A wide temperature range supercapacitor electrode material and device and preparation method
NiCo-MOF material was prepared by activated carbon felt and one-step hydrothermal method, combining ultra-thin MnO2 and gel electrolyte, and the problem of insufficient stability and conductivity of supercapacitor electrode materials was solved, and flexible non-infrastructure of high energy density and power density was achieved Symmetric supercapacitor, suitable for portable devices.
Patent Information
- Application Number
- CN202210545659.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-05-19
AI Technical Summary
The existing supercapacitor electrode materials have poor cyclic stability, low conductivity, and it is difficult to design and prepare nanoelectrode materials with high specific surface area and uniform morphology, which limits their application in the energy field.
Using mixed acid activated carbon felt, NiCo-MOF bimetallic organic frame material was prepared as the positive electrode material by one-step hydrothermal method. Combined with the laboratory's self-made ultra-thin MnO2 and PVA/KOH gel electrolyte, a flexible asymmetric supercapacitor was designed, and three-dimensional three-dimensional Structural and gel electrolytes enhance electrochemical performance.
It has achieved high pseudocapacitance performance, stable working voltage, good flexibility and temperature resistance, with a maximum energy density of 66Wh/kg and a maximum power density of 11700W/kg, which is suitable for energy support for portable wearable devices.
Smart Images

Figure CN114743802B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a supercapacitor, and in particular to a wide temperature range supercapacitor electrode material and device and a preparation method thereof. Background Art
[0002] As an emerging energy storage device, supercapacitors have many advantages such as fast charging and discharging speed and long service life. Supercapacitors are mainly composed of three parts: electrode materials, electrolytes, and diaphragms. The electrode material is the most critical factor in determining the performance of its device. According to the different energy storage mechanisms of electrode materials, supercapacitors can be divided into three categories: double-layer capacitors, Faraday pseudocapacitors, and hybrids. Double-layer capacitors and Faraday pseudocapacitors have their own advantages and disadvantages. Single double-layer materials, such as activated carbon and carbon cloth, have good stability and good rate capability, but low specific capacitance. Single pseudocapacitor materials, such as manganese-based and copper-based materials, have high specific capacitance, but the structure is easy to collapse and ions are easy to accumulate. Therefore, researchers currently focus on the diversified and multi-dimensional composite of pseudocapacitor materials and other materials to give full play to the advantages of both, while suppressing the exposure of their defects, and preparing devices with excellent performance.
[0003] Among the many pseudocapacitive electrode materials, metal-organic framework (MOF) materials have the characteristics of both inorganic and organic materials, with advantages such as high porosity, large specific surface area, and adjustable structure and function. However, most of the MOFs prepared so far are solid powder materials with poor cycle stability and poor conductivity, which are not conducive to the performance and seriously hinder their application in the energy field. Therefore, it is necessary to take measures such as modification of MOF to improve its electrochemical performance.
[0004] In addition, the performance of electrode materials is closely related to their microscopic morphology, and their microstructure determines the number of binding sites for the surface active substances (such as oxygen-containing functional groups) of the electrode materials. How to design and prepare nano-electrode materials with uniform size, uniform morphology, and large specific surface area, which can fully and stably load their surface active substances, is one of the key problems in current research. MOFs are mostly two-dimensional and three-dimensional structures. Compared with low-dimensional materials, three-dimensional materials have more advantages in overall size, specific surface area, ion transport, charge distribution, etc., which facilitates the movement of anions and cations in the electrolyte inside the electrode material, and kinetically promotes the electrochemical reaction between anions and cations and the electrode material.
[0005] On the other hand, with the help of carbon fiber felt with a three-dimensional structure, the performance of the device has been comprehensively improved: (1) The three-dimensional conductive carbon felt with a rich pore structure can enhance the conductivity of MOF and improve the energy density and power density of the device. (2) The introduction of carbon felt with good flexibility and excellent mechanical properties makes it possible to prepare micro-flexible all-solid-state devices, which can promote the multifunctional development of devices.
[0006] At present, the preparation of morphology-controllable composite structural materials based on single metal MOF as electrode materials has been preliminarily studied, but the research on bimetallic MOF-based electrode materials prepared by the synergistic coupling of bimetallic is still relatively rare. Therefore, designing and developing a stable and reliable method to prepare NiCo-MOF supercapacitor electrode materials with bimetallic ion organic framework structure and high pseudocapacitive performance, and using this binary material as the positive electrode material of flexible devices, is of great significance for promoting the development of supercapacitor electrode materials and the practical application of devices. Summary of the invention
[0007] The present invention proposes to use mixed acid to activate commercial carbon felt to make it rich in functional groups, and then use a one-step hydrothermal method to prepare NiCo-MOF bimetallic organic framework material, which is used as the positive electrode material to design and assemble a new flexible asymmetric supercapacitor.
