Benzoxazine resin and its preparation method and resin composition

Through the condensation polymerization reaction of phenolic compounds and primary amine compounds, benzoxazine resins with suitable dielectric constant and dielectric loss are prepared, and combined with epoxy resins and bismaleimide resins to form high-frequency The resin composition for printed circuit boards solves the problems of high dielectric loss and poor processability of existing benzoxazine resins and achieves good dielectric properties and heat resistance.

CN114763401BActive Publication Date: 2024-10-25NANYA PLASTICS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110062143.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-01-13
Filing Date
2021-01-18
Publication Date
2024-10-25
Estimated Expiration
2041-01-18

AI Technical Summary

Technical Problem

The dielectric loss of existing benzoxazine resin in high-frequency printed circuit boards is too high and cannot meet the demand for low dielectric loss. At the same time, its processability is poor.

Method used

Through the condensation polymerization reaction of phenolic compounds (dicyclopentadienphenol and phenolmethane) and primary amine compounds (2,6-dimethylaniline and m-xylylenediamine), the dielectric constant is between 2.6 and 3.2. A benzoxazine resin with a dielectric loss of 0.015 to 0.021 is combined with an epoxy resin and a bismaleimide resin to form a resin composition.

Benefits of technology

The good dielectric characteristics and heat resistance of benzoxazine resin are achieved, the dielectric loss is reduced, it is suitable for high-frequency printed circuit boards, and the processability is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The present invention discloses a benzoxazine resin and a preparation method thereof and a resin composition. The benzoxazine resin is prepared by condensation polymerization reaction using phenolic compounds, formaldehyde and primary amine compounds as reactants. Wherein, the phenolic compounds include dicyclopentadiene phenol resin and phenol methane, and the primary amine compounds include 2,6-dimethylaniline and meta-phenylenediamine. The resin composition includes benzoxazine resin, epoxy resin and bismaleimide resin. Wherein, the total weight of benzoxazine resin, epoxy resin and bismaleimide resin is 100 parts by weight, and the content of benzoxazine resin is 30 to 50 parts by weight. The benzoxazine resin of the present invention can be used as a material for a copper foil substrate, and has the characteristics of good heat resistance, low water absorption, low dielectric constant and low dielectric loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a benzoxazine resin, a preparation method thereof and a resin composition, and in particular to a benzoxazine resin with good dielectric properties and heat resistance, a preparation method thereof and a resin composition. Background Art

[0002] With the advancement of technology, electronic components are developing towards the goal of being light, thin, short and small. In addition, the advent of the fifth generation mobile networks (5G) has increased the industry's demand for high-frequency transmission, high-speed signal transmission and low latency. Therefore, the relevant fields are currently committed to developing substrate materials with high glass transition temperature (glass transition temperature, Tg), low dielectric constant, low dielectric loss and good heat resistance to meet the requirements of electronic substrates for dielectric properties (low dielectric constant, low dielectric loss) and heat resistance.

[0003] Common substrate materials such as polyphenylene ether resin, bismaleimide resin or cyanate resin have good dielectric properties, but they are highly reactive, have a fast reaction rate, and have a gel point that is difficult to determine, resulting in poor processability.

[0004] Benzoxazine resin has good processability, but its dielectric properties are poor, and it cannot be applied to products with high dielectric loss requirements (dielectric loss less than 0.004). For example, a benzoxazine resin is disclosed in the prior art, and this benzoxazine resin contains a molecular structure of dicyclopentadiene. However, the dielectric loss of printed circuit boards made with this benzoxazine resin is greater than 0.008, which cannot meet the requirements of high-frequency printed circuit boards. Therefore, the benzoxazine resin currently on the market still needs to be improved. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a benzoxazine resin and a preparation method thereof, as well as a resin composition in view of the deficiencies in the prior art.

