 cm 2 A mesh with a magnetic pole area of more than 1.2T and magnetized to more than 1.2T.
[0078] The net is a flat plate in the shape of a mesh and is an electromagnet magnetized to 1.2T or more by electric current, with a length of 30cm. 2 The greater the magnetic force and the area of the magnetic pole, the higher the effect of magnetic separation in removing magnetic foreign matter. Therefore, there is no upper limit on the magnetic force and the area of the magnetic pole. Here, in order to remove magnetic fine powders less than 1 mm with a high probability, an opening of 5 mm or less × 8 mm or less and 30 cm 2 The magnetic pole area is greater than 1.2T and is magnetized to greater than 1.2T.
[0079] By performing magnetic separation under the above conditions, magnetic foreign matter can be reliably removed from the surface of hexagonal boron nitride particles, or, even if magnetic foreign matter exists on particles of particle aggregates of hexagonal boron nitride powder, the magnetic foreign matter can be removed together with the particles, and hexagonal boron nitride powder with a highly reduced total content of magnetic foreign matter can be obtained.
[0080] The electromagnetic sieve device is a device capable of overlapping and using 20 or more of the aforementioned nets at specific intervals, for example, the following device: the inner side wall of the longitudinal cylindrical device is provided with a protrusion for holding the aforementioned net, after all the nets are set, the powder is added from the top, and the entire device is vibrated, so that the aforementioned powder falls due to gravity and passes through all the nets, thereby performing magnetic separation. The more the number of nets, the higher the effect of magnetic separation for removing magnetic foreign matter, so the upper limit of the number of nets is not limited, and it is preferably 45 or less in consideration of production efficiency.
[0081] The present invention includes a step of filling the magnetically separated powder into a packaging bag.
[0082] The magnetically separated powder is in a state where magnetic foreign matter is highly removed, and therefore it is preferred to fill the magnetically separated powder into a packaging bag so that the magnetic foreign matter does not re-enter and cause contamination.
[0083] By going through the above-mentioned steps, it is possible to obtain hexagonal boron nitride powder in which the elements Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn, and Al, which are elements whose compounds containing the elements themselves will form magnetic foreign matter or may be contained in magnetic foreign matter, are highly reduced.
[0084] Example
[0085] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to these examples.
[0086] <Preparation of Raw Material Mixture and Reduction Nitriding Reaction Step>
[0087] 14 kg of boron oxide, 6 kg of carbon black, 4 kg of calcium carbonate, and 1.5 kg of boron carbide were mixed in a ball mill. The mixture was heated to 1500°C at 15°C / min in a nitrogen atmosphere using a graphite Tamman furnace, and kept at 1500°C for 6 hours. After being kept at 1500°C, the mixture was heated to 1830°C at 15°C / min, and kept at 1830°C for 2 hours to obtain a boron nitride powder subjected to reduction nitridation treatment.
[0088] <Acid washing, water washing and drying process>
[0089] Next, the hexagonal boron nitride powder treated with the above-mentioned reduction nitridation is placed in a polyethylene cylindrical container, and a hydrochloric acid aqueous solution (hydrochloric acid concentration 10 weight %) 10 times the amount of the hexagonal boron nitride powder is added, and stirred at a speed of 300 rpm for 15 hours. After the acid washing, the acid is filtered, and the pure water with a resistivity of 1MΩ·cm at 25°C and 300 times the amount of the hexagonal boron nitride powder is used for washing again, and then dehydrated by suction-based filtration until the water content in the filtered powder is less than 50wt%. After the pure water washing, the obtained powder is dried under reduced pressure at a pressure of 1kPaA at 200°C for 15 hours to obtain a high-purity hexagonal boron nitride powder.