[0008] The flexible asymmetric supercapacitor comprises a positive electrode, a negative electrode and a gel electrolyte, characterized in that the positive electrode is a NiCo-MOF electrode material with high pseudocapacitance performance. This electrode material is obtained by adjusting the ratio of the two main metal ions of Ni and Co to obtain a NiCo-MOF ball similar to a raspberry. There are a large number of ultra-thin nanosheets on the surface of the ball, which have an ultra-high specific surface area, and there are certain gaps between the nanosheet layers. This non-fully enclosed three-dimensional structure provides a large amount of space for the free flow of anions and cations in the electrolyte, and directly contacts with the electrode material, thereby improving the activity of the electrode material, improving the electrochemical reaction rate of the electrode material, and making the pseudocapacitance effect more significant. The negative electrode is a laboratory-made ultra-thin MnO2. The gel electrolyte is a PVA / KOH gel electrolyte. Compared with aqueous electrolytes, gel electrolytes significantly broaden the operating voltage range due to the addition of organic polymers. In addition, the all-solid structure of the gel electrolyte can solve the problems of device volume expansion and electrolyte overflow, laying the foundation for the preparation and practical application of flexible supercapacitors.
[0009] The method for preparing the flexible asymmetric supercapacitor comprises the following steps:
[0010] (1) Cleaning and activation of carbon felt surface: The commercial carbon felt was ultrasonically cleaned with ethanol solution and deionized water in turn; then H2SO4 solution and HNO3 solution were prepared respectively and poured into the beaker containing the carbon felt in turn; the beaker was stirred at room temperature and then transferred to a 70°C water bath and continued to stir at a constant speed; after the stirring was completed, the carbon felt was taken out and cleaned three times with ethanol solution; finally, the carbon felt was placed in an oven to dry and then taken out and weighed for later use.
[0011] (2) Preparation of bimetallic NiCo-MOF positive electrode material: First, a certain amount of Ni(NO3)2·6H2O, Co(NO3)2·6H2O and H3BTC were dissolved in DMF solution. After stirring at room temperature, the mixed solution was transferred to a reactor, heated to 120°C at a rate of 5°C / min, and subjected to hydrothermal reaction at this temperature. After the reaction was completed and naturally cooled to room temperature, the sample was centrifuged in a centrifuge and rinsed with DMF, deionized water and ethanol solution in turn. Finally, the obtained precipitate was placed in a drying oven and dried to obtain a NiCo-MOF sample.
[0012] (3) Preparation of asymmetric devices: First, NiCo-MOF, acetylene black and PVDF were weighed in turn and poured into a mortar containing NMP solvent and ground into a slurry; then the obtained slurry was coated on carbon felt and dried overnight for use; similarly, laboratory-made ultra-thin MnO2, acetylene black and PVDF were weighed, poured into a mortar containing NMP solvent, ground into a slurry, coated on carbon felt and dried overnight as the negative electrode material; then, PVA, KOH, deionized water, K3[Fe(CN)6] and C3H8O3 were weighed in a water bath at 85°C to synthesize a PVA / KOH gel electrolyte; finally, the positive and negative electrodes were immersed in the gel electrolyte respectively; after taking out, the two electrodes were aligned and closed; a layer of plastic film was wrapped on the surface of the electrode and pressure was applied to the device to obtain an all-solid-state supercapacitor.
[0013] In the above step (1), the ultrasonic cleaning time is controlled at 15 min; the concentration of the ethanol solution is 95 wt %; the concentrations of the H2SO4 solution and the HNO3 solution are both 3 mol / L, and the volume ratio of the H2SO4 solution to the HNO3 solution is 3:1; and the oven temperature is 65°C.
[0014] In the above step (2), the molar ratios of Ni(NO3)2·6H2O, Co(NO3)2·6H2O and H3BTC are 1:1:1, 1:2:1, 2:1:1 and 4:1:1 respectively; DMF is used as an activator, H3BTC is used as an initiator and inducer, and the stirring speed is 900 rpm / min.