[0006] In order to solve the above technical problems, one of the technical solutions adopted by the present invention is to provide a benzoxazine resin. The benzoxazine resin is prepared by condensation polymerization of phenolic compounds, formaldehyde and primary amine compounds as reactants. Among them, the phenolic compounds include dicyclopentadiene phenol resin and phenol methane, and the primary amine compounds include 2,6-dimethylaniline and m-xylylenediamine.

[0007] Preferably, the structural formula of the benzoxazine resin is:

[0008]

[0009] ; wherein the average values ​​of x, y and z are each from 0 to less than 5, and at least one of x and y is not 0, and at least one of y and z is not 0.

[0010] Among them, R 1 yes R 2 yes n is an integer between 0 and 5.

[0011] Preferably, the ratio of the molar number of hydroxyl groups in the dicyclopentadiene phenol resin to the molar number of hydroxyl groups in the phenol methane is 0.22 to 1.22.

[0012] Preferably, the ratio of the molar number of amine groups in 2,6-dimethylaniline to the molar number of amine groups in m-xylylenediamine is 1 to 9.

[0013] Preferably, the benzoxazine resin has a weight average molecular weight of 750 to 2750 g / mol.

[0014] Preferably, the molar number of hydroxyl groups in the dicyclopentadiene phenol resin is 18% to 55% of the total molar number of hydroxyl groups in the phenolic compound.

[0015] Preferably, the molar number of hydroxyl groups in the phenol methane is 45% to 82% of the total molar number of hydroxyl groups in the phenolic compounds.

[0016] Preferably, the molar number of the amine groups of 2,6-dimethylaniline is 50% to 90% of the total molar number of the amine groups in the primary amine compound.

[0017] Preferably, the molar number of the amine groups of meta-xylylenediamine is 10% to 50% of the total molar number of the amine groups in the primary amine compound.

[0018] Preferably, the dielectric constant (1 GHz) of the benzoxazine resin is 2.6 to 3.2, and the dielectric loss (1 GHz) of the benzoxazine resin is 0.015 to 0.021.

[0019] In order to solve the above technical problems, another technical solution adopted by the present invention is to provide a method for preparing a benzoxazine resin. The method for preparing a benzoxazine resin comprises the following steps: mixing a phenolic compound, formaldehyde, a primary amine compound and a solvent, and performing a condensation reaction at a temperature of 60 to 100° C. to prepare a benzoxazine resin; wherein the phenolic compound comprises dicyclopentadiene phenol and phenol methane, and the primary amine compound comprises 2,6-dimethylaniline and m-xylylenediamine.

[0020] Preferably, the benzoxazine resin has a weight average molecular weight of 750 to 2750 g / mol.

[0021] Preferably, the molar number of hydroxyl groups in the dicyclopentadiene phenol resin is 18% to 55% of the total molar number of hydroxyl groups in the phenolic compound.

[0022] Preferably, the molar number of hydroxyl groups of phenol methane is 45% to 82% of the total molar number of hydroxyl groups in the phenolic compounds.

[0023] Preferably, the molar number of amine groups in 2,6-dimethylaniline is 50% to 90% of the total molar number of amine groups in the primary amine compound.

[0024] Preferably, the molar number of amine groups in meta-xylylenediamine is 10% to 50% of the total molar number of amine groups in the primary amine compound.

[0025] In order to solve the above technical problems, another technical solution adopted by the present invention is to provide a resin composition. The resin composition includes a benzoxazine resin, an epoxy resin and a bismaleimide resin. Wherein, the total weight of the benzoxazine resin, the epoxy resin and the bismaleimide resin is 100 parts by weight, and the content of the benzoxazine resin is 30 to 50 parts by weight.

[0026] Preferably, based on 100 parts by weight of the total weight of the benzoxazine resin, the epoxy resin and the bismaleimide resin, the content of the epoxy resin is 5 to 15 parts by weight, and the content of the bismaleimide resin is 40 to 60 parts by weight.