[0090] <Step of Classifying to Adjust Particle Size>
[0091] Next, the hexagonal boron nitride powder was classified with a final sieve of 90 μm using a circular vibrating sieving machine (Kowa Kogyo Co., Ltd.) to adjust the particle size. The hexagonal boron nitride powder obtained at this stage was designated as the hexagonal boron nitride powder of Comparative Example 1.
[0092] <Magnetic separation process using electromagnetic sieving device>
[0093] Next, use the overlapping 40 Thickness 10mm, opening 5mm×8mm, with 54cm 2 The hexagonal boron nitride powder having the above-mentioned particle size adjustment was magnetically separated by an electromagnetic sieve device having a magnetic pole area of 1.6 T and a mesh magnetized to obtain the hexagonal boron nitride powder of Example 1.
[0094] <Step of filling magnetically separated powder into packaging bags>
[0095] Next, the hexagonal boron nitride powder subjected to the magnetic separation is filled into a commonly used packaging bag such as a paper bag, thereby producing a hexagonal boron nitride powder with a reduced content of magnetic foreign matter.
[0096] (1) Determination of particle size distribution
[0097] The particle size distribution of the hexagonal boron nitride powder is measured using a particle size distribution measuring device MT3000 manufactured by Nikkiso Co., Ltd. It should be noted that the measurement sample is prepared by the method shown below. First, 20 g of ethanol is added to a 50 mL threaded tube bottle as a dispersion medium, and 1 g of hexagonal boron nitride powder is dispersed in ethanol. Then, the particle size distribution of the measurement sample subjected to ultrasonic treatment is measured. The average particle sizes of the hexagonal boron nitride powders of Example 1 and Comparative Example 1 are 26 μm and 27 μm, respectively.
[0098] (2) ICP determination of total dissolution of hexagonal boron nitride powder
[0099] Ten samples, 0.5 g each, were collected from any part of the hexagonal boron nitride powder, and each sample was put into a pressurized decomposition container together with 10 ml of hydrofluoric acid, 1.25 ml of sulfuric acid and 0.25 ml of nitric acid. After being placed in a dryer at 160°C for 20 hours, the solution was transferred to a platinum dish, and the temperature was raised to 220°C over 1 hour. After heating at 220°C for 5 hours until no white smoke was emitted, 1.25 ml of hydrochloric acid and 1.25 ml of ultrapure water were added and recovered, and ultrapure water was added to a 25 ml polypropylene volumetric flask to make the volume constant. The amount of Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn and Al in the solution was determined by an ICP luminescence device (manufactured by Thermo Fisher Scientific KK: ICAP6500), and the content of each sample was calculated. The average value of the ten samples is shown in Table 1.
[0100] (3) ICP analysis of hexagonal boron nitride powder extracted with aqueous sulfuric acid solution
[0101] 2 g of hexagonal boron nitride powder was put into 50 ml of a sulfuric acid aqueous solution with a concentration of 0.02 mol / L, and 2.5 ml of the extract obtained by placing it at 25°C for 120 minutes was diluted with 1 ml of concentrated sulfuric acid and 46.5 ml of ultrapure water. The obtained sample was analyzed using an ICP luminescence device (manufactured by Thermo Fisher Scientific KK: ICAP6500), and the elution amounts of boron, dissolved calcium, sodium, and silicon converted into B2O3 in each sample are shown in Table 2. At this time, for the hexagonal boron nitride powder of Example 1, the 10 elements of the above-mentioned total dissolution ICP test items were not detected (below the detection limit), and for the hexagonal boron nitride powder of Comparative Example 1, Fe was detected as 7 ppm and Cr was detected as 1 ppm.
[0102] (4) Ion Chromatographic Determination of Hexagonal Boron Nitride Powder by Aqueous Solution Extraction
[0103] The chloride ion concentration of the aqueous solution obtained by immersing 2 g of the hexagonal boron nitride powder in 50 ml of water at 25° C. for 120 minutes was analyzed by ion chromatography (ICS-2100 manufactured by Nippon Dionex KK). The chloride ion concentration is shown in Table 2 as the amount of eluted chlorine in each sample.