[0015] In the above step (2), the hydrothermal reaction time of the reactor is controlled at 15h; the centrifuge speed is 10000rpm / min, and the centrifugation time is 3min; the concentration of the ethanol solution is 95wt%; the drying oven temperature is 60°C, and the drying time is 24h.
[0016] In the above step (3), the net mass of the prepared NiCo-MOF cathode material is 1.89-2.33 mg / cm 2 .
[0017] In step (3), the mass ratio of NiCo-MOF, acetylene black and PVDF is 8:1:1, and the mass ratio of ultra-thin MnO2, acetylene black and PVDF is 8:1:1; the size of the carbon felt is 1 cm×3 cm, and the drying temperature is 70°C.
[0018] In the above step (3), the negative electrode ultra-thin MnO2 loading is 4.2-5.18 mg / cm 2 The ratio of PVA, KOH, deionized water, K3[Fe(CN)6] and C3H8O3 is 3g:1.52g:30g:0.329-0.658g:3mL. K3[Fe(CN)6] and C3H8O3 are used as additives.
[0019] In the above step (3), after the PVA is stirred in a water bath at 85° C. for 1 h, the KOH solution is added dropwise.
[0020] In the above step (3), the immersion time is 20-30 minutes; when assembling the device, the pressure applied is 0.1-0.15 MPa; and the maintenance time is 10-15 minutes.
[0021] Therefore, the flexible all-solid-state asymmetric supercapacitor obtained by the present invention has the following advantages: (1) Excellent electrochemical performance: the operating voltage is stable at 1.3V, the maximum energy density reaches 66Wh / kg, the maximum power density reaches 11700W / kg, and two devices connected in series can light up an LED bulb, showing good practicality. (2) The device is lightweight, has good flexibility and temperature resistance, and the extreme operating temperature can reach -20°C and 40°C, which is expected to provide energy support for portable wearable devices. (3) The positive and negative electrode materials are widely available and low in cost. (4) The preparation of gel electrolytes, the assembly process of the device is simple, stable, safe and controllable. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the electrode material and device experimental process route adopted by the present invention.
[0023] Figure 2These are selected-area scanning electron microscope images of the NiCo-MOF series composite materials prepared in the present invention: a. Sample of Example 1; b. Sample of Example 2; c. Sample of Example 4; d. Sample of Example 3.
[0024] Figure 3 These are scanning electron microscope images of selected areas of the NiCo-MOF composite material prepared in Example 3 of the present invention at different magnifications: ab. scanning electron microscope images at 10 μm; c. scanning electron microscope image at 2 μm; d. scanning electron microscope image at 400 nm; e. scanning electron microscope image at 100 nm; f. scanning electron microscope image at 50 nm.
[0025] Figure 4 The flexible test and temperature resistance test curves of the flexible asymmetric device assembled by the present invention are: a. 0°, 45°, 90°, 135° test schematic diagram; b. 0°, 45°, 90°, 135°C V test curve; c. 0°, 45°, 90°, 135°GCD test curve; d. -20°C, 40°C test schematic diagram; e. -20°C, 40°C CV test curve; f. -20°C, 40°C GCD test curve. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described below in conjunction with specific implementation cases.
[0027] Embodiment 1:
[0028] (1) Cleaning and activation of carbon felt surface: A 1 cm × 3 cm piece of commercial carbon felt was ultrasonically cleaned with 95% mass concentration ethanol solution and deionized water for 15 min respectively; then, 3 mol / L H2SO4 solution and 3 mol / L HNO3 solution were prepared respectively, and 60 mL and 20 mL of the two were measured in a volume ratio of 3:1 and poured into a beaker containing carbon felt; the beaker was stirred at room temperature for 20 min and then transferred to a 70°C water bath and continued to stir at a constant speed for 20 min; after the stirring was completed, the carbon felt was taken out and cleaned three times with 95% mass concentration ethanol solution; finally, the carbon felt was placed in an oven and dried at 65°C for 5 h and then taken out, and its mass M1 was weighed to be 0.236 g.