[0027] Preferably, the epoxy resin is a novolac type epoxy resin.

[0028] Preferably, the reactants for synthesizing the epoxy resin include at least one of 2,6-dimethylphenol and dicyclopentadiene.

[0029] One of the beneficial effects of the present invention is that the benzoxazine resin, the preparation method thereof and the resin composition provided by the present invention can achieve good heat resistance and dielectric properties through the technical scheme of "phenolic compounds including dicyclopentadiene phenol resin and phenol methane" and "primary amine compounds including 2,6-dimethylaniline and meta-phenylenediamine".

[0030] To further understand the features and technical contents of the present invention, please refer to the following detailed description of the present invention. However, the detailed description provided is only for reference and illustration and is not intended to limit the present invention. DETAILED DESCRIPTION

[0031] The following is an explanation of the implementation methods of the "benzoxazine resin, its preparation method and resin composition" disclosed in the present invention through specific examples. Those skilled in the art can understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and the details in this specification can also be modified and changed in various ways based on different viewpoints and applications without departing from the concept of the present invention. The following implementation methods will further explain the relevant technical content of the present invention in detail, but the disclosed content is not intended to limit the scope of protection of the present invention. In addition, the term "or" used in this article may include any one or more combinations of the associated listed items depending on the actual situation.

[0032] The benzoxazine resin of the present invention has good dielectric properties and heat resistance, and also has low water absorption and good dimensional stability. Thus, the benzoxazine resin of the present invention can not only solve the problem of poor processability when using polyphenylene ether resin, bismaleimide resin and cyanate resin in the past, but also can be applied to high-frequency printed circuit boards.

[0033] [Benzoxazine resin]

[0034] The benzoxazine resin of the present invention is prepared by a condensation polymerization reaction (Mannich reaction) using a phenolic compound, formaldehyde and a primary amine compound as reactants. In addition, the dielectric constant (1 GHz) of the benzoxazine resin of the present invention is 2.6 to 3.2, and the dielectric loss (1 GHz) of the benzoxazine resin is 0.015 to 0.021.

[0035] The method for preparing the benzoxazine resin of the present invention comprises the following steps: First, a phenolic compound, a primary amine compound and a solvent are mixed at a temperature of 60 to 100° C. to form a raw material mixture.

[0036] In the raw material mixture, the total hydroxyl mole number of the phenolic compound is equal to or almost equal to the total amine mole number of the primary amine compound. The solvent is selected from the group consisting of toluene, methylisobutyl ketone (MIBK), methyl ethyl ketone (MEK) and proprylene glycol monomethyl ether (PM). However, the present invention is not limited to the above examples.

[0037] Next, formaldehyde is added to the raw material mixture, and a condensation polymerization reaction is carried out at a temperature of 60 to 100° C. for 1 to 10 hours to obtain the benzoxazine resin of the present invention.

[0038] The added molar number of formaldehyde is 2 to 2.3 times the total molar number of hydroxyl groups of the phenolic compound (or the total molar number of amino groups of the primary amine compound). The formaldehyde can be a formaldehyde solution with a concentration of 30 to 40 weight percent or polyoxymethylene. However, the method of adding formaldehyde is not limited to the above.

[0039] In some embodiments, after adding formaldehyde, the raw material mixture is reacted at a temperature of 70 to 90° C. for 1 to 5 hours to obtain the benzoxazine resin of the present invention.

[0040] The weight average molecular weight of the benzoxazine resin of the present invention measured by gel permeation chromatograph (GPC) is 750 to 2750 g / mol. The gel chromatograph is calibrated with polystyrene of standard molecular weight, the flow rate is set to 1.0 ml / min, and tetrahydrofuran is used as the mobile phase. In addition, the minimum molecular weight ratio of the benzoxazine resin measured by the gel chromatograph is 20% to 40%. "Minimum molecular weight ratio" refers to the area percentage of the last peak appearing in the chromatographic result pattern.