[0104] (5) Dielectric strength measurement
[0105] Hexagonal boron nitride was mixed in epoxy resin to prepare a resin composition, and thermal conductivity was evaluated. 100 parts by mass of epoxy resin (JER828 manufactured by Mitsubishi Chemical Corporation) and 5 parts by mass of curing agent (imidazole curing agent, Curesol 2E4MZ manufactured by Shikoku Chemical Co., Ltd.) were used, and 210 parts by mass of methyl ethyl ketone were added as a solvent to prepare a varnish-like mixture. Next, a rotation / revolution mixer (MAZERUSTAR manufactured by KURABO INDUSTRIES LTD.) was used to mix the varnish-like mixture with the hexagonal boron nitride powder in a manner of 30% by volume of epoxy resin and 70% by volume of hexagonal boron nitride powder to obtain a resin composition.
[0106] The resin composition was coated on a PET film with a thickness of about 250 to 300 μm using an automatic coating machine PI-1210 manufactured by TESTER SANGYO CO., LTD. and dried. The film was cured under reduced pressure at a temperature of 200°C, a pressure of 5 MPa and a holding time of 30 minutes to prepare a sheet with a thickness of 200 μm. The dielectric strength was measured using a withstand voltage tester (manufactured by Tama Denso Co., Ltd.). The results are shown in Table 2.
[0107] [Table 1]
[0108] Results of the total dissolved impurity determination of boron nitride powder
[0109]
[0110] [Table 2]
[0111] Results of ICP and dielectric strength test of boron nitride powder extracted with sulfuric acid
[0112]
[0113] As shown in Table 1, the total contents of Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn and Al in Example 1 and Comparative Example 1 are 5.6 ppm and 60.9 ppm, respectively. Compared with Comparative Example 1 which has not undergone the magnetic separation process, the total content of magnetic foreign matter mainly composed of Fe in Example 1 which has undergone the magnetic separation process using an electromagnetic sieve device is greatly reduced.
[0114] In addition, as shown in Table 2, there is no significant difference between Example 1 and Comparative Example 1 in the dissolution amount of each component in the ICP measurement of sulfuric acid aqueous solution extraction and the ion chromatography measurement of aqueous solution extraction. However, in the insulation strength measurement, the insulation strength (kV / mm) of Example 1 and Comparative Example 1 are 75 and 35, respectively, so it is obvious that Example 1 has excellent electrical insulation.
[0115] As described above, the hexagonal boron nitride powder of the present invention has a very low content of magnetic foreign matter and therefore has high electrical insulation and excellent dielectric strength, and is therefore suitable for use as a heat dissipating filler or the like to be blended in a resin material.
[0116] In addition, the production method of the present invention can produce hexagonal boron nitride powder having a reduced total content of magnetic foreign matter at low cost, and is therefore extremely useful industrially.
Claims
1. A method for producing hexagonal boron nitride powder with reduced magnetic foreign matter, the method comprising the following steps: A process for preparing hexagonal boron nitride powder by reduction nitridation; The hexagonal boron nitride powder is acid-washed, water-washed and dried; and The step of preparing an electromagnetic sieve device to magnetically separate the powder after the particle size adjustment, wherein the electromagnetic sieve device has 20 or more overlapping openings of 5 mm or less and 8 mm or less and a length of 30 cm 2 The magnetic pole area is above and the mesh is magnetized to above 1.2T.
Citation Information
Patent Citations
Production of sintered ceramics and apparatus therefor
JP1995082033A
Highly delaminated hexagonal boron nitride powder, process for making, and use thereof
JP2008280243A
Hexagonal boron nitride powder and method for producing the same
JP2011098882A
Hexagonal boron nitride powder and manufacturing method therefor
JP2019182737A
Hexagonal boron nitride powder and method for producing same
US20120196128A1