[0029] (2) Preparation of bimetallic NiCo-MOF cathode material: First, 1.5mmol Ni(NO3)2·6H2O, 1.5mmol Co(NO3)2·6H2O and 1.5mmol H3BTC were dissolved in 60mL DMF solution and stirred at 900rpm / min for 10min at room temperature; then, the mixed solution was transferred to a 100mL reactor, heated to 120℃ at a rate of 5℃ / min, and hydrothermal at this temperature for 15h; after the reaction was completed and naturally cooled to room temperature, the sample was placed in a centrifuge and centrifuged at 10000rpm / min for 3min; then rinsed with DMF, deionized water and 95% mass concentration ethanol solution three times in turn; finally, the obtained precipitate was placed in a drying oven and dried at 60℃ for 24h. After drying, the electrochemical test showed that the NiCo-MOF specific capacitance was 469F / g.
[0030] (3) Preparation of asymmetric devices: First, NiCo-MOF, acetylene black and PVDF were weighed in a mass ratio of 80wt%, 10wt% and 10wt% respectively, and poured into a mortar containing NMP solvent for grinding into a slurry; then the obtained slurry was coated on a 1cm×3cm carbon felt and dried at 70℃ for 24h; its mass was weighed as M2, which was 0.242g. The net loading of the NiCo-MOF sample was M + =1.95mg / cm 2 .
[0031] According to the positive electrode loading and the law of charge conservation, the negative electrode loading is calculated as M - =4.33mg / cm 2 . Similarly, the laboratory-made ultra-thin MnO2, acetylene black and PVDF were weighed in the same mass ratio and ground into slurry and coated on the carbon felt of the same size as the negative electrode material; then, 3g PVA, 1.68g KOH, 3mL C3H8O3, and 30mL deionized water were weighed, and after the PVA was stirred in a water bath at 85°C for 1h, KOH solution was added dropwise, and then C3H8O3 was added dropwise to synthesize PVA / KOH gel electrolyte; finally, the positive and negative electrodes were immersed in the gel electrolyte for 20min respectively; after taking out, the two poles were aligned and closed; after a layer of plastic film was wrapped on the surface of the electrode, the device was maintained at 0.1MPa for 10min to obtain a full solid-state supercapacitor. After testing, the device operating voltage was 0-1.3V and the energy density was 39.25Wh / kg.
[0032] Embodiment 2:
[0033] (1) Cleaning and activating the carbon felt surface: This step is the same as that in Example 1, and its mass M3 is 0.225 g.
[0034] (2) Preparation of bimetallic NiCo-MOF cathode material: First, 1.5mmol Ni(NO3)2·6H2O, 3mmol Co(NO3)2·6H2O and 1.5mmol H3BTC were dissolved in 60ml DMF solution and stirred at 900rpm / min for 10min at room temperature; then, the mixed solution was transferred to a 100mL reactor, heated to 120℃ at a rate of 5℃ / min, and hydrothermal at this temperature for 15h; after the reaction was completed and naturally cooled to room temperature, the sample was placed in a centrifuge and centrifuged at 10000rpm / min for 3min; then rinsed with DMF, deionized water and 95% mass concentration ethanol solution three times in turn; finally, the obtained precipitate was placed in a drying oven and dried at 60℃ for 24h. After drying, the electrochemical test showed that the NiCo-MOF specific capacitance was 532F / g.
[0035] (3) Preparation of asymmetric device: This step is the same as that in Example 1, and the total mass of the positive electrode is M4, which is 0.232 g. Thus, the net loading of the NiCo-MOF sample is M + =2.26mg / cm 2 According to the positive electrode loading and the law of charge conservation, the negative electrode loading is calculated as M - =5.02mg / cm 2 . Similarly, the laboratory-made ultra-thin MnO2, acetylene black and PVDF were weighed in the same mass ratio and ground into slurry and coated on the carbon felt of the same size as the negative electrode material; then, 3g PVA, 1.68g KOH, 3mL C3H8O3, and 30mL deionized water were weighed, and after the PVA was stirred in a water bath at 85°C for 1h, KOH solution was added dropwise, and then C3H8O3 was added dropwise to synthesize PVA / KOH gel electrolyte; finally, the positive and negative electrodes were immersed in the gel electrolyte for 20min respectively; after taking out, the two poles were aligned and closed; after wrapping a layer of plastic film on the surface of the electrode, the device was maintained at 0.1MPa for 10min to obtain a full solid-state supercapacitor. After testing, the device operating voltage was 0-1.3V and the energy density was 47.69Wh / kg.
[0036] Embodiment 3:
[0037] (1) Cleaning and activating the carbon felt surface: This step is the same as that in Example 1, and its mass M5 is 0.215 g.