[0041] When the weight average molecular weight of the benzoxazine resin is higher than 2750 g / mol, the benzoxazine resin is difficult to mix with other resins to form a resin composition, and has the problem of being difficult to operate. When the weight average molecular weight of the benzoxazine resin is lower than 750 g / mol, the glass transition temperature of the benzoxazine resin is low, and it is easy to have the problem of poor heat resistance.

[0042] In a preferred embodiment, the weight average molecular weight of the benzoxazine resin is 1000 to 2500 g / mol, and more preferably, the weight average molecular weight of the benzoxazine resin is 1500 to 2400 g / mol.

[0043] The aforementioned phenolic compounds include at least two phenolic compounds, and the phenolic compounds may have one or more hydroxyl groups. Preferably, the phenolic compounds have one or two hydroxyl groups, or the average number of hydroxyl groups of the phenolic compounds is between 1 and 2.

[0044] In the present invention, the phenolic compounds include dicyclopentadiene phenol resin (DCPD phenol resin) and bisphenol A (BPA). Among the phenolic compounds, the molar number of hydroxyl groups of the DCPD phenol resin is 18% to 55% of the total molar number of hydroxyl groups of the phenolic compounds, and the molar number of hydroxyl groups of the bisphenol A is 45% to 82% of the total molar number of hydroxyl groups of the phenolic compounds.

[0045] Furthermore, the addition amount of the dicyclopentadiene phenol resin and phenol methane can be adjusted according to the property requirements. In a preferred embodiment, the ratio of the molar number of hydroxyl groups in the dicyclopentadiene phenol resin to the molar number of hydroxyl groups in phenol methane is 0.22 to 1.22.

[0046] The aforementioned primary amine compound comprises at least two amine compounds, and the primary amine compound may have one or more amine groups. Preferably, the primary amine compound has one or two amine groups.

[0047] In the present invention, the primary amine compound includes 2,6-dimethylaniline and m-xylenediamine. In the primary amine compound, the amine group mole number of 2,6-dimethylaniline is 50% to 90% of the total amine group mole number of the primary amine compound, and the amine group mole number of m-xylenediamine is 10% to 50% of the total amine group mole number of the primary amine compound.

[0048] Furthermore, the addition amount of 2,6-dimethylaniline and m-xylylenediamine can be adjusted according to the characteristic requirements. In a preferred embodiment, the addition amount of 2,6-dimethylaniline is greater than or equal to the addition amount of m-xylylenediamine. Specifically, the ratio of the number of moles of the amino groups of 2,6-dimethylaniline to the number of moles of the amino groups of m-xylylenediamine is 1 to 9.

[0049] According to the above-mentioned preparation method, the benzoxazine resin of the present invention can be represented by the following formula (I).

[0050]

[0051] In formula (I), the average value of x is 0 to less than 5, the average value of y is 0 to less than 5, and the average value of z is 0 to less than 5. Moreover, at least one of x and y is not 0, and at least one of y and z is not 0. In a preferred embodiment, x, y and z are all greater than 0.

[0052] In formula (I), R 1 yes R 2 yes n is an integer between 0 and 5.

[0053] From the structure of formula (I), it can be seen that dicyclopentadiene phenol resin has a low polarity structure, so it can reduce the dielectric constant and dielectric loss of benzoxazine resin. In addition, 2,6-dimethylaniline has a highly symmetrical structure with a low molecular dipole moment, which can further reduce the dielectric constant and dielectric loss of benzoxazine resin. In this way, the benzoxazine resin of the present invention can meet the market demand for high-frequency printed circuit boards.

[0054] For the convenience of understanding the present invention, please refer to the contents of the following Synthesis Example 1 and Synthesis Example 2.

[0055] [Synthesis example 1]

[0056] A temperature controller, a heating bag, an electric stirrer and a condenser are installed on a four-necked glass reaction tank with a capacity of one liter. 76.5 grams (containing 0.45 moles of hydroxyl groups) of dicyclopentadiene phenol resin, 63 grams (containing 0.55 moles of hydroxyl groups) of phenol methane, 31.6 grams (containing 0.45 moles of amino groups) of m-xylylenediamine, 66 grams (containing 0.55 moles of amino groups) of 2,6-dimethylaniline and 460 grams of toluene (solvent) are added to the four-necked glass reaction tank, and the temperature of the four-necked glass reaction tank is raised to 60 to 100° C. to dissolve the reactants.

[0057] Next, 67 g (2.1 mol) of polyoxymethylene was added to a four-necked glass reaction vessel, and a condensation polymerization reaction was carried out at a temperature of 60 to 100° C. for 1 to 5 hours. After the reaction was completed, the temperature was maintained at 60 to 100° C. for 4 to 10 hours, and then the temperature was raised to 105 to 115° C. to remove the water and part of the solvent produced by the reaction, and a benzoxazine resin with a solid content of 64 to 66 wt % was obtained.

[0058] After gel chromatography analysis, the weight average molecular weight of the benzoxazine resin is 1724 g / mol, the minimum molecular weight ratio is 27%, the dielectric constant (1 GHz) of the benzoxazine resin is 2.9, and the dielectric loss (1 GHz) of the benzoxazine resin is 0.0195.

[0059] [Synthesis example 2]

[0060] A temperature controller, a heating bag, an electric stirrer and a condenser are installed on a four-necked glass reaction tank with a capacity of one liter. 31 grams (containing 0.18 moles of hydroxyl groups) of dicyclopentadiene phenol resin, 93.5 grams (containing 0.82 moles of hydroxyl groups) of phenol methane, 31.6 grams (containing 0.45 moles of amino groups) of m-xylylenediamine, 66 grams (containing 0.55 moles of amino groups) of 2,6-dimethylaniline and 460 grams of toluene (solvent) are added to the four-necked glass reaction tank, and the temperature of the four-necked glass reaction tank is raised to 60 to 100° C. to dissolve the reactants.

[0061] Next, 67.3 g (2.1 mol) of polyoxymethylene was added to a four-necked glass reaction vessel, and a condensation polymerization reaction was carried out at a temperature of 60 to 100° C. for 1 to 5 hours. After the reaction was completed, the temperature was maintained at 60 to 100° C. for 4 to 10 hours, and then the temperature was raised to 105 to 115° C. to remove the water and part of the solvent produced by the reaction, and a benzoxazine resin with a solid content of 64 to 66 wt % was obtained.

[0062] After gel chromatography analysis, the weight average molecular weight of the benzoxazine resin is 2344 g / mol, the minimum molecular weight ratio is 21.9%, the dielectric constant (1 GHz) of the benzoxazine resin is 2.7, and the dielectric loss (1 GHz) of the benzoxazine resin is 0.0153.

[0063] [Resin composition]

[0064] The benzoxazine resin of the present invention has good dielectric properties and heat resistance, and can be added to a resin composition for making a high-frequency substrate. In addition, the benzoxazine resin of the present invention can be added in a relatively high amount in the resin composition.

[0065] In the present invention, based on the total weight of the resin composition as 100 parts by weight, the content of the benzoxazine resin can reach 25 parts by weight or more, preferably, the content of the benzoxazine resin can reach 30 parts by weight or more, and more preferably, the content of the benzoxazine resin can reach 35 parts by weight or more.

[0066] The resin composition of the present invention comprises a benzoxazine resin, an epoxy resin and a bismaleimide resin. Taking the total weight of the resin composition as 100 parts by weight, the content of the benzoxazine resin is 30 to 50 parts by weight, the content of the epoxy resin is 5 to 15 parts by weight, and the content of the bismaleimide resin is 40 to 60 parts by weight.