[0038] (2) Preparation of bimetallic NiCo-MOF cathode material: First, 3mmol Ni(NO3)2·6H2O, 1.5mmol Co(NO3)2·6H2O and 1.5mmol H3BTC were dissolved in 60ml DMF solution and stirred at 900rpm / min for 10min at room temperature; then, the mixed solution was transferred to a 100mL reactor, heated to 120℃ at a rate of 5℃ / min, and hydrothermal at this temperature for 15h; after the reaction was completed and naturally cooled to room temperature, the sample was placed in a centrifuge and centrifuged at 10000rpm / min for 3min; then rinsed with DMF, deionized water and 95% mass concentration ethanol solution three times in sequence; finally, the obtained precipitate was placed in a drying oven and dried at 60℃ for 24h. After drying, the electrochemical test showed that the specific capacitance of NiCo-MOF was 639F / g.
[0039] (3) Preparation of asymmetric device: This step is the same as that in Example 1, and the total mass of the positive electrode is M6, which is 0.222 g. Thus, the net loading of the NiCo-MOF sample is M + =2.19mg / cm 2 According to the positive electrode loading and the law of charge conservation, the negative electrode loading is calculated as M - =4.87mg / cm 2 . Similarly, the laboratory-made ultra-thin MnO2, acetylene black and PVDF were weighed in the same mass ratio and ground into slurry and coated on the carbon felt of the same size as the negative electrode material; then, 3g PVA, 1.68g KOH, 3mL C3H8O3 and 30mL deionized water were weighed, and after the PVA was stirred in a water bath at 85°C for 1h, KOH solution was added dropwise, and then C3H8O3 was added dropwise to synthesize PVA / KOH gel electrolyte; finally, the positive and negative electrodes were immersed in the gel electrolyte for 20min respectively; after taking out, the two poles were aligned and closed; after wrapping a layer of plastic film on the surface of the electrode, the device was maintained at 0.1MPa for 10min to obtain a full solid-state supercapacitor. After testing, the device operating voltage was 0-1.3V and the energy density was 58.93Wh / kg.
[0040] Embodiment 4:
[0041] (1) Cleaning and activating the carbon felt surface: This step is the same as that in Example 1, and the mass M7 is 0.223 g.
[0042] (2) Preparation of bimetallic NiCo-MOF cathode material: First, 6mmol Ni(NO3)2·6H2O, 1.5mmol Co(NO3)2·6H2O and 1.5mmol H3BTC were dissolved in 60mL DMF solution and stirred at 900rpm / min for 10min at room temperature; then, the mixed solution was transferred to a 100mL reactor, heated to 120℃ at a rate of 5℃ / min, and hydrothermal at this temperature for 15h; after the reaction was completed and naturally cooled to room temperature, the sample was placed in a centrifuge and centrifuged at 10000rpm / min for 3min; then rinsed with DMF, deionized water and 95% mass concentration ethanol solution three times in sequence; finally, the obtained precipitate was placed in a drying oven and dried at 60℃ for 24h. After drying, the electrochemical test showed that the NiCo-MOF specific capacitance was 639F / g.
[0043] (3) Preparation of asymmetric device: This step is the same as that in Example 1, and the total mass of the positive electrode is M8, which is 0.229 g. Thus, the net loading of the NiCo-MOF sample is M + =2mg / cm 2 According to the positive electrode loading and the law of charge conservation, the negative electrode loading is calculated as M - =4.44mg / cm 2 . Similarly, the laboratory-made ultra-thin MnO2, acetylene black and PVDF were weighed in the same mass ratio and ground into slurry and coated on the carbon felt of the same size as the negative electrode material; then, 3g PVA, 1.68g KOH, 3mL C3H8O3, and 30mL deionized water were weighed, and after the PVA was stirred in a water bath at 85°C for 1h, KOH solution was added dropwise, and then C3H8O3 was added dropwise to synthesize PVA / KOH gel electrolyte; finally, the positive and negative electrodes were immersed in the gel electrolyte for 10min respectively; after taking out, the two poles were aligned and closed; after a layer of plastic film was wrapped on the surface of the electrode, the device was maintained at 0.1MPa for 20min to obtain a full solid-state supercapacitor. After testing, the device operating voltage was 0-1.3V and the energy density was 35.42Wh / kg.
[0044] Implementation cases 1-4 are to compare the effects of different Ni and Co molar ratios on the electrochemical performance of NiCo-MOF cathode materials. It can be concluded that when the Ni / Co molar ratio is 2:1, NiCo-MOF cathode materials have the best electrochemical performance. Similar to electrode materials, the device exhibits the best energy density at the corresponding ratio.