[0067] The epoxy resin may include one or more epoxy resins. In a preferred embodiment, the epoxy resin is a phenolic epoxy resin, and the epoxy resin includes two phenolic epoxy resins, for example: dicyclopentadiene-dimethylphenolic epoxy resin or dimethylphenolic resin. In other words, the reactants for synthesizing the epoxy resin may include at least one of 2,6-dimethylphenol and dicyclopentadiene. However, the present invention is not limited thereto. In some embodiments, the weight average molecular weight of the epoxy resin is 500 to 3000 g / mol.

[0068] The bismaleimide resin may include one or more bismaleimide resins, such as phenylmethane bismaleimide resin. However, the present invention is not limited thereto. In some embodiments, the weight average molecular weight of the bismaleimide resin is 350 to 750 g / mol.

[0069] In addition to the above-mentioned benzoxazine resin, epoxy resin and bismaleimide resin, the resin composition may further selectively include a hardener, a flame retardant, a filler, a coupling agent and a promoter. For example, the hardener may be a phosphorus-containing phenolic resin hardener or a phenolic resin hardener. The flame retardant may be a phosphorus-based flame retardant. The filler may be silicon dioxide. The coupling agent may be a silane coupling agent. The promoter may be dimethylimidazole. However, the present invention is not limited thereto.

[0070] In order to facilitate the understanding of the present invention, the present invention prepares the resin compositions of Experimental Examples 1 and 2 and Comparative Examples 1 and 2, and uses the resin compositions as materials for making a copper foil substrate. The difference between Experimental Examples 1 and 2 and Comparative Examples 1 and 2 is that the compositions of Experimental Examples 1 and 2 contain the benzoxazine resin of the present invention, while the compositions of Comparative Examples 1 and 2 contain other benzoxazine resins on the market (4,4'-methylenedianiline type benzoxazine resin or dicyclopentadienephenol type benzoxazine resin). In addition, the composition of Experimental Example 1 contains the benzoxazine resin of Synthesis Example 1, and the composition of Experimental Example 2 contains the benzoxazine resin of Synthesis Example 2. The component ratios of the resin compositions of Experimental Examples 1 and 2 and Comparative Examples 1 and 2 are listed in Table 1. Unless otherwise specified, the units of each component in Table 1 are parts by weight.

[0071] The manufacturing method of the copper foil substrate includes the following steps. First, a glass fiber cloth is impregnated with a resin composition, and after drying and semi-curing, a prepreg is obtained. The melt viscosity of the prepreg is 4000 poise to 12000 poise. Then, four prepregs are stacked between two 35-micron copper foils, and the copper foil substrate is prepared by a hot pressing process with staged temperature increase. In the hot pressing process, the temperature is first raised to 85°C and 7kg / cm 2 Then, the temperature was raised to 195°C and the pressure was 25kg / cm 2 The copper foil substrate was obtained by hot pressing at a pressure of 2 hours. After the copper foil substrate was obtained, the glass transition temperature, heat resistance, water absorption, dielectric constant and dielectric loss of the copper foil substrate were measured, and the measurement results are listed in Table 1.

[0072] In Table 1, the characteristics of the copper foil substrate are evaluated as follows:

[0073] (1) Glass transition temperature: The glass transition temperature of the copper foil substrate was measured using a differential scanning calorimeter (DSC) at a heating rate of 20° C. per minute.

[0074] (2) Heat resistance: The copper foil substrate was cut into square test pieces with a side length of 6.35 mm. The pieces were baked at 105°C for 2 hours. The pieces were then placed in a thermomechanical analyzer test bench and heated to 288°C at a rate of 10°C per minute. The temperature was maintained at 288°C and the time required for the test pieces to explode and delaminate was recorded.

[0075] (3) Water absorption: Cut the copper foil substrate into square test pieces with a side length of 5 cm, bake them at 105°C for 2 hours, and weigh the initial weight of the test piece. Then, place the test piece in a pressure cooker (120°C, 2 atmospheres) for 2 hours, and weigh the weight of the test piece again. The water absorption of the test piece is the weight difference before and after the pressure cooker divided by the initial weight of the test piece.

[0076] (4) Dielectric constant (3 GHz): The copper foil substrate was cut into square test pieces with a side length of 5 cm and baked at 105°C for 2 hours. The thickness of the test piece was first measured with a thickness meter. The dielectric constant of the test piece was then measured at three locations with an impedance analyzer (Agilent E4991A) and the average was taken.

[0077] (5) Dielectric loss (3 GHz): The copper foil substrate was cut into square test pieces with a side length of 5 cm and baked at 105°C for 2 hours. The thickness of the test piece was first measured with a thickness gauge. The dielectric loss of the test piece at three locations was then measured with an impedance analyzer (Agilent E4991A) and the average was taken.

[0078] Table 1

[0079]

[0080]

[0081] According to the results in Table 1, the benzoxazine resin of the present invention can be used as a material for a copper foil substrate, and can have the characteristics of good heat resistance, low water absorption, low dielectric constant and low dielectric loss. Moreover, compared with the benzoxazine resins currently on the market (4,4'-methylenedianiline type benzoxazine resin or dicyclopentadienephenol type benzoxazine resin), it has lower dielectric loss.

[0082] Specifically, the glass transition temperature of the copper foil substrate is greater than or equal to 210°C, preferably, the glass transition temperature of the copper foil substrate is greater than or equal to 215°C, so the copper foil substrate of the present invention has good heat resistance. The water absorption rate of the copper foil substrate is less than or equal to 0.50, preferably, the water absorption rate of the copper foil substrate is less than or equal to 0.48. The dielectric constant of the copper foil substrate is less than or equal to 4, preferably, the dielectric constant of the copper foil substrate is less than or equal to 3.95, and the dielectric loss of the copper foil substrate is less than or equal to 0.005, preferably, the dielectric loss of the copper foil substrate is less than or equal to 0.0045, and more preferably, the dielectric loss of the copper foil substrate is less than or equal to 0.0043, so the copper foil substrate of the present invention has good dielectric properties.

[0083] [Beneficial Effects of Embodiments]

[0084] One of the beneficial effects of the present invention is that the benzoxazine resin, the preparation method thereof and the resin composition provided by the present invention can achieve good heat resistance and dielectric properties through the technical scheme of "the phenolic compound includes dicyclopentadiene phenol resin and phenol methane" and "the primary amine compound includes 2,6-dimethylaniline and meta-phenylenediamine".

[0085] The contents disclosed above are only preferred feasible embodiments of the present invention, and are not intended to limit the protection scope of the claims of the present invention. Therefore, all equivalent technical changes made using the contents of the present invention specification are included in the protection scope of the claims of the present invention.

Claims

1. A benzoxazine resin, characterized in that The benzoxazine resin is prepared by condensation polymerization of phenolic compounds, formaldehyde and primary amine compounds as reactants; wherein the phenolic compounds include dicyclopentadiene phenol resin and phenol methane, and the primary amine compounds include 2,6-dimethylaniline and m-xylylenediamine; Wherein, the structural formula of the benzoxazine resin is: wherein the average values ​​of x, y and z are each from 0 to less than 5, and at least one of x and y is not 0, and at least one of y and z is not 0; Among them, R 1 yes R 2 yes n is an integer between 0 and 5.

2. The benzoxazine resin according to claim 1, characterized in that The ratio of the molar number of hydroxyl groups in the dicyclopentadiene phenol resin to the molar number of hydroxyl groups in the phenol methane is 0.22 to 1.

22.

3. The benzoxazine resin according to claim 1, characterized in that The ratio of the mole number of amine groups in the 2,6-dimethylaniline to the mole number of amine groups in the meta-xylylenediamine is 1 to 9.