[0045] Embodiment 5:
[0046] (1) Cleaning and activating the carbon felt surface: This step is the same as that in Example 3, and its mass M9 is 0.229 g.
[0047] (2) Preparation of bimetallic NiCo-MOF positive electrode material: This step is the same as the process in Example 3. After drying, electrochemical testing was performed to obtain a specific capacitance of NiCo-MOF of 628 F / g.
[0048] (3) Preparation of asymmetric device: This step is the same as that in Example 3. The total mass of the positive electrode is M 10 The net loading of the NiCo-MOF sample is M + =2.08mg / cm 2 According to the positive electrode loading and the law of charge conservation, the negative electrode loading is calculated as M - =4.62mg / cm 2 . Similarly, the laboratory-made ultra-thin MnO2, acetylene black and PVDF were weighed in the same mass ratio and ground into slurry and coated on the carbon felt of the same size as the negative electrode material; then, 3g PVA, 1.68g KOH, 0.329g K3[Fe(CN)6], 3mL C3H8O3, and 30mL deionized water were weighed, and after the PVA was stirred in a water bath at 85°C for 1h, KOH solution was added dropwise, followed by K3[Fe(CN)6] solution and C3H8O3 dropwise to synthesize PVA / KOH gel electrolyte; finally, the positive and negative electrodes were immersed in the gel electrolyte for 20min respectively; after taking out, the two poles were aligned and closed; after a layer of plastic film was wrapped on the surface of the electrode, the device was maintained at 0.1MPa for 10min to obtain a fully solid-state supercapacitor. After testing, the device operating voltage was 0-1.3V and the energy density was 61.37Wh / kg.
[0049] Embodiment 6:
[0050] (1) Cleaning and Activating the Carbon Felt Surface: This step is the same as that in Example 3. The mass M of the carbon felt is measured. 11 It is 0.237g.
[0051] (2) Preparation of bimetallic NiCo-MOF positive electrode material: This step is the same as the process in Example 3. After drying, electrochemical testing was performed to obtain a specific capacitance of NiCo-MOF of 635 F / g.
[0052] (3) Preparation of asymmetric device: This step is the same as that in Example 3. The total mass of the positive electrode is M 12 The net loading of the NiCo-MOF sample is M + =2.33mg / cm 2According to the positive electrode loading and the law of charge conservation, the negative electrode loading is calculated as M - =5.18mg / cm 2 . Similarly, the laboratory-made ultra-thin MnO2, acetylene black and PVDF were weighed in the same mass ratio and ground into slurry and coated on the carbon felt of the same size as the negative electrode material; then, 3g PVA, 1.68g KOH, 3mL C3H8O3, 0.658g K3[Fe(CN)6] and 30mL deionized water were weighed, and after the PVA was stirred in a water bath at 85℃ for 1h, KOH solution was added dropwise, followed by K3[Fe(CN)6] solution and C3H8O3 dropwise to synthesize PVA / KOH gel electrolyte; finally, the positive and negative electrodes were immersed in the gel electrolyte for 20min respectively; after taking out, the two electrodes were aligned and closed; after wrapping a layer of plastic film on the surface of the electrode, the device was maintained at 0.1MPa for 10min to obtain a full solid-state supercapacitor. After testing, the device operating voltage was 0-1.3V and the energy density was 66.52Wh / kg.
[0053] Implementation cases 3, 5, and 6 are intended to explore the effect of the amount of redox electron pairs added to the gel electrolyte on the energy density of the device. It can be concluded that the additional redox electron pairs introduced by the gel electrolyte play a role in improving the energy density of the device. As the amount added increases, the energy density of the device is improved.
Claims
1. A supercapacitor with a wide temperature range supercapacitor electrode material as the positive electrode, characterized in that: The specific steps of the preparation method of the supercapacitor are as follows: first, weigh NiCo-MOF, acetylene black and PVDF in turn, pour them into a mortar containing NMP solvent and grind them into slurry; then apply the obtained slurry on carbon felt, dry overnight for use; similarly, weigh MnO2, acetylene black and PVDF, pour them into a mortar containing NMP solvent, grind them into slurry, apply them on carbon felt and dry overnight as negative electrode material; then, weigh PVA, KOH, deionized water, K3[Fe(CN)6] and C3H8O3 in a water bath at 85°C to synthesize PVA / KOH gel electrolyte; finally, immerse the positive and negative electrodes in the gel electrolyte respectively; after taking them out, align the two electrodes and close them; after wrapping a layer of plastic film on the surface of the electrode, apply pressure to the device to obtain an all-solid-state supercapacitor; the electrode material is NiCo-MOF high pseudocapacitance electrode material, which can change Ni and Co The ratio of the two main metal ions, the electrode material is a raspberry-shaped NiCo-MOF ball. There are a large number of ultra-thin nanosheets on the surface of the NiCo-MOF ball, which has an ultra-high specific surface area, and there are certain gaps between the nanosheet layers. This non-fully enclosed three-dimensional structure provides a large amount of space for the free flow of anions and cations in the electrolyte, and directly contacts with the electrode material, thereby enhancing the activity of the electrode material, increasing the electrochemical reaction rate of the electrode material, and making the pseudocapacitance effect more significant.
2. The supercapacitor according to claim 1, comprising a positive electrode, a negative electrode and a gel electrolyte, characterized in that: The negative electrode is MnO2, and the gel electrolyte is PVA / KOH gel electrolyte.
3. The supercapacitor according to claim 1, characterized in that The preparation method of the electrode material comprises the following specific steps: (1) Cleaning and activation of carbon felt surface: The commercial carbon felt was ultrasonically cleaned with ethanol solution and deionized water in turn; then H2SO4 solution and HNO3 solution were prepared respectively and poured into the beaker containing the carbon felt in turn; the beaker was stirred at room temperature and then transferred to a 70°C water bath and continued to stir at a constant speed; after the stirring was completed, the carbon felt was taken out and cleaned three times with ethanol solution; finally, the carbon felt was placed in an oven to dry and then taken out and weighed for later use; (2) Preparation of bimetallic NiCo-MOF positive electrode material: First, Ni(NO3)2•6H2O, Co(NO3)2•6H2O and H3BTC were dissolved in DMF solution. After stirring at room temperature, the mixed solution was transferred to a reactor, heated to 120℃ at a rate of 5℃ / min, and subjected to hydrothermal reaction at this temperature. After the reaction was completed and naturally cooled to room temperature, the sample was centrifuged and rinsed with DMF, deionized water and ethanol solution in turn. Finally, the obtained precipitate was placed in a drying oven and dried to obtain a NiCo-MOF sample.
4. The supercapacitor according to claim 3, characterized in that In step (1), the ultrasonic cleaning time is controlled at 15 min; the concentration of the ethanol solution is 95 wt %; the concentrations of the H2SO4 solution and the HNO3 solution are both 3 mol / L, and the volume ratio of the H2SO4 solution to the HNO3 solution is 3:1; and the oven temperature is 65°C.
5. The supercapacitor according to claim 3, characterized in that In step (2), the molar ratio of Ni(NO3)2·6H2O, Co(NO3)2·6H2O and H3BTC is 1:1:1, 1:2:1, 2:1:1, 4:1:1; DMF was used as an activator, H3BTC as an initiator and inducer, and the stirring speed was 900 rpm; the hydrothermal reaction time in the reactor was controlled at 15 h; the centrifuge speed was 10,000 rpm, and the centrifugation time was 3 min; the concentration of the ethanol solution was 95 wt %; the drying oven temperature was 60 ° C, and the drying time was 24 h.
6. The supercapacitor according to claim 1, characterized in that The net mass of the prepared NiCo-MOF cathode material is 1.89-2.33 mg / cm 2 The negative electrode MnO2 loading is 4.2-5.18 mg / cm 2 .
7. The supercapacitor according to claim 1, wherein: The mass ratio of NiCo-MOF, acetylene black and PVDF is 8:1:1, and the mass ratio of MnO2, acetylene black and PVDF is 8:1:1; the size of the carbon felt is 1cm×3cm, and the drying temperature is 70°C; the ratio of PVA, KOH, deionized water, K3[Fe(CN)6] and C3H8O3 is 3g: 1.52g:30g:0.329-0.658g:3mL, K3[Fe(CN)6] and C3H8O3 as additives.
8. The supercapacitor according to claim 1, characterized in that: After the PVA is stirred in a water bath at 85°C for 1 hour, KOH solution is added dropwise; the immersion time is 20-30 minutes; when assembling the device, the pressure applied is 0.1-0.15 MPa; and the maintenance time is 10-15 minutes.