4. The benzoxazine resin according to claim 1, characterized in that The weight average molecular weight of the benzoxazine resin is 750 to 2750 g / mol.

5. The benzoxazine resin according to claim 1, characterized in that The molar number of hydroxyl groups in the dicyclopentadiene phenol resin is 18% to 55% of the total molar number of hydroxyl groups in the phenolic compound.

6. The benzoxazine resin according to claim 1, characterized in that The molar number of hydroxyl groups in the phenol methane is 45% to 82% of the total molar number of hydroxyl groups in the phenolic compounds.

7. The benzoxazine resin according to claim 1, characterized in that The molar number of the amine groups of the 2,6-dimethylaniline is 50% to 90% of the total molar number of the amine groups in the primary amine compound.

8. The benzoxazine resin according to claim 1, wherein The mole number of the amine groups of the meta-xylylenediamine is 10% to 50% of the total mole number of the amine groups in the primary amine compound.

9. The benzoxazine resin according to claim 1, characterized in that The dielectric constant of the benzoxazine resin under the measurement condition of 1 GHz is 2.6 to 3.2, and the dielectric loss of the benzoxazine resin under the measurement condition of 1 GHz is 0.015 to 0.

021.

10. A method for preparing a benzoxazine resin, characterized in that: The preparation method of the benzoxazine resin comprises: Mixed phenolic compounds, formaldehyde, primary amine compounds and solvents; and Carrying out a condensation reaction at a temperature of 60 to 100° C. to prepare the benzoxazine resin according to any one of claims 1 to 9; The phenolic compounds include dicyclopentadiene phenol and phenol methane, and the primary amine compounds include 2,6-dimethylaniline and meta-xylylenediamine.

11. The method for preparing a benzoxazine resin according to claim 10, wherein: The weight average molecular weight of the benzoxazine resin is 750 to 2750 g / mol.

12. The method for preparing a benzoxazine resin according to claim 10, wherein: The molar number of hydroxyl groups in the dicyclopentadiene phenol resin is 18% to 55% of the total molar number of hydroxyl groups in the phenolic compound.

13. The method for preparing a benzoxazine resin according to claim 10, wherein: The molar number of hydroxyl groups in the phenol methane is 45% to 82% of the total molar number of hydroxyl groups in the phenolic compounds.

14. The method for preparing a benzoxazine resin according to claim 10, wherein: The molar number of amine groups in the 2,6-dimethylaniline is 50% to 90% of the total molar number of amine groups in the primary amine compound.

15. The method for preparing a benzoxazine resin according to claim 10, wherein: The molar number of the amine groups in the meta-xylylenediamine is 10% to 50% of the total molar number of the amine groups in the primary amine compound.

16. A resin composition, characterized in that The resin composition comprises: a benzoxazine resin according to any one of claims 1 to 9, an epoxy resin and a bismaleimide resin; wherein the content of the benzoxazine resin is 30 to 50 parts by weight based on the total weight of the benzoxazine resin, the epoxy resin and the bismaleimide resin being 100 parts by weight.

17. The resin composition according to claim 16, characterized in that Based on the total weight of the benzoxazine resin, the epoxy resin and the bismaleimide resin being 100 parts by weight, the content of the epoxy resin is 5 to 15 parts by weight, and the content of the bismaleimide resin is 40 to 60 parts by weight.

18. The resin composition according to claim 16, characterized in that The epoxy resin is a novolac epoxy resin.

19. The resin composition according to claim 16, characterized in that The reactants for synthesizing the epoxy resin include at least one of 2,6-dimethylphenol and dicyclopentadiene.

Citation Information

Patent Citations

  • Preparation and application of dicyclopentadiene-phenol and 2,6-dimethyl phenol copolymer epoxy resin

    EP3354672A1

  • Resin composition, copper-clad laminate and printed circuit sheet using the same

    JP2017020011A

  • Low dialectric composite material and laminate and printed circuit board thereof

    US20160021739